A copper alloy for a heat exchanger of a refrigeration device, a method of production and use thereof
By controlling the content and ratio of Sn, Ni, P, Fe, Si and Mg, and employing fine grain strengthening and precipitation strengthening, the problem of balancing strength and thermal conductivity in the thin-wall process of refrigeration heat exchange copper tubes was solved, thus achieving a comprehensive improvement in the performance of copper alloys.
Patent Information
- Application Number
- CN202611459617.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-20
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2046-09-20
AI Technical Summary
In the process of thinning existing refrigeration and heat exchange copper tubes, it is difficult to balance strength, thermal conductivity and plasticity, which can easily lead to problems such as dents, corrosion and leakage. Existing alloying methods result in a decrease in thermal conductivity and plasticity.
By controlling the content and ratio of Sn, Ni, P, Fe, Si and Mg, fine grain strengthening and precipitation strengthening are used as the main methods, supplemented by a small amount of solid solution strengthening, to form a fine and dispersed second phase, refine the grains, and improve the strength and thermal conductivity of the alloy.
Under low alloying conditions, the strength, thermal conductivity, plasticity and corrosion resistance of copper alloys have been comprehensively improved, making them suitable for the thin-wall manufacturing of refrigeration equipment.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of equipment heat exchange technology, specifically relating to a copper alloy for heat exchangers in refrigeration equipment, its preparation method, and its applications. Background Technology
[0002] Refrigeration equipment heat exchangers have long been developing towards miniaturization, high efficiency, low charge volume, and lightweight design. Thinning of copper tube walls can reduce copper consumption and weight per unit product, but thinning is not simply a matter of reducing wall thickness. As tube walls become thinner, the requirements for strength, hardness, dent resistance, expansion stability, pressure resistance, and corrosion resistance during manufacturing, transportation, installation, and service simultaneously increase.
[0003] Most existing refrigeration heat exchange copper tubes are made of oxygen-free copper or TP2 phosphorus deoxidized copper. These materials have good thermal conductivity and processing plasticity, but their soft strength and surface damage resistance are limited. Under the combined effects of refrigerant pressure, thermal cycling, vibration, bending, flaring, tube expansion, and construction loads, if the wall thickness is further reduced, risks such as local dents, out-of-round cross-sections, damage to the internal thread teeth, fatigue cracks, or corrosion leaks are likely to occur.
[0004] A common method to improve the strength and corrosion resistance of copper tubes is to increase the content of alloying elements. However, high alloying mainly relies on solid solution strengthening. When the content of alloying elements is high, it can easily lead to a decrease in thermal conductivity and plasticity, which is not conducive to efficient heat exchange and complex tube processing. If low alloying still relies mainly on a small amount of solid solution strengthening, although it can maintain good thermal conductivity, the extent of solid solution strengthening is limited and it is difficult to fully support the further thinning of refrigeration heat exchange copper tubes.
[0005] Therefore, under the premise of low total alloy content, how to improve the strength of copper alloy while maintaining high thermal conductivity, good plasticity and tube processing performance, so as to provide a material basis for further thinning of refrigeration and heat exchange copper tubes, is an urgent technical problem to be solved. Summary of the Invention
[0006] To solve at least one of the above-mentioned technical problems, the present invention reduces the damage to thermal conductivity and plasticity caused by high content of solid solution elements by controlling the content and ratio of Sn, Ni, P, Fe, Si and Mg, and improves the strength of the alloy by refining the grains and precipitating fine second phases.
[0007] The technical solution adopted by this invention to solve its technical problem includes: In a first aspect, the present invention provides a copper alloy for heat exchangers in refrigeration equipment, comprising, by weight percentage: Sn: 0.15%–0.50%, Ni: 0.05%–0.10%, P: 0.005%–0.035%, Fe: 0.0003%–0.005%, Si: 0.015%–0.085%, Mg: 0.001%–0.006%, with unavoidable impurities totaling no more than 0.025%, and the balance being Cu and Ag, with the total content of Cu and Ag not less than 99.2%. The copper alloy satisfies the following proportional relationship: [Fe] / [P] = 0.2–1.0, [Ni] / [Si] = 1–8, and 100 × [Mg] / [Sn] = 0.5–5.0, where [X] represents the mass percentage of element X.
[0008] Preferably, by mass percentage, it includes: Sn: 0.28%, Ni: 0.08%, P: 0.018%, Fe: 0.004%, Si: 0.018%, Mg: 0.004%, with unavoidable impurities totaling no more than 0.025%, and the balance being Cu and Ag, with the total content of Cu and Ag being no less than 99.2%.
[0009] Preferably, the copper alloy satisfies the following proportional relationship: [Fe] / [P] = 0.2~0.35, [Ni] / [Si] = 3~6, 100×[Mg] / [Sn] = 1~3, where [X] represents the mass percentage of element X.
[0010] Preferably, Sn, Ni, P, Fe, Si and Mg are added using a copper-based master alloy.
[0011] Preferably, Sn, Ni, P, Fe, Si and Mg are added in the form of copper-tin master alloy, copper-nickel master alloy, copper-phosphorus master alloy, copper-iron master alloy, copper-silicon master alloy and copper-magnesium master alloy, respectively.
[0012] Preferably, the Fe content in the copper-iron master alloy is not higher than 4%, and the proportion of Fe existing in solid solution is not less than 90%; and / or, The Mg content in the copper-magnesium master alloy is not higher than 4.2%, and the proportion of Mg existing in solid solution is not less than 80%; and / or, The Si content in the copper-silicon master alloy is not higher than 5.3%, and the proportion of Si existing in solid solution is not less than 90%; and / or, The average grain size of the copper alloy is 0.010–0.025 mm.
[0013] Preferably, it further includes Ti, with a Ti content of 0.001% to 0.006%; and / or, It also includes Y (yttrium), with a Y content of 0.001% to 0.006%.
[0014] Secondly, the present invention provides a method for preparing the copper alloy for a heat exchanger in a refrigeration device as described above, comprising: Provide molten electrolytic copper solution; A copper-based master alloy with the corresponding components as described above is added to an electrolytic copper solution to obtain a copper alloy melt. The copper alloy is obtained through refining, degassing, and casting.
