Polyvinyl alcohol-triterpene saponin synergistically modified fly ash cement-based supercapacitor and preparation method thereof

By synergistic modification of fly ash cement-based supercapacitors with polyvinyl alcohol and triterpenoid saponins, a continuous and interconnected ion transport channel is constructed and deeply wetted with electrolyte. This solves the problem of the difficulty in synergistic relationship between pore structure and mechanical properties of cement-based supercapacitors, improves specific capacitance and cycle stability, and is suitable for energy storage applications in building structures.

CN122950313BActive Publication Date: 2026-11-20SHANDONG JIANZHU UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611433364.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-09-16
Publication Date
2026-11-20
Estimated Expiration
2046-09-16

AI Technical Summary

Technical Problem

Existing cement-based supercapacitors suffer from problems such as difficulty in synergizing pore structure and mechanical properties, insufficient electrolyte wetting, and poor cycle stability, resulting in low specific capacitance and high interfacial charge transfer impedance, which limits their application in building structures.

Method used

A fly ash cement-based supercapacitor was modified using polyvinyl alcohol and triterpenoid saponins. The triterpenoid saponins were used to induce air and construct a continuous and interconnected ion transport channel. Polyvinyl alcohol was used to toughen and strengthen the pore walls. The micro-aggregate effect of fly ash was combined to refine the pore size distribution. The electrolyte was deeply saturated and wetted through a vacuum negative pressure impregnation process.

Benefits of technology

It achieves a synergistic improvement in electrochemical energy storage performance and structural mechanical performance, increases specific capacitance, reduces interfacial charge transfer impedance, enhances cycle stability and mechanical load-bearing capacity, and is suitable for integrated structural and energy storage applications in building structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122950313B_ABST
    Figure CN122950313B_ABST
Patent Text Reader

Abstract

The present application relates to the field of civil engineering materials and electrochemical energy storage cross technology, specifically relates to a kind of polyvinyl alcohol-triterpene saponin synergistic modified fly ash cement-based supercapacitor and its preparation method.The capacitor includes electrode layer and the cement-based functional layer between electrode layer, cement-based functional layer raw material includes Portland cement, fly ash, polyvinyl alcohol, triterpene saponin air entraining agent, water reducing agent and water, water-binder ratio 0.35~0.45, fly ash content 10%~20%, polyvinyl alcohol content 1.0%~3.0%, triterpene saponin air entraining agent content 0.04%~0.12%.The present application also provides a kind of polyvinyl alcohol-triterpene saponin synergistic modified fly ash cement-based supercapacitor preparation method.The cement-based supercapacitor prepared by the present application has excellent electrical performance, and the capacity retention rate is still ≥80% after 10000 times of charge-discharge cycle, and the 28-day compressive strength is stable to reach ≥65MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the interdisciplinary field of civil engineering materials and electrochemical energy storage, specifically to a polyvinyl alcohol-triterpenoid saponin synergistic modification fly ash cement-based supercapacitor and its preparation method. Background Technology

[0002] With the rapid development of building-integrated photovoltaics (BIPV) and distributed energy, the integration of energy storage functionality into building structures has become a research hotspot in the field of civil engineering. Supercapacitors, with their advantages of high power density, long cycle life, and fast charge / discharge rates, are well-suited for integration with building structures to achieve structural and energy storage integration. Cement-based materials, as the most widely used building materials, possess characteristics such as low cost, good durability, and excellent mechanical properties. Ion transport channels can be constructed through pore control and electrolyte impregnation, and combined with built-in electrodes, cement-based supercapacitors can be fabricated, possessing both load-bearing and energy storage functions.

[0003] In recent years, researchers have conducted extensive research in the field of cement-based supercapacitors. However, existing cement-based supercapacitors still suffer from two major problems: First, it is difficult to coordinate pore structure and mechanical properties. Increasing porosity through gas entrainment often leads to a significant decrease in the compressive strength of the matrix, failing to meet structural load-bearing requirements. Second, the poor connectivity of pores within the cement matrix results in insufficient electrolyte wetting under normal pressure, leading to high interfacial charge transfer impedance, which in turn causes low specific capacitance and poor cycle stability. Single modification methods cannot simultaneously achieve pore structure optimization, mechanical property assurance, and electrochemical performance improvement, thus limiting the engineering application of cement-based supercapacitors. Summary of the Invention

[0004] To address the technical problems of existing cement-based supercapacitors, such as difficulty in achieving synergistic mechanical and electrical properties, insufficient electrolyte wetting, and poor cycle stability, this invention provides a polyvinyl alcohol-triterpenoid saponin synergistic modification fly ash cement-based supercapacitor and its preparation method. The invention utilizes triterpenoid saponins to induce air flow and construct continuously connected ion transport channels, while polyvinyl alcohol toughens and strengthens the pore walls to compensate for the strength loss caused by air induction. The fly ash micro-aggregate effect refines the pore size distribution, and a vacuum negative pressure impregnation process achieves deep saturation wetting of the pores by the electrolyte, effectively reducing interfacial charge transfer resistance. This results in a synergistic improvement in both electrochemical energy storage performance and structural mechanical properties.

