AI Technical Summary
CN115323205A公开了一种提高ASME CY40镍基合金机械性能的熔炼方法,其通过内控化学成分和气体含量控制来提升合金的力学性能,但该专利仅关注合金力学性能的提升,未涉及铸造过程中热裂纹的抑制,更未提及通过微合金化手段改善抗热裂性能
(1)本发明通过在CY40合金中同时添加Ti、Zr、B三种晶粒细化元素并控制Ti:Zr=3:1~5:1,利用Ti与Zr在熔体中预先形成(Ti,Zr)(C,N)复合形核核心,该复合形核核心与镍基体的晶格错配度小于5%,可在凝固过程中作为非均质形核基底显著细化奥氏体晶粒,经固溶处理后铸件平均晶粒度可达ASTM 4级或更细;同时B的晶界偏聚进一步增强了晶界结合力,从合金本质层面降低了热裂敏感性,克服了现有技术中Zr、B添加易导致热裂的技术偏见。
Smart Images

Figure FT_1 
Figure SMS_34 
Figure SMS_35
Abstract
Description
Technical Field
[0001] This invention belongs to the field of nickel-based alloy casting technology, specifically relating to a casting and smelting process for CY40 material. Background Technology
[0002] CY40 nickel-based alloy (ASTM A494 Grade CY40, corresponding to UNS N06040) is a Ni-Cr-Fe solid solution strengthened corrosion-resistant alloy with excellent corrosion resistance, high-temperature strength, and resistance to chloride stress corrosion cracking. It can operate for extended periods at temperatures up to 1093°C and is widely used in critical hot-end components in chemical, heat treatment, electrical, nuclear energy, and aerospace industries, such as valves, pump bodies, and pipeline castings. This alloy has a high nickel content (≥70%) and a wide solidification range, and is typically used for investment casting to produce complex-shaped valve body castings.
[0003] However, CY40 alloy is highly susceptible to hot cracking defects during casting. Its wide solidification range, long solid-liquid phase coexistence time, and concentrated shrinkage stress make it prone to hot spots in castings (especially at the root of the ingate). Simultaneously, nickel-based alloys are prone to oxidation and gas absorption during high-temperature melting; if deoxidation and degassing are insufficient, gases and inclusions in the melt will further exacerbate the hot cracking tendency. Current technologies typically reduce hot cracking by adjusting the casting process (e.g., changing from bottom-pouring to top-pouring and using a split-flow casting method), controlling pouring temperature and cooling rate, and improving the mold's collapsibility. However, these methods only optimize the casting process and fail to address the inherent hot cracking problem at the alloy level. CN115323205A discloses a smelting method for improving the mechanical properties of ASME CY40 nickel-based alloy. This method enhances the alloy's mechanical properties through internal control of chemical composition and gas content. However, this patent only focuses on improving the alloy's mechanical properties and does not address the suppression of hot cracking during casting, nor does it mention improving hot crack resistance through microalloying. CY40 is a standard composition solid solution-strengthened alloy, and its ASTM standard chemical composition does not contain grain-refining elements such as Ti, Zr, and B. There are no existing reports of systematically suppressing hot cracking in CY40 alloys by using microalloying combined with melt refining and advanced casting processes.
[0004] In summary, the existing technology lacks a casting and smelting process for CY40 materials that can refine grains at the alloy's intrinsic level, deeply purify the melt, and eliminate stress concentration at the casting process level. This restricts the further improvement of the yield and reliability of CY40 castings. Summary of the Invention
[0005] To address the aforementioned problems in the existing technology, this invention provides a casting and smelting process for CY40 material.
