A method for improving tensile properties of PVA-ECC material after sub-high temperature damage

By leveraging the synergistic effect of trivalent iron ion crosslinking curing and modified inorganic seed material, the problem of decreased tensile properties of PVA-ECC materials after sub-high temperature damage was solved, restoring their tensile properties and toughness, and significantly improving the material's ability to crack multiple cracks.

CN122940482BActive Publication Date: 2026-11-20INNER MONGOLIA UNIV OF TECH +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611424589.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-09-15
Publication Date
2026-11-20
Estimated Expiration
2046-09-15

AI Technical Summary

Technical Problem

Existing technologies are insufficient to restore the fiber bridging effect and interfacial bonding properties of PVA-ECC materials after sub-high temperature damage, resulting in a significant decrease in their tensile toughness and multi-crack cracking ability.

Method used

The modified matrix precursor was crosslinked and cured using a trivalent iron ion aqueous solution, and combined with modified inorganic seed material, and the PVA-ECC material damaged by sub-high temperature was treated by vacuum infiltration to restore its structural damage and stress characteristics.

Benefits of technology

It effectively restored the tensile properties of PVA-ECC materials after sub-high temperature damage, with the ultimate tensile strength and ultimate tensile strain restored to near the undamaged state, and significantly improved the material's multi-crack initiation ability and tensile toughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122940482B_ABST
    Figure CN122940482B_ABST
Patent Text Reader

Abstract

This invention relates to the field of building material reinforcement and repair technology, and in particular to a method for improving the tensile properties of PVA-ECC materials damaged by sub-high temperatures. The method involves first cleaning and wetting the surface of the damaged PVA-ECC material until it is saturated and surface-dry, then pre-curing it in a humid and hot environment with a relative humidity of 95%-98% for 4-12 hours. Next, a modified matrix precursor, a modified inorganic seed material, and an aqueous solution containing ferric ions are sequentially applied using a vacuum infiltration method. The modified matrix precursor is prepared by reacting oxidized tannic acid grafted with aminated hyperbranched polyglycerol and then with sodium alginate. The modified inorganic seed material is prepared by modifying C-S-H seed crystals with a silane coupling agent and a nonionic surfactant. This invention utilizes the ferric ion crosslinking and curing of the modified matrix precursor, synergistically repairing structural damage with the modified inorganic seed material, restoring fiber bridging and strain hardening capabilities, and improving the tensile properties and toughness of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of building material reinforcement and repair technology, specifically a method for improving the tensile properties of PVA-ECC materials after sub-high temperature damage. Background Technology

[0002] Polyvinyl alcohol fiber-reinforced cementitious composites (PVA-ECC) are widely used in civil engineering due to their excellent strain hardening properties. During service, when exposed to sub-high temperatures of 200°C or below, PVA fibers undergo thermal degradation over time, leading to a decrease in tensile strength. Simultaneously, the fiber bridging effect and fiber-matrix interfacial bonding deteriorate, significantly weakening the material's ability to develop multiple cracks and drastically reducing its ultimate tensile strain. While this sub-high temperature damage does not cause irreversible strain softening, damaged PVA-ECC retains some strain hardening characteristics, but its tensile toughness and multi-crack development performance are severely diminished.

[0003] Currently, cement-based materials are mainly used for crack filling in ambient temperature environments, and they are well-suited for handling conventional damage. However, they have limitations when dealing with materials damaged at sub-high temperatures: conventional repair materials are unable to improve the deterioration state of the fiber-matrix interface, and are unable to restore the effective bridging effect of fibers and the multi-crack mechanism, resulting in the inability to substantially restore the ultimate tensile strain and tensile toughness of the repaired material.

[0004] Therefore, there is an urgent need in this field to develop a performance enhancement method that can improve the deterioration state of the fiber-matrix interface, restore the effective bridging effect of the fiber, and enable the material to meet the strain hardening criterion again, so as to solve the problem that the tensile toughness and multi-crack ability of PVA-ECC materials are greatly reduced due to interface matching deterioration after sub-high temperature damage. Summary of the Invention

[0005] The purpose of this invention is to provide a method for improving the tensile properties of PVA-ECC materials after sub-high temperature damage, so as to solve the problems mentioned in the background art.

[0006] To achieve the above objectives, the present invention provides the following technical solution: A method for improving the tensile properties of PVA-ECC materials after sub-high temperature damage includes the following steps: S1. Clean the surface of the PVA-ECC material after it has been damaged by sub-high temperature, and wet the PVA-ECC material until it is saturated and surface-dry with no visible water. S2. Place the PVA-ECC material treated in S1 under a relative humidity of 95%-98% for pre-curing for 4-12 hours; S3. For the PVA-ECC material cured by S2, the modified matrix precursor, modified inorganic seed material and aqueous solution containing ferric ions are applied sequentially by vacuum infiltration. S4. Curing the PVA-ECC material treated in S3 under sealed conditions and relative humidity of 95%-98% for 24-48 hours, and then placing it under conditions of 20-25℃ and relative humidity of 50%-60% for another 12-48 hours.