[0005] The technical solution of this invention is as follows: In a first aspect, the present invention provides a polyvinyl alcohol-triterpenoid saponin synergistic modified fly ash cement-based supercapacitor, comprising an electrode layer and a cement-based functional layer disposed between the electrode layers; the raw materials of the cement-based functional layer include cement, fly ash, polyvinyl alcohol, triterpenoid saponin air-entraining agent, water-reducing agent, and water; the water-cement ratio of the cement-based functional layer is 0.35~0.45, the amount of fly ash is 10%~20% of the cement mass, the amount of polyvinyl alcohol is 1.0%~3.0% of the cement mass, the amount of triterpenoid saponin air-entraining agent is 0.04%~0.12% of the cement mass, and the amount of water-reducing agent is 0.05%~0.15% of the cement mass.

[0006] This invention uses silicate cement with fly ash as the cementitious system. The fly ash leverages its micro-aggregate effect and pozzolanic activity to refine the matrix pore size distribution and improve pore wall density. Triterpenoid saponins are used as air-entraining agents to introduce uniform and stable micron-sized bubbles, constructing a continuous and interconnected pore network that provides channels for electrolyte storage and ion migration. Polyvinyl alcohol is used as a polymer toughening component, forming a flexible polymer film within the cement hydration products. This film bridges microcracks and strengthens the pore wall structure, while also synergizing with triterpenoid saponins to stabilize bubble morphology and inhibit the formation of harmful macropores. This ensures pore connectivity while compensating for strength loss caused by air entrainment. The synergistic effect of these components achieves precise control of the pore structure and simultaneous improvement of mechanical and electrical properties.

[0007] Furthermore, the mass ratio of cement to fly ash is 20:3, the water-cement ratio is 0.4, the polyvinyl alcohol content is 2.0% of the cement mass, the triterpenoid saponin air-entraining agent content is 0.08% of the cement mass, and the water-reducing agent content is 0.1% of the cement mass. Under this ratio, the matrix pore structure is optimal, and the mechanical and electrochemical properties achieve the best balance.

[0008] Furthermore, the electrode layer is an electrode with a nickel foam-supported activated carbon slurry coating; the raw materials for the activated carbon slurry coating include activated carbon, conductive carbon black, polyvinylidene fluoride (PVDF), and N-methylpyrrolidone solvent. The three-dimensional porous structure of the nickel foam reduces contact resistance, activated carbon provides high specific surface area double-layer energy storage sites, conductive carbon black constructs an electronic conductivity network, and PVDF acts as a binder to ensure the stability of the electrode structure.

[0009] Furthermore, the mass ratio of activated carbon, conductive carbon black, and polyvinylidene fluoride is 7:2:1.

[0010] Furthermore, the thickness of the activated carbon slurry coating is 100~200μm; the coating area of ​​the activated carbon slurry layer is 1cm². 2 .

[0011] Secondly, the present invention provides a method for preparing the above-mentioned cement-based supercapacitor, comprising the following steps: (1) Electrode preparation: The nickel foam was cut and ultrasonically cleaned with ethanol and deionized water and then dried; activated carbon, conductive carbon black, polyvinylidene fluoride and N-methylpyrrolidone were mixed to prepare activated carbon slurry, which was coated on the surface of the nickel foam and vacuum dried to obtain the electrode with activated carbon slurry coating on nickel foam. (2) Preparation of polyvinyl alcohol solution: Add polyvinyl alcohol to deionized water, place it in a magnetic stirrer, stir at 100℃ and 2500r / min until completely dissolved, cool to room temperature and set aside; (3) Preparation of triterpenoid saponin gas-entraining agent dilution: Add the triterpenoid saponin gas-entraining agent to deionized water and stir until completely dissolved, then set aside. (4) Preparation of cement-based slurry: Weigh various raw materials according to the proportion. First, mix cement, fly ash and water-reducing agent and dry mix evenly to obtain dry material. Mix polyvinyl alcohol solution cooled to room temperature with the remaining water evenly and pour it into dry material. After slow stirring, switch to fast stirring. Slowly drip the triterpenoid saponin air-entraining agent dilution into the slurry and continue stirring until evenly mixed to obtain cement-based slurry. (5) Molding and curing: Cement-based slurry is poured into the mold. Half of the slurry is poured in first, then the electrode is inserted and fixed in position. The remaining slurry is then poured in. After vibration molding, the mold is left to stand at room temperature. After demolding, the mold is transferred to a standard curing box for curing to obtain cement-based matrix components. (6) Vacuum impregnation of electrolyte: The cured cement-based matrix component is immersed in potassium hydroxide solution and placed in a vacuum environment for negative pressure impregnation. After impregnation, it is taken out and the excess electrolyte on the surface is wiped off to obtain a cement-based supercapacitor.

[0012] In the above preparation method, polyvinyl alcohol is pre-dissolved at high temperature and high speed to ensure complete dispersion of the polymer without agglomeration; the air-entraining agent is introduced by slow dripping and rapid stirring to form uniform micro-bubbles and avoid the generation of large bubbles; the layered casting method of the electrode ensures accurate electrode position and tight bonding with the substrate; the vacuum impregnation process displaces air in the pores by negative pressure to achieve deep wetting of the electrolyte and significantly improve ion transport efficiency.

[0013] Furthermore, in step (4), the dry mixing time is 1~2 min; the slow mixing speed is 60 r / min; the time is 90 s; the fast mixing speed is 120 r / min; the time is 90 s.

[0014] Furthermore, in step (4), the dropping rate of the triterpenoid saponin gas-entraining agent dilution is 0.5~1mL / s, and after the dropping is completed, the mixture is stirred at a speed of 120r / min for 1~2min to ensure that the bubbles are uniformly dispersed and have stable size.