[0015] Thirdly, the present invention provides a heat exchange tube made of a copper alloy as described above for use in heat exchangers of refrigeration equipment.
[0016] Fourthly, the present invention provides a heat exchanger for a refrigeration device, including the heat exchange tubes described above.
[0017] The beneficial effects of this invention include: In this invention, Sn, Ni, P, Fe, Si, and Mg are all controlled components, and unavoidable impurities are not considered. This invention does not achieve strength by significantly increasing the total amount of alloying elements, but instead employs a low-content microalloying system. It modifies the strengthening mechanism by primarily using grain refinement and precipitation strengthening, supplemented by a controlled amount of solid solution strengthening. Through the synergistic reaction between trace elements, some elements that were originally dissolved in the copper matrix and could significantly reduce thermal conductivity are transformed into fine, dispersed second phases. Simultaneously, the influence of elements such as Fe and Mg on the solidification and recrystallization structures refines the grains. Thus, at a lower degree of alloying, the strength loss due to reduced solid solution elements is effectively compensated. Grain refinement and precipitation strengthening improve the strengthening efficiency per unit alloying element, avoiding reliance solely on increasing the content of solid solution elements, thereby achieving a synergistic improvement in both strength and thermal conductivity.
[0018] Furthermore, refining the grain size helps improve strength and maintain uniform deformation capacity. Moreover, since elements that easily reduce thermal conductivity, such as Sn, Ni, and P, are controlled within a low range, and elements such as Si, Fe, and Mg synergistically promote the formation of a second phase from some solutes, the copper alloy of this invention has good thermal conductivity, achieving a comprehensive balance of strength, thermal conductivity, plasticity, processability, and corrosion resistance. Detailed Implementation
[0019] The technical features of the embodiments of the present invention will be clearly and completely described below in conjunction with the technical solutions in the embodiments of the present invention. All embodiments are based on the core technical solutions of the present invention and are not intended to limit the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0020] To better understand the embodiments provided by the present invention, the technical content involved in the present invention will first be introduced.
[0021] In a first aspect, the present invention provides a copper alloy for heat exchangers in refrigeration equipment, comprising, by weight percentage: Sn: 0.15%–0.50%, Ni: 0.05%–0.10%, P: 0.005%–0.035%, Fe: 0.0003%–0.005%, Si: 0.015%–0.085%, Mg: 0.001%–0.006%, with unavoidable impurities totaling no more than 0.025%, and the balance being Cu and Ag, with the total content of Cu and Ag not less than 99.2%. The copper alloy satisfies the following proportional relationship: [Fe] / [P] = 0.2–1.0, [Ni] / [Si] = 1–8, and 100 × [Mg] / [Sn] = 0.5–5.0, where [X] represents the mass percentage of element X.
[0022] In this invention, Sn, Ni, P, Fe, Si, and Mg are all controlled components, and unavoidable impurities are not considered. This invention does not achieve strength by significantly increasing the total amount of alloying elements, but instead employs a low-content microalloying system. It modifies the strengthening mechanism by primarily using grain refinement and precipitation strengthening, supplemented by a controlled amount of solid solution strengthening. Through the synergistic reaction between trace elements, some elements that were originally dissolved in the copper matrix and could significantly reduce thermal conductivity are transformed into fine, dispersed second phases. Simultaneously, the influence of elements such as Fe and Mg on the solidification and recrystallization structures refines the grains. Thus, at a lower degree of alloying, the strength loss due to reduced solid solution elements is effectively compensated. Grain refinement and precipitation strengthening improve the strengthening efficiency per unit alloying element, avoiding reliance solely on increasing the content of solid solution elements, thereby achieving a synergistic improvement in both strength and thermal conductivity.
[0023] Furthermore, refining the grain size helps improve strength and maintain uniform deformation capacity. Moreover, since elements that easily reduce thermal conductivity, such as Sn, Ni, and P, are controlled within a low range, and elements such as Si, Fe, and Mg synergistically promote the formation of a second phase from some solutes, the copper alloy of this invention has good thermal conductivity, achieving a comprehensive balance of strength, thermal conductivity, plasticity, processability, and corrosion resistance.
[0024] Specifically: The copper alloy of this invention has a soft tensile strength of 235-285 MPa and a soft elongation after fracture of 45%-53%. It can pass the flattening and 35% flaring tests. In the comparative test of φ9.52 mm × 0.30 mm, the ultimate compressive strength can reach at least 16.1 MPa. Under acidic test conditions of pH 3.0-3.1, the corrosion initiation time is at least 410 h, and under pH 6.5-7.2 conditions, it exceeds 720 h. No performance loss of the copper material of this invention is shown under neutral conditions. The soft room temperature thermal conductivity can be maintained above 380 W / (m·K).
[0025] The following explains the reasons for the limitations of each component in this invention, where % represents mass.
[0026] [Sn] The Sn content is 0.15%–0.50%, for example, it can be 0.15%, 0.20%, 0.25%, 0.30%, 0.35%, 0.40%, 0.45%, or 0.50%. Sn is beneficial for improving the corrosion resistance of copper alloys and inhibiting grain coarsening, thus improving the stability of the microstructure. At the same time, Sn and Mg synergistically form a Mg-Sn nanoscale second phase, which produces a precipitation strengthening effect through dispersed distribution.
[0027] If the Sn content is too low (e.g., below 0.15%), the corrosion resistance and synergistic strengthening effect will be insufficient; if the Sn content is too high (e.g., above 0.50%), excessive Sn solution will significantly reduce thermal conductivity and increase deformation resistance, which is not conducive to the drawing and subsequent bending of the pipe. Therefore, the present invention limits the Sn content to 0.15% to 0.50%.