[0007] Preferably, the preparation method of the modified matrix precursor includes the following steps: S11. Dissolve 5-10 parts of tannic acid in 200-500 parts of deionized water by mass, add sodium periodate, and pre-oxidize for 0.5-2 hours under light-protected conditions and a pH of 6-8 to obtain an aqueous solution of oxidized tannic acid; disperse or dissolve the modified core framework substrate in deionized water to obtain an aqueous solution of modified core framework substrate with a mass fraction of 1%-5%; S12. Add the modified core framework substrate aqueous solution to the oxidized tannic acid aqueous solution, adjust the pH value to 8-9, react for 4-12 hours, and after purification, collect the retentate containing the tannic acid grafting product. S13. Adjust the pH of the retentate to 5.0-6.5, add sodium alginate, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDC·HCl) and N-hydroxysuccinimide, react for 6-12 h, and after purification, obtain the modified matrix precursor.

[0008] Preferably, the preparation method of the modified inorganic seed material includes the following steps: S21. According to the molar ratio of calcium to silicon (0.8-1.2):1, the sodium silicate solution and calcium nitrate solution are mixed, the pH is adjusted to 11-13, stirred for 20-60 min, and after centrifugation-redispersion treatment, the resulting solid product is dispersed in deionized water to prepare a seed suspension with a mass concentration of 0.5%-3%. S22. Dissolve γ-aminopropyltriethoxysilane in an ethanol-water mixed solvent, adjust the pH to 3-6 with acetic acid, and hydrolyze at 20-40℃ for 0.5-3 hours to obtain a silane hydrolysate. S23. Under stirring conditions, add a nonionic surfactant with HLB of 8-16 to the seed crystal suspension, then add silane hydrolysate, and ultrasonically disperse for 10-30 min. After ultrasonic dispersion, mature at 40-80℃ for 0.5-6 h to obtain modified inorganic seed crystal material.

[0009] Preferably, the method for preparing the modified core framework substrate includes the following steps: S111. Using 0.5-20 parts by mass of sodium hydroxide as a catalyst, 10 parts of trimethylolpropane and 280-1100 parts of glycidyl ether are reacted at 80-120℃ under nitrogen protection for 12-48 hours. After purification, the mixture is dried at 40-60℃ for 12-24 hours to obtain hyperbranched polyglycerol. S112. Dissolve hyperbranched polyglycerol in anhydrous dimethyl sulfoxide to prepare a solution with a mass concentration of 10%-30%, add an alkaline acid-binding agent, then add p-toluenesulfonyl chloride, react at 0-5℃ for 4-8h, then add ethylenediamine and react at 60-80℃ for 12-24h to obtain aminated hyperbranched polyglycerol. S113. The reaction product is purified in deionized water for 24-72 hours and then freeze-dried at -80℃ to -40℃ for 24-48 hours to obtain the modified core framework substrate.

[0010] Preferably, the aqueous solution containing ferric ions is either ferric nitrate solution or ferric sulfate solution, and the concentration of ferric ions is 0.05-0.5 mol / L.

[0011] Preferably, the vacuum permeation control vacuum degree is -0.06~-0.09MPa, each permeate is permeated and held at pressure for 15-30 minutes, and after the three permeates complete one round of permeation, they are allowed to stand for 30 minutes before the next round of circulation, and the whole permeation cycle is 2-3 times.

[0012] Preferably, the mass ratio of sodium periodate to tannic acid is (0.05-0.5):1; The mass ratio of tannic acid to modified core framework substrate is (0.5-2):1, based on the solid mass of tannic acid and the solid mass of modified core framework substrate. The mass ratio of sodium alginate to the modified core framework substrate is (0.5-2.0):1; The mass ratio of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride to sodium alginate is (0.5-2.0):1; The mass ratio of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride to N-hydroxysuccinimide is (2-5.0):1.

[0013] Preferably, in step S22, the mass ratio of ethanol, water and γ-aminopropyltriethoxysilane in the ethanol-water mixed solvent is (5-20):(1-10):1; The mass ratio of the nonionic surfactant to the seed crystal is (0.05-0.2):1, based on the oven-dry mass of the seed crystal; The mass ratio of γ-aminopropyltriethoxysilane to seed crystals is (0.1-0.5):1.

[0014] Preferably, the nonionic surfactant is selected from at least one of polyoxyethylene sorbitan fatty acid ester, alkylphenol polyoxyethylene ether, polyoxyethylene-polyoxypropylene block copolymer, and fatty alcohol polyoxyethylene ether.

[0015] Preferably, the alkaline acid-binding agent in step S112 is selected from at least one of triethylamine, pyridine, N,N-diisopropylethylamine and 4-dimethylaminopyridine; The mass ratio of the hyperbranched polyglycerol to p-toluenesulfonyl chloride is (0.5-1.5):1; The molar ratio of the alkaline acid-binding agent to the p-toluenesulfonyl chloride is (1.0-3.0):1; The mass ratio of the ethylenediamine to the p-toluenesulfonyl chloride is (1.6-4.0):1.