[0006] The objective of this invention can be achieved through the following technical solutions: A casting and smelting process for CY40 material includes the following steps: (1) Batching and microalloying: Batching is carried out according to the chemical composition of CY40 nickel-based alloy. The chemical composition of CY40 nickel-based alloy by weight percentage is: C≤0.40%, Si≤3.00%, Mn≤1.50%, P≤0.03%, S≤0.03%, Cr14.0~17.0%, Fe≤11.0%, with the balance being Ni and unavoidable impurities; At the same time, the following grain refining elements by weight percentage are added to the batching: Ti 0.03~0.15wt%, Zr 0.01~0.08wt%, B 0.001~0.006wt%, and the weight ratio of Ti to Zr is controlled between 3:1 and 5:1; (2) Melting and refining: The prepared raw materials are placed in a vacuum induction melting furnace, a vacuum is drawn, and a protective gas is introduced. The temperature is raised to melt and clear the raw materials to obtain the initial molten liquid. A composite refining agent is added to the initial molten liquid for refining. The refining temperature is 1480~1520℃, and the refining time is 10~15 minutes. The composite refining agent is composed of the following components by weight percentage: 5~8wt%, 2~5wt%, 40~50wt%, 25~35wt%, The amount of the composite refining agent added is 10-20 wt%, which is 0.2-0.5 wt% of the initial molten liquid weight. (3) Casting and solidification: Cool the refined molten liquid to 1360~1400℃, and fill the preheated mold shell from bottom to top with a filling pressure of 0.04~0.08MPa; after filling, apply a holding pressure of 0.5~1.0MPa until the casting is completely solidified, and obtain the billet after cooling; (4) Solution treatment: The billet is solution treated at 1120~1140℃, and then cooled after holding at the temperature.
[0007] As a preferred technical solution of the present invention, in step (3), the bottom-up filling is achieved by using anti-gravity casting.
[0008] As a preferred technical solution of the present invention, in step (2), the composite refining agent is baked at 800~900℃ for no less than 2 hours before being added.
[0009] As a preferred technical solution of the present invention, in step (2), the crucible of the vacuum induction melting furnace is a magnesium oxide crucible or a calcium oxide crucible.
[0010] As a preferred technical solution of the present invention, in step (2), the composite refining agent contains and The weight ratio is 2:1 to 3:1.
[0011] As a preferred technical solution of the present invention, in step (3), the preheating temperature of the shell is 750~950℃.
[0012] As a preferred technical solution of the present invention, in step (1), the weight ratio of Ti to Zr is 3:1 to 5:1, which enables the formation of a (Ti,Zr)(C,N) composite nucleation core in situ during the smelting process. The lattice mismatch between the composite nucleation core and the nickel matrix is less than 5%, and it serves as a heterogeneous nucleation substrate during solidification to promote the refinement of austenite grains.
[0013] As a preferred technical solution of the present invention, in step (2), the composite refining agent generates rare earth oxygen sulfide during the refining process. The rare earth oxygen sulfide serves as the nucleation substrate for the carbonitride formed by Ti, Zr, and B elements in step (1), thereby achieving the synergistic generation of refining products and grain refinement cores.
[0014] As a preferred technical solution of the present invention, in step (1), the amount of Ti added is further limited to 0.05~0.10wt%; the synergistic addition of Ti, Zr and B in step (1) makes the average grain size of the casting reach ASTM grade 4 or finer after the solution treatment in step (4).
[0015] Application of a CY40 material casting and melting process in the preparation of CY40 nickel-based alloy valve body castings.
[0016] The present invention has the following beneficial effects: (1) This invention adds three grain-refining elements, Ti, Zr and B, to CY40 alloy and controls the Ti:Zr ratio to be 3:1 to 5:1. The (Ti,Zr)(C,N) composite nucleation core is pre-formed in the melt by Ti and Zr. The lattice mismatch between the composite nucleation core and the nickel matrix is less than 5%. It can significantly refine the austenite grains as a heterogeneous nucleation substrate during solidification. After solution treatment, the average grain size of the casting can reach ASTM grade 4 or finer. At the same time, the grain boundary segregation of B further enhances the grain boundary bonding force, reduces the hot cracking sensitivity from the perspective of the alloy itself, and overcomes the technical prejudice that the addition of Zr and B in the prior art easily leads to hot cracking.
[0017] (2) This invention directly adds [material] during the vacuum induction melting process. , , , and Refining is carried out using a composite refining agent. and Nanoscale rare earth oxysulfides are generated by dual rare earth oxides under vacuum reduction environment. These rare earth oxysulfides can not only deeply remove oxygen and sulfur from the melt, but also serve as a nucleation substrate for carbonitrides formed by Ti, Zr and B elements. This achieves the synergistic generation of refining products and grain refinement cores, eliminating crack sources at the melt level.
[0018] (3) This invention effectively resolves the contradiction between low-temperature casting and mold integrity by cooling the refined molten liquid to 1360~1400℃ for low-temperature casting, combined with an anti-gravity filling pressure of 0.04~0.08MPa and a holding solidification pressure of 0.5~1.0MPa. This ensures the density of the casting while obtaining fine equiaxed crystals, thus preventing the initiation of cracks from the casting process level. The synergistic effect of these three levels effectively suppresses hot cracking in CY40 castings, significantly improving yield and reliability. Attached Figure Description
[0019] To facilitate understanding by those skilled in the art, the present invention will be further described below with reference to the accompanying drawings.