[0028] [Ni] The Ni content is 0.05%–0.10%, for example, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, or 0.10%. Ni can improve the corrosion resistance and microstructure stability of copper alloys, but Ni dissolved in the copper matrix increases the probability of electron scattering, which has a significant adverse effect on thermal conductivity. This invention controls the Ni content and adds an appropriate amount of Si so that some Ni exists in the form of a Ni-Si system second phase, thereby reducing the influence of free dissolved Ni on thermal conductivity. Furthermore, the dispersed distribution of the Ni-Si system second phase generates a precipitation strengthening effect, synergistically improving the strength and corrosion resistance of the alloy.
[0029] If the Ni content is too low (e.g., below 0.05%), the precipitation strengthening effect will be insufficient, making it difficult to form a sufficient number of Ni-Si second phases. If the Ni content is too high (e.g., above 0.10%), it will exceed the solid solution control range of the low alloying system of this invention, and some Ni will not be fully precipitated and will remain in the matrix, resulting in a significant decrease in thermal conductivity. Therefore, this invention limits the Ni content to 0.05% to 0.10%.
[0030] [P] The phosphorus (P) content is 0.005% to 0.035%, for example, it can be 0.005%, 0.010%, 0.015%, 0.020%, 0.025%, 0.030%, or 0.035%. P acts as a deoxidizer, helping to improve the corrosion resistance of copper alloys in specific corrosive environments. It also synergistically forms a Fe-P-rich second phase with P, exerting a dual effect of grain refinement and precipitation strengthening. If the P content is too low (e.g., below 0.005%), the deoxidation effect and corrosion resistance improvement are insufficient; if the P content is too high (e.g., above 0.035%), excessive solid solution of P will significantly increase electron scattering, leading to a significant decrease in electrical and thermal conductivity. Therefore, this invention limits the P content to 0.005% to 0.035%.
[0031] [Fe] The Fe content is 0.0003% to 0.005%, for example, it can be 0.0003%, 0.0005%, 0.0008%, 0.001%, 0.003%, 0.004%, or 0.005%. In this invention, Fe is mainly used for microstructure control. An appropriate amount of Fe is beneficial for grain refinement and synergistically forms a Fe-P-rich second phase with P, exerting a dual effect of grain refinement and precipitation strengthening.
[0032] If the Fe content is too low (e.g., below 0.0003%), the grain refinement effect and Fe-P synergistic effect will be insufficient; if the Fe content is too high (e.g., above 0.005%), it will exceed the control range of the low-content microalloying system of this invention, easily forming coarse Fe-containing particles, reducing thermal conductivity and affecting the surface quality of the pipe. Therefore, this invention limits the Fe content to 0.003% to 0.005%.
[0033] [Si] The Si content is 0.015% to 0.085%, for example, it can be 0.015%, 0.025%, 0.035%, 0.045%, 0.055%, 0.065%, 0.075%, or 0.085%. Si is mainly used to synergistically form a Ni-Si system second phase (such as Ni2Si) with Ni, playing a precipitation strengthening role. If the Si content is too low (e.g., below 0.015%), it is difficult to form a sufficient number of Ni-Si second phases with Ni, resulting in insufficient precipitation strengthening effect; if the Si content is too high (e.g., above 0.085%), the residual solid solution Si will increase electron scattering and may also form coarse second phase particles, significantly reducing thermal conductivity and plasticity, and affecting the surface quality of the pipe. Therefore, the present invention limits the Si content to 0.015% to 0.085%.
[0034] [Mg] The Mg content is 0.001% to 0.006%, for example, 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, or 0.006%. Trace amounts of Mg can influence the solidification nucleation, grain boundary state, and recrystallization behavior of copper alloys, and synergistically form a Mg-Sn second phase with Sn, playing a role in microstructure regulation and precipitation strengthening. If the Mg content is too low (e.g., below 0.001%), it is difficult to effectively regulate the solidification microstructure and recrystallization, and the amount of Mg-Sn second phase is insufficient; if the Mg content is too high (e.g., above 0.006%), due to the reactive nature of Mg, it is easily oxidized and burned off, increasing the difficulty of smelting control. Therefore, this invention limits the Mg content to 0.001% to 0.006%.
[0035] [Cu+Ag] Silver is present as an accompanying element in copper raw materials. In this invention, the total content of Cu and Ag is controlled to be no less than 99.2% in order to maintain the high thermal conductivity, plasticity and processing performance of the copper matrix.
[0036] In this scheme, the mass percentage ratio of Fe to P, [Fe] / [P], is 0.2 to 1.0, for example, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or 1.0. By controlling the Fe / P ratio within this range, some P can exist in the form of a Fe-P-rich second phase, thereby reducing the proportion of free solid-solid P in the copper matrix and mitigating its adverse effects on thermal conductivity. Simultaneously, the dispersed distribution of the Fe-P-rich second phase can exert a synergistic effect of precipitation strengthening and grain refinement, helping to compensate for the strength loss due to the reduction of solid-solid elements. If the Fe / P ratio is too low (e.g., below 0.2), the Fe content is insufficient to effectively fix P, leading to an increase in free solid-solid P and a decrease in thermal conductivity. If the Fe / P ratio is too high (e.g., above 1.0), it exceeds the solid-solidity limit of Fe in the copper matrix, and excess Fe may precipitate in the form of coarse Fe-containing particles, reducing thermal conductivity and affecting the surface quality of the pipe. Therefore, the present invention controls the Fe / P ratio to be between 0.2 and 1.0.
[0037] The mass percentage ratio of Ni to Si, [Ni] / [Si], is between 1 and 8, for example, 1, 2, 3, 4, 5, 6, 7, or 8. The [Ni] / [Si] ratio is a key synergistic parameter controlling the precipitation behavior of the second phase (such as Ni₂Si) in the Ni-Si system. By controlling the [Ni] / [Si] ratio within this range, Ni can fully combine with Si and precipitate completely, minimizing the damage to thermal conductivity caused by free Ni and residual Si. Simultaneously, the dispersed distribution of the Ni-Si second phase generates a precipitation strengthening effect, synergistically improving the alloy's strength. If the [Ni] / [Si] ratio is too low (e.g., below 1), Si becomes relatively excessive, increasing residual Si and decreasing thermal conductivity and plasticity. If the Ni / [Si] ratio is too high (e.g., above 8), Ni becomes relatively excessive, increasing free Ni, which also exacerbates electron scattering and reduces thermal conductivity. Therefore, this invention controls the [Ni] / [Si] ratio between 1 and 8.