[0016] Compared with the prior art, the beneficial effects of the present invention are: This invention employs a trivalent iron ion aqueous solution to crosslink and cure a modified matrix precursor, combined with the synergistic effect of modified inorganic seed crystals, to specifically address the core challenge of significant deterioration in the tensile mechanical properties of PVA-ECC materials after exposure to sub-high temperatures. Specifically, the modified matrix precursor, after crosslinking and curing with trivalent iron ions, effectively repairs the structural damage caused by sub-high temperatures, stabilizes the overall stress system, and provides a reliable foundation for the material's tensile load-bearing capacity. The modified inorganic seed crystals, as functional additives, work in conjunction with the crosslinking and curing system to optimize the overall stress characteristics of the material, synergistically improve the tensile load transfer effect, and effectively restore the tensile properties of PVA-ECC materials damaged by sub-high temperatures. Attached Figure Description

[0017] Figure 1 This is a flowchart of the method for improving the tensile properties of PVA-ECC materials after sub-high temperature damage according to the present invention; Figure 2 This is a process flow diagram for preparing the modified matrix precursor of the present invention; Figure 3 This is a flow chart of the preparation process of the modified inorganic seed material of the present invention; Figure 4 This is a process flow diagram for preparing the modified core framework substrate of the present invention; Figure 5 The tensile stress-strain curve of the PVA-ECC material used in this invention after damage under sub-high temperature conditions; Figure 6 The tensile stress-strain curve of the PVA-ECC material damaged at sub-high temperature after repair by the process of Example 3 of this invention. Detailed Implementation

[0018] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0019] Please see Figures 1-6 The present invention provides a technical solution: I. Preparation of Experimental Materials and Substrate Materials In this specific embodiment, a uniform PVA-ECC substrate material was prepared, and a sub-high temperature damage environment was simulated. The specific preparation process is as follows: (1) Preparation of original materials without damage Raw materials: P.O42.5 ordinary Portland cement, Grade I fly ash, finely ground quartz sand (particle size 0.075-0.12mm), polyvinyl alcohol (PVA) fiber, hydroxypropyl methylcellulose (HPMC) thickener, early strength agent, modified polycarboxylate high-efficiency water-reducing agent, and high-efficiency defoamer. The PVA fiber has a length of 12mm, a diameter of 0.04mm, a tensile strength of 1600MPa, an elastic modulus of 40GPa, an elongation of 6%, and an aspect ratio of 300. The PVA fiber is incorporated at a volumetric dosage of 2% in the mix design.

[0020] Mix proportions: The water-cement ratio is 0.24, and the fly ash content is 80% (based on the mass of cementitious materials). The material usage per cubic meter of PVA-ECC is as follows: cement 252.6kg, fly ash 1010.5kg, quartz sand 454.7kg, thickener 1.4kg, early strength agent 40kg, defoamer 3.8kg, water-reducing agent 17.7kg, water 303.2kg, and PVA fiber 26kg.

[0021] Mixing and Molding Process: Weigh cement, fly ash, quartz sand, accelerator, and thickener according to the mixing ratio and add them to the mortar mixer. Dry mix at low speed until the dry materials are uniformly mixed. Add defoamer and water-reducing agent to the mixing water, stir evenly, and then slowly add them to the dry materials while stirring at low speed, continuing to stir until the slurry is uniform. Then add PVA fiber and continue stirring until the fiber is evenly dispersed and there are no obvious lumps. For molding, the mixture is poured into the mold in two layers: first, about 1 / 2 volume of the mixture is poured in, manually vibrated to remove air and initially leveled; then the remaining mixture is poured in, placed on a vibrating table for vibration molding, and finally the surface is scraped smooth.

[0022] Specimen specifications: The specimen is dog bone shaped with overall dimensions of 330mm×60mm×15mm. The gauge length is 90mm, and the gauge length transitions naturally to the loading clamping section through a 61mm diameter arc.

[0023] Curing: After the molded material was covered with a film and left to stand for 24 hours, the mold was removed, and the casting surface of the material was smoothed with an angle grinder to ensure the material dimensions were standard. Subsequently, it was placed at room temperature and cured with a film for 28 days to obtain the original material without damage. This group of materials served as the baseline control group for the initial state of the material.

[0024] (2) Preparation of sub-high temperature damage materials A portion of PVA-ECC reference material cured for 28 days was placed in a forced-air drying oven for sub-high temperature damage treatment. The specific steps are as follows: ①Heat to 200℃ at a heating rate of 10℃ / min; ② After reaching the target temperature, maintain the temperature for 1 hour; ③After the constant temperature period is over, remove the material and place it in a ventilated area to cool naturally to room temperature; ④ After cooling, let stand for 48 hours to obtain PVA-ECC material after sub-high temperature damage.

[0025] To verify the effectiveness of the above preparation and damage simulation processes, uniaxial tensile tests were performed on the PVA-ECC material after it underwent sub-high temperature damage. The tensile stress-strain curves are shown below. Figure 5 As shown.

