A method for synthesizing a metal-modified molybdenum-based composite sulfide catalyst and its application
The metal-modified molybdenum-based composite sulfide catalyst prepared by the complex gel method solves the problems of complex preparation and uneven distribution of active phase in the existing technology of Mo-based catalysts, and realizes efficient CO hydrogenation reaction and selectivity of methanethiol.
Patent Information
- Application Number
- CN202611363807.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-10
AI Technical Summary
Existing Mo-based catalysts have complex preparation processes, high costs, limited dispersion of active components, and separation of the sulfidation process from the catalyst forming process, resulting in uneven distribution of the active phase and affecting catalytic performance.
Metal-modified molybdenum-based composite sulfide catalysts were prepared by complexation gel method. Citric acid and polyethylene glycol were added to a soluble salt solution to form a sol, which was then dried and heat-treated in an oxygen-free atmosphere. Alkali metal sulfides were physically mixed to form tightly cross-linked composite sulfide catalysts.
It achieves high activity and high selectivity of catalyst, with CO conversion rate ≥50% and methanethiol selectivity ≥70% in CO hydrogenation reaction, significantly improving catalytic performance.
Smart Images

Figure CN123059664A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of producing methanethiol from hydrogen sulfide and syngas (a mixture of hydrogen and carbon monoxide), and particularly to the field of catalysts used in the production of methanethiol from hydrogen sulfide and syngas. Background Technology
[0002] Methanethiol (CH3SH) is an important chemical raw material for the synthesis of methionine, pharmaceuticals, and pesticides, and a key intermediate in the production of the feed additive methionine. Traditional methanethiol production processes mainly involve the reaction of potassium hydrosulfide with halomethanes or the thiolation reaction of methanol with H2S, which suffer from long process routes and high costs. A one-step synthesis of methanethiol from syngas containing H2S (CO / H2) is a short process route with great industrial application potential. In recent years, sulfur-resistant Mo-based catalysts have attracted widespread attention due to their excellent catalytic performance in CO / H2 / H2S systems. Studies have shown that alkali metal-promoted MoS2 catalysts are the most promising catalytic system for the direct production of methanethiol from syngas.
[0003] In existing technologies, the preparation of Mo-based catalysts mostly adopts impregnation or co-precipitation methods, which result in limited dispersion of active components and separation of the sulfidation process from the catalyst forming process, leading to uneven distribution of the active phase. Summary of the Invention
[0004] The technical problem to be solved by this invention is: how to provide a metal-modified molybdenum-based composite sulfide catalyst for the production of methanethiol from hydrogen sulfide and syngas (a mixture of hydrogen and carbon monoxide) with simple preparation process, low cost and excellent catalytic performance.
[0005] The technical solution adopted in this invention is: a method for synthesizing a metal-modified molybdenum-based composite sulfide catalyst, which is carried out according to the following steps: Step 1: Add citric acid to the homogeneous aqueous solution of the soluble salt corresponding to element X, and stir to form a transparent first solution, wherein the molar ratio of element X to citric acid is 0.2-1; Step 2: The molar ratio of polyethylene glycol to citric acid is 0.1-2. Polyethylene glycol is added to the first solution as an esterifying agent and stirred continuously to form a sol solution. After stirring the sol solution continuously at 70-100℃ for 1-5 hours, a gel is obtained. The gel is dried at 100-150℃ to form a dry gel. The dry gel is heat-treated at 300-800℃ for 2-8 hours in an oxygen-free atmosphere to obtain a solid powder for later use. Step 3: Add citric acid to the homogeneous aqueous solution of ammonium molybdate and stir to form a transparent second solution, wherein the molar ratio of molybdenum to citric acid is 0.2-1; Step 4: With a molar ratio of polyethylene glycol to citric acid of 0.1-2, polyethylene glycol is added to the second solution as an esterifying agent. With a molar ratio of element X to molybdenum of 0.1-10, the prepared solid powder is added to the second solution. After stirring continuously at 70-100℃ for 1-5 hours, a gel is obtained. This gel is dried at 100-150℃ to form a dry gel. With a mass ratio of dry gel to sulfide corresponding to alkali metal element Y of 0.1-10, this dry gel and the sulfide corresponding to alkali metal element Y are physically mixed. Then, under an oxygen-free atmosphere, it is heat-treated at 300-800℃ for 2-8 hours to obtain the YX-Mo composite sulfide catalyst, i.e., the metal-modified molybdenum-based composite sulfide catalyst.
[0006] The element X is one of Be, Mg, Ca, Ba, Co, Ni, Cu, Nb, Rh, Pd, Pt, Cd, Ga, La, In, Ru, Ti, Zr, Ce, Zn, Fe, Cr, W, Ag, Si, or Al; the alkali metal element Y is one of Li, Na, K, Rb, or Cs.
[0007] The soluble salts corresponding to element X are beryllium chloride, beryllium nitrate, beryllium sulfate, magnesium chloride, magnesium nitrate, magnesium sulfate, calcium chloride, calcium nitrate, barium chloride, barium nitrate, cobalt chloride, cobalt nitrate, cobalt sulfate, nickel chloride, nickel nitrate, nickel sulfate, copper chloride, copper nitrate, copper sulfate, niobium chloride, niobium nitrate, niobium sulfate, rhodium chloride, rhodium nitrate, rhodium sulfate, palladium chloride, palladium nitrate, palladium sulfate, platinum chloride, platinum nitrate, platinum sulfate, cadmium chloride, cadmium nitrate, cadmium sulfate, gallium chloride, gallium nitrate, gallium sulfate, lanthanum chloride, and nitrate. Lanthanum sulfate, lanthanum nitrate, indium sulfate, indium chloride, ruthenium nitrate, ruthenium sulfate, ruthenium chloride, titanium nitrate, zirconium chloride, zirconium nitrate, zirconium sulfate, cerium chloride, cerium nitrate, cerium sulfate, zinc chloride, zinc nitrate, zinc sulfate, ferric chloride, ferric nitrate, ferric sulfate, chromium chloride, chromium nitrate, chromium sulfate, silver nitrate, lithium silicate, sodium silicate, potassium silicate, aluminum chloride, aluminum nitrate, or aluminum sulfate; the sulfide corresponding to the alkali metal element Y is one of lithium sulfide, sodium sulfide, potassium sulfide, rubidium sulfide, or cesium sulfide.