[0020] Figure 1 This is a schematic diagram of the main steps of the present invention. Detailed Implementation
[0021] To further illustrate the technical means and effects of the present invention in achieving its intended purpose, the following detailed description of the specific implementation methods, structures, features, and effects of the present invention, in conjunction with the accompanying drawings and preferred embodiments, is provided.
[0022] Example 1 Please see Figure 1 This invention provides a casting and smelting process for CY40 material, comprising the following steps.
[0023] Batching and Microalloying: Batching was carried out according to the chemical composition of CY40 nickel-based alloy. The chemical composition of the CY40 nickel-based alloy, by weight percentage, is: C≤0.40%, Si≤3.00%, Mn≤1.50%, P≤0.03%, S≤0.03%, Cr14.0~17.0%, Fe≤11.0%, with the balance being Ni and unavoidable impurities. Simultaneously, grain-refining elements were added to the batching, with Ti added at 0.08wt%, Zr at 0.02wt%, and B at 0.003wt%, with a Ti to Zr weight ratio of 4:1.
[0024] Smelting and refining: Place the prepared raw materials in a vacuum induction melting furnace and evacuate to a vacuum level not exceeding 1×10⁻⁶. -The mixture is heated to 1580°C with high-purity argon gas as a protective gas at 2Pa to obtain an initial molten liquid. A composite refining agent is then added to the initial molten liquid for refining. The composite refining agent consists of the following components by weight percentage: 6wt%, 3wt%, 45wt%, 30wt%, 16 wt%. The composite refining agent was baked at 850°C for 3 hours before being added. The amount of the composite refining agent added was 0.3 wt% of the initial molten liquid weight. The refining temperature was 1500°C, and the refining time was 12 minutes. After standing, the refined molten liquid was obtained. The crucible of the vacuum induction melting furnace was a magnesium oxide crucible.
[0025] Casting and Solidification: The refined molten metal is cooled to 1380℃ and filled from bottom to top using anti-gravity casting. Under a filling pressure of 0.06 MPa, the molten metal fills the preheated mold shell from bottom to top. The preheating temperature of the mold shell is 850℃. After filling, a holding pressure of 0.8 MPa is applied until the casting is completely solidified. The casting is then slowly cooled to room temperature along with the mold shell to obtain the cast billet.
[0026] Solution treatment: The billet is solution treated at 1130℃, and the holding time is calculated as 2h / 25mm based on the maximum wall thickness of the casting, followed by oil quenching.
[0027] The CY40 nickel-based alloy castings prepared by the above process are used to prepare valve body castings.
[0028] Example 2 This embodiment provides a casting and smelting process for CY40 material, which differs from Embodiment 1 in that the boundary values of the process parameters are different.
[0029] In the batching and microalloying stage: the amount of Ti added is 0.03 wt%, the amount of Zr added is 0.01 wt%, the amount of B added is 0.001 wt%, and the weight ratio of Ti to Zr is 3:1.
[0030] Melting and refining stage: The temperature for heating and clearing is 1550℃. The composite refining agent consists of the following components by weight percentage: 5wt%, 2wt%, 48wt%, 28wt%, 17 wt%. The composite refining agent is baked at 800°C for 3 hours before being added. The amount of the composite refining agent added is 0.2 wt% of the initial molten liquid weight. The refining temperature is 1480°C, and the refining time is 15 minutes. The crucible of the vacuum induction melting furnace is a calcium oxide crucible.
[0031] Casting and solidification stage: The refined molten metal is cooled to 1360℃. The molten metal is then filled from bottom to top into the preheated mold shell at a filling pressure of 0.04 MPa. The preheating temperature of the mold shell is 750℃. After filling, a holding pressure of 0.5 MPa is applied until the casting is completely solidified.
[0032] Solution treatment stage: The billet is solution treated at 1120℃, and the holding time is calculated as 2h / 25mm based on the maximum wall thickness of the casting, followed by water quenching.
[0033] The remaining steps are the same as in Example 1.
[0034] Example 3 This embodiment provides a casting and smelting process for CY40 material, which differs from Embodiment 1 in that the boundary values of the process parameters are different.
[0035] In the batching and microalloying stage: the amount of Ti added was 0.15 wt%, the amount of Zr added was 0.08 wt%, the amount of B added was 0.006 wt%, and the weight ratio of Ti to Zr was 5:1.
