A heat-sealable self-adhesive high-strength medical dialysis paper and a processing method thereof

CN122980269APending Publication Date: 2026-10-27CHANGZHOU MAGNET NEW MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611202662.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-10
Publication Date
2026-10-27

AI Technical Summary

Technical Problem

现有技术存在三大痛点:一是热封性能与自粘性难以兼顾,单一涂胶层易出现热封强度不足或开袋纸屑残留问题;二是高强度与透气性存在矛盾,增加纤维用量或添加增强剂会导致透气度下降,影响灭菌效率;三是耐灭菌稳定性差,经121℃/20min蒸汽灭菌后,湿抗张强度和热封剥离力衰减明显

Benefits of technology

[0027]1、通过核心的双效协同改性剂,有效增强纤维间结合力,提升纸张整体结构强度,改善耐湿性能,确保包装在灭菌、运输、储存全流程中保持结构完整,避免医疗器械污染;

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present application relates to the technical field of medical packaging materials, and particularly relates to a heat-seal self-adhesive high-strength medical dialysis paper, which comprises a paper base layer and a stepped heat-seal layer; the paper base layer is made of the following raw materials in parts by weight: coniferous pulp 50-70 parts, broadleaf wood pulp 10-15 parts, Lyocell fiber 8-12 parts, bamboo pulp fiber 5-8 parts, double-effect synergistic modifier 3-6 parts, auxiliary modifier 2.3-4.5 parts, and functional additive 6.3-11.8 parts; the stepped heat-seal layer comprises a primer layer and a surface rubber layer, the primer layer is a water-based polyurethane-acrylate copolymer, and the coating amount is 8-12 g / m 2 The present application realizes the synergistic breakthrough of the strength, heat-sealability, sterilization stability and air permeability of the medical dialysis paper through the synergism of the double-effect synergistic modifier and the processes such as stepped heat-sealing and double-stage beating, the dry and wet strength, sealing easy-open property and sterilization stability are significantly improved, the raw materials are green and safe, the industrialization cost is controllable, the present application is suitable for various medical sterilization packaging scenes, and has significant technical advantages and economic and social benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of medical packaging materials technology, and in particular to a heat-sealable self-adhesive high-strength medical dialysis paper and its processing method. Background Technology

[0002] Medical dialysis paper, as a key material for sterilization packaging of medical devices, must simultaneously meet four core requirements: breathability and sterilization, antibacterial protection, physical strength, and heat-sealing performance. Existing technologies suffer from three major drawbacks: First, it is difficult to balance heat-sealing performance and self-adhesion; a single adhesive layer is prone to insufficient heat-sealing strength or paper residue residue upon opening the bag. Second, there is a contradiction between high strength and breathability; increasing fiber content or adding reinforcing agents leads to decreased breathability, affecting sterilization efficiency. Third, it exhibits poor sterilization stability; after steam sterilization at 121℃ for 20 minutes, wet tensile strength and heat-sealing peel strength show significant decreases.

[0003] Existing patent CN113089373B discloses a high-strength dialysis paper containing green orange peel extract, but does not involve heat-sealing self-adhesive function; CN213949323U designs a double-layer glued heat-sealing structure, but the strength improvement is insufficient and the problem of performance degradation after sterilization is not solved.

[0004] Therefore, we propose a heat-sealing self-adhesive high-strength medical dialysis paper. Summary of the Invention

[0005] The purpose of this invention is to address the shortcomings of existing technologies by proposing a heat-sealing self-adhesive high-strength medical dialysis paper.

[0006] To achieve the above objectives, the present invention adopts the following technical solution:

[0007] A heat-sealable self-adhesive high-strength medical dialysis paper, comprising a paper base layer and a stepped heat-sealable layer;

[0008] The paper base layer is made from the following raw materials in parts by weight: 50-70 parts softwood pulp, 10-15 parts hardwood pulp, 8-12 parts Lyocell fiber, 5-8 parts bamboo pulp fiber, 3-6 parts dual-effect synergistic modifier, 2.3-4.5 parts auxiliary modifier, and 6.3-11.8 parts functional additives;

[0009] The stepped heat-sealing layer includes a base layer and a topcoat layer. The base layer is a water-based polyurethane-acrylate copolymer with a coating weight of 8-12 g / m². 2 The topcoat layer consists of medical-grade hot melt adhesive, polyethylene glycol monomethyl ether graft modifier, and nano zinc oxide, with a coating weight of 5-8 g / m². 2 The amount of nano zinc oxide added is 0.5-1% of the total mass of the adhesive layer.

[0010] As a preferred technical solution of this application, the dual-effect synergistic modifier is a ternary complex of green tangerine peel extract-polydopamine-chitosan.

[0011] As a preferred technical solution of this application, the auxiliary modifier is a mixture of 1.5-3 parts of ethyl 3-propionate and 0.8-1.5 parts of medical-grade polycaprolactone.

[0012] As a preferred technical solution of this application, the functional additives include 2-4 parts of polyvinylpyrrolidone, 1-2 parts of cationic starch, 0.3-0.8 parts of wet strength agent, and 2-3 parts of inorganic pigment.

[0013] As a preferred technical solution of this application, the wet strength agent is polyamide epichlorohydrin, the inorganic pigment is nano silica with a particle size of 50-100nm; in the ternary complex of green tangerine peel extract-polydopamine-chitosan, the mass ratio of green tangerine peel extract, polydopamine and chitosan is 3:(1-2):(1-3).

[0014] As a preferred technical solution of this application, the preparation method of the dual-effect synergistic modifier includes the following steps:

[0015] Step S1: Preparation of green tangerine peel extract: Pulverize green tangerine peel to 80 mesh, reflux extract with 70% ethanol solution twice, 2 hours each time, with a material-to-liquid ratio of 1:15, combine the extracts, concentrate under reduced pressure to a paste, and after purification, control the limonene content in the green tangerine peel extract to be at least 30 mg / g.