[0015] Furthermore, in step (5), vibration molding is performed using a 50Hz vibration table. After the air bubbles are expelled, the surface is naturally vibrated for 2-3 minutes. The electrode insertion position is fixed by an insulating partition. The static time is 24 hours, and the curing time is 3-28 days. This ensures that the substrate is dense and the electrode position does not shift.

[0016] Furthermore, in step (6), the molar concentration of the potassium hydroxide solution is 6 mol / L.

[0017] Furthermore, in step (6), the specific conditions for negative pressure impregnation are as follows: the vacuum degree is -0.09~-0.1MPa, first evacuate for 60 minutes to remove air from the pores, then maintain the vacuum state for impregnation for 24 hours, and the impregnation temperature is 20~25℃. This ensures that the electrolyte fully fills the internal pores. The internal pores of the cement-based functional layer are filled with potassium hydroxide electrolyte through vacuum impregnation, and the electrolyte pore filling rate is ≥90%; the high-concentration alkaline electrolyte provides sufficient ion carriers, and the vacuum negative pressure impregnation can completely remove air from the pores, achieving deep wetting of the pores by the electrolyte and significantly reducing the interfacial charge transfer resistance.

[0018] The beneficial effects of this invention are as follows: (1) This invention overcomes the contradiction between increased porosity and decreased mechanical strength through the synergistic effect of polyvinyl alcohol toughening and triterpenoid saponin air induction. Triterpenoid saponins introduce uniform micropores to construct ion transport channels, while polyvinyl alcohol strengthens the pore walls and bridges microcracks, and the micro-aggregate effect of fly ash refines the pore size. Test results show that the 28-day compressive strength of the composite system is about 22% higher than that of the single-component triterpenoid saponin system, reaching 65.2 MPa; the areal capacitance can reach 840 mF / cm². 2 Compared to the control group, it improved by 147%; the areal energy density was 116 μWh / cm². 2 After 10,000 charge-discharge cycles, the capacity retention rate is still ≥80%, achieving synergistic optimization of mechanical load-bearing capacity and electrochemical energy storage.

[0019] (2) This invention uses negative pressure vacuum impregnation with 6 mol / L potassium hydroxide electrolyte, which effectively removes air from the pores inside the cement matrix. The electrolyte pore filling rate can reach more than 90%, which greatly reduces the charge transfer impedance at the electrode-matrix interface. Compared with atmospheric pressure impregnation, the specific capacitance is increased by more than 35%, the electrochemical impedance is significantly reduced, and the rate performance and cycle stability are greatly improved.

[0020] (3) The preparation process of this invention is highly compatible with the traditional cement paste construction process. The electrode is cast in situ and formed without the need for additional diaphragms and complex assembly processes. Fly ash partially replaces cement, realizing the resource utilization of industrial solid waste. The low dosage and wide availability of polyvinyl alcohol and triterpenoid saponins are beneficial to reducing material costs and are suitable for large-scale engineering applications. Attached Figure Description

[0021] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0022] Figure 1 These are constant current charge-discharge (GCD) curves of Embodiment 1 and Comparative Examples 1-3 of the present invention.

[0023] Figure 2 This is a cyclic voltammetry (CV) curve of Comparative Example 1 of the present invention at different scan rates.

[0024] Figure 3 This is a cyclic voltammetry (CV) curve of Comparative Example 2 of the present invention at different scan rates.

[0025] Figure 4 This is a cyclic voltammetry (CV) curve of Comparative Example 3 of the present invention at different scan rates.

[0026] Figure 5 This is a cyclic voltammetry (CV) curve at different scan rates for Embodiment 1 of the present invention.

[0027] Figure 6 The Nyquist plots of electrochemical impedance spectroscopy (EIS) for Example 1 and Comparative Examples 1-3 of this invention are shown.

[0028] Figure 7 The graphs show the capacity retention rates of Embodiment 1 and Comparative Examples 1-3 after 10,000 charge-discharge cycles.

[0029] Figure 8 This is a comparison diagram of the compressive strength of Example 1 and Comparative Examples 1-3 of the present invention at different curing ages. Detailed Implementation

[0030] To enable those skilled in the art to better understand the technical solutions of this invention, the technical solutions of the embodiments of this invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this invention, and not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of this invention.

[0031] I. Implementation Examples Example 1 A method for preparing a polyvinyl alcohol-triterpenoid saponin synergistic modified fly ash cement-based supercapacitor includes the following steps: (1) Electrode preparation: The nickel foam was cut into 20mm×45mm pieces, ultrasonically cleaned with anhydrous ethanol and deionized water for 15min each, and vacuum dried at 60℃ for 12h; activated carbon, conductive carbon black and polyvinylidene fluoride were weighed in a mass ratio of 7:2:1, and an appropriate amount of N-methylpyrrolidone solvent was added. The mixture was magnetically stirred for 2h to prepare a uniform slurry; the slurry was coated on the surface of the nickel foam, and the effective coating area was controlled to be 1cm². 2 An electrode with a nickel foam-supported activated carbon coating was prepared by vacuum drying at 60°C for 24 hours with a coating thickness of approximately 150 μm.

[0032] (2) Preparation of polyvinyl alcohol solution: Add 9g of polyvinyl alcohol (the mass of polyvinyl alcohol is 2% of the mass of cement) to deionized water, stir magnetically at 100℃ and 2500r / min until completely dissolved, and cool to room temperature.

[0033] (3) Preparation of diluent for air-entraining agent: Dissolve 0.36g of triterpenoid saponin air-entraining agent in 20g of deionized water and stir evenly. The amount of triterpenoid saponin air-entraining agent is 0.08% of the cement mass.