[0008] The oxygen-free atmosphere is any one of nitrogen, argon, helium, hydrogen, methane, or carbon monoxide.
[0009] An application of a metal-modified molybdenum-based composite sulfide catalyst for the production of methanethiol from H2S and syngas is described. The catalyst, prepared with a 40-60 mesh metal element modification, is uniformly mixed with quartz sand and then loaded into a fixed-bed reactor. The H2 / CO ratio in the H2S and syngas is controlled at 0.1-10 using a mass flow meter, and the molar ratio of H2S to (H2+CO) is also 0.1-10. The volume hourly space velocity (VHSV) is 300-15000 h⁻¹. -1The reaction conditions are: reaction temperature 200-400℃, reaction pressure 2.5-12MPa, and reaction time 5-100 hours.
[0010] The beneficial effects of the present invention are: the metal-modified molybdenum-based composite sulfide catalyst prepared by the present invention has excellent CO hydrogenation catalytic activity and methanethiol selectivity. In the production of methanethiol from H2S and syngas, the CO conversion rate is generally ≥50% and the methanethiol selectivity is generally ≥70%.
[0011] This invention utilizes a complexation-gel process to tightly crosslink metal elements with a molybdenum-based composite, achieving uniform mixing at the microscale. Simultaneously, sulfidation under oxygen-free conditions is completed in both time and dimension through the action of sulfides, causing the catalyst particles to undergo sulfidation reactions. This process yields a metal-modified molybdenum-based composite sulfide catalyst exhibiting extremely high activity towards syngas and selectivity for methanethiol. By using the sulfide and metal composite phase as the main active components, highly stable and highly selective catalytic synthesis of methanethiol from syngas is achieved.
[0012] In this invention, the introduction of alkali metals (such as Li, Na, K, Rb, Cs, etc.) significantly enhances the performance of MoS2 in catalytic synthesis of methanethiol. The introduction of transition metals (such as Co, Ni, Fe, La, Ce, etc.) further improves catalytic activity and selectivity. This invention achieves molecular-level homogeneous mixing of multiple components through a complexation gel method, followed by in-situ sulfidation to form a highly active composite sulfide phase, fully leveraging the synergistic catalytic effect among the components. Attached Figure Description
[0013] Figure 1 The results are from the 100-hour reaction of the Cs-La-Mo composite sulfide catalyst in Example 33. Detailed Implementation
[0014] The present invention will be further illustrated below through specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. All technologies implemented based on the above description of the present invention fall within the scope of the present invention.
[0015] Example 1: A method for synthesizing a metal-modified molybdenum-based composite sulfide catalyst, comprising the following steps. Step 1: Dissolve 10g of nickel nitrate (Ni(NO3)2·6H2O) in 100mL of deionized water to obtain a homogeneous aqueous solution of nickel nitrate. Add citric acid to the homogeneous aqueous solution of nickel nitrate and stir to form a transparent first solution. The molar ratio of elemental nickel to citric acid is 1. Step 2: The molar ratio of polyethylene glycol to citric acid is 0.1. Polyethylene glycol is added to the first solution as an esterifying agent and continuously stirred to form a sol solution. After stirring this sol solution continuously at 70°C for 5 hours, a gel is obtained. This gel is dried at 100°C to form a dry gel. The dry gel is heat-treated at 300°C for 8 hours in an oxygen-free atmosphere to obtain a solid powder for later use. Step 3: Add citric acid to the homogeneous aqueous solution of ammonium molybdate and stir to form a transparent second solution, wherein the molar ratio of molybdenum to citric acid is 1. Step 4: With a molar ratio of polyethylene glycol to citric acid of 0.1, polyethylene glycol is added to the second solution as an esterifying agent. With a molar ratio of nickel to molybdenum of 0.1, the prepared solid powder is added to the second solution. After stirring continuously at 70°C for 5 hours, a gel is obtained. This gel is dried at 100°C to form a dry gel. With a mass ratio of dry gel to potassium sulfide of 0.1, this dry gel and potassium sulfide are physically mixed. Then, under an oxygen-free atmosphere, it is heat-treated at 300°C for 8 hours to obtain a metal-modified molybdenum-based composite sulfide catalyst (K-Ni-Mo composite sulfide catalyst).
[0016] An application of a metal-modified molybdenum-based composite sulfide catalyst for the production of methanethiol from H2S and syngas is described. A 40-60 mesh K-Ni-Mo composite sulfide catalyst is uniformly mixed with quartz sand and then loaded into a fixed-bed reactor. The reactor is operated with an H2 / CO ratio of 0.1, an H2S / (H2+CO) molar ratio of 0.1, and a volume hourly space velocity (VHSV) of 300 h⁻¹. -1 The reaction was carried out at a temperature of 200℃ and a pressure of 2.5MPa for 5 hours. The CO conversion rate was 52%, and the methanethiol selectivity was 72 wt.%.