[0026] like Figure 5 As shown, the tensile stress-strain curves of PVA-ECC after damage under sub-high temperature conditions are as follows: ECC still exhibits strain hardening characteristics after 1 hour of exposure at 200℃. In the initial loading stage, the stress rapidly rises to approximately 3 MPa, subsequently entering a multi-crack stage. The curve shows continuous sawtooth fluctuations, accompanied by a slow overall increase in stress, indicating that the specimen can continue to transfer stress and induce new crack formation through the bridging effect of PVA fibers after the initial cracking of the matrix. With increasing tensile deformation, the peak tensile stress is approximately 4.40 MPa, and the ultimate tensile strain is approximately 2.00%. Afterward, the stress rapidly decreases, indicating that the cracks gradually localize and form a main crack, ultimately leading to a decrease in load-bearing capacity. Compared to the room temperature state, ECC still maintains strain hardening behavior after 1 hour of exposure at 200℃, but its peak tensile stress and ultimate tensile strain are significantly reduced. This indicates that the sub-high temperature weakens the bridging load-bearing capacity of PVA fibers and the force transmission performance of the fiber-matrix interface, significantly affecting the material's multi-crack cracking ability and tensile ductility.

[0027] All Examples 1-3 and Comparative Examples 1-5 below use the above-mentioned "PVA-ECC material after sub-high temperature damage" as the base material for corresponding repair treatment or as a blank control.

[0028] Example 1 This embodiment provides a method for improving the tensile properties of PVA-ECC materials after sub-high temperature damage. The specific steps are as follows: (I) Preparation of modified core framework substrate S111. Take 10g of trimethylolpropane, 280g of glycidyl ether, and 0.5g of sodium hydroxide. React at 80℃ under nitrogen protection for 12h. After the reaction is completed, purify the mixture and dry it at 40℃ for 12h to obtain hyperbranched polyglycerol. S112. Take 20g of hyperbranched polyglycerol, add 180g of anhydrous dimethyl sulfoxide to prepare a 10% solution, add 21.23g of triethylamine, then add 40g of p-toluenesulfonyl chloride, and react at 0℃ for 4h; then add 64g of ethylenediamine, and react at 60℃ for 12h to obtain aminated hyperbranched polyglycerol.

[0029] S113. The reaction product was purified in deionized water for 24 hours and then freeze-dried at -40°C for 24 hours to obtain the modified core framework substrate.

[0030] (II) Preparation of modified matrix precursor S11. Dissolve 5g of tannic acid in 200g of deionized water, add 0.25g of sodium periodate, and pre-oxidize for 0.5h under light-protected conditions and pH 6 to obtain an aqueous solution of oxidized tannic acid; take 2.5g of modified core framework substrate, add 247.5g of deionized water, and prepare an aqueous solution of modified core framework substrate with a mass fraction of 1%.

[0031] S12. Take 51.31g of oxidized tannic acid aqueous solution and add it to 250g of modified core framework substrate aqueous solution. Adjust the pH value to 8 and react for 4h. After dialysis purification, collect the retentate containing tannic acid grafting product.

[0032] S13. Adjust the pH of the retentate to 5.0, add 1.25g sodium alginate, 0.625g EDC·HCl and 0.31g NHS, react for 6h, and after dialysis purification, obtain the modified matrix precursor.

[0033] (III) Preparation of modified inorganic seed material S21. Take 3.9g of anhydrous sodium silicate and 4.2g of anhydrous calcium nitrate, prepare them into aqueous solutions, mix them, adjust the pH to 11 after mixing, stir for 20min, and after centrifugation-redispersion treatment, disperse the resulting solid product in 995g of deionized water to prepare a seed suspension with a mass concentration of about 0.5%.

[0034] S22. Take 0.5g of γ-aminopropyltriethoxysilane, dissolve it in a mixed solvent consisting of 2.5g of ethanol and 0.5g of water, add acetic acid to adjust the pH to 3, and hydrolyze at 20℃ for 0.5h to obtain silane hydrolysate.

[0035] S23. Under stirring conditions, add 0.25g of polyoxyethylene sorbitan fatty acid ester (Tween-20) to the seed crystal suspension, then add silane hydrolysate, ultrasonically disperse for 10min, and then mature at 40℃ for 0.5h to obtain modified inorganic seed crystal material.

[0036] (iv) Tensile property enhancement treatment S1. Clean the surface of the PVA-ECC material after it has been damaged by sub-high temperature, remove dust and loose particles, and wet it until the surface is saturated and dry with no visible water. S2. Place the PVA-ECC material treated in S1 under a relative humidity of 95% for 4 hours for pre-curing. S3. Take 20.2g of ferric nitrate nonahydrate, dissolve it in deionized water and bring the volume to 1L to prepare an aqueous solution of ferric nitrate with a ferric ion concentration of 0.05mol / L; apply the above modified matrix precursor, modified inorganic seed material and ferric nitrate aqueous solution sequentially by vacuum permeation; control the vacuum degree of vacuum permeation at -0.06MPa, maintain the pressure for 15min for each permeation solution, and let stand for 30min after completing one round of permeation for the three permeation solutions before the next round of circulation, and perform two overall permeation cycles; S4. Seal the PVA-ECC material treated in S3 and cure it at a relative humidity of 95% for 24 hours, then continue to place it at a temperature of 20℃ and a relative humidity of 50% for 12 hours.