[0036] Melting and refining stage: The heating and melting temperature is 1600℃. The composite refining agent consists of the following components by weight percentage: 8wt%, 5wt%, 42wt%, 32wt%, 13 wt%. The composite refining agent is baked at 900°C for 3 hours before being added. The amount of the composite refining agent added is 0.5 wt% of the initial molten liquid weight. The refining temperature is 1520°C, and the refining time is 10 minutes. The crucible of the vacuum induction melting furnace is a magnesium oxide crucible.
[0037] Casting and solidification stage: The refined molten metal is cooled to 1400℃. The molten metal is then filled from bottom to top into the preheated mold shell at a filling pressure of 0.08 MPa. The preheating temperature of the mold shell is 950℃. After filling, a holding pressure of 1.0 MPa is applied until the casting is completely solidified.
[0038] Solution treatment stage: The billet is solution treated at 1140℃, and the holding time is calculated as 2h / 25mm based on the maximum wall thickness of the casting, followed by oil quenching and cooling.
[0039] The remaining steps are the same as in Example 1.
[0040] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that no grain-refining elements such as Ti, Zr, and B are added during the batching and microalloying stages, while the other conditions are the same as in Example 1.
[0041] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that no composite refining agent is added during the smelting and refining stages, while the other conditions are the same as in Example 1.
[0042] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that the conventional gravity casting method was used in the pouring and solidification stages, the pouring temperature was 1550℃, no holding pressure was applied, and the other conditions were the same as in Example 1.
[0043] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that only 0.08 wt% Ti was added during the batching and microalloying stages, and Zr and B were not added. The other conditions were the same as in Example 1.
[0044] Performance testing and characterization The following performance tests and microstructure characterization were performed on the castings obtained in Examples 1-3 and Comparative Examples 1-4.
[0045] As-cast grain size test: The as-cast grain size was determined according to ASTM E112 standard. After grinding and polishing, the austenite grain boundaries were revealed using a suitable etchant, and the grain size grade was determined under an optical microscope using the intercept method or comparison method. The test results are shown in Table 1.
[0046] Grain size test after solution treatment: The average grain size of the castings after solution treatment was determined according to ASTM E112 standard. The solution-treated casting samples were ground, polished, and etched, and then observed and measured for grain size grade under an optical microscope. The test results are shown in Table 1.
[0047] Hot crack evaluation: Fluorescent penetrant testing was used to inspect the surface of the casting, and the number and total length of hot cracks were counted. The test results are shown in Table 1.
[0048] Mechanical property testing: Room temperature tensile strength, yield strength, and elongation were tested according to ASTM A494 standard. The test results are shown in Table 1.
[0049] Melt purity analysis: The oxygen content in the refined melt was determined using an oxygen, nitrogen, and hydrogen analyzer. The test results are shown in Table 1.
[0050] Lattice mismatch determination: Phase analysis of the casting samples was performed using X-ray diffraction. First, samples were cut from the casting and prepared into flat, stress-free diffraction samples through mechanical grinding and electrolytic polishing. A quadriaxial X-ray diffractometer was used with a Cu-Kα radiation source, performing step scans within the 2θ angle range of 20°–100° to obtain diffraction patterns. Based on the diffraction peak positions, the phase mismatch was determined according to Bragg's equation. Calculate the interplanar spacing and lattice constant of the (Ti,Zr)(C,N) composite nucleation core, and simultaneously calculate the lattice constant of the austenitic nickel matrix. The lattice mismatch is calculated according to the formula... Calculation, where The lattice constant of the (Ti,Zr)(C,N) composite nucleation core is given. is the lattice constant of the austenitic nickel matrix. The test results are shown in Table 2.
[0051] Microstructural observation: Transmission electron microscopy (TEM) combined with X-ray energy dispersive spectroscopy (EDS) was used to observe the microstructure and analyze the composition of the casting samples. First, a 0.3 mm thick slice was cut from the casting and mechanically thinned to below 50 μm. Then, TEM samples were prepared using double-jet electrolytic thinning or ion thinning methods. The morphology, size, and distribution of the precipitated phases were observed under TEM, and the phase structure was determined by selected area electron diffraction (SED). EDS was used to analyze the composition of the precipitated phases, confirming the elemental composition of rare earth oxysulfides and Ti-Zr carbonitrides. The spatial relationship between rare earth oxysulfides and Ti-Zr carbonitrides was observed to confirm the presence of a core-shell structure.