[0017] Example 2: A method for synthesizing a metal-modified molybdenum-based composite sulfide catalyst, comprising the following steps. Step 1: Dissolve 15g of cobalt nitrate (Co(NO3)2·6H2O) in 120mL of deionized water to obtain a homogeneous aqueous solution of cobalt nitrate. Add citric acid to the homogeneous aqueous solution of cobalt nitrate and stir to form a transparent first solution. The molar ratio of elemental cobalt to citric acid is 1:3. Step 2: The molar ratio of polyethylene glycol to citric acid is 1.0. Polyethylene glycol is added to the first solution as an esterifying agent and stirred continuously to form a sol solution. After stirring the sol solution continuously at 85°C for 3 hours, a gel is obtained. The gel is dried at 125°C to form a dry gel. The dry gel is heat-treated at 550°C for 5 hours in an oxygen-free atmosphere to obtain a solid powder for later use. Step 3: Add citric acid to the homogeneous aqueous solution of ammonium molybdate and stir to form a transparent second solution, wherein the molar ratio of molybdenum to citric acid is 1:3; Step 4: With a molar ratio of polyethylene glycol to citric acid of 1.0, polyethylene glycol is added to the second solution as an esterifying agent. With a molar ratio of cobalt to molybdenum of 5, the prepared solid powder is added to the second solution. After stirring continuously at 85°C for 3 hours, a gel is obtained. This gel is dried at 125°C to form a dry gel. With a mass ratio of dry gel to sodium sulfide of 5, this dry gel and sodium sulfide are physically mixed. Then, under an oxygen-free atmosphere, it is heat-treated at 300°C for 8 hours to obtain a metal-modified molybdenum-based composite sulfide catalyst (Na-Co-Mo composite sulfide catalyst).
[0018] An application of a metal-modified molybdenum-based composite sulfide catalyst for the production of methanethiol from H2S and syngas involves uniformly mixing a 40-60 mesh Na-Co-Mo composite sulfide catalyst with quartz sand and then loading the mixture into a fixed-bed reactor. The reactor is operated with an H2 / CO ratio of 5, an H2S / (H2+CO) molar ratio of 5, and a volume hourly space velocity of 7500 h⁻¹. -1 The reaction was carried out at a temperature of 300℃ and a pressure of 7MPa for 50 hours. The CO conversion rate was 65%, and the methanethiol selectivity was 85 wt.%.
[0019] Example 3: A method for synthesizing a metal-modified molybdenum-based composite sulfide catalyst, comprising the following steps. Step 1: Dissolve 20g of lanthanum nitrate (La(NO3)3•6H2O) in 150mL of deionized water to obtain a homogeneous aqueous solution of lanthanum nitrate. Add citric acid to the homogeneous aqueous solution of lanthanum nitrate and stir to form a transparent first solution. The molar ratio of elemental lanthanum to citric acid is 1:5. Step 2: The molar ratio of polyethylene glycol to citric acid is 2.0. Polyethylene glycol is added to the first solution as an esterifying agent and stirred continuously to form a sol solution. After stirring the sol solution continuously at 100°C for 1 hour, a gel is obtained. The gel is dried at 150°C to form a dry gel. The dry gel is heat-treated at 800°C for 2 hours in an oxygen-free atmosphere to obtain a solid powder for later use. Step 3: Add citric acid to the homogeneous aqueous solution of ammonium molybdate and stir to form a transparent second solution, wherein the molar ratio of molybdenum to citric acid is 1:5; Step 4: With a molar ratio of polyethylene glycol to citric acid of 2.0, polyethylene glycol is added to the second solution as an esterifying agent. With a molar ratio of lanthanum to molybdenum of 10, the prepared solid powder is added to the second solution. After stirring continuously at 100°C for 1 hour, a gel is obtained. This gel is dried at 150°C to form a dry gel. With a mass ratio of dry gel to cesium sulfide of 10, this dry gel and cesium sulfide are physically mixed. Then, under an oxygen-free atmosphere, it is heat-treated at 300°C for 8 hours to obtain a metal-modified molybdenum-based composite sulfide catalyst (Cs-La-Mo composite sulfide catalyst).
[0020] An application of a metal-modified molybdenum-based composite sulfide catalyst for the production of methanethiol from H2S and syngas involves uniformly mixing a 40-60 mesh Na-Co-Mo composite sulfide catalyst with quartz sand and then loading the mixture into a fixed-bed reactor. The reactor is operated with an H2 / CO ratio of 10, an H2S / (H2+CO) molar ratio of 10, and a volume hourly space velocity (VHSV) of 15000 h⁻¹. -1 The reaction was carried out at a temperature of 400℃ and a pressure of 12MPa for 100 hours. The CO conversion rate was 72%, and the methanethiol selectivity was 96 wt.%.
[0021] Example 4: The same preparation method as in Example 1 was used, except that element X was Fe (ferric nitrate), alkali metal Y was K, the molar ratio of X to citric acid was 1:1, the molar ratio of polyethylene glycol to citric acid was 0.1, the molar ratio of X to Mo was 0.1, the mass ratio of dry gel to sulfide was 0.1, the heat treatment temperature was 300℃, and the heat treatment time was 8 hours.
[0022] The application conditions are the same as in Example 1, with a CO conversion rate of 50% and a methanethiol selectivity of 70 wt.%.
[0023] Example 5: The same preparation method as in Example 2 was used, except that element X was Ce (cerium nitrate), alkali metal Y was K, the molar ratio of X to citric acid was 1:3, the molar ratio of polyethylene glycol to citric acid was 1.0, the molar ratio of X to Mo was 5, the mass ratio of dry gel to sulfide was 5, the heat treatment temperature was 550℃, and the heat treatment time was 5 hours.