[0034] (4) Preparation of cement-based slurry: Weigh 450g of silicate cement (P·O 52.5) ​​and 67.5g of fly ash according to a cement-to-fly ash mass ratio of 20:3. Add 0.45g of water-reducing agent (0.1% of cement mass) and dry mix in a cement paste mixer for 2 minutes until uniform to obtain dry material. Mix the cooled polyvinyl alcohol solution with the remaining water evenly and pour it into the dry material. Stir slowly at 60r / min for 90s. Then switch to 120r / min for rapid stirring. Use a dropper to slowly drip the diluted triterpenoid saponin air-entraining agent into the slurry at a rate of 0.5~1mL / s. After the dripping is complete, continue stirring at 120r / min for 2 minutes to obtain cement-based slurry. The water-cement ratio in the system is 0.4.

[0035] (5) Casting and curing: First, inject half of the cement-based slurry into a 30mm×30mm×30mm steel mold, then insert two prepared nickel-foamed activated carbon-coated electrodes in parallel with a spacing of 2mm, and fix their positions with an insulating partition; then inject the remaining slurry until it is flush with the mold. Place it on a 50Hz vibrating table and vibrate for 2 minutes; after standing at room temperature for 24 hours, demold it and place it in a standard curing box with a temperature of 20±2℃ and a relative humidity of ≥95% for curing for 3 days, 7 days and 28 days respectively.

[0036] (6) Vacuum impregnation electrolyte: Prepare a 6mol / L KOH solution, completely immerse the electrode test block that has been cured for 28 days in the electrolyte, place it in a vacuum drying oven, evacuate to -0.095MPa and maintain for 20min, and keep it in a vacuum state for 24h; after taking it out, wipe off the excess electrolyte on the surface to obtain the polyvinyl alcohol-triterpenoid saponin synergistic modified fly ash cement-based supercapacitor.

[0037] Example 2 A method for preparing a polyvinyl alcohol-triterpenoid saponin synergistic modified fly ash cement-based supercapacitor includes the following steps: (1) Electrode preparation: The nickel foam was cut into 20mm×45mm pieces, ultrasonically cleaned with anhydrous ethanol and deionized water for 15min each, and vacuum dried at 60℃ for 12h; activated carbon, conductive carbon black and polyvinylidene fluoride were weighed in a mass ratio of 7:2:1, and an appropriate amount of N-methylpyrrolidone solvent was added. The mixture was magnetically stirred for 2h to prepare a uniform slurry; the slurry was coated on the surface of the nickel foam, and the effective coating area was controlled to be 1cm². 2 An electrode with a nickel foam-supported activated carbon coating was prepared by vacuum drying at 60°C for 24 hours with a coating thickness of approximately 150 μm.

[0038] (2) Preparation of polyvinyl alcohol solution: Add 13.5g of polyvinyl alcohol (the mass of polyvinyl alcohol is 3% of the mass of cement) to deionized water, stir magnetically at 100℃ and 2500r / min until completely dissolved, and cool to room temperature.

[0039] (3) Preparation of diluent for air-entraining agent: Dissolve 0.36g of triterpenoid saponin air-entraining agent in 20g of deionized water and stir evenly. The amount of triterpenoid saponin air-entraining agent is 0.08% of the cement mass.

[0040] (4) Preparation of cement-based slurry: Weigh 450g of silicate cement (P·O 52.5) ​​and 67.5g of fly ash according to a cement-to-fly ash mass ratio of 20:3. Add 0.45g of water-reducing agent (0.1% of cement mass) and dry mix in a paste mixer for 2 minutes until uniform to obtain dry material. Mix the cooled polyvinyl alcohol solution with the remaining water evenly and pour it into the dry material. Stir slowly at 60r / min for 90s. Then switch to 120r / min for rapid stirring. Use a dropper to slowly drip the diluted triterpenoid saponin air-entraining agent into the slurry at a rate of 0.5~1mL / s. After the dripping is complete, continue to stir rapidly at 120r / min for 2 minutes to obtain cement-based slurry. The water-cement ratio in the system is 0.4.

[0041] (5) Casting and curing: First, inject half of the cement-based slurry into a 30mm×30mm×30mm steel mold, then insert two prepared nickel-foamed activated carbon-coated electrodes in parallel with a spacing of 2mm, and fix their positions with an insulating partition; then inject the remaining slurry until it is flush with the mold. Place it on a 50Hz vibrating table and vibrate for 2 minutes; after standing at room temperature for 24 hours, demold it and place it in a standard curing box with a temperature of 20±2℃ and a relative humidity of ≥95% for curing for 3 days, 7 days and 28 days respectively.

[0042] (6) Vacuum impregnation electrolyte: Prepare a 6mol / L KOH solution, completely immerse the electrode test block that has been cured for 28 days in the electrolyte, place it in a vacuum drying oven, evacuate to -0.095MPa and maintain for 20min, and keep it in a vacuum state for 24h; after taking it out, wipe off the excess electrolyte on the surface to obtain the polyvinyl alcohol-triterpenoid saponin synergistic modified fly ash cement-based supercapacitor.