[0037] Example 2 This embodiment provides a method for improving the tensile properties of PVA-ECC materials after sub-high temperature damage. The specific steps are as follows: (I) Preparation of modified core framework substrate S111. Take 10g of trimethylolpropane, 1100g of glycidyl ether, and 20g of sodium hydroxide. React at 120℃ under nitrogen protection for 48h. After the reaction is completed, purify the mixture and dry it at 60℃ for 24h to obtain hyperbranched polyglycerol.

[0038] S112. Take 30g of the above hyperbranched polyglycerol, add 70g of anhydrous dimethyl sulfoxide to prepare a solution with a mass concentration of 30%, add 31.85g of triethylamine, then add 20g of p-toluenesulfonyl chloride, and react at 5℃ for 8h; then add 80g of ethylenediamine, and react at 80℃ for 24h to obtain aminated hyperbranched polyglycerol.

[0039] S113. The reaction product was purified in deionized water for 72 hours and then freeze-dried at -80°C for 48 hours to obtain the modified core framework substrate.

[0040] (II) Preparation of modified matrix precursor S11. Dissolve 10g of tannic acid in 500g of deionized water, add 5g of sodium periodate, and pre-oxidize for 2h under light-protected conditions and pH 8 to obtain an aqueous solution of oxidized tannic acid; take 10g of modified core framework substrate, add 190g of deionized water, and prepare an aqueous solution of modified core framework substrate with a mass fraction of 5%.

[0041] S12. Add 515g of oxidized tannic acid aqueous solution to 100g of modified core framework substrate aqueous solution, adjust the pH value to 9, react for 12h, and after dialysis purification, collect the retentate containing tannic acid grafting product.

[0042] S13. Adjust the pH of the retentate to 6.5, add 10g of sodium alginate, 20g of EDC·HCl and 4g of NHS, react for 12h, and after dialysis purification, obtain the modified matrix precursor.

[0043] (III) Preparation of modified inorganic seed material S21. Take 6.1g of anhydrous sodium silicate and 9.9g of anhydrous calcium nitrate, prepare them into aqueous solutions, mix them, adjust the pH to 13, stir for 60min, and after centrifugation-redispersion treatment, disperse the resulting solid product in 242.5g of deionized water to prepare a seed suspension with a mass concentration of about 3%.

[0044] S22. Take 3.75g of γ-aminopropyltriethoxysilane, dissolve it in a mixed solvent consisting of 75g of ethanol and 37.5g of water, add acetic acid to adjust the pH to 6, and hydrolyze at 40℃ for 3h to obtain silane hydrolysate.

[0045] S23. Under stirring conditions, 1.5g of polyoxyethylene sorbitan fatty acid ester (Tween-20) was added to the seed crystal suspension, followed by the addition of silane hydrolysate. The mixture was ultrasonically dispersed for 30min and then matured at 80℃ for 6h to obtain the modified inorganic seed crystal material.

[0046] (iv) Tensile property enhancement treatment S1. Clean the surface of the PVA-ECC material after it has been damaged by sub-high temperature, remove dust and loose particles, and wet it until the surface is saturated and dry with no visible water. S2. Place the PVA-ECC material treated in S1 under a relative humidity of 98% for 12 hours for pre-curing. S3. Take 100g of ferric sulfate, dissolve it in deionized water and bring the volume to 1L to prepare a ferric sulfate aqueous solution with a ferric ion concentration of 0.5mol / L. Apply the modified matrix precursor, modified inorganic seed material and ferric sulfate aqueous solution sequentially by vacuum permeation. Control the vacuum degree of vacuum permeation at -0.09MPa. Hold the pressure for 30min for each permeation solution. After completing one round of permeation with the three permeation solutions, let it stand for 30min before starting the next round of circulation. The entire permeation cycle is repeated 3 times. S4. Seal the PVA-ECC material treated in S3 and cure it at a relative humidity of 98% for 48 hours, then continue to place it at a temperature of 25℃ and a relative humidity of 60% for another 48 hours.

[0047] Example 3 This embodiment provides a method for improving the tensile properties of PVA-ECC materials after sub-high temperature damage. The specific steps are as follows: (I) Preparation of modified core framework substrate S111. Take 10g of trimethylolpropane, 600g of glycidyl ether, and 10g of sodium hydroxide. React them at 100℃ under nitrogen protection for 24h. After the reaction is completed, purify the mixture and dry it at 50℃ for 18h to obtain hyperbranched polyglycerol.

[0048] S112. Take 20g of the above hyperbranched polyglycerol, add 80g of anhydrous dimethyl sulfoxide to prepare a solution with a mass concentration of 20%, add 21.23g of triethylamine, then add 20g of p-toluenesulfonyl chloride, and react at 2℃ for 6h; then add 50g of ethylenediamine, and react at 70℃ for 18h to obtain aminated hyperbranched polyglycerol.

[0049] S113. The reaction product was purified in deionized water for 48 hours and then freeze-dried at -60°C for 36 hours to obtain the modified core framework substrate.

[0050] (II) Preparation of modified matrix precursor S11. Dissolve 5g of tannic acid in 300g of deionized water, add 1.25g of sodium periodate, and pre-oxidize for 1h under light-protected conditions and pH 7 to obtain an aqueous solution of oxidized tannic acid; take 5g of modified core framework substrate, add 161.7g of deionized water, and prepare an aqueous solution of modified core framework substrate with a mass fraction of 3%.