[0052] Table 1 Performance test results of the examples and comparative examples
[0053] Table 2. Lattice constants and mismatches of the (Ti,Zr)(C,N) composite nucleation core and nickel matrix in Example 1.
[0054] As shown in Table 2, the lattice mismatch between the (Ti,Zr)(C,N) composite nucleation core and the austenitic nickel matrix is 4.2%, which is less than 5%.
[0055] Microscopic tissue observation results Transmission electron microscopy (TEM) observation of the casting sample from Example 1 revealed a large number of finely dispersed precipitates within the austenite grains and near the grain boundaries. Selected area electron diffraction (SED) analysis confirmed that the core phase was a (Ti,Zr)(C,N) composite carbonitride with a face-centered cubic structure. Surrounding the (Ti,Zr)(C,N) core was a shell composed of cerium and lanthanum oxysulfides, forming a core-shell structure. X-ray energy dispersive spectroscopy (EDS) analysis confirmed that the core region was enriched in Ti, Zr, C, and N elements, while the shell region was enriched in Ce, La, O, and S elements.
[0056] The above results indicate that: in composite refining agents and Nanoscale rare-earth oxysulfides were generated from dual rare-earth oxides under vacuum reduction conditions. These rare-earth oxysulfides served as a precursor nucleation substrate for carbonitrides formed by Ti, Zr, and B elements, achieving the synergistic generation of refined products and grain refinement nuclei. The formation mechanism of this core-shell structure is as follows: rare-earth oxides first react with oxygen and sulfur in the melt to generate fine rare-earth oxysulfide particles; subsequently, Ti, Zr, C, and N undergo heterogeneous nucleation on the surface of the rare-earth oxysulfide particles, growing to form a (Ti,Zr)(C,N) composite carbonitride shell. Since the lattice mismatch between (Ti,Zr)(C,N) and the austenitic nickel matrix is less than 5%, these core-shell structure particles can serve as a highly efficient heterogeneous nucleation substrate, significantly promoting austenite grain refinement during solidification.
[0057] Results Analysis As shown in Table 1: The as-cast grain size of Examples 1-3 reached ASTM grade 5.0-6.0, and after solution treatment, it still maintained ASTM grade 4.5-5.5, significantly better than Comparative Example 1 (as-cast grade 3.0, solution-treated grade 2.5). This indicates that the synergistic addition of Ti / Zr / B ternary elements has a significant grain refinement effect, and the grain growth tendency is effectively suppressed after solution treatment. This is attributed to the pinning effect of the (Ti,Zr)(C,N) composite nucleation cores pre-formed by Ti and Zr in the melt on grain boundaries during high-temperature solution treatment.
[0058] The number and total length of hot cracks in Examples 1-3 were significantly lower than those in the comparative examples, with no hot cracks detected in Examples 1 and 3. Comparative Example 1, without the addition of Ti / Zr / B grain-refining elements, had coarse as-cast grains and the highest number of hot cracks. Comparative Example 2, without the addition of the composite refining agent, had a melt oxygen content as high as 68 ppm, resulting in a large number of hot cracks. Comparative Example 3, using conventional gravity casting and high-temperature pouring, although with a lower oxygen content, still had significantly more hot cracks than the examples. Comparative Example 4, with only Ti added but without Zr and B, showed significantly weaker grain refinement and hot crack suppression effects than Examples 1-3. These results indicate that the present invention effectively suppresses hot cracking in CY40 castings through the synergistic effects of Ti / Zr / B ternary synergistic microalloying, deep purification with the composite refining agent, and anti-gravity low-temperature pouring and pressure-holding solidification.
[0059] The tensile strength of Examples 1-3 was 610-635 MPa, the yield strength was 470-495 MPa, and the elongation was 33-36%, all of which met the mechanical property requirements of ASTM A494 standard for CY40 alloy. Moreover, the elongation was significantly better than that of Comparative Examples 1-4 (28-31%), indicating that grain refinement improved plasticity while increasing strength.
[0060] The melt oxygen content of Examples 1-3 was 10-15 ppm, significantly better than that of Comparative Example 2 (68 ppm), indicating that the oxygen content in the melt was... and The composite refining agent of rare earth oxides has excellent deep deoxidation effect.