[0016] Step S2: Polydopamine pretreatment: Dissolve dopamine hydrochloride in Tris-HCl buffer at pH 8.5 at a concentration of 2 mg / mL, stir for 30 min to form a polydopamine precursor solution;

[0017] Step S3: Ternary complex reaction: The green tangerine peel extract and chitosan were mixed at a mass ratio of 2:1, and polydopamine precursor solution was added. The total mass ratio of the three was 3:(1-2):(1-3). The mixture was stirred at 50℃ for 2 hours, the pH was adjusted to 7.0, and the mixture was centrifuged at 8000 r / min for 15 minutes. The precipitate was freeze-dried at -40℃ for 24 hours to obtain the green tangerine peel extract-polydopamine-chitosan ternary complex.

[0018] A method for processing heat-sealable self-adhesive high-strength medical dialysis paper includes the following steps:

[0019] Step S1: Two-stage pulping: Mix softwood pulp, hardwood pulp and bamboo pulp fibers for one-stage pulping with a freeness of 25-30°SR. After adding Lyocell fibers, perform a second-stage pulping with a freeness of 40-45°SR, controlling the average fiber length to 0.8-1.2mm.

[0020] Step S2: Pulp preparation: Add the dual-effect synergistic modifier and auxiliary modifier to the pulped fiber, stir at 45-50℃ for 30 min, then add the functional additives, stir for 15 min, and adjust the concentration to 3-5%;

[0021] Step S3: Forming: Papermaking on an inclined wire paper machine, with a wire speed of 80-100 m / min, a press pressure of 0.3-0.5 MPa, and a pre-drying temperature of 80-90℃, yielding a basis weight of 45-60 g / m². 2 Dialysis paper substrate;

[0022] Step S4: Gradient coating: First apply the primer layer and dry at 100-110℃ for 2 minutes, then apply the topcoat layer and dry at 80-90℃ for 1.5 minutes;

[0023] Step S5: Ultraviolet crosslinking: Irradiate with 254nm ultraviolet light at an intensity of 30-50mJ / cm. 2 The time is 30-60 seconds, and the cross-linking degree of the adhesive layer is controlled to be ≥60%.

[0024] Step S6: Post-processing: 0.2-0.3MPa soft calendering, edge trimming and winding.

[0025] As a preferred technical solution of this application, the fiber coarseness after the two-stage pulping in step S1 is 15-20 μm; the surface adhesive layer is coated using a micro-gravure coating process with a coating accuracy of ±0.2 g / m. 2 .

[0026] The beneficial effects of this invention are as follows:

[0027] 1. Through the core dual-effect synergistic modifier, the bonding force between fibers is effectively enhanced, the overall structural strength of the paper is improved, and the moisture resistance is improved, ensuring that the packaging maintains structural integrity throughout the entire process of sterilization, transportation, and storage, and avoiding contamination of medical devices;

[0028] 2. Through the combined action of the stepped heat-sealing layer design and modifier, and the addition of a base coating to strengthen the adhesion to the paper base, the dual requirements of sealing and easy opening are achieved. This ensures no leakage during high-temperature and high-pressure sterilization, allows medical staff to easily open the packaging, and prevents paper residue from contaminating medical devices, making it suitable for clinical use scenarios.

[0029] 3. Through the synergistic effect of the ternary composite system during the preparation of the dual-effect synergistic modifier and the ultraviolet cross-linking process, the product's anti-sterilization attenuation ability is effectively improved. After high temperature and high pressure steam sterilization, the core performance of the product does not decrease significantly and it is not prone to yellowing and aging. The antibacterial protection effect is stable and continuous, effectively extending the shelf life of medical device packaging, ensuring that the product maintains reliable performance within the validity period, and reducing the risk of medical use.

[0030] 4. The dual-effect synergistic modifier uses natural extracts and biocompatible materials, with no toxic or harmful substances released, meeting the safety standards for medical materials. The formula and process are compatible with existing paper machine production lines, enabling industrialization without the need for large-scale new equipment. The production process is green and environmentally friendly with no pollutant emissions. The product not only meets the stringent safety and environmental protection requirements of the medical field, but also has the advantage of controllable cost. It can be widely adapted to various medical device sterilization packaging scenarios, combining technical value and market competitiveness.

[0031] This invention achieves a synergistic breakthrough in the strength, heat-sealing properties, sterilization stability, and air permeability of medical dialysis paper through the synergistic effect of dual-effect modifiers and processes such as stepped heat sealing and two-stage pulping. The dry and wet strength, sealing ease, and sterilization stability are significantly improved. Moreover, the raw materials are green and safe, and the industrialization cost is controllable. It is suitable for various medical sterilization packaging scenarios and has significant technical advantages and economic and social benefits. Detailed Implementation

[0032] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.

[0033] Experimental Design

[0034] Three examples, two comparative examples, and one blank group were set up to conduct three groups of directional experiments on physical strength, heat-sealing self-adhesive performance, and sterilization resistance stability. The test standards refer to YY / T 0698.2-2017 and GB / T 458-2008.

[0035] Example 1

[0036] A heat-sealable self-adhesive high-strength medical dialysis paper, comprising a paper base layer and a stepped heat-sealable layer;

[0037] The paper base layer is made from the following raw materials in parts by weight: 50 parts softwood pulp, 10 parts hardwood pulp, 8 parts Lyocell fiber, 5 parts bamboo pulp fiber, 4 parts dual-effect synergistic modifier, 3 parts auxiliary modifier, and 6.5 parts functional additives.