[0043] Example 3 A method for preparing a polyvinyl alcohol-triterpenoid saponin synergistic modified fly ash cement-based supercapacitor includes the following steps: (1) Electrode preparation: The nickel foam was cut into 20mm×45mm pieces, ultrasonically cleaned with anhydrous ethanol and deionized water for 15min each, and vacuum dried at 60℃ for 12h; activated carbon, conductive carbon black and polyvinylidene fluoride were weighed in a mass ratio of 7:2:1, and an appropriate amount of N-methylpyrrolidone solvent was added. The mixture was magnetically stirred for 2h to prepare a uniform slurry; the slurry was coated on the surface of the nickel foam, and the effective coating area was controlled to be 1cm². 2 The coating thickness was approximately 150 μm, and the electrode was vacuum dried at 60 °C for 24 h to obtain a nickel foam-supported activated carbon coating.

[0044] (2) Preparation of polyvinyl alcohol solution: Add 9g of polyvinyl alcohol (the mass of polyvinyl alcohol is 2% of the mass of cement) to deionized water, stir magnetically at 100℃ and 2500r / min until completely dissolved, and cool to room temperature.

[0045] (3) Preparation of diluent for air-entraining agent: Dissolve 0.54g of triterpenoid saponin air-entraining agent in 20g of deionized water and stir evenly. The amount of triterpenoid saponin air-entraining agent is 0.12% of the cement mass.

[0046] (4) Preparation of cement-based slurry: Weigh 450g of silicate cement (P·O 52.5) ​​and 67.5g of fly ash according to a cement-to-fly ash mass ratio of 20:3. Add 0.45g of water-reducing agent (0.1% of cement mass) and dry mix in a cement paste mixer for 2 minutes until uniform to obtain dry material. Mix the cooled polyvinyl alcohol solution with the remaining water evenly and pour it into the dry material. Stir slowly at 60r / min for 90s. Then switch to 120r / min for rapid stirring. Use a dropper to slowly drip the diluted triterpenoid saponin air-entraining agent into the slurry at a rate of 0.5~1mL / s. After the dripping is complete, continue to stir rapidly at 120r / min for 2 minutes to obtain cement-based slurry. The water-cement ratio in the system is 0.4.

[0047] (5) Casting and curing: First, inject half of the cement-based slurry into a 30mm×30mm×30mm steel mold, then insert two prepared nickel-foamed activated carbon-coated electrodes in parallel with a spacing of 2mm, and fix their positions with an insulating partition; then inject the remaining slurry until it is flush with the mold. Place it on a 50Hz vibrating table and vibrate for 2 minutes; after standing at room temperature for 24 hours, demold it and place it in a standard curing box with a temperature of 20±2℃ and a relative humidity of ≥95% for curing for 3 days, 7 days and 28 days respectively.

[0048] (6) Vacuum impregnation electrolyte: Prepare a 6mol / L KOH solution, completely immerse the electrode test block that has been cured for 28 days in the electrolyte, place it in a vacuum drying oven, evacuate to -0.095MPa and maintain for 20min, and keep it in a vacuum state for 24h; after taking it out, wipe off the excess electrolyte on the surface to obtain the polyvinyl alcohol-triterpenoid saponin synergistic modified fly ash cement-based supercapacitor.

[0049] II. Comparative Example Comparative Example 1 Comparative Example 1 is the same as Example 1, except that 9g of polyvinyl alcohol (2% of cement mass) and 0.36g of triterpenoid saponin air-entraining agent (0.08% of cement mass) are not added in the preparation of cement-based slurry.

[0050] The specific preparation steps are as follows: (1) Electrode preparation: The nickel foam was cut into 20mm×45mm pieces, ultrasonically cleaned with anhydrous ethanol and deionized water for 15min each, and vacuum dried at 60℃ for 12h; activated carbon, conductive carbon black and polyvinylidene fluoride were weighed in a mass ratio of 7:2:1, and an appropriate amount of N-methylpyrrolidone solvent was added. The mixture was magnetically stirred for 2h to prepare a uniform slurry; the slurry was coated on the surface of the nickel foam, and the effective coating area was controlled to be 1cm². 2 The coating thickness was approximately 150 μm, and the electrode was vacuum dried at 60 °C for 24 h to obtain a nickel foam-supported activated carbon coating.

[0051] (2) Preparation of cement-based slurry: Weigh 450g of silicate cement (P·O 52.5) ​​and 67.5g of fly ash according to the mass ratio of cement to fly ash of 20:3, add 0.45g of water-reducing agent of 0.1% of cement mass, put them into a neat slurry mixer and dry mix for 2min until uniform; add 207g of deionized water according to the water-binder ratio of 0.4, stir slowly for 90s and then stir quickly for 2min to obtain cement-based slurry.

[0052] (3) Casting and curing: First, inject half of the cement-based slurry into a 30mm×30mm×30mm steel mold, then insert two prepared nickel-foamed activated carbon-coated electrodes in parallel with a spacing of 2mm, and fix their positions with an insulating partition; then inject the remaining slurry until it is flush with the mold. Place it on a 50Hz vibrating table and vibrate for 2 minutes; after standing at room temperature for 24 hours, demold it and place it in a standard curing box with a temperature of 20±2℃ and a relative humidity of ≥95% for curing for 3 days, 7 days and 28 days respectively.

[0053] (4) Vacuum impregnation electrolyte: Prepare a 6mol / L KOH solution, completely immerse the electrode test block that has been cured for 28 days in the electrolyte, place it in a vacuum drying oven, evacuate to -0.095MPa and maintain for 20min, and keep it in a vacuum state for 24h; after taking it out, wipe off the excess electrolyte on the surface to obtain the polyvinyl alcohol-triterpenoid saponin synergistic modified fly ash cement-based supercapacitor.