[0051] S12. Measure 183.75g of oxidized tannic acid aqueous solution and add it to 100g of modified core framework substrate aqueous solution. Adjust the pH value to 8.5 and react for 8 hours. After dialysis purification, collect the retentate containing tannic acid grafting product.

[0052] S13. Adjust the pH of the retentate to 5.5, add 4.5g of sodium alginate, 4.5g of EDC·HCl and 1.5g of NHS, react for 9h, and after dialysis purification, obtain the modified matrix precursor.

[0053] (III) Preparation of modified inorganic seed material S21. Take 6.1g of anhydrous sodium silicate and 8.2g of anhydrous calcium nitrate, prepare them into aqueous solutions, mix them, adjust the pH to 12 after mixing, stir for 40min, and after centrifugation-redispersion treatment, disperse the obtained solid product in 541.75g ​​of deionized water to prepare a seed suspension with a mass concentration of about 1.5%.

[0054] S22. Take 2.5g of γ-aminopropyltriethoxysilane, dissolve it in a mixed solvent consisting of 30g of ethanol and 12.5g of water, add acetic acid to adjust the pH to 4, and hydrolyze it at 30℃ for 1.5h to obtain silane hydrolysate.

[0055] S23. Under stirring conditions, add 0.825g of polyoxyethylene sorbitan fatty acid ester (Tween-20) to the seed crystal suspension, then add silane hydrolysate, ultrasonically disperse for 20min, and then mature at 60℃ for 3h to obtain modified inorganic seed crystal material.

[0056] (iv) Tensile property enhancement treatment S1. Clean the surface of the PVA-ECC material after it has been damaged by sub-high temperature, remove dust and loose particles, and wet it until the surface is saturated and dry with no visible water. S2. Place the PVA-ECC material treated in S1 under a relative humidity of 96% for 8 hours for pre-curing. S3. Take 80.8g of ferric nitrate nonahydrate, dissolve it in deionized water and bring the volume to 1L to prepare an aqueous solution of ferric nitrate with a ferric ion concentration of 0.2mol / L. Apply the modified matrix precursor, modified inorganic seed material and ferric nitrate aqueous solution sequentially by vacuum permeation. Control the vacuum degree of vacuum permeation at -0.08MPa. Hold the pressure for 20min for each permeation solution. After completing one round of permeation with the three permeation solutions, let it stand for 30min before the next round of circulation. The entire permeation cycle is repeated 3 times.

[0057] S4. Seal the PVA-ECC material treated in S3 and cure it at a relative humidity of 96% for 36 hours, then continue to place it at a temperature of 22℃ and a relative humidity of 55% for 24 hours.

[0058] Comparative Example 1 The difference between this comparative example and Example 3 is that in the vacuum permeation treatment in step S3, the application of the modified matrix precursor is omitted, and only the modified inorganic seed material and the aqueous solution containing ferric ions (0.2 mol / L ferric nitrate aqueous solution) are applied sequentially. The remaining steps and parameters are exactly the same as in Example 3.

[0059] Comparative Example 2 The difference between this comparative example and Example 3 is that in the vacuum permeation treatment in step S3, the application of modified inorganic seed material is omitted, and only the modified matrix precursor and an aqueous solution containing ferric ions (a ferric nitrate aqueous solution with a concentration of 0.2 mol / L) are applied sequentially. The remaining steps and parameters are exactly the same as in Example 3.

[0060] Comparative Example 3 The difference between this comparative example and Example 3 is that in the vacuum permeation treatment of step S3, the application of the aqueous solution containing ferric ions is omitted, and only the modified matrix precursor and the modified inorganic seed material are applied in sequence. The remaining steps and parameters are exactly the same as those in Example 3.

[0061] Comparative Example 4 (Unrepaired) The difference between this comparative example and Example 3 is that the PVA-ECC material that has been damaged by sub-high temperature (e.g., 200℃) is not subjected to any repair treatment (i.e., the surface cleaning, pre-curing, vacuum infiltration application of penetrant and subsequent curing operations in steps S1 to S4 are completely omitted), and it is directly used as a blank control group for performance testing.

[0062] Comparative Example 5 The difference between this comparative example and Example 3 is that a commercially available conventional cement-based penetrating crystalline repair agent (model: CCCW-Ⅰ, the main components of which are silicate cement, quartz sand and active chemical substances, conforming to GB 18445-2012 "Cement-based penetrating crystalline waterproof materials") was used to perform conventional brushing and grouting repair on the PVA-ECC material that had been damaged by sub-high temperature, in accordance with the product instructions. The other curing conditions were the same as in Example 3.

[0063] Performance testing methods Performance tests were conducted on the undamaged original material (basic control group), PVA-ECC materials treated in Examples 1-3 and Comparative Examples 1-5, and the test criteria are as follows: Ultimate tensile strength and ultimate tensile strain: In accordance with the provisions of "Tensile Properties Test" in "JC / T 2461-2018 High Toughness Fiber Reinforced Cement-Based Composite Materials", uniaxial tensile tests were conducted using dog-bone shaped specimens; the test environment conditioning and general data processing principles were in accordance with "GB / T 50081-2019 Standard for Test Methods of Physical and Mechanical Properties of Concrete". Performance test results Performance tests were conducted on the undamaged original material (basic control group), PVA-ECC materials treated in Examples 1-3 and Comparative Examples 1-5, and the test results are shown in Table 1.