[0038] The stepped heat-sealing layer consists of a base coat and a top coat. The base coat is a water-based polyurethane-acrylate copolymer with a coating weight of 8 g / m². 2 The topcoat layer consists of medical-grade hot melt adhesive, polyethylene glycol monomethyl ether graft modifier, and nano zinc oxide, with a coating weight of 5 g / m². 2 The amount of nano zinc oxide added is 0.7% of the total mass of the adhesive layer.

[0039] Furthermore, the dual-effect synergistic modifier is a ternary complex of green tangerine peel extract, polydopamine, and chitosan.

[0040] Furthermore, the auxiliary modifier is a mixture of 2 parts ethyl 3-propionate and 1 part medical-grade polycaprolactone.

[0041] Furthermore, the functional additives include 2 parts polyvinylpyrrolidone, 1 part cationic starch, 0.3 parts wet strength agent, and 2 parts inorganic pigment.

[0042] Furthermore, the wet strength agent is polyamide epichlorohydrin, and the inorganic pigment is nano-silica with a particle size of 50 nm; in the ternary complex of green tangerine peel extract-polydopamine-chitosan, the mass ratio of green tangerine peel extract, polydopamine, and chitosan is 3:1:1.

[0043] Furthermore, the preparation method of the dual-effect synergistic modifier includes the following steps:

[0044] Step S1: Preparation of green tangerine peel extract: Pulverize green tangerine peel to 80 mesh, reflux extract with 70% ethanol solution twice, 2 hours each time, with a material-to-liquid ratio of 1:15, combine the extracts, concentrate under reduced pressure to a paste, and after purification, control the limonene content in the green tangerine peel extract to be at least 30 mg / g.

[0045] Step S2: Polydopamine pretreatment: Dissolve dopamine hydrochloride in Tris-HCl buffer at pH 8.5 at a concentration of 2 mg / mL, stir for 30 min to form a polydopamine precursor solution;

[0046] Step S3: Ternary complex reaction: The green tangerine peel extract and chitosan were mixed at a mass ratio of 2:1, and polydopamine precursor solution was added. The mixture was stirred at 50°C for 2 hours, the pH was adjusted to 7.0, and the mixture was centrifuged at 8000 r / min for 15 minutes. The precipitate was freeze-dried at -40°C for 24 hours to obtain the green tangerine peel extract-polydopamine-chitosan ternary complex.

[0047] A method for processing heat-sealable self-adhesive high-strength medical dialysis paper includes the following steps:

[0048] Step S1: Two-stage pulping: Mix softwood pulp, hardwood pulp and bamboo pulp fibers for one-stage pulping with a freeness of 30°SR. After adding Lyocell fibers, perform a second-stage pulping with a freeness of 45°SR, controlling the average fiber length to 1.0 mm.

[0049] Step S2: Pulp preparation: Add a dual-effect synergistic modifier and an auxiliary modifier to the pulped fiber, stir at 45°C for 30 minutes, then add the functional additives, stir for 15 minutes, and adjust the concentration to 4%;

[0050] Step S3: Forming: Papermaking on an inclined wire paper machine, wire speed 100m / min, press pressure 0.5MPa, pre-drying temperature 90℃, to obtain a basis weight of 50g / m². 2 Dialysis paper substrate;

[0051] Step S4: Gradient coating: First apply the primer layer and dry at 100℃ for 2 minutes, then apply the topcoat layer and dry at 85℃ for 1.5 minutes;

[0052] Step S5: Ultraviolet crosslinking: Irradiation with 254nm ultraviolet light at an intensity of 40mJ / cm 2 Time: 45 seconds; control the crosslinking degree of the adhesive layer to ≥60%.

[0053] Step S6: Post-processing: 0.3MPa soft calendering, edge trimming and winding.

[0054] Furthermore, in step S1, the fiber thickness after the second-stage pulping is 20 μm; the surface adhesive layer is coated using a micro-gravure coating process with a coating accuracy of ±0.2 g / m. 2 .

[0055] Example 2

[0056] A heat-sealable self-adhesive high-strength medical dialysis paper, comprising a paper base layer and a stepped heat-sealable layer;

[0057] The paper base layer is made from the following raw materials in parts by weight: 60 parts softwood pulp, 12 parts hardwood pulp, 10 parts Lyocell fiber, 6.5 parts bamboo pulp fiber, 4.5 parts dual-effect synergistic modifier, 3.2 parts auxiliary modifier, and 8 parts functional additives.

[0058] The stepped heat-sealing layer consists of a base coat and a top coat. The base coat is a water-based polyurethane-acrylate copolymer with a coating weight of 10 g / m². 2 The topcoat layer consists of medical-grade hot melt adhesive, polyethylene glycol monomethyl ether graft modifier, and nano zinc oxide, with a coating weight of 6 g / m². 2 The amount of nano zinc oxide added is 0.8% of the total mass of the adhesive layer.

[0059] Furthermore, the dual-effect synergistic modifier is a ternary complex of green tangerine peel extract, polydopamine, and chitosan.

[0060] Furthermore, the auxiliary modifier is a mixture of 2 parts ethyl 3-propionate and 1.2 parts medical-grade polycaprolactone.

[0061] Furthermore, the functional additives include 3 parts polyvinylpyrrolidone, 1.5 parts cationic starch, 0.5 parts wet strength agent, and 2.5 parts inorganic pigment.

[0062] Furthermore, the wet strength agent is polyamide epichlorohydrin, and the inorganic pigment is nano-silica with a particle size of 80 nm; in the ternary complex of green tangerine peel extract-polydopamine-chitosan, the mass ratio of green tangerine peel extract, polydopamine, and chitosan is 3:1:2.