[0054] Comparative Example 2 Comparative Example 2 is the same as Example 1, except that in the cement-based slurry preparation step, 0.36g of triterpenoid saponin air-entraining agent (0.08% of cement mass) was added, and 9g of polyvinyl alcohol (2% of cement mass) was not added.

[0055] The specific preparation steps are as follows: (1) Electrode preparation: The nickel foam was cut into 20mm×45mm pieces, ultrasonically cleaned with anhydrous ethanol and deionized water for 15min each, and vacuum dried at 60℃ for 12h; activated carbon, conductive carbon black and polyvinylidene fluoride were weighed in a mass ratio of 7:2:1, and an appropriate amount of N-methylpyrrolidone solvent was added. The mixture was magnetically stirred for 2h to prepare a uniform slurry; the slurry was coated on the surface of the nickel foam, and the effective coating area was controlled to be 1cm². 2 The coating thickness was approximately 150 μm, and the electrode was vacuum dried at 60 °C for 24 h to obtain a nickel foam-supported activated carbon coating.

[0056] (2) Preparation of polyvinyl alcohol solution: Add 9g of polyvinyl alcohol (the mass of polyvinyl alcohol is 2% of the mass of cement) to deionized water, stir magnetically at 100℃ and 2500r / min until completely dissolved, and cool to room temperature.

[0057] (3) Preparation of air-entraining agent dilution: Dissolve 0.36g of triterpenoid saponin air-entraining agent in a portion of deionized water and stir evenly. The amount of triterpenoid saponin air-entraining agent is 0.08% of the cement mass.

[0058] (4) Preparation of cement-based slurry: Weigh 450g of silicate cement (P·O 52.5) ​​and 67.5g of fly ash according to the mass ratio of cement to fly ash of 20:3. Add 0.45g of water-reducing agent (0.1% of cement mass) and put it into a paste mixer and dry mix for 2min until uniform to obtain dry material. Use a dropper to slowly drip the diluted triterpenoid saponin air-entraining agent into the slurry at a rate of 0.5mL / s. After the dripping is completed, continue to stir at a speed of 120r / min for 2min to obtain cement-based slurry.

[0059] (5) Casting and curing: First, inject half of the cement-based slurry into a 30mm×30mm×30mm steel mold, then insert two prepared nickel-foamed activated carbon-coated electrodes in parallel with a spacing of 2mm, and fix their positions with an insulating partition; then inject the remaining slurry until it is flush with the mold. Place it on a 50Hz vibrating table and vibrate for 2 minutes; after standing at room temperature for 24 hours, demold it and place it in a standard curing box with a temperature of 20±2℃ and a relative humidity of ≥95% for curing for 3 days, 7 days and 28 days respectively.

[0060] (6) Vacuum impregnation electrolyte: Prepare a 6 mol / L KOH solution, completely immerse the electrode test block that has been cured for 28 days in the electrolyte, place it in a vacuum drying oven, evacuate to -0.095 MPa and maintain for 20 min, and keep it in a vacuum state for 24 h; after taking it out, wipe off the excess electrolyte on the surface to obtain the polyvinyl alcohol-triterpenoid saponin synergistic modified fly ash cement-based supercapacitor.

[0061] Comparative Example 3 Comparative Example 3 is the same as Example 1, except that in the cement-based slurry preparation step, 9g of polyvinyl alcohol (2% of the cement mass) is added, but 0.36g of triterpenoid saponin air-entraining agent (0.08% of the cement mass) is not added.

[0062] The specific preparation steps are as follows: (1) Electrode preparation: The nickel foam was cut into 20mm×45mm pieces, ultrasonically cleaned with anhydrous ethanol and deionized water for 15min each, and vacuum dried at 60℃ for 12h; activated carbon, conductive carbon black and polyvinylidene fluoride were weighed in a mass ratio of 7:2:1, and an appropriate amount of N-methylpyrrolidone solvent was added. The mixture was magnetically stirred for 2h to prepare a uniform slurry; the slurry was coated on the surface of the nickel foam, and the effective coating area was controlled to be 1cm². 2 The coating thickness was approximately 150 μm, and the electrode was vacuum dried at 60 °C for 24 h to obtain a nickel foam-supported activated carbon coating.

[0063] (2) Preparation of polyvinyl alcohol solution: Add 9g of polyvinyl alcohol (the mass of polyvinyl alcohol is 2% of the mass of cement) to deionized water, stir magnetically at 100℃ and 2500r / min until completely dissolved, and cool to room temperature.

[0064] (3) Preparation of air-entraining agent dilution: Dissolve 0.36g of triterpenoid saponin air-entraining agent in a portion of deionized water and stir evenly. The amount of triterpenoid saponin air-entraining agent is 0.08% of the cement mass.

[0065] (4) Preparation of cement-based slurry: Weigh 450g of silicate cement (P·O 52.5) ​​and 67.5g of fly ash according to the mass ratio of cement to fly ash of 20:3. Add 0.45g of water-reducing agent of 0.1% of cement mass and put it into a paste mixer and dry mix for 2min until uniform to obtain dry material. Mix the polyvinyl alcohol solution cooled to room temperature with the remaining water evenly and pour it into the dry material. Stir slowly at a speed of 60r / min for 90s, and then stir quickly for 2min to obtain cement-based slurry.