[0038] The mass percentage ratio of 100×Mg to Sn, 100×[Mg] / [Sn], is 0.5–5.0, for example, it can be 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, or 5.0. The 100×[Mg] / [Sn] ratio is a key synergistic parameter controlling the precipitation behavior of the Mg-Sn system second phase. By controlling this ratio within the above range, trace amounts of Mg and Sn can be fully combined to form the Mg-Sn system second phase, exerting a synergistic effect of microstructure regulation and precipitation enhancement. If the 100×[Mg] / [Sn] ratio is too low (e.g., below 0.5), the Mg content is severely insufficient relative to Sn, making it difficult to form a sufficient amount of Mg-Sn second phase, thus limiting the effects of microstructure control and precipitation strengthening. If the 100×[Mg] / [Sn] ratio is too high (e.g., above 5.0), Mg is relatively excessive, exceeding the amount of Mg that Sn can bind, increasing the amount of free dissolved Mg. Simultaneously, excessively high Mg content will exacerbate oxidation loss during the smelting process, increasing the difficulty of composition control. Therefore, this invention controls the 100×[Mg] / [Sn] ratio between 0.5 and 5.0.
[0039] The three sets of ratios mentioned above correspond to the three synergistic systems of Fe-P, Ni-Si, and Mg-Sn, respectively. These ratios, while ensuring the basic functions of each element (such as corrosion resistance, structural stability, and deoxidation effect), can reduce the damage to thermal conductivity caused by excessive free solid solution elements, thereby achieving a fine, dispersed, and controllable precipitation strengthening effect.
[0040] In a preferred embodiment of the present invention, the copper alloy comprises, by weight percentage: Sn: 0.28%, Ni: 0.08%, P: 0.018%, Fe: 0.004%, Si: 0.018%, Mg: 0.004%, with unavoidable impurities totaling no more than 0.025%, and the balance being Cu and Ag, with the total content of Cu and Ag being no less than 99.2%.
[0041] In this preferred scheme, the synergistic precipitation and grain refinement of multiple elements such as Sn-Mg, Ni-Si, and Fe-P achieve significant strengthening effects while maintaining a low total alloy content. Simultaneously, the content of each element is controlled within appropriate levels within their respective ranges, avoiding excessive scattering of thermally conductive electrons and phonons by excessive solid solution atoms. Furthermore, the high-purity copper matrix with a total Cu and Ag content of not less than 99.2% further ensures unobstructed heat conduction channels. Therefore, this scheme achieves a good balance of strength, thermal conductivity, and processing performance under low alloying conditions, making it particularly suitable for the further thinning of refrigeration heat exchange copper tubes.
[0042] In a preferred embodiment of the present invention, the copper alloy satisfies the following proportional relationship: [Fe] / [P] = 0.2–0.35, [Ni] / [Si] = 3–6, 100×[Mg] / [Sn] = 1–3, where [X] represents the mass percentage of element X. Within the preferred ratio range of this invention, the three synergistic systems of Fe / P, Ni / Si, and Mg / Sn are each in their optimal matching range: Fe / P is controlled at 0.2–0.35, so that Fe is just enough to convert free solid solution P into a Fe-P rich second phase, avoiding thermal conductivity deterioration caused by excess P, and preventing excessive Fe from forming coarse particles; Ni / Si is controlled at 3–6, ensuring that Ni and Si fully precipitate as a Ni-Si system second phase (such as Ni2Si), minimizing the damage to thermal conductivity and plasticity caused by free solid solution Ni and residual solid solution Si; 100×[Mg] / [Sn] is controlled at 1–3, so that trace amounts of Mg can synergistically form a Mg-Sn system second phase with Sn at extremely low content, exerting a dual effect of microstructure refinement and precipitation strengthening. The three proportions work together to ensure that each alloying element retains its basic functions such as corrosion resistance, structural stability and deoxidation, while also contributing to the strengthening effect in the form of a second phase. This achieves a synergistic match of high strength, high thermal conductivity and excellent processing performance under the condition that the total alloy content is less than 0.5%, making it particularly suitable for the thin-wall manufacturing of refrigeration heat exchange copper tubes.
[0043] To improve the efficiency and uniformity of trace element addition, Sn, Ni, P, Fe, Si, and Mg are preferably added using copper-based master alloys. The purpose of using master alloys is to ensure that the target elements are already relatively uniformly distributed in the copper matrix before addition, reducing oxidation loss, segregation due to density differences, and refractory particle residue caused by direct addition of the elements. In a preferred embodiment of the present invention, Sn, Ni, P, Fe, Si, and Mg are added in the form of copper-tin master alloys, copper-nickel master alloys, copper-phosphorus master alloys, copper-iron master alloys, copper-silicon master alloys, and copper-magnesium master alloys, respectively.
[0044] During the smelting process, some Fe may be introduced through iron tools or equipment parts that come into contact with the molten copper, but the final copper alloy composition must be controlled within the range of 0.0003% to 0.005%. If the introduced amount is insufficient, a copper-iron master alloy is used to make up the difference.
[0045] In a preferred embodiment of the present invention, the Fe content in the copper-iron master alloy is no higher than 4%, and the proportion of Fe existing in solid solution is no less than 90%. The Fe content refers to mass percentage. Using a copper-iron master alloy with low Fe content and a high proportion of solid solution allows for rapid and uniform dissolution of Fe during subsequent smelting and dilution processes. This avoids uneven Fe distribution or the formation of large Fe-containing particles in the final ingot due to excessively high Fe content or the presence of coarse Fe-rich phases in the master alloy, thereby ensuring the thermal conductivity and surface quality of the pipe. The content refers to mass percentage.