[0024] The application conditions were the same as in Example 2, with a CO conversion rate of 63% and a methanethiol selectivity of 82 wt.%.
[0025] Example 6: The same preparation method as in Example 3 was used, except that element X was Zn (zinc nitrate), alkali metal Y was K, the molar ratio of X to citric acid was 1:5, the molar ratio of polyethylene glycol to citric acid was 2.0, the molar ratio of X to Mo was 10, the mass ratio of dry gel to sulfide was 10, the heat treatment temperature was 800℃, and the heat treatment time was 2 hours.
[0026] The application conditions were the same as in Example 3, with a CO conversion rate of 68% and a methanethiol selectivity of 91 wt.%.
[0027] Example 7: The same preparation method as in Example 1 was used, except that element X was Mg (magnesium nitrate), alkali metal Y was K, the molar ratio of X to citric acid was 1:2, the molar ratio of polyethylene glycol to citric acid was 0.5, the molar ratio of X to Mo was 1, the mass ratio of dry gel to sulfide was 2, the heat treatment temperature was 400℃, and the heat treatment time was 6 hours. The sol stirring temperature was 80℃, and the stirring time was 4 hours; the gel drying temperature was 120℃.
[0028] An application of a metal-modified molybdenum-based composite sulfide catalyst for the production of methanethiol from H2S and syngas involves uniformly mixing a 40-60 mesh K-Mg-Mo composite sulfide catalyst with quartz sand and then loading the mixture into a fixed-bed reactor. The reactor is operated with an H2 / CO ratio of 2, an H2S / (H2+CO) molar ratio of 2, and a volume hourly space velocity of 3000 h⁻¹. -1 The reaction was carried out at a temperature of 250℃ and a pressure of 5MPa for 20 hours. The CO conversion rate was 58%, and the methanethiol selectivity was 78 wt.%.
[0029] Example 8: The same preparation method as in Example 2 was used, except that element X was Ca (calcium nitrate) and alkali metal Y was K. The molar ratio of X to citric acid was 1:4, the molar ratio of polyethylene glycol to citric acid was 1.5, the molar ratio of X to Mo was 3, the mass ratio of dry gel to sulfide was 3, the heat treatment temperature was 600℃, and the heat treatment time was 4 hours.
[0030] An application of a metal-modified molybdenum-based composite sulfide catalyst for the production of methanethiol from H2S and syngas involves uniformly mixing a 40-60 mesh K-Ca-Mo composite sulfide catalyst with quartz sand and then loading the mixture into a fixed-bed reactor. The reactor is operated with an H2 / CO ratio of 3, an H2S / (H2+CO) molar ratio of 3, and a volume hourly space velocity of 5000 h⁻¹. -1 The reaction was carried out at a temperature of 280℃ and a pressure of 6MPa for 20 hours. The CO conversion rate was 60%, and the methanethiol selectivity was 80 wt.%.
[0031] Example 9: The same preparation method as in Example 3 was used, except that element X was Ba (barium nitrate) and alkali metal Y was K. The molar ratio of X to citric acid was 1:1, the molar ratio of polyethylene glycol to citric acid was 0.2, the molar ratio of X to Mo was 0.5, the mass ratio of dry gel to sulfide was 1, the heat treatment temperature was 350℃, and the heat treatment time was 7 hours.
[0032] An application of a metal-modified molybdenum-based composite sulfide catalyst for the production of methanethiol from H2S and syngas involves uniformly mixing a 40-60 mesh K-Ba-Mo composite sulfide catalyst with quartz sand and then loading the mixture into a fixed-bed reactor. The reactor is operated with an H2 / CO ratio of 1, an H2S / (H2+CO) molar ratio of 1, and a volume hourly space velocity (VHSV) of 1000 h⁻¹. -1 The reaction was carried out at a temperature of 220℃ and a pressure of 3MPa for 10 hours. The CO conversion rate was 54%, and the methanethiol selectivity was 74 wt.%.
[0033] Example 10: The same preparation method as in Example 1 was used, except that element X was Cu (copper nitrate) and alkali metal Y was K. The molar ratio of X to citric acid was 1:3, the molar ratio of polyethylene glycol to citric acid was 0.8, the molar ratio of X to Mo was 2, the mass ratio of dry gel to sulfide was 4, the heat treatment temperature was 500℃, and the heat treatment time was 5 hours.
[0034] An application of a metal-modified molybdenum-based composite sulfide catalyst for the production of methanethiol from H2S and syngas involves uniformly mixing a 40-60 mesh K-Cu-Mo composite sulfide catalyst with quartz sand and then loading the mixture into a fixed-bed reactor. The reactor is operated with an H2 / CO ratio of 4, an H2S / (H2+CO) molar ratio of 4, and a volume hourly space velocity of 6000 h⁻¹. -1 The reaction was carried out at a temperature of 290℃ and a pressure of 8MPa for 40 hours. The CO conversion rate was 62%, and the methanethiol selectivity was 83 wt.%.
[0035] Example 11: The same preparation method as in Example 2 was used, except that element X was Nb (niobium nitrate) and alkali metal Y was K. The molar ratio of X to citric acid was 1:2, the molar ratio of polyethylene glycol to citric acid was 1.2, the molar ratio of X to Mo was 4, the mass ratio of dry gel to sulfide was 6, the heat treatment temperature was 650℃, and the heat treatment time was 3 hours.