[0063] Furthermore, the preparation method of the dual-effect synergistic modifier includes the following steps:

[0064] Step S1: Preparation of green tangerine peel extract: Pulverize green tangerine peel to 80 mesh, reflux extract with 70% ethanol solution twice, 2 hours each time, with a material-to-liquid ratio of 1:15, combine the extracts, concentrate under reduced pressure to a paste, and after purification, control the limonene content in the green tangerine peel extract to be at least 30 mg / g.

[0065] Step S2: Polydopamine pretreatment: Dissolve dopamine hydrochloride in Tris-HCl buffer at pH 8.5 at a concentration of 2 mg / mL, stir for 30 min to form a polydopamine precursor solution;

[0066] Step S3: Ternary complex reaction: The green tangerine peel extract and chitosan were mixed at a mass ratio of 2:1, and polydopamine precursor solution was added. The mixture was stirred at 50°C for 2 hours, the pH was adjusted to 7.0, and the mixture was centrifuged at 8000 r / min for 15 minutes. The precipitate was freeze-dried at -40°C for 24 hours to obtain the green tangerine peel extract-polydopamine-chitosan ternary complex.

[0067] A method for processing heat-sealable self-adhesive high-strength medical dialysis paper includes the following steps:

[0068] Step S1: Two-stage pulping: Mix softwood pulp, hardwood pulp and bamboo pulp fibers for one-stage pulping with a freeness of 30°SR. After adding Lyocell fibers, perform a second-stage pulping with a freeness of 45°SR, controlling the average fiber length to 1.0 mm.

[0069] Step S2: Pulp preparation: Add a dual-effect synergistic modifier and an auxiliary modifier to the pulped fiber, stir at 45°C for 30 minutes, then add the functional additives, stir for 15 minutes, and adjust the concentration to 4%;

[0070] Step S3: Forming: Papermaking on an inclined wire paper machine, wire speed 100m / min, press pressure 0.5MPa, pre-drying temperature 90℃, to obtain a basis weight of 50g / m². 2 Dialysis paper substrate;

[0071] Step S4: Gradient coating: First apply the primer layer and dry at 100℃ for 2 minutes, then apply the topcoat layer and dry at 85℃ for 1.5 minutes;

[0072] Step S5: UV crosslinking: Irradiation with 254nm UV light at an intensity of 45mJ / cm 2 Time: 45 seconds; control the crosslinking degree of the adhesive layer to ≥60%.

[0073] Step S6: Post-processing: 0.3MPa soft calendering, edge trimming and winding.

[0074] Furthermore, in step S1, the fiber thickness after the second-stage pulping is 20 μm; the surface adhesive layer is coated using a micro-gravure coating process with a coating accuracy of ±0.2 g / m. 2 .

[0075] Example 3

[0076] A heat-sealable self-adhesive high-strength medical dialysis paper, comprising a paper base layer and a stepped heat-sealable layer;

[0077] The paper base layer is made from the following raw materials in parts by weight: 70 parts softwood pulp, 15 parts hardwood pulp, 12 parts Lyocell fiber, 8 parts bamboo pulp fiber, 5 parts dual-effect synergistic modifier, 4 parts auxiliary modifier, and 10 parts functional additives.

[0078] The stepped heat-sealing layer consists of a base coat and a top coat. The base coat is a water-based polyurethane-acrylate copolymer with a coating weight of 12 g / m². 2 The topcoat layer consists of medical-grade hot melt adhesive, polyethylene glycol monomethyl ether graft modifier, and nano zinc oxide, with a coating weight of 8 g / m². 2 The amount of nano zinc oxide added is 1.0% of the total mass of the adhesive layer.

[0079] Furthermore, the dual-effect synergistic modifier is a ternary complex of green tangerine peel extract, polydopamine, and chitosan.

[0080] Furthermore, the auxiliary modifier is a mixture of 2 parts ethyl 3-propionate and 1.5 parts medical-grade polycaprolactone.

[0081] Furthermore, the functional additives include 4 parts polyvinylpyrrolidone, 2 parts cationic starch, 0.8 parts wet strength agent, and 3 parts inorganic pigment.

[0082] Furthermore, the wet strength agent is polyamide epichlorohydrin, and the inorganic pigment is nano-silica with a particle size of 100 nm; in the ternary complex of green tangerine peel extract-polydopamine-chitosan, the mass ratio of green tangerine peel extract, polydopamine, and chitosan is 3:1:2.

[0083] Furthermore, the preparation method of the dual-effect synergistic modifier includes the following steps:

[0084] Step S1: Preparation of green tangerine peel extract: Pulverize green tangerine peel to 80 mesh, reflux extract with 70% ethanol solution twice, 2 hours each time, with a material-to-liquid ratio of 1:15, combine the extracts, concentrate under reduced pressure to a paste, and after purification, control the limonene content in the green tangerine peel extract to be at least 30 mg / g.

[0085] Step S2: Polydopamine pretreatment: Dissolve dopamine hydrochloride in Tris-HCl buffer at pH 8.5 at a concentration of 2 mg / mL, stir for 30 min to form a polydopamine precursor solution;

[0086] Step S3: Ternary complex reaction: The green tangerine peel extract and chitosan were mixed at a mass ratio of 2:1, and polydopamine precursor solution was added. The mixture was stirred at 50°C for 2 hours, the pH was adjusted to 7.0, and the mixture was centrifuged at 8000 r / min for 15 minutes. The precipitate was freeze-dried at -40°C for 24 hours to obtain the green tangerine peel extract-polydopamine-chitosan ternary complex.

[0087] A method for processing heat-sealable self-adhesive high-strength medical dialysis paper includes the following steps:

[0088] Step S1: Two-stage pulping: Mix softwood pulp, hardwood pulp and bamboo pulp fibers for one-stage pulping with a freeness of 30°SR. After adding Lyocell fibers, perform a second-stage pulping with a freeness of 45°SR, controlling the average fiber length to 1.0 mm.