[0064] Table 1: Tensile property test results of each embodiment and comparative example As shown in Table 1, after being subjected to sub-high temperature damage at 200℃ for 1 hour, the ultimate tensile strength of the untreated Comparative Example 4 was only 4.40 MPa, a decrease of approximately 41.3% compared to the undamaged original material (7.50 MPa), and the ultimate tensile strain was only 2.00%, a decrease of approximately 58.3% compared to the original material (4.80%). This indicates that the sub-high temperature damage significantly reduced the strain hardening capacity of PVA-ECC. Examples 1-3 treated with the method of this invention recovered their ultimate tensile strengths to 6.37 MPa, 6.42 MPa, and 6.50 MPa, respectively, reaching 84.9%, 85.6%, and 86.7% of the strength of the undamaged original material; their ultimate tensile strains recovered to 3.71%, 3.72%, and 3.80%, respectively, reaching 77.3%, 77.5%, and 79.2% of the original material. Example 3 showed the best repair effect.

[0065] The ultimate tensile strengths of Comparative Example 1 (omitting the modified matrix precursor) and Comparative Example 2 (omitting the modified inorganic seed material) were 5.58 MPa and 5.65 MPa, respectively, and the ultimate tensile strains were 3.18% and 3.13%, respectively. The ultimate tensile strength of Comparative Example 3 (omitting the aqueous solution containing ferric ions) was only 5.52 MPa, and the ultimate tensile strain was only 3.10%, indicating that the synergistic effect of the three components is indispensable.

[0066] In addition, although the ultimate tensile strength of Comparative Example 5, which uses commercially available conventional repair agents, was restored to 5.60 MPa, the ultimate tensile strain was only 3.08%, indicating that conventional repair methods cannot control the excessive bonding state of the interface caused by sub-high temperature. In contrast, Example 3 of the present invention is significantly better than Comparative Example 5 in terms of both strength recovery rate (86.7%) and strain recovery rate (79.2%).

[0067] This invention selects Example 3, which exhibits the best repair effect, and performs uniaxial tensile stress-strain characterization. The corresponding tensile stress-strain curves are shown below. Figure 6 As shown.

[0068] like Figure 6As shown, the tensile stress-strain curve of the PVA-ECC material after repair in Example 3 exhibits typical strain hardening characteristics: in the initial loading stage, the stress increases rapidly with strain. After the matrix reaches the initial crack strength, the curve enters the multi-crack initiation stage, and the stress continues to rise overall amidst local fluctuations. Subsequently, as the PVA fibers continue to play a bridging role, the specimen can continuously form new microcracks while existing cracks stably propagate, allowing the material to maintain its load-bearing capacity under large tensile deformation. The curve shows obvious sawtooth fluctuations, which are closely related to the gradual initiation and propagation of cracks, as well as fiber bridging and interface slip processes. As can be seen from the figure, the ultimate tensile strain of ECC is approximately 3.8%, and the peak tensile stress is approximately 6.5 MPa, indicating that the material has good multi-crack initiation capability and tensile ductility under room temperature conditions. After reaching the peak stress, the curve shows a certain degree of decline, indicating that local cracks gradually develop into main cracks, eventually leading to the unstable failure of the specimen.

[0069] The above results demonstrate that the present invention achieves effective recovery of the tensile properties and toughness of PVA-ECC materials after sub-high temperature damage through the synergistic effect of modified matrix precursor, modified inorganic seed material, and aqueous solution containing ferric ions.