[0036] An application of a metal-modified molybdenum-based composite sulfide catalyst for the production of methanethiol from H2S and syngas involves uniformly mixing a 40-60 mesh K-Nb-Mo composite sulfide catalyst with quartz sand and then loading the mixture into a fixed-bed reactor. The reactor is operated with an H2 / CO ratio of 6, an H2S / (H2+CO) molar ratio of 6, and a volume hourly space velocity (VHSV) of 9000 h⁻¹. -1 The reaction was carried out at a temperature of 320℃ and a pressure of 9MPa for 60 hours. The CO conversion rate was 66%, and the methanethiol selectivity was 88 wt.%.
[0037] Example 12: The same preparation method as in Example 3 was used, except that element X was Rh (rhodium nitrate) and alkali metal Y was K. The molar ratio of X to citric acid was 1:4, the molar ratio of polyethylene glycol to citric acid was 1.8, the molar ratio of X to Mo was 8, the mass ratio of dry gel to sulfide was 8, the heat treatment temperature was 700℃, and the heat treatment time was 2 hours.
[0038] An application of a metal-modified molybdenum-based composite sulfide catalyst for the production of methanethiol from H2S and syngas involves uniformly mixing a 40-60 mesh K-Rh-Mo composite sulfide catalyst with quartz sand and then loading the mixture into a fixed-bed reactor. The reactor is operated with an H2 / CO ratio of 8, an H2S / (H2+CO) molar ratio of 8, and a volume hourly space velocity (VHSV) of 12000 h⁻¹. -1 The reaction was carried out at a temperature of 350℃ and a pressure of 10MPa for 80 hours. The CO conversion rate was 70%, and the methanethiol selectivity was 94 wt.%.
[0039] Example 13: The same preparation method as in Example 1 was used, except that element X was Pd (palladium nitrate) and alkali metal Y was K. The molar ratio of X to citric acid was 1:5, the molar ratio of polyethylene glycol to citric acid was 2.0, the molar ratio of X to Mo was 10, the mass ratio of dry gel to sulfide was 10, the heat treatment temperature was 800℃, and the heat treatment time was 2 hours.
[0040] An application of a metal-modified molybdenum-based composite sulfide catalyst for the production of methanethiol from H2S and syngas involves uniformly mixing a 40-60 mesh K-Pd-Mo composite sulfide catalyst with quartz sand and then loading the mixture into a fixed-bed reactor. The reactor is operated with an H2 / CO ratio of 10, an H2S / (H2+CO) molar ratio of 10, and a volume hourly space velocity (VHSV) of 15000 h⁻¹. -1 The reaction was carried out at a temperature of 400℃ and a pressure of 12MPa for 100 hours. The CO conversion rate was 73%, and the methanethiol selectivity was 97 wt.%.
[0041] Example 14: The same preparation method as in Example 2 was used, except that element X was Pt (platinum nitrate) and alkali metal Y was Na. The molar ratio of X to citric acid was 1:1, the molar ratio of polyethylene glycol to citric acid was 0.1, the molar ratio of X to Mo was 0.1, the mass ratio of dry gel to sulfide was 0.1, the heat treatment temperature was 300℃, and the heat treatment time was 8 hours.
[0042] The application conditions were the same as in Example 1, with a CO conversion rate of 51% and a methanethiol selectivity of 71 wt.%.
[0043] Example 15: The same preparation method as in Example 3 was used, except that element X was Cd (cadmium nitrate) and alkali metal Y was Na. The molar ratio of X to citric acid was 1:3, the molar ratio of polyethylene glycol to citric acid was 1.0, the molar ratio of X to Mo was 5, the mass ratio of dry gel to sulfide was 5, the heat treatment temperature was 550℃, and the heat treatment time was 5 hours.
[0044] The application conditions were the same as in Example 2, with a CO conversion rate of 64% and a methanethiol selectivity of 84 wt.%.
[0045] Example 16: The same preparation method as in Example 1 was used, except that element X was Ga (gallium nitrate) and alkali metal Y was Na. The molar ratio of X to citric acid was 1:5, the molar ratio of polyethylene glycol to citric acid was 2.0, the molar ratio of X to Mo was 10, the mass ratio of dry gel to sulfide was 10, the heat treatment temperature was 800℃, and the heat treatment time was 2 hours.
[0046] The application conditions were the same as in Example 3, with a CO conversion rate of 69% and a methanethiol selectivity of 92 wt.%.
[0047] Example 17: The same preparation method as in Example 2 was used, except that element X was In (indium nitrate) and alkali metal Y was Na. The molar ratio of X to citric acid was 1:2, the molar ratio of polyethylene glycol to citric acid was 0.5, the molar ratio of X to Mo was 1, the mass ratio of dry gel to sulfide was 2, the heat treatment temperature was 400℃, and the heat treatment time was 6 hours.
[0048] The application conditions were the same as in Example 7, with a CO conversion rate of 59% and a methanethiol selectivity of 79 wt.%.
[0049] Example 18: The same preparation method as in Example 3 was used, except that element X was Ru (ruthenium nitrate) and alkali metal Y was Na. The molar ratio of X to citric acid was 1:4, the molar ratio of polyethylene glycol to citric acid was 1.5, the molar ratio of X to Mo was 3, the mass ratio of dry gel to sulfide was 3, the heat treatment temperature was 600℃, and the heat treatment time was 4 hours.
[0050] The application conditions were the same as in Example 8, with a CO conversion rate of 61% and a methanethiol selectivity of 81 wt.%.
[0051] Example 19: The same preparation method as in Example 1 was used, except that element X was Ti (titanium nitrate) and alkali metal Y was Na. The molar ratio of X to citric acid was 1:1, the molar ratio of polyethylene glycol to citric acid was 0.2, the molar ratio of X to Mo was 0.5, the mass ratio of dry gel to sulfide was 1, the heat treatment temperature was 350℃, and the heat treatment time was 7 hours.