[0089] Step S2: Pulp preparation: Add a dual-effect synergistic modifier and an auxiliary modifier to the pulped fiber, stir at 45°C for 30 minutes, then add the functional additives, stir for 15 minutes, and adjust the concentration to 4%;

[0090] Step S3: Forming: Papermaking on an inclined wire paper machine, wire speed 100m / min, press pressure 0.5MPa, pre-drying temperature 90℃, to obtain a basis weight of 50g / m². 2 Dialysis paper substrate;

[0091] Step S4: Gradient coating: First apply the primer layer and dry at 100℃ for 2 minutes, then apply the topcoat layer and dry at 85℃ for 1.5 minutes;

[0092] Step S5: Ultraviolet crosslinking: Irradiation with 254nm ultraviolet light at an intensity of 50mJ / cm 2 Time: 45 seconds; control the crosslinking degree of the adhesive layer to ≥60%.

[0093] Step S6: Post-processing: 0.3MPa soft calendering, edge trimming and winding.

[0094] Furthermore, in step S1, the fiber thickness after the second-stage pulping is 20 μm; the surface adhesive layer is coated using a micro-gravure coating process with a coating accuracy of ±0.2 g / m. 2 .

[0095] Comparative Example 1

[0096] A heat-sealable self-adhesive high-strength medical dialysis paper, comprising a paper base layer and a stepped heat-sealable layer;

[0097] The paper base layer is made from the following raw materials in parts by weight: 60 parts softwood pulp, 12 parts hardwood pulp, 10 parts Lyocell fiber, 6.5 parts bamboo pulp fiber, 4.5 parts dual-effect synergistic modifier, 3.2 parts auxiliary modifier, and 8 parts functional additives.

[0098] The stepped heat-sealing layer consists of a base coat and a top coat. The base coat is a water-based polyurethane-acrylate copolymer with a coating weight of 10 g / m². 2 The topcoat layer consists of medical-grade hot melt adhesive, polyethylene glycol monomethyl ether graft modifier, and nano zinc oxide, with a coating weight of 6 g / m². 2 The amount of nano zinc oxide added is 0.8% of the total mass of the adhesive layer.

[0099] Furthermore, the dual-effect synergistic modifier is an extract of green tangerine peel.

[0100] Furthermore, the auxiliary modifier is a mixture of 2 parts ethyl 3-propionate and 1.2 parts medical-grade polycaprolactone.

[0101] Furthermore, the functional additives include 3 parts polyvinylpyrrolidone, 1.5 parts cationic starch, 0.5 parts wet strength agent, and 2.5 parts inorganic pigment.

[0102] Furthermore, the wet strength agent is polyamide epichlorohydrin, and the inorganic pigment is nano-silica with a particle size of 80nm.

[0103] Furthermore, the preparation method of the dual-effect synergistic modifier includes the following steps:

[0104] Preparation of green tangerine peel extract: The green tangerine peel was crushed to 80 mesh and extracted twice with 70% ethanol solution for 2 hours each time, with a material-to-liquid ratio of 1:15. The extracts were combined and concentrated under reduced pressure to a paste. After purification, the limonene content in the green tangerine peel extract was controlled to be at least 30 mg / g.

[0105] A method for processing heat-sealable self-adhesive high-strength medical dialysis paper includes the following steps:

[0106] Step S1: Two-stage pulping: Mix softwood pulp, hardwood pulp and bamboo pulp fibers for one-stage pulping with a freeness of 30°SR. After adding Lyocell fibers, perform a second-stage pulping with a freeness of 45°SR, controlling the average fiber length to 1.0 mm.

[0107] Step S2: Pulp preparation: Add a dual-effect synergistic modifier and an auxiliary modifier to the pulped fiber, stir at 45°C for 30 minutes, then add the functional additives, stir for 15 minutes, and adjust the concentration to 4%;

[0108] Step S3: Forming: Papermaking on an inclined wire paper machine, wire speed 100m / min, press pressure 0.5MPa, pre-drying temperature 90℃, to obtain a basis weight of 50g / m². 2 Dialysis paper substrate;

[0109] Step S4: Gradient coating: First apply the primer layer and dry at 100℃ for 2 minutes, then apply the topcoat layer and dry at 85℃ for 1.5 minutes;

[0110] Step S5: UV crosslinking: Irradiation with 254nm UV light at an intensity of 45mJ / cm 2 Time: 45 seconds; control the crosslinking degree of the adhesive layer to ≥60%.

[0111] Step S6: Post-processing: 0.3MPa soft calendering, edge trimming and winding.

[0112] Furthermore, in step S1, the fiber thickness after the second-stage pulping is 20 μm; the surface adhesive layer is coated using a micro-gravure coating process with a coating accuracy of ±0.2 g / m. 2 .

[0113] Comparative Example 2

[0114] A heat-sealable self-adhesive high-strength medical dialysis paper, comprising a paper base layer and a stepped heat-sealable layer;

[0115] The paper base layer is made from the following raw materials in parts by weight: 60 parts softwood pulp, 12 parts hardwood pulp, 10 parts Lyocell fiber, 6.5 parts bamboo pulp fiber, 4.5 parts dual-effect synergistic modifier, 3.2 parts auxiliary modifier, and 8 parts functional additives.

[0116] The stepped heat-sealing layer consists of a base coat and a top coat. The base coat is a water-based polyurethane-acrylate copolymer with a coating weight of 10 g / m². 2 The topcoat layer consists of medical-grade hot melt adhesive, polyethylene glycol monomethyl ether graft modifier, and nano zinc oxide, with a coating weight of 6 g / m². 2 The amount of nano zinc oxide added is 0.8% of the total mass of the adhesive layer.