[0070] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for improving the tensile properties of PVA-ECC materials after sub-high temperature damage, characterized in that, Includes the following steps: S1. Clean the surface of the PVA-ECC material after it has been damaged by sub-high temperature, and wet the PVA-ECC material until it is saturated and surface-dry with no visible water. S2. Place the PVA-ECC material treated in S1 under a relative humidity of 95%-98% for pre-curing for 4-12 hours; S3. For the PVA-ECC material cured by S2, the modified matrix precursor, modified inorganic seed material and aqueous solution containing ferric ions are applied sequentially by vacuum infiltration. S4. The PVA-ECC material treated in S3 is cured in a sealed environment with a relative humidity of 95%-98% for 24-48 hours, and then placed in a temperature of 20-25℃ and a relative humidity of 50%-60% for another 12-48 hours. The preparation method of the modified matrix precursor includes the following steps: S11. Dissolve 5-10 parts of tannic acid in 200-500 parts of deionized water by mass, add sodium periodate, and pre-oxidize for 0.5-2 hours under light-protected conditions and a pH of 6-8 to obtain an aqueous solution of oxidized tannic acid; disperse or dissolve the modified core framework substrate in deionized water to obtain an aqueous solution of modified core framework substrate with a mass fraction of 1%-5%; S12. Add the modified core framework substrate aqueous solution to the oxidized tannic acid aqueous solution, adjust the pH value to 8-9, react for 4-12 hours, and after purification, collect the retentate containing the tannic acid grafting product. S13. Adjust the pH of the retentate to 5.0-6.5, add sodium alginate, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide, react for 6-12 h, and after purification, obtain the modified matrix precursor. The preparation method of the modified inorganic seed material includes the following steps: S21. According to the molar ratio of calcium to silicon (0.8-1.2):1, the sodium silicate solution and calcium nitrate solution are mixed, the pH is adjusted to 11-13, stirred for 20-60 min, and after centrifugation-redispersion treatment, the resulting solid product is dispersed in deionized water to prepare a seed suspension with a mass concentration of 0.5%-3%. S22. Dissolve γ-aminopropyltriethoxysilane in an ethanol-water mixed solvent, adjust the pH to 3-6 with acetic acid, and hydrolyze at 20-40℃ for 0.5-3 hours to obtain a silane hydrolysate. S23. Under stirring conditions, add a nonionic surfactant with HLB of 8-16 to the seed crystal suspension, then add silane hydrolysate, and ultrasonically disperse for 10-30 min. After ultrasonic dispersion, mature at 40-80℃ for 0.5-6 h to obtain modified inorganic seed crystal material. The method for preparing the modified core framework substrate includes the following steps: S111. Using 0.5-20 parts by mass of sodium hydroxide as a catalyst, 10 parts of trimethylolpropane and 280-1100 parts of glycidyl ether are reacted at 80-120℃ under nitrogen protection for 12-48 hours. After purification, the mixture is dried at 40-60℃ for 12-24 hours to obtain hyperbranched polyglycerol. S112. Dissolve hyperbranched polyglycerol in anhydrous dimethyl sulfoxide to prepare a solution with a mass concentration of 10%-30%, add an alkaline acid-binding agent, then add p-toluenesulfonyl chloride, react at 0-5℃ for 4-8h, then add ethylenediamine and react at 60-80℃ for 12-24h to obtain aminated hyperbranched polyglycerol. S113. The reaction product is purified in deionized water for 24-72 hours and then freeze-dried at -80℃ to -40℃ for 24-48 hours to obtain the modified core framework substrate.

2. The method for improving the tensile properties of PVA-ECC materials after sub-high temperature damage according to claim 1, characterized in that, The aqueous solution containing ferric ions is either ferric nitrate solution or ferric sulfate solution, and the concentration of ferric ions is 0.05-0.5 mol / L.

3. The method for improving the tensile properties of PVA-ECC materials after sub-high temperature damage according to claim 1, characterized in that, The vacuum permeation control vacuum degree is -0.06~-0.09MPa. Each permeate is held at pressure for 15-30 minutes per permeation. After the three permeates complete one round of permeation, they are allowed to stand for 30 minutes before the next round of circulation. The entire permeation cycle is 2-3 times.

4. The method for improving the tensile properties of PVA-ECC materials after sub-high temperature damage according to claim 1, characterized in that, The mass ratio of sodium periodate to tannic acid is (0.05-0.5):1; The mass ratio of tannic acid to modified core framework substrate is (0.5-2):1, based on the solid mass of tannic acid and the solid mass of modified core framework substrate. The mass ratio of sodium alginate to the modified core framework substrate is (0.5-2.0):1; The mass ratio of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride to sodium alginate is (0.5-2.0):1; The mass ratio of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride to N-hydroxysuccinimide is (2-5.0):

1.

5. The method for improving the tensile properties of PVA-ECC materials after sub-high temperature damage according to claim 1, characterized in that, In step S22, the mass ratio of ethanol, water and γ-aminopropyltriethoxysilane in the ethanol-water mixed solvent is (5-20):(1-10):1; The mass ratio of the nonionic surfactant to the seed crystal is (0.05-0.2):1, based on the oven-dry mass of the seed crystal; The mass ratio of γ-aminopropyltriethoxysilane to seed crystals is (0.1-0.5):

1.

6. The method for improving the tensile properties of PVA-ECC materials after sub-high temperature damage according to claim 1, characterized in that, The nonionic surfactant is selected from at least one of polyoxyethylene sorbitan fatty acid ester, alkylphenol polyoxyethylene ether, polyoxyethylene-polyoxypropylene block copolymer and fatty alcohol polyoxyethylene ether.

7. The method for improving the tensile properties of PVA-ECC materials after sub-high temperature damage according to claim 1, characterized in that, The alkaline acid-binding agent in step S112 is selected from at least one of triethylamine, pyridine, N,N-diisopropylethylamine and 4-dimethylaminopyridine; The mass ratio of the hyperbranched polyglycerol to p-toluenesulfonyl chloride is (0.5-1.5):1; The molar ratio of the alkaline acid-binding agent to the p-toluenesulfonyl chloride is (1.0-3.0):1; The mass ratio of the ethylenediamine to the p-toluenesulfonyl chloride is (1.6-4.0):1.

Citation Information

Patent Citations

  • Method for preparing hydrogel based on metal coordination physical mixing and hydrogel

    CN114276562A

  • High-tensile adhesive sodium alginate / polyacrylamide / tannic acid hydrogel as well as preparation method and application thereof