[0052] The application conditions are the same as in Example 9, with a CO conversion rate of 55% and a methanethiol selectivity of 75 wt.%.
[0053] Example 20: The same preparation method as in Example 2 was used, except that element X was Zr (zirconium nitrate) and alkali metal Y was Na. The molar ratio of X to citric acid was 1:3, the molar ratio of polyethylene glycol to citric acid was 0.8, the molar ratio of X to Mo was 2, the mass ratio of dry gel to sulfide was 4, the heat treatment temperature was 500℃, and the heat treatment time was 5 hours.
[0054] The application conditions were the same as in Example 10, with a CO conversion rate of 63% and a methanethiol selectivity of 83 wt.%.
[0055] Example 21: The same preparation method as in Example 3 was used, except that element X was Cr (chromium nitrate) and alkali metal Y was Na. The molar ratio of X to citric acid was 1:2, the molar ratio of polyethylene glycol to citric acid was 1.2, the molar ratio of X to Mo was 4, the mass ratio of dry gel to sulfide was 6, the heat treatment temperature was 650℃, and the heat treatment time was 3 hours.
[0056] The application conditions were the same as in Example 11, with a CO conversion rate of 67% and a methanethiol selectivity of 89 wt.%.
[0057] Example 22: The same preparation method as in Example 1 was used, except that element X was W (ammonium tungstate) and alkali metal Y was Na. The molar ratio of X to citric acid was 1:4, the molar ratio of polyethylene glycol to citric acid was 1.8, the molar ratio of X to Mo was 8, the mass ratio of dry gel to sulfide was 8, the heat treatment temperature was 700℃, and the heat treatment time was 2 hours.
[0058] The application conditions were the same as in Example 12, with a CO conversion rate of 71% and a methanethiol selectivity of 95 wt.%.
[0059] Example 23: The same preparation method as in Example 2 was used, except that element X was Ag (silver nitrate) and alkali metal Y was Li. The molar ratio of X to citric acid was 1:1, the molar ratio of polyethylene glycol to citric acid was 0.1, the molar ratio of X to Mo was 0.1, the mass ratio of dry gel to sulfide was 0.1, the heat treatment temperature was 300℃, and the heat treatment time was 8 hours.
[0060] The application conditions were the same as in Example 3, with a CO conversion rate of 74% and a methanethiol selectivity of 94 wt.%.
[0061] Example 24: The same preparation method as in Example 3 was used, except that element X was Si (lithium silicate) and alkali metal Y was Li. The molar ratio of X to citric acid was 1:3, the molar ratio of polyethylene glycol to citric acid was 1.0, the molar ratio of X to Mo was 5, the mass ratio of dry gel to sulfide was 5, the heat treatment temperature was 550℃, and the heat treatment time was 5 hours.
[0062] The application conditions were the same as in Example 2, with a CO conversion rate of 62% and a methanethiol selectivity of 82 wt.%.
[0063] Example 25: The same preparation method as in Example 1 was used, except that element X was Al (aluminum nitrate) and alkali metal Y was Li. The molar ratio of X to citric acid was 1:5, the molar ratio of polyethylene glycol to citric acid was 2.0, the molar ratio of X to Mo was 10, the mass ratio of dry gel to sulfide was 10, the heat treatment temperature was 800℃, and the heat treatment time was 2 hours.
[0064] The application conditions were the same as in Example 3, with a CO conversion rate of 67% and a methanethiol selectivity of 90 wt.%.
[0065] Example 26: The same preparation method as in Example 2 was used, except that element X was Be (beryllium nitrate) and alkali metal Y was Li. The molar ratio of X to citric acid was 1:2, the molar ratio of polyethylene glycol to citric acid was 0.5, the molar ratio of X to Mo was 1, the mass ratio of dry gel to sulfide was 2, the heat treatment temperature was 400℃, and the heat treatment time was 6 hours.
[0066] The application conditions were the same as in Example 7, with a CO conversion rate of 57% and a methanethiol selectivity of 77 wt.%.
[0067] Example 27: The same preparation method as in Example 3 was used, except that element X was Co (cobalt nitrate) and alkali metal Y was Rb. The molar ratio of X to citric acid was 1:1, the molar ratio of polyethylene glycol to citric acid was 0.2, the molar ratio of X to Mo was 0.5, the mass ratio of dry gel to sulfide was 1, the heat treatment temperature was 350°C, and the heat treatment time was 7 hours.
[0068] The application conditions were the same as in Example 9, with a CO conversion rate of 56% and a methanethiol selectivity of 76 wt.%.
[0069] Example 28: The same preparation method as in Example 1 was used, except that element X was Ni (nickel nitrate) and alkali metal Y was Rb. The molar ratio of X to citric acid was 1:3, the molar ratio of polyethylene glycol to citric acid was 0.8, the molar ratio of X to Mo was 2, the mass ratio of dry gel to sulfide was 4, the heat treatment temperature was 500℃, and the heat treatment time was 5 hours.
[0070] The application conditions were the same as in Example 10, with a CO conversion rate of 64% and a methanethiol selectivity of 84 wt.%.
[0071] Example 29: The same preparation method as in Example 2 was used, except that element X was La (lanthanum nitrate) and alkali metal Y was Rb. The molar ratio of X to citric acid was 1:4, the molar ratio of polyethylene glycol to citric acid was 1.5, the molar ratio of X to Mo was 3, the mass ratio of dry gel to sulfide was 3, the heat treatment temperature was 600℃, and the heat treatment time was 4 hours.