[0046] In a preferred embodiment of the present invention, the Mg content in the copper-magnesium master alloy is no higher than 4.2%, and the proportion of Mg existing in solid solution is no less than 80%. The Mg content refers to mass percentage. Because Mg is chemically reactive and easily oxidized and burned off, direct addition is difficult to control stably. Therefore, the present invention preferably adds Mg in the form of a copper-magnesium master alloy with low Mg content and predominantly in solid solution to improve the yield and distribution uniformity of Mg, and avoid compositional fluctuations caused by Mg oxidation and burning off. The content refers to mass percentage.
[0047] In a preferred embodiment of the present invention, the Si content in the copper-silicon master alloy is no higher than 5.3%, and the proportion of Si existing in solid solution is no less than 90%. The Si content refers to mass percentage. Using a copper-silicon master alloy with low Si content and a high proportion of solid solution can avoid the incomplete dissolution of coarse silicide particles in conventional high-Si master alloys during the smelting process, thus preventing their inheritance to the final product and ensuring the consistency of the copper tube's plasticity, surface quality, and precipitation strengthening effect. The content refers to mass percentage.
[0048] This invention specifies requirements for the content and solid solution ratio of intermediate alloys used for elements such as Fe, Mg, and Si, in order to improve the uniformity and effectiveness of trace element addition and reduce the risks of burn-off, segregation, or coarse particles that may result from direct addition of elemental particles. Furthermore, for trace elements with low solid solubility in copper or prone to segregation, oxidation, and burn-off, specifying only the final content without controlling the addition carrier and state can easily lead to problems such as low element utilization, uneven distribution, coarse particles, or localized segregation, making it difficult to consistently achieve the microalloying effect of "small addition, significant effect." Improving utilization efficiency through intermediate alloy state control helps reduce raw material costs and production control difficulties.
[0049] In a preferred embodiment of the present invention, the average grain size of the copper alloy is 0.010–0.025 mm. This average grain size is significantly finer than that of conventional copper tubing (typically 0.030–0.080 mm). The fine-grained structure provides a strengthening effect while retaining good plastic deformation capacity, resulting in excellent crack resistance during drawing and bending processes. Furthermore, the fine-grained structure means an increased total grain boundary area, which is beneficial for grain boundary strengthening and uniform deformation, further ensuring the yield of thin-walled copper tubing.
[0050] In a preferred embodiment of the present invention, the copper alloy further includes Ti, the Ti content of which is 0.001% to 0.006%, for example, 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, or 0.006%. The content is a mass percentage.
[0051] Trace amounts of Ti can deoxidize and refine grains, further purifying the copper matrix and refining the as-cast microstructure. Simultaneously, it can form a multi-component composite second phase with Sn and Mg, enhancing precipitation strengthening and also contributing to improved corrosion resistance. If the Ti content is too low (e.g., below 0.001%), the deoxidation and grain refinement effects are insufficient; if the Ti content is too high (e.g., above 0.006%), it exceeds the control range of the ultra-low content microalloying system of this invention, and residual dissolved Ti will reduce thermal conductivity. Therefore, this invention limits the Ti content to 0.001%–0.006%. Preferably, the Ti is added in the form of a copper-titanium master alloy.
[0052] In a preferred embodiment of the present invention, the copper alloy further includes Y (yttrium), with a Y content of 0.001% to 0.006%, for example, 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, or 0.006%. The content is a mass percentage.
[0053] Trace amounts of Y can play a dual role in refining grains and purifying molten copper: on the one hand, Y accumulates at the solid-liquid interface during solidification, inhibiting grain growth and refining the as-cast and final recrystallized structures, complementing the grain-refining effect of Fe; on the other hand, Y has a strong affinity for impurity elements such as O and S, forming high-melting-point compounds that float to the surface and are removed, reducing contamination of the copper matrix by impurities, thus helping to maintain the thermal conductivity and processing plasticity of the copper alloy. If the Y content is too low (e.g., below 0.001%), the refining and purification effects are insufficient; if the Y content is too high (e.g., above 0.006%), it exceeds the control range of the ultra-low content microalloying system of this invention, potentially forming coarse Y-rich phases, which adversely affects the uniformity of the microstructure and thermal conductivity. Therefore, this invention limits the Y content to 0.001%–0.006%.
[0054] Preferably, the Y is added in the form of a copper-yttrium master alloy.
[0055] In addition to Y, this invention does not optionally add other rare earth elements, thereby reducing costs and avoiding rare earth agglomeration.
[0056] Secondly, the present invention provides a method for preparing a copper alloy, comprising: Provide molten electrolytic copper solution; A copper-based master alloy with the corresponding components as described above is added to an electrolytic copper solution to obtain a copper alloy melt. The copper alloy billet is obtained through refining, degassing, and casting.
[0057] In this invention, an exemplary method for preparing electrolytic copper liquid includes: adding electrolytic copper into a smelting furnace, preheating it to 600°C to 700°C at a heating rate of 60°C / min to 80°C / min, and continuing to heat it to 1150°C to 1250°C to fully melt the copper material.
[0058] In a preferred embodiment of the present invention, a copper-based master alloy with the corresponding components as described above is added to the electrolytic copper solution. After addition, the solution is stirred at a speed of 60 r / min to 80 r / min for 15 min to 25 min to ensure that the alloying elements are uniformly distributed in the electrolytic copper solution. In actual production, the alloying elements can be added in batches according to their burn-off characteristics, but the final composition and synergistic relationship must not be changed.
[0059] In a preferred embodiment of the present invention, refining and degassing: the copper alloy melt is controlled at 1120℃~1180℃ and held for 30 min~50 min for refining. Degassing is performed using a graphite degassing rod, and surface oxide slag is removed to obtain a refined copper alloy melt with uniform composition, controlled gas content and inclusions.
[0060] In a preferred embodiment of the present invention, casting involves introducing refined copper alloy molten metal into a semi-continuous casting equipment and casting at 1100°C to 1180°C, with a cooling rate of 50°C / s to 80°C / s.
[0061] Thirdly, the present invention provides a heat exchange tube made of a copper alloy as described above for use in refrigeration equipment heat exchangers.
[0062] Fourthly, the present invention provides a heat exchanger for refrigeration equipment, including the heat exchange tubes described above. The present invention is applicable to heat exchange systems of air conditioners, heat pumps, and other refrigeration equipment.