[0117] Furthermore, the dual-effect synergistic modifier is a binary complex of green tangerine peel extract and polydopamine.

[0118] Furthermore, the auxiliary modifier is a mixture of 2 parts ethyl 3-propionate and 1.2 parts medical-grade polycaprolactone.

[0119] Furthermore, the functional additives include 3 parts polyvinylpyrrolidone, 1.5 parts cationic starch, 0.5 parts wet strength agent, and 2.5 parts inorganic pigment.

[0120] Furthermore, the wet strength agent is polyamide epichlorohydrin, the inorganic pigment is nano-silica with a particle size of 80 nm; in the green tangerine peel extract-polydopamine complex, the mass ratio of green tangerine peel extract to polydopamine is 3:1.

[0121] Furthermore, the preparation method of the dual-effect synergistic modifier includes the following steps:

[0122] Step S1: Preparation of green tangerine peel extract: Pulverize green tangerine peel to 80 mesh, reflux extract with 70% ethanol solution twice, 2 hours each time, with a material-to-liquid ratio of 1:15, combine the extracts, concentrate under reduced pressure to a paste, and after purification, control the limonene content in the green tangerine peel extract to be at least 30 mg / g.

[0123] Step S2: Polydopamine pretreatment: Dissolve dopamine hydrochloride in Tris-HCl buffer at pH 8.5 at a concentration of 2 mg / mL, stir for 30 min to form a polydopamine precursor solution;

[0124] Step S3: Binary complex reaction: Add the green tangerine peel extract to the polydopamine precursor solution, stir and react at 50℃ for 2h, adjust the pH to 7.0, centrifuge at 8000r / min for 15min, and freeze-dry the precipitate at -40℃ for 24h to obtain the green tangerine peel extract-polydopamine binary complex.

[0125] A method for processing heat-sealable self-adhesive high-strength medical dialysis paper includes the following steps:

[0126] Step S1: Two-stage pulping: Mix softwood pulp, hardwood pulp and bamboo pulp fibers for one-stage pulping with a freeness of 30°SR. After adding Lyocell fibers, perform a second-stage pulping with a freeness of 45°SR, controlling the average fiber length to 1.0 mm.

[0127] Step S2: Pulp preparation: Add a dual-effect synergistic modifier and an auxiliary modifier to the pulped fiber, stir at 45°C for 30 minutes, then add the functional additives, stir for 15 minutes, and adjust the concentration to 4%;

[0128] Step S3: Forming: Papermaking on an inclined wire paper machine, wire speed 4100m / min, press pressure 0.5MPa, pre-drying temperature 90℃, to obtain a basis weight of 50g / m². 2 Dialysis paper substrate;

[0129] Step S4: Gradient coating: First apply the primer layer and dry at 100℃ for 2 minutes, then apply the topcoat layer and dry at 85℃ for 1.5 minutes;

[0130] Step S5: UV crosslinking: Irradiation with 254nm UV light at an intensity of 45mJ / cm 2 Time: 45 seconds; control the crosslinking degree of the adhesive layer to ≥60%.

[0131] Step S6: Post-processing: 0.3MPa soft calendering, edge trimming and winding.

[0132] Furthermore, in step S1, the fiber thickness after the second-stage pulping is 20 μm; the surface adhesive layer is coated using a micro-gravure coating process with a coating accuracy of ±0.2 g / m. 2 .

[0133] Blank group

[0134] A heat-sealable self-adhesive high-strength medical dialysis paper comprises the following raw materials in parts by weight: 70 parts softwood pulp and 30 parts hardwood pulp.

[0135] A method for processing heat-sealable self-adhesive high-strength medical dialysis paper includes the following steps:

[0136] Step S1: Mix and beat the softwood pulp and hardwood pulp to a beatness of 35°SR;

[0137] Step S2: After pulping, add water to dilute and adjust the pulp concentration to 4%, then stir for 10 minutes;

[0138] Step S3: Forming: Papermaking on an inclined wire paper machine, wire speed 100m / min, press pressure 0.2MPa, pre-drying temperature 80℃, to obtain a basis weight of 50g / m². 2 Dialysis paper;

[0139] Step S4: Post-processing: 0.3MPa soft calendering, edge trimming and winding.

[0140] Experimental Results and Analysis

[0141] Table 1 Results of Physical Strength Orientation Experiment

[0142] Units: Dry tensile strength kN / m; Wet tensile strength kN / m; Tear strength mN

[0143]

[0144] The test methods in the table above are as follows:

[0145] 1. Dry / Wet Tensile Strength (Longitudinal): Tested using a tensile testing machine according to Clause 5.3 of YY / T0698.2-2017 "Terminally Sterilized Medical Device Packaging Part 2: Requirements and Test Methods for Sterilization Wrapping Materials":

[0146] Sample size: 15mm × 180mm (width × length), longitudinal sampling;

[0147] Dry strength test: After the sample is kept at constant temperature and humidity for 24 hours at 23℃ and 50%RH, the test speed is 100mm / min, the maximum force at the time of fracture is recorded, and the tensile strength (kN / m) is calculated.

[0148] Wet strength test: After immersing the sample in distilled water at 23℃ for 30 minutes, the surface moisture is absorbed with filter paper, and the test is immediately carried out under dry strength test conditions. The maximum breaking force is recorded.

[0149] 2. Tear strength (longitudinal): According to clause 5.4 of YY / T 0698.2-2017, the Elemandorf tear strength tester was used for testing.

[0150] Sample size: 63mm×50mm, longitudinal sampling, performed according to the instrument operating procedures, and the maximum tearing force (mN) during the tearing process was recorded.

[0151] 3. Wet-to-dry strength ratio: Calculated by the formula (wet tensile strength ÷ dry tensile strength) × 100%, no additional separate test is required.