[0072] The application conditions were the same as in Example 8, with a CO conversion rate of 62% and a methanethiol selectivity of 82 wt.%.
[0073] Example 30: The same preparation method as in Example 3 was used, except that element X was Ce (cerium nitrate) and alkali metal Y was Rb. The molar ratio of X to citric acid was 1:2, the molar ratio of polyethylene glycol to citric acid was 1.2, the molar ratio of X to Mo was 4, the mass ratio of dry gel to sulfide was 6, the heat treatment temperature was 650°C, and the heat treatment time was 3 hours.
[0074] The application conditions are the same as in Example 11, with a CO conversion rate of 68% and a methanethiol selectivity of 90 wt.%.
[0075] Example 31: The same preparation method as in Example 1 was used, except that element X was Fe (ferric nitrate) and alkali metal Y was Cs. The molar ratio of X to citric acid was 1:1, the molar ratio of polyethylene glycol to citric acid was 0.1, the molar ratio of X to Mo was 0.1, the mass ratio of dry gel to sulfide was 0.1, the heat treatment temperature was 300℃, and the heat treatment time was 8 hours.
[0076] The application conditions were the same as in Example 1, with a CO conversion rate of 53% and a methanethiol selectivity of 73 wt.%.
[0077] Example 32: The same preparation method as in Example 2 was used, except that element X was Co (cobalt nitrate) and alkali metal Y was Cs. The molar ratio of X to citric acid was 1:3, the molar ratio of polyethylene glycol to citric acid was 1.0, the molar ratio of X to Mo was 5, the mass ratio of dry gel to sulfide was 5, the heat treatment temperature was 550℃, and the heat treatment time was 5 hours.
[0078] The application conditions were the same as in Example 2, with a CO conversion rate of 67% and a methanethiol selectivity of 87 wt.%.
[0079] Example 33: The same preparation method as in Example 3 was used, except that element X was La (lanthanum nitrate) and alkali metal Y was Cs. The molar ratio of X to citric acid was 1:5, the molar ratio of polyethylene glycol to citric acid was 2.0, the molar ratio of X to Mo was 10, the mass ratio of dry gel to sulfide was 10, the heat treatment temperature was 800℃, and the heat treatment time was 2 hours.
[0080] The application conditions were the same as in Example 3, with a CO conversion rate of 74% and a methanethiol selectivity of 98 wt.%.
[0081] Example 34: The same preparation method as in Example 1 was used, except that the oxygen-free atmosphere was hydrogen atmosphere, and the other conditions were the same as in Example 1.
[0082] The application conditions are the same as in Example 1, with a CO conversion rate of 55% and a methanethiol selectivity of 74 wt.%.
[0083] Example 35: The same preparation method as in Example 2 was used, except that the oxygen-free atmosphere was a methane atmosphere, and the other conditions were the same as in Example 2.
[0084] The application conditions were the same as in Example 2, with a CO conversion rate of 66% and a methanethiol selectivity of 86 wt.%.
[0085] Example 36: The same preparation method as in Example 3 was used, except that the oxygen-free atmosphere was a carbon monoxide atmosphere, and the other conditions were the same as in Example 3.
[0086] The application conditions were the same as in Example 3, with a CO conversion rate of 71% and a methanethiol selectivity of 95 wt.%.
[0087] Example 37: The same preparation method as in Example 1 was used, except that in step two, the sol stirring temperature was 90°C, the stirring time was 2 hours, the gel drying temperature was 130°C, and the other conditions were the same as in Example 1.
[0088] The application conditions were the same as in Example 1, with a CO conversion rate of 53% and a methanethiol selectivity of 73 wt.%.
[0089] Example 38: The same preparation method as in Example 2 was used, except that in step two, the sol stirring temperature was 75°C, the stirring time was 4 hours, the gel drying temperature was 110°C, and the other conditions were the same as in Example 2.
[0090] The application conditions were the same as in Example 2, with a CO conversion rate of 64% and a methanethiol selectivity of 84 wt.%.
[0091] Example 39: The same preparation method as in Example 3 was used, except that in step two, the sol stirring temperature was 95°C, the stirring time was 1.5 hours, the gel drying temperature was 140°C, and the other conditions were the same as in Example 3.
[0092] The application conditions were the same as in Example 3, with a CO conversion rate of 72% and a methanethiol selectivity of 96 wt.%.
[0093] Example 40: The same preparation method as in Example 1 was used, except that element X was a Ni and Co mixed metal in a mass ratio of 1:1 (nickel nitrate and cobalt nitrate were mixed in equimolar amounts), alkali metal Y was K, the molar ratio of X to citric acid was 1:3 (based on the total molar amount of X), the molar ratio of polyethylene glycol to citric acid was 1.0, the molar ratio of X to Mo was 3 (based on the total molar amount of X), the mass ratio of dry gel to sulfide was 5, the heat treatment temperature was 550℃, and the heat treatment time was 5 hours.
[0094] The application conditions are the same as in Example 2, with a CO conversion rate of 68% and a methanethiol selectivity of 90 wt.%.
[0095] Comparative Examples: To better illustrate the technical effects of the present invention, the following comparative examples are provided: Comparative Example 1: Mo-SK / SiO2 catalyst was prepared according to the method of Chinese Patent ZL98118186.4, and the application conditions were the same as in Example 1, with CO conversion of 35% and methanethiol selectivity of 58 wt.%.
[0096] Comparative Example 2: K-Ni-Mo / SiO2 catalyst was prepared by conventional impregnation method (without complexing gel-sulfidation coupling process), and the application conditions were the same as in Example 1, with CO conversion of 40% and methanethiol selectivity of 62 wt.%.