[0063] The following are specific embodiments and comparative examples.
[0064] Example 1 A copper alloy was prepared according to the following composition: Sn 0.28 wt%, Ni 0.08 wt%, P 0.018 wt%, Fe 0.004 wt%, Si 0.018 wt%, Mg 0.004 wt%, with the balance being Cu and unavoidable impurities, and the total Cu+Ag content being not less than 99.2 wt%. In this embodiment, [Fe] / [P] = 0.22, [Ni] / [Si] = 4.44, and 100 × [Mg] / [Sn] = 1.43.
[0065] The method for preparing the copper alloy as described above includes: S1 Raw Material Inspection and Melting: Composition and surface quality inspections are conducted on electrolytic copper, copper-tin master alloy, copper-nickel master alloy, copper-phosphorus master alloy, copper-iron master alloy, copper-silicon master alloy, and copper-magnesium master alloy. Specifically, the Fe content in copper-iron master alloy shall not exceed 4%, and the proportion of Fe existing in solid solution shall not be less than 90%; the Mg content in copper-magnesium master alloy shall not exceed 4.2%, and the proportion of Mg existing in solid solution shall not be less than 80%; the Si content in copper-silicon master alloy shall not exceed 5.3%, and the proportion of Si existing in solid solution shall not be less than 90%.
[0066] After passing the inspection, electrolytic copper is added to the smelting furnace and preheated to 650°C at a heating rate of 70°C / min. The temperature is then further increased to 1200°C to fully melt the copper.
[0067] S2 Alloying and Homogenization: Add copper-tin master alloy, copper-nickel master alloy, copper-phosphorus master alloy, copper-iron master alloy, copper-silicon master alloy and copper-magnesium master alloy in sequence according to the target composition, and stir at 70 r / min for 20 min to make the alloying elements uniformly distributed in the copper liquid.
[0068] S3 Refining and Degassing: The copper alloy melt is controlled at 1160℃ and held for 40 minutes for refining. A graphite degassing rod is used for degassing, and the surface oxide slag is removed to obtain a refined copper alloy melt with uniform composition, controlled gas content and inclusions.
[0069] S4 Casting: Refined copper alloy molten metal is introduced into a semi-continuous casting equipment and cast at 1150℃ with a cooling rate of 65℃ / s. After casting, the chemical composition is tested, and copper alloy billets are obtained if they pass the test.
[0070] Example 2 Everything else is the same as in Example 1, except for the following differences: A copper alloy was prepared according to the following composition: Sn 0.35 wt%, Ni 0.075 wt%, P 0.015 wt%, Fe 0.003 wt%, Si 0.032 wt%, Mg 0.003 wt%, with the balance being Cu and unavoidable impurities, and the total Cu+Ag content being not less than 99.2 wt%. In this embodiment, [Fe] / [P] = 0.2, [Ni] / [Si] = 2.34, and 100 × [Mg] / [Sn] = 0.86.
[0071] Example 3 Everything else is the same as in Example 1, except for the following differences: A copper alloy was prepared according to the following composition: Sn 0.15 wt%, Ni 0.05 wt%, P 0.025 wt%, Fe 0.005 wt%, Si 0.015 wt%, Mg 0.003 wt%, with the balance being Cu and unavoidable impurities, and the total Cu+Ag content being not less than 99.2 wt%. In this embodiment, [Fe] / [P] = 0.2, [Ni] / [Si] = 3.33, and 100 × [Mg] / [Sn] = 2.
[0072] Example 4 Everything else is the same as in Example 1, except for the following differences: The composition is as follows: Sn 0.28 wt%, Ni 0.08 wt%, P 0.018 wt%, Fe 0.004 wt%, Si 0.018 wt%, Mg 0.004 wt%, Ti 0.003%, with the balance being Cu and unavoidable impurities. The total Cu+Ag content is not less than 99.2 wt%. In this embodiment, [Fe] / [P] = 0.22, [Ni] / [Si] = 4.44, and 100 × [Mg] / [Sn] = 1.43.
[0073] Example 5 Everything else is the same as in Example 1, except for the following differences: The composition is Sn 0.28 wt%, Ni 0.08 wt%, P 0.018 wt%, Fe 0.004 wt%, Si 0.018 wt%, Mg 0.004 wt%, Y 0.003%, with the balance being Cu and unavoidable impurities. The total Cu+Ag content is not less than 99.2 wt%. In this embodiment, [Fe] / [P] = 0.22, [Ni] / [Si] = 4.44, and 100 × [Mg] / [Sn] = 1.43.
[0074] Example 6 Everything else is the same as in Example 1, except for the following differences: The composition is as follows: Sn 0.28 wt%, Ni 0.08 wt%, P 0.018 wt%, Fe 0.004 wt%, Si 0.018 wt%, Mg 0.004 wt%, Ti 0.003%, Y 0.003%, with the balance being Cu and unavoidable impurities. The total Cu+Ag content is not less than 99.2 wt%. In this embodiment, [Fe] / [P] = 0.22, [Ni] / [Si] = 4.44, and 100 × [Mg] / [Sn] = 1.43.
[0075] Example 7 Everything else is the same as in Example 1, except for the following differences: A copper alloy was prepared according to the following composition: Sn 0.45 wt%, Ni 0.05 wt%, P 0.005 wt%, Fe 0.004 wt%, Si 0.025 wt%, Mg 0.004 wt%, with the balance being Cu and unavoidable impurities, and the total Cu+Ag content being not less than 99.2 wt%. In this embodiment, [Fe] / [P] = 0.8, [Ni] / [Si] = 2, and 100 × [Mg] / [Sn] = 0.88.
[0076] Example 8 Everything else is the same as in Example 1, except for the following differences: A copper alloy was prepared according to the following composition: Sn 0.20 wt%, Ni 0.07 wt%, P 0.005 wt%, Fe 0.001 wt%, Si 0.016 wt%, Mg 0.004 wt%, with the balance being Cu and unavoidable impurities, and the total Cu+Ag content being not less than 99.2 wt%. In this embodiment, [Fe] / [P] = 0.2, [Ni] / [Si] = 4.44, and 100 × [Mg] / [Sn] = 1.43.