[0152] Results analysis:

[0153] 1. Example 2 showed the best performance, with dry and wet tensile strengths of 9.5 kN / m and 4.9 kN / m, respectively, which were 21.8% and 28.9% higher than Comparative Example 2, and 131.7% and 226.7% higher than the blank group, respectively, proving that the synergistic enhancement effect of the ternary composite was significant.

[0154] 2. The wet-to-dry strength ratio is a key indicator of dialysis paper. Example 2 achieved 51.6%, which is much higher than the 36.6% of the blank group. The core reason is that the amino group of chitosan forms a three-dimensional hydrogen bond network with the hydroxyl groups of cellulose and polydopamine phenolic hydroxyl groups, which strengthens the bonding force between fibers.

[0155] 3. In Example 3, due to the excessive amount of chitosan added, some fibers agglomerated, and the strength was slightly lower than that in Example 2, indicating that there is an optimal ratio range for the ternary complex.

[0156] Table 2. Results of the orientation test for heat-sealing self-adhesive properties

[0157] Units: Heat seal peel force (N / 15mm); Self-adhesive opening force (N / 15mm)

[0158]

[0159] The test methods in the table above are as follows:

[0160] 1. Heat seal peel force: According to clause 5.5 of YY / T0698.2-2017, a combination of heat sealer and tensile testing machine is used for testing.

[0161] Heat sealing conditions: Heat seal the sample according to the temperature / pressure / time parameters marked in the table, with a heat sealing area of ​​15mm × 100mm;

[0162] Peel test: After heat sealing, the sample was left to stand for 24 hours at 23℃ and 50%RH, and then peeled at 180° at a speed of 300mm / min. The average peel force was recorded.

[0163] 2. Self-adhesive opening force: The test method is the same as the heat seal peel force. A 180° peel test is performed on the self-adhesive interface of the heat seal layer, and the average force at the opening is recorded.

[0164] 3. Paper scrap-free rate after opening: Select 100 heat-sealed samples, manually open them along the heat-sealed edge, count the number of samples with no visible paper scraps after opening, and calculate the percentage.

[0165] 4. Heat sealing uniformity: The ratio of the standard deviation to the average value of the heat sealing peel force test data of 10 samples in the same group is calculated to reflect the bonding consistency of the heat sealing layer.

[0166] Results analysis:

[0167] 1. Example 2: The heat-sealing peel force reaches 4.3N / 15mm, and the self-adhesive opening force is controlled at 2.3N / 15mm, achieving "easy to open and not easy to break". The paper-free opening rate reaches 99%. The core benefit is the synergy between the gradient heat-sealing layer and the ternary composite: the bottom layer has strong adhesion to avoid delamination, and the top layer is modified hot melt adhesive + nano zinc oxide to improve the heat-sealing uniformity.

[0168] 2. In Example 3, the heat-sealing temperature was reduced to 128°C, but the heat-sealing strength was still high, indicating that the addition of chitosan optimized the interfacial compatibility between the heat-sealing layer and the paper base.

[0169] 3. Comparative Example 1, lacking the reinforcement of a ternary compound, requires a higher heat-sealing temperature to achieve a similar peel strength, and its paper-free opening rate is only 91%, indicating poor heat-sealing uniformity.

[0170] Table 3 Results of the sterilization stability orientation test

[0171] After steam sterilization at 121℃ for 20 minutes

[0172]

[0173] The test methods in the table above are as follows:

[0174] 1. Sterilization treatment: According to clause 5.7 of YY / T0698.2-2017, a high temperature and high pressure steam sterilizer was used to sterilize the samples at 121℃, 20min, and 0.1MPa. After sterilization, the samples were cooled at 23℃ and 50%RH for 24h.

[0175] 2. Retention rate of wet tensile strength / retention rate of heat-sealing peel force: The wet tensile strength and heat-sealing peel force were tested before and after sterilization, respectively, and the results were obtained using the formula...

[0176] (Value after sterilization ÷ Value before sterilization) × 100%

[0177] Calculate the retention rate.

[0178] 3. Air permeability and attenuation rate: Tested according to the "Bentessen method" in GB / T458-2008 "Determination of air permeability of paper and paperboard":

[0179] Sample size: 120 mm in diameter. After standing for 24 hours at 23℃ and 50%RH, the air permeability was tested using a Bentley air permeability meter.

[0180] Air permeability decay rate: calculated using the formula (air permeability before sterilization - air permeability after sterilization) ÷ air permeability before sterilization × 100%.

[0181] 4. Antibacterial rate: According to clause 5.6 of YY / T0698.2-2017, membrane filtration method is adopted:

[0182] The sterilized sample was mixed with an E. coli suspension at a concentration of 10. 5 CFU / mL, after 24 hours of contact, filtered and cultured under aseptic conditions, and the colony count was determined.

[0183] The bacterial inhibition rate (%) is calculated as follows: (number of colonies in the blank group - number of colonies in the sample group) ÷ number of colonies in the blank group × 100%.

[0184] 5. Yellowing Index ΔE: According to GB / T2409-2008 "Determination of Yellowing Index of Plastics", a colorimeter was used to test the yellowing index of samples before and after sterilization. , , The value is calculated using the yellow index formula, ΔE ( This reflects the degree of yellowing of the sample after sterilization.

[0185] Results analysis:

[0186] 1. Example 2 exhibits the best sterilization stability, with a wet tensile strength retention rate of 97.2% and a heat-sealing peel strength retention rate of 94.8%, representing improvements of 8% and 3.6% respectively compared to Comparative Example 2. The core reason is that the three-dimensional cross-linking structure of the ternary compound synergistically inhibits molecular chain degradation during sterilization.