[0061] in conclusion As can be seen from the above embodiments and comparative examples, the present invention, by simultaneously adding three grain-refining elements—Ti, Zr, and B—to the CY40 alloy and controlling the Ti:Zr ratio to be 3:1~5:1, combined with... and The composite refining agent of two rare earth oxides is used for vacuum induction melting and refining, followed by anti-gravity low-temperature casting and pressure-holding solidification. This achieves a systematic and synergistic effect, refining grains at the alloy's intrinsic level, deeply purifying the melt, and eliminating stress concentration at the casting process level. CY40 castings prepared using this invention exhibit significantly refined grains, effectively suppress hot cracking, meet standard requirements for mechanical properties, and show significantly improved yield and reliability.
[0062] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Any person skilled in the art can make some modifications or alterations to the disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention, without departing from the scope of the present invention, shall still fall within the protection scope of the present invention.
Claims
1. A casting and smelting process for CY40 material, characterized in that, Includes the following steps: (1) Batching and microalloying: Batching is carried out according to the chemical composition of CY40 nickel-based alloy. The chemical composition of CY40 nickel-based alloy by weight percentage is: C≤0.40%, Si≤3.00%, Mn≤1.50%, P≤0.03%, S≤0.03%, Cr 14.0~17.0%, Fe≤11.0%, with the balance being Ni and unavoidable impurities; At the same time, the following grain refining elements by weight percentage are added to the batching: Ti 0.03~0.15wt%, Zr 0.01~0.08wt%, B 0.001~0.006wt%, and the weight ratio of Ti to Zr is controlled between 3:1 and 5:1; (2) Melting and refining: The prepared raw materials are placed in a vacuum induction melting furnace, a vacuum is drawn, and a protective gas is introduced. The temperature is raised to melt and clear the raw materials to obtain the initial molten liquid. A composite refining agent is added to the initial molten liquid for refining. The refining temperature is 1480~1520℃, and the refining time is 10~15 minutes. The composite refining agent is composed of the following components by weight percentage: 5~8wt%, 2~5wt%, 40~50wt%, 25~35wt%, The amount of the composite refining agent added is 10-20 wt%, which is 0.2-0.5 wt% of the initial molten liquid weight. (3) Casting and solidification: Cool the refined molten liquid to 1360~1400℃, and fill the preheated mold shell from bottom to top with a filling pressure of 0.04~0.08MPa; after filling, apply a holding pressure of 0.5~1.0MPa until the casting is completely solidified, and obtain the billet after cooling; (4) Solution treatment: The billet is solution treated at 1120~1140℃, and then cooled after holding at the temperature.
2. The casting and smelting process for CY40 material according to claim 1, characterized in that: In step (3), the bottom-up filling is achieved by using anti-gravity casting.
3. The casting and smelting process for CY40 material according to claim 1, characterized in that: In step (2), the composite refining agent is baked at 800~900℃ for no less than 2 hours before being added.
4. The casting and smelting process for CY40 material according to claim 1, characterized in that: In step (2), the crucible of the vacuum induction melting furnace is a magnesium oxide crucible or a calcium oxide crucible.
5. The casting and smelting process for CY40 material according to claim 1, characterized in that: In step (2), the composite refining agent contains and The weight ratio is 2:1 to 3:
1.
6. The casting and smelting process for CY40 material according to claim 1, characterized in that: In step (3), the preheating temperature of the shell is 750~950℃.
7. The casting and smelting process for CY40 material according to claim 1, characterized in that: In step (1), the weight ratio of Ti to Zr is 3:1 to 5:1, which enables the formation of a (Ti,Zr)(C,N) composite nucleation core in situ during the smelting process. The lattice mismatch between the composite nucleation core and the nickel matrix is less than 5%, and it serves as a heterogeneous nucleation substrate during solidification to promote the refinement of austenite grains.
8. The casting and smelting process for CY40 material according to claim 1, characterized in that: In step (2), the composite refining agent generates rare earth oxygen sulfides during the refining process. The rare earth oxygen sulfides serve as the nucleation substrate for the carbonitrides formed by Ti, Zr, and B elements in step (1), thereby achieving the synergistic generation of refining products and grain refinement cores.
9. The casting and smelting process for CY40 material according to claim 1, characterized in that: In step (1), the amount of Ti added is further limited to 0.05~0.10wt%; the synergistic addition of Ti, Zr and B in step (1) makes the average grain size of the casting reach ASTM grade 4 or finer after the solution treatment in step (4).
10. The application of the CY40 material casting and smelting process according to any one of claims 1 to 9 in the preparation of CY40 nickel-based alloy valve body castings.
Citation Information
Patent Citations
Smelting method for improving mechanical performance of ASME CY40 nickel-based alloy