[0077] Comparative Example 1 Everything else is the same as in Example 1, except for the following differences: A copper alloy was prepared according to the following composition: Sn 0.15 wt%, Ni 0.08 wt%, P 0.035 wt%, Fe 0.004 wt%, Si 0.075 wt%, Mg 0.004 wt%, with the balance being Cu and unavoidable impurities, and the total Cu+Ag content being not less than 99.2 wt%. In this embodiment, [Fe] / [P] = 0.11, [Ni] / [Si] = 1.07, and 100 × [Mg] / [Sn] = 2.66.
[0078] Comparative Example 2 Everything else is the same as in Example 1, except for the following differences: A copper alloy was prepared according to the following composition: Sn 0.28 wt%, Ni 0.05 wt%, P 0.018 wt%, Fe 0.004 wt%, Si 0.085 wt%, Mg 0.004 wt%, with the balance being Cu and unavoidable impurities, and the total Cu+Ag content being not less than 99.2 wt%. In this embodiment, [Fe] / [P] = 0.22, [Ni] / [Si] = 0.59, and 100 × [Mg] / [Sn] = 1.43.
[0079] Comparative Example 3 Everything else is the same as in Example 1, except for the following differences: A copper alloy was prepared according to the following composition: Sn 0.50 wt%, Ni 0.08 wt%, P 0.018 wt%, Fe 0.004 wt%, Si 0.018 wt%, Mg 0.001 wt%, with the balance being Cu and unavoidable impurities, and the total Cu+Ag content being not less than 99.2 wt%. In this embodiment, [Fe] / [P] = 0.22, [Ni] / [Si] = 4.44, and 100 × [Mg] / [Sn] = 0.2.
[0080] Comparative Example 4 Alloys were prepared according to the following composition: Copper: Balance; Tin: 0.30%; Nickel: 0.20%; Phosphorus: 0.020%; Unavoidable impurities: ≤0.05%.
[0081] The copper alloys obtained in the examples and comparative examples were used to prepare copper tubes with an outer diameter of φ9.52 mm and a wall thickness of 0.30 mm.
[0082] Test method: Tensile strength and elongation at break: The room temperature tensile test was conducted in accordance with GB / T 34505-2017 "Tension test method for copper and copper alloy materials at room temperature" to determine the tensile strength and elongation at break of soft (fully annealed) copper alloy specimens.
[0083] Average grain size: GB / T 6394-2017 "Method for determination of average grain size of metals", the metallographic cross section method was used for determination.
[0084] Thermal conductivity: determined by the laser flash method.
[0085] Corrosion resistance test: Refer to JB / T 7901 "Metallic Materials Laboratory Uniform Corrosion Full Immersion Test Method", adjust the pH to 3.0-3.1 and 6.5-7.2 respectively, and record the time when the first corrosion pit is observed on the sample surface under a 10x magnifying glass as the corrosion start time.
[0086] Pressure resistance test: The copper alloy is made into a copper tube with an outer diameter of 9.52 mm and a wall thickness of 0.30 mm. The water pressure burst test is carried out according to GB / T 241-2025, and the burst pressure (i.e. ultimate pressure resistance strength) is measured.
[0087] Table 1
[0088] Compared to Example 1, the Ni / Si ratio in Example 2 deviates from the preferred range, resulting in reduced precipitation of the Ni-Si second phase and increased residual dissolved Si, leading to a decrease in both tensile strength and thermal conductivity. This comparison indicates that controlling the Ni / Si ratio within the preferred range is beneficial for promoting the full precipitation of Ni-Si, reducing the scattering effect of free dissolved Si on the heat conduction channels, and thus maintaining the high thermal conductivity of the alloy.
[0089] In Example 3, Sn, Ni, and Si are all taken as the lower limit of the scope of this invention, and the total alloy content is 0.248%. However, the content of each component is not within the preferred range. Compared with Example 1, all performance indicators are slightly lower.
[0090] Compared with Example 1, Example 4 added 0.003% Ti. Ti promoted grain refinement by forming TiC / TiN particles, reducing the average grain size from 0.018 mm to 0.017 mm, increasing the tensile strength from 255 MPa to 262 MPa, the ultimate pressure resistance from 16.4 MPa to 16.7 MPa, and the elongation from 48% to 49%. However, the portion of Ti remaining in the matrix in a solid solution state caused lattice distortion and scattering of conduction electrons, resulting in a slight decrease in thermal conductivity from 415 W / (m·K) to 412 W / (m·K), while the corrosion resistance remained basically the same.
[0091] Compared to Example 1, Example 5 added 0.003% Y. On the one hand, Y is enriched at the solid-liquid interface to inhibit grain growth, refining the average grain size from 0.018 mm to 0.017 mm and increasing the tensile strength from 255 MPa to 260 MPa. On the other hand, Y has a strong affinity for impurity elements such as O and S, and is removed by forming high-melting-point compounds that float to the surface, thus purifying the copper matrix and reducing the scattering of thermally conductive electrons by impurities. The addition of Y, through the dual mechanism of "matrix purification + grain refinement", can achieve a comprehensive and simultaneous improvement in strength, plasticity, thermal conductivity, and corrosion resistance.
[0092] Compared to Example 1, Example 6 simultaneously added 0.003% Ti and 0.003% Y. Ti provides nucleation sites by forming TiC / TiN particles, while Y inhibits grain growth by accumulating at the solid-liquid interface. Both work together to refine the grains from the two directions of "nucleation" and "growth," resulting in a significant improvement in all properties. This indicates that the simultaneous addition of Ti and Y has a synergistic effect, which can optimize the overall performance of the alloy.