[0066] (5) Casting and curing: First, inject half of the cement-based slurry into a 30mm×30mm×30mm steel mold, then insert two prepared nickel-foamed activated carbon-coated electrodes in parallel with a spacing of 2mm, and fix their positions with an insulating partition; then inject the remaining slurry until it is flush with the mold. Place it on a 50Hz vibrating table and vibrate for 2 minutes; after standing at room temperature for 24 hours, demold it and place it in a standard curing box with a temperature of 20±2℃ and a relative humidity of ≥95% for curing for 3 days, 7 days and 28 days respectively.

[0067] (6) Vacuum impregnation electrolyte: Prepare a 6mol / L KOH solution, completely immerse the electrode test block that has been cured for 28 days in the electrolyte, place it in a vacuum drying oven, evacuate to -0.095MPa and maintain for 20min, and keep it in a vacuum state for 24h; after taking it out, wipe off the excess electrolyte on the surface to obtain the polyvinyl alcohol-triterpenoid saponin synergistic modified fly ash cement-based supercapacitor.

[0068] III. Test Examples 1. The prepared cement-based capacitors were subjected to constant current charge-discharge and cyclic voltammetry tests using an electrochemical workstation (instrument model: CHI660E). A two-electrode system was used, and the samples prepared in Example 1 and Comparative Examples 1-3 of this invention were subjected to constant current charge-discharge tests at a voltage window of 0-1V and a current density of 1A / g. The results are as follows: Figure 1 As shown.

[0069] Depend on Figure 1It can be seen that Example 1 has the longest discharge time, indicating that it has the highest specific capacitance; Comparative Example 1 has the shortest discharge time, and the discharge times of Comparative Example 2 and Comparative Example 3 are progressively longer. Calculations show that the specific capacitance of Example 1 is 105% higher than that of Comparative Example 1, 46% higher than that of Comparative Example 2, and 5% higher than that of Comparative Example 3, indicating that the co-doping of polyvinyl alcohol and triterpenoid saponins can effectively improve the energy storage capacity.

[0070] Cyclic voltammetry tests were performed within a voltage window of 0–0.6 V at scan rates of 10, 20, 30, 50, and 100 mV / s. The test results for Example 1 and Comparative Examples 1–3 are as follows: Figures 2-5 As shown in the figure; the test results show that the CV curves of each group of samples exhibit a rectangular characteristic, demonstrating typical double-layer energy storage behavior; as the scan rate increases, the curves still maintain good symmetry, indicating good reversibility of the electrode reaction. At the same scan rate, Example 1 has the largest response current, indicating that it has the fastest ion transport rate and the best capacitance characteristics.

[0071] 2. The electrochemical performance of the samples was tested using an electrochemical workstation (instrument model: CHI660E). The test frequency range was 10 Hz at open-circuit voltage. -2 ~10 5 Hz, AC amplitude 5mV, test results as follows Figure 6 As shown.

[0072] Depend on Figure 6 The Nyquist plot shows that the semicircle diameter in the high-frequency region represents the charge transfer resistance, while the slope of the straight line in the low-frequency region represents the ion diffusion rate. Example 1 has the smallest semicircle diameter and the largest slope in the low-frequency region, indicating that the multi-doped system has the lowest charge transfer resistance and the fastest ion diffusion within the pores. Comparative Example 1 has the largest semicircle diameter, while Comparative Example 2 and Comparative Example 3 show progressively smaller diameters.

[0073] Capacity retention was tested by performing 10,000 constant current charge-discharge cycles at a current density of 1 A / g, and the results are as follows: Figure 7 As shown.

[0074] Depend on Figure 7 It can be seen that Comparative Example 1 exhibited the fastest capacity decay, with a capacity retention of only about 40% after 10,000 cycles. The cycling stability of Comparative Examples 2 and 3 improved sequentially. Example 1 demonstrated the best cycling stability, with a capacity retention of over 82% after 10,000 cycles, more than double that of Comparative Example 1. This is because the sample prepared in Example 1 possessed a uniform pore structure, sufficient electrolyte wetting, and the reinforcing effect of polyvinyl alcohol on the pore walls, effectively suppressing structural degradation and performance decay during cycling.

[0075] 3. Referring to the "Test Method for Strength of Cement Mortar (ISO Method)" (GB / T 17671-1999), the compressive strength of electrodeless specimens at 3 days, 7 days, and 28 days of age was tested, and the results are as follows: Figure 8 As shown.

[0076] Depend on Figure 8 It can be seen that Comparative Example 1 has the highest compressive strength, reaching over 72 MPa after 28 days; Comparative Example 2, which is doped with triterpenoid saponins, shows a significant decrease in strength, reaching approximately 56 MPa after 28 days; Comparative Example 3, which is doped with polyvinyl alcohol, shows a slight decrease in strength, reaching approximately 68 MPa after 28 days; The compressive strength of Example 1 after 28 days is approximately 65 MPa, which is about 16% higher than that of Comparative Example 2, indicating that polyvinyl alcohol can effectively compensate for the strength loss caused by air entrainment and achieve a balance between porosity and mechanical properties.

[0077] 4. Referring to the "Test Methods for Volume Resistivity and Surface Resistivity of Solid Insulating Materials" (GB / T 1410-2006), and using an electrochemical workstation (instrument model: CHI660E), the electrical performance of the cement-based capacitors prepared in Examples 1-3 and Comparative Examples 1-3 was tested. The test items included volume resistivity, specific capacitance, energy density, and capacity retention rate after 10,000 charge-discharge cycles. The test results are shown in Table 1 below.