[0187] 2. The antibacterial rate of the example group remained at 100%, and the yellowing index ΔE ≤ 1.2, which was much lower than that of Comparative Example 1 and the blank group. This indicates that the limonene in the ternary complex and the nano zinc oxide synergistically improved the antibacterial stability and anti-yellowing performance.

[0188] 3. The air permeability decay rate is controlled within 3.2%, which not only meets the sterilization steam permeation requirements, but also avoids the deterioration of air permeability after sterilization through the uniform pore structure, achieving a synergy of "high stability and high air permeability".

[0189] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A heat-sealable self-adhesive high-strength medical dialysis paper, characterized in that, Includes a paper base layer and a stepped heat seal layer; The paper base layer is made from the following raw materials in parts by weight: 50-70 parts softwood pulp, 10-15 parts hardwood pulp, 8-12 parts Lyocell fiber, 5-8 parts bamboo pulp fiber, 3-6 parts dual-effect synergistic modifier, 2.3-4.5 parts auxiliary modifier, and 6.3-11.8 parts functional additives; The stepped heat-sealing layer includes a base layer and a topcoat layer. The base layer is a water-based polyurethane-acrylate copolymer with a coating weight of 8-12 g / m². 2 The topcoat layer consists of medical-grade hot melt adhesive, polyethylene glycol monomethyl ether graft modifier, and nano zinc oxide, with a coating weight of 5-8 g / m². 2 The amount of nano zinc oxide added is 0.5-1% of the total mass of the adhesive layer.

2. The heat-sealable self-adhesive high-strength medical dialysis paper according to claim 1, characterized in that, The dual-effect synergistic modifier is a ternary complex of green tangerine peel extract, polydopamine, and chitosan.

3. The heat-sealable self-adhesive high-strength medical dialysis paper according to claim 1, characterized in that, The auxiliary modifier is a mixture of 1.5-3 parts of ethyl 3-propionate and 0.8-1.5 parts of medical-grade polycaprolactone.

4. The heat-sealing self-adhesive high-strength medical dialysis paper according to claim 1, characterized in that, The functional additives include 2-4 parts of polyvinylpyrrolidone, 1-2 parts of cationic starch, 0.3-0.8 parts of wet strength agent, and 2-3 parts of inorganic pigment.

5. The heat-sealable self-adhesive high-strength medical dialysis paper according to claim 1, characterized in that, The wet strength agent is polyamide epichlorohydrin, and the inorganic pigment is nano-silica with a particle size of 50-100nm; in the ternary complex of green tangerine peel extract-polydopamine-chitosan, the mass ratio of green tangerine peel extract, polydopamine and chitosan is 3:(1-2):(1-3).

6. The heat-sealable self-adhesive high-strength medical dialysis paper according to claim 2, characterized in that, The preparation method of the dual-effect synergistic modifier includes the following steps: Step S1: Preparation of green tangerine peel extract: Pulverize green tangerine peel to 80 mesh, reflux extract with 70% ethanol solution twice, 2 hours each time, with a material-to-liquid ratio of 1:15, combine the extracts, concentrate under reduced pressure to a paste, and after purification, control the limonene content in the green tangerine peel extract to be at least 30 mg / g. Step S2: Polydopamine pretreatment: Dissolve dopamine hydrochloride in Tris-HCl buffer at pH 8.5 at a concentration of 2 mg / mL, stir for 30 min to form a polydopamine precursor solution; Step S3: Ternary complex reaction: The green tangerine peel extract and chitosan were mixed at a mass ratio of 2:1, and polydopamine precursor solution was added. The total mass ratio of the three was 3:(1-2):(1-3). The mixture was stirred at 50℃ for 2 hours, the pH was adjusted to 7.0, and the mixture was centrifuged at 8000 r / min for 15 minutes. The precipitate was freeze-dried at -40℃ for 24 hours to obtain the green tangerine peel extract-polydopamine-chitosan ternary complex.

7. A method for processing heat-sealable self-adhesive high-strength medical dialysis paper according to any one of claims 1-6, characterized in that, Includes the following steps: Step S1: Two-stage pulping: Mix softwood pulp, hardwood pulp and bamboo pulp fibers for one-stage pulping with a freeness of 25-30°SR. After adding Lyocell fibers, perform a second-stage pulping with a freeness of 40-45°SR, controlling the average fiber length to 0.8-1.2mm. Step S2: Pulp preparation: Add the dual-effect synergistic modifier and auxiliary modifier to the pulped fiber, stir at 45-50℃ for 30 min, then add the functional additives, stir for 15 min, and adjust the concentration to 3-5%; Step S3: Forming: Papermaking on an inclined wire paper machine, with a wire speed of 80-100 m / min, a press pressure of 0.3-0.5 MPa, and a pre-drying temperature of 80-90℃, yielding a basis weight of 45-60 g / m². 2 Dialysis paper substrate; Step S4: Gradient coating: First apply the primer layer and dry at 100-110℃ for 2 minutes, then apply the topcoat layer and dry at 80-90℃ for 1.5 minutes; Step S5: Ultraviolet crosslinking: Irradiate with 254nm ultraviolet light at an intensity of 30-50mJ / cm. 2 The time is 30-60 seconds, and the cross-linking degree of the adhesive layer is controlled to be ≥60%. Step S6: Post-processing: 0.2-0.3MPa soft calendering, edge trimming and winding.

8. The processing method of a heat-sealing self-adhesive high-strength medical dialysis paper according to claim 7, characterized in that, In step S1, the fiber coarseness after the two-stage pulping is 15-20 μm; the surface adhesive layer is coated using a micro-gravure coating process with a coating accuracy of ±0.2 g / m. 2 .

Citation Information

Patent Citations

  • A high-strength medical dialysis paper and its preparation method

    CN113089373B

  • Glued dialyzing paper for sterilizing and packaging medical instruments

    CN213949323U