[0093] Compared to Example 1, the ratios [Fe] / [P] = 0.80, [Ni] / [Si] = 2.00, and 100×[Mg] / [Sn] = 0.88 in Example 7 all deviate from the preferred range. The deviation of the Ni / Si ratio from the preferred range leads to a decrease in the precipitation of the Ni-Si system second phase and an increase in residual dissolved Si; the Fe / P ratio exceeding the upper limit of the preferred range weakens the synergistic refining effect of Fe-P; and the Mg / Sn ratio falling below the lower limit of the preferred range reduces the amount of Mg-Sn second phase. The synchronous weakening performance of the three synergistic systems is lower than that of Example 1.
[0094] Compared to Example 1, the Fe content in Example 8 was 0.001%. This example demonstrates that even with extremely low Fe content, a certain Fe-P synergistic effect can still be achieved because the [Fe] / [P] ratio still meets the requirement of 0.2 to 1.0.
[0095] Compared with Example 1, the [Fe] / [P] ratio of Comparative Example 1 is 0.10 (below the lower limit of the basic range of 0.15). The Fe / P ratio is lower than the lower limit of the basic range, which means that Fe cannot effectively fix P, the amount of free solid solution P increases, the Fe-P synergistic refining effect disappears, the average grain size increases, and other properties decrease.
[0096] Compared with Example 1, the [Ni] / [Si] ratio of Comparative Example 2 is 0.59. The Ni / Si ratio is lower than the lower limit of the basic range, resulting in very little precipitation of the second phase in the Ni-Si system. The residual solid solution Si increases significantly, which increases the average grain size and reduces other properties.
[0097] Compared with Example 1, Comparative Example 3 has a ratio of 100×[Mg] / [Sn] = 0.2. The Mg / Sn ratio is lower than the lower limit of the basic range, which leads to a significant reduction in the amount of the second phase of the Mg-Sn system. Its contribution to solidification structure regulation, grain boundary pinning and grain refinement is significantly weakened, resulting in an increase in average grain size and a decrease in other properties.
[0098] Compared to Example 1, Comparative Example 4 is a Cu-0.30Sn-0.20Ni-0.020P ternary alloy, free of Fe, Si, and Mg. Because it lacks Fe, Si, and Mg, there is no Fe-P, Ni-Si, or Mg-Sn synergistic system; it relies solely on the traditional Cu-Ni-P age-hardening mechanism. Excessive Ni solution leads to strong scattering of thermally conductive electrons, significantly reducing thermal conductivity, elongation at break, and corrosion resistance, while increasing the average grain size. Simply increasing the Ni content to improve strength comes at the cost of sacrificing thermal conductivity, plasticity, and corrosion resistance.
[0099] It should be noted that the above description is only a preferred embodiment of the present invention and is not limited to the description in the specification and embodiments. Therefore, all equivalent changes or modifications made to the structure, features and principles described in the claims of this invention should be included within the scope of this patent application.
Claims
1. A copper alloy for use in heat exchangers of refrigeration equipment, characterized in that, In terms of mass percentage, it includes: Sn: 0.15%–0.50%, Ni: 0.05%–0.10%, P: 0.005%–0.035%, Fe: 0.0003%–0.005%, Si: 0.015%–0.085%, Mg: 0.001%–0.006%, with unavoidable impurities totaling no more than 0.025%, and the balance being Cu and Ag, where Ag is an accompanying element of Cu raw material, and the total content of Cu and Ag is no less than 99.2%. The copper alloy satisfies the following proportional relationship: [Fe] / [P] = 0.2–1.0, [Ni] / [Si] = 1–6.0, and 100×[Mg] / [Sn] = 0.5–3.0, where [X] represents the mass percentage of element X.
2. The copper alloy as described in claim 1, characterized in that, In terms of mass percentage, it includes: Sn: 0.28%, Ni: 0.08%, P: 0.018%, Fe: 0.004%, Si: 0.018%, Mg: 0.004%, with unavoidable impurities totaling no more than 0.025%, and the balance being Cu and Ag, with the total content of Cu and Ag being no less than 99.2%.
3. The copper alloy as described in claim 1, characterized in that, The copper alloy satisfies the following proportional relationship: [Fe] / [P] = 0.2~0.35, [Ni] / [Si] = 3~6, 100×[Mg] / [Sn] = 1~3, where [X] represents the mass percentage of element X.
4. The copper alloy as described in claim 1, characterized in that, The Sn, Ni, P, Fe, Si and Mg are added using a copper-based master alloy.
5. The copper alloy as described in claim 4, characterized in that, Sn, Ni, P, Fe, Si and Mg are added in the form of copper-tin master alloy, copper-nickel master alloy, copper-phosphorus master alloy, copper-iron master alloy, copper-silicon master alloy and copper-magnesium master alloy, respectively.
6. The copper alloy as described in claim 5, characterized in that, The Fe content in the copper-iron master alloy is not higher than 4%, and the proportion of Fe existing in solid solution is not less than 90%; and / or, The Mg content in the copper-magnesium master alloy is not higher than 4.2%, and the proportion of Mg existing in solid solution is not less than 80%; and / or, The Si content in the copper-silicon master alloy is not higher than 5.3%, and the proportion of Si existing in solid solution is not less than 90%; and / or, The average grain size of the copper alloy is 0.010–0.025 mm.
7. The copper alloy as described in claim 1, characterized in that, It also includes Ti, with a Ti content of 0.001% to 0.006%; and / or, It also includes Y, with a Y content of 0.001% to 0.006%.
8. A method for preparing a copper alloy for a heat exchanger in a refrigeration device as described in any one of claims 1-7, characterized in that, include: Provide molten electrolytic copper solution; According to the composition of the copper alloy as described in any one of claims 1-7, a copper-based master alloy having the corresponding composition is added to an electrolytic copper solution to obtain a copper alloy melt. The copper alloy is obtained through refining, degassing, and casting.
9. A heat exchange tube, characterized in that, It is made of a copper alloy for heat exchangers in refrigeration equipment as described in any one of claims 1-7.
10. A heat exchanger for refrigeration equipment, characterized in that, Includes the heat exchange tube as described in claim 9.
Citation Information
Patent Citations
Precipitation-hardening copper alloy and application thereof
CN108285988A
Tin brass alloy and preparation method thereof
CN113073229A