[0097] Comparative Example 3: Sulfation treatment without the addition of alkali metal sulfides (in-situ sulfidation only under H2S / H2 atmosphere before reaction), with the same application conditions as Example 2, CO conversion rate of 42%, and methanethiol selectivity of 55 wt.%.
[0098] The comparative examples above show that the YX-Mo composite sulfide catalyst prepared by the complexation gel-sulfidation coupling process of the present invention is significantly superior to the prior art in terms of CO conversion and methanethiol selectivity.
Claims
1. A method for synthesizing a metal-modified molybdenum-based composite sulfide catalyst, characterized in that, Follow these steps: Step 1: Add citric acid to the homogeneous aqueous solution of the soluble salt corresponding to element X, and stir to form a transparent first solution, wherein the molar ratio of element X to citric acid is 0.2-1; Step 2: The molar ratio of polyethylene glycol to citric acid is 0.1-2. Polyethylene glycol is added to the first solution as an esterifying agent and stirred continuously to form a sol solution. After stirring the sol solution continuously at 70-100℃ for 1-5 hours, a gel is obtained. The gel is dried at 100-150℃ to form a dry gel. The dry gel is heat-treated at 300-800℃ for 2-8 hours in an oxygen-free atmosphere to obtain a solid powder for later use. Step 3: Add citric acid to the homogeneous aqueous solution of ammonium molybdate and stir to form a transparent second solution, wherein the molar ratio of molybdenum to citric acid is 0.2-1; Step 4: With a molar ratio of polyethylene glycol to citric acid of 0.1-2, polyethylene glycol is added to the second solution as an esterifying agent. With a molar ratio of element X to molybdenum of 0.1-10, the prepared solid powder is added to the second solution. After stirring continuously at 70-100℃ for 1-5 hours, a gel is obtained. This gel is dried at 100-150℃ to form a dry gel. With a mass ratio of dry gel to sulfide corresponding to alkali metal element Y of 0.1-10, this dry gel and the sulfide corresponding to alkali metal element Y are physically mixed. Then, under an oxygen-free atmosphere, it is heat-treated at 300-800℃ for 2-8 hours to obtain the YX-Mo composite sulfide catalyst, i.e., the metal-modified molybdenum-based composite sulfide catalyst.
2. The method for synthesizing a metal-modified molybdenum-based composite sulfide catalyst according to claim 1, characterized in that: The element X is one of Be, Mg, Ca, Ba, Co, Ni, Cu, Nb, Rh, Pd, Pt, Cd, Ga, La, In, Ru, Ti, Zr, Ce, Zn, Fe, Cr, W, Ag, Si, or Al; the alkali metal element Y is one of Li, Na, K, Rb, or Cs.
3. The method for synthesizing a metal-modified molybdenum-based composite sulfide catalyst according to claim 2, characterized in that: The soluble salts corresponding to element X are beryllium chloride, beryllium nitrate, beryllium sulfate, magnesium chloride, magnesium nitrate, magnesium sulfate, calcium chloride, calcium nitrate, barium chloride, barium nitrate, cobalt chloride, cobalt nitrate, cobalt sulfate, nickel chloride, nickel nitrate, nickel sulfate, copper chloride, copper nitrate, copper sulfate, niobium chloride, niobium nitrate, niobium sulfate, rhodium chloride, rhodium nitrate, rhodium sulfate, palladium chloride, palladium nitrate, palladium sulfate, platinum chloride, platinum nitrate, platinum sulfate, cadmium chloride, cadmium nitrate, cadmium sulfate, gallium chloride, gallium nitrate, gallium sulfate, lanthanum chloride, and nitrate. Lanthanum sulfate, lanthanum nitrate, indium sulfate, indium chloride, ruthenium nitrate, ruthenium sulfate, ruthenium chloride, titanium nitrate, zirconium chloride, zirconium nitrate, zirconium sulfate, cerium chloride, cerium nitrate, cerium sulfate, zinc chloride, zinc nitrate, zinc sulfate, ferric chloride, ferric nitrate, ferric sulfate, chromium chloride, chromium nitrate, chromium sulfate, silver nitrate, lithium silicate, sodium silicate, potassium silicate, aluminum chloride, aluminum nitrate, or aluminum sulfate; the sulfide corresponding to the alkali metal element Y is one of lithium sulfide, sodium sulfide, potassium sulfide, rubidium sulfide, or cesium sulfide.
4. The method for synthesizing a metal-modified molybdenum-based composite sulfide catalyst according to claim 1, characterized in that: The oxygen-free atmosphere is any one of nitrogen, argon, helium, hydrogen, methane, or carbon monoxide.
5. The application of a metal-modified molybdenum-based composite sulfide catalyst prepared by the synthesis method according to any one of claims 1-4, characterized in that: For the production of methanethiol from H2S and syngas, a metal element-modified Mo-based composite sulfide catalyst prepared with a mesh size of 40-60 is uniformly mixed with quartz sand and then loaded into a fixed-bed reactor. The H2 / CO ratio in the H2S and syngas is controlled at 0.1-10 using a mass flow meter, and the molar ratio of H2S to (H2+CO) is 0.1-10, with a volume hourly space velocity of 300-15000 h⁻¹. -1 The reaction conditions are: reaction temperature 200-400℃, reaction pressure 2.5-12MPa, and reaction time 5-100 hours.
Citation Information
Patent Citations
Catalyst for synthesizing methyl mercaptan from synthesized gas contg. hydrogen sulfide
CN1207957A