[0078] Table 1 - Electrical properties of samples prepared in Examples 1-3 and Comparative Examples 1-3

[0079] Although the present invention has been described in detail with reference to the accompanying drawings and preferred embodiments, the present invention is not limited thereto. Various equivalent modifications or substitutions can be made to the embodiments of the present invention by those skilled in the art without departing from the spirit and essence of the invention, and such modifications or substitutions should all be within the scope of the present invention. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should also be covered within the protection scope of the present invention.

Claims

1. A polyvinyl alcohol-triterpenoid saponin synergistic modification fly ash cement-based supercapacitor, characterized in that, The device includes an electrode layer and a cement-based functional layer disposed between the electrode layers. The raw materials of the cement-based functional layer include cement, fly ash, polyvinyl alcohol, triterpenoid saponin air-entraining agent, water-reducing agent, and water. The water-cement ratio of the cement-based functional layer is 0.35~0.45, the amount of fly ash is 10%~20% of the cement mass, the amount of polyvinyl alcohol is 1.0%~3.0% of the cement mass, the amount of triterpenoid saponin air-entraining agent is 0.04%~0.12% of the cement mass, and the amount of water-reducing agent is 0.05%~0.15% of the cement mass. The internal pores of the cement-based functional layer are filled with 6 mol / L potassium hydroxide electrolyte through vacuum impregnation.

2. The polyvinyl alcohol-triterpenoid saponin synergistic modification fly ash cement-based supercapacitor as described in claim 1, characterized in that, The electrode layer is an electrode coated with nickel foam-supported activated carbon slurry; the raw materials for the activated carbon slurry coating include activated carbon, conductive carbon black, polyvinylidene fluoride, and N-methylpyrrolidone solvent.

3. The polyvinyl alcohol-triterpenoid saponin synergistic modification fly ash cement-based supercapacitor as described in claim 2, characterized in that, The mass ratio of activated carbon, conductive carbon black and polyvinylidene fluoride is 7:2:

1.

4. The polyvinyl alcohol-triterpenoid saponin synergistic modification fly ash cement-based supercapacitor as described in claim 2, characterized in that, The thickness of the activated carbon slurry coating is 100~200μm; the coating area of ​​the activated carbon slurry coating is 1cm². 2 .

5. A method for preparing a polyvinyl alcohol-triterpenoid saponin synergistic modified fly ash cement-based supercapacitor as described in any one of claims 1 to 4, characterized in that, Includes the following steps: (1) Electrode preparation: The nickel foam was cut and ultrasonically cleaned with ethanol and deionized water and then dried; activated carbon, conductive carbon black, polyvinylidene fluoride and N-methylpyrrolidone were mixed to prepare activated carbon slurry, which was coated on the surface of the nickel foam and vacuum dried to obtain the electrode with activated carbon slurry coating on nickel foam. (2) Preparation of polyvinyl alcohol solution: Add polyvinyl alcohol to deionized water, place it in a magnetic stirrer, stir at 100℃ and 2500r / min until completely dissolved, cool to room temperature and set aside; (3) Preparation of triterpenoid saponin gas-entraining agent dilution: Add the triterpenoid saponin gas-entraining agent to deionized water and stir until completely dissolved, then set aside. (4) Preparation of cement-based slurry: Weigh various raw materials according to the proportion. First, mix cement, fly ash and water-reducing agent and dry mix evenly to obtain dry material. Mix polyvinyl alcohol solution cooled to room temperature with the remaining water evenly and pour it into dry material. After slow stirring, switch to fast stirring. Slowly drip the triterpenoid saponin air-entraining agent dilution into the slurry and continue stirring until evenly mixed to obtain cement-based slurry. (5) Molding and curing: Cement-based slurry is poured into the mold. Half of the slurry is poured in first, then the electrode is inserted and fixed in position. The remaining slurry is then poured in. After vibration molding, the mold is left to stand at room temperature. After demolding, the mold is transferred to a standard curing box for curing to obtain cement-based matrix components. (6) Vacuum impregnation of electrolyte: The cured cement-based matrix component is immersed in potassium hydroxide solution and placed in a vacuum environment for negative pressure impregnation. After impregnation, it is taken out and the excess electrolyte on the surface is wiped off to obtain a cement-based supercapacitor.

6. The method as described in claim 5, characterized in that, In step (4), the dry mixing time is 1~2 min; the slow mixing speed is 60 r / min; the time is 90 s; the fast mixing speed is 120 r / min; the time is 90 s.

7. The method as described in claim 5, characterized in that, In step (4), the dropping rate of the triterpenoid saponin gas-entraining agent dilution is 0.5~1mL / s, and after the dropping is completed, the mixture is stirred at a speed of 120r / min for 1~2min.

8. The method as described in claim 5, characterized in that, In step (5), a vibration table with a frequency of 50Hz is used for vibration molding. After the air bubbles are expelled, the surface is naturally vibrated for 2-3 minutes. The electrode insertion position is fixed by an insulating partition. The static time is 24 hours and the curing time is 3-28 days.

9. The method as described in claim 5, characterized in that, In step (6), the molar concentration of the potassium hydroxide solution is 6 mol / L.

10. The method as described in claim 5, characterized in that, In step (6), the specific conditions for negative pressure impregnation are: vacuum degree is -0.09~-0.1MPa, first evacuate the vacuum for 60 minutes to remove the air in the pores, then maintain the vacuum state for impregnation for 24 hours, and the impregnation temperature is 20~25℃.

Citation Information

Patent Citations

  • Waterproof anti-cracking fully-recycled aggregate foamed block based on macro-micro double-pore structure and preparation method thereof

    CN110818357A

  • Concrete admixture and preparation method therefor

    WO2024138911A1