A method and apparatus for forming a solid-state electrolyte composite electrode sheet

By designing a multi-roller pressing mechanism, the problems of difficult and complex separation of solid electrolyte from the support carrier were solved, enabling efficient and environmentally friendly production of solid electrolyte composite electrodes and improving production efficiency and product performance.

CN123073005APending Publication Date: 2026-11-10CHAOWEI POWER GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610587040.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-04-29
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing solid electrolyte preparation and composite processes suffer from problems such as difficulty in peeling, complex processes, low yield, difficulty in accurately adjusting film thickness, and a narrow range of film thickness. In particular, during the roll transfer process, the solid electrolyte is difficult to peel from the support carrier, which affects production efficiency and product yield.

Method used

The rolling mechanism, which uses multiple non-contact pressure rollers, achieves continuous molding and compounding of solid electrolytes by gradually adjusting the gap between the pressure rollers and the difference in rotation speed. This avoids the dependence on the support carrier in traditional processes, simplifies the production process, and enables precise control of film thickness and compaction density through surface support of the rolling mechanism.

Benefits of technology

It achieves high yield (>99.7%), high-efficiency production (10m/min~20m/min), wide range of control over film thickness and compaction density, reduces equipment footprint and energy consumption costs, avoids solvent emissions, and improves electrical and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123073005A_ABST
    Figure CN123073005A_ABST
Patent Text Reader

Abstract

The application discloses a solid electrolyte composite electrode piece forming method and a forming device. The forming device comprises a first rolling mechanism. The first rolling mechanism comprises a plurality of pressure rollers arranged in close proximity without contact. The axes of the plurality of pressure rollers are parallel and coplanar, and the plurality of pressure rollers are arranged in parallel along the vertical direction of the axes. Adjacent pressure rollers are in close proximity without contact, and the rotating directions are different. The film is formed from powder to composite, and is supported and transferred by the surface of the rolling mechanism throughout the process. No self-supporting or additional support carrier is needed, there is no risk of broken tape and composite defects, and the problems of electrolyte peeling difficulty, complex process, low yield, difficulty in accurately adjusting the film thickness, and narrow film thickness range in the prior art when rolling and transferring to the electrode are solved.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This invention patent application is based on the prior patent application filed on May 9, 2025, with application number 202510596706.7 and invention title "A method and apparatus for forming a solid electrolyte composite electrode". Technical Field

[0002] This invention relates to the field of composite material molding technology, and in particular to a method and apparatus for molding solid electrolyte composite electrodes. Background Technology

[0003] Solid-state lithium-ion batteries, due to their use of solid-state electrolytes instead of traditional liquid electrolytes, possess higher energy density, thermal stability, and chemical resistance, reducing the risk of thermal runaway and improving battery safety. In existing technologies, the main preparation and lamination method for solid-state electrolytes is roll forming: this process first prepares a solid electrolyte slurry, coats it onto a support carrier, dries it, and then roll-forms the solid electrolyte film onto the electrode sheet while simultaneously peeling off the support carrier. Figure 1 As shown.

[0004] Existing solid-state electrolyte preparation and composite processes still face several major challenges: First, during the roll transfer process, the solid-state electrolyte is difficult to separate from the support carrier, which not only affects production efficiency but also leads to a decrease in the yield of solid-state electrolyte films with broken strips. Second, the preparation and composite process of the solid-state electrolyte in this technology involves steps such as slurry preparation, coating, drying, winding, transfer, and peeling, which is complex and requires numerous equipment, resulting in high costs and limiting its large-scale application. Third, this process is based on wet slurry preparation, making it difficult to apply to solvent-sensitive sulfide solid-state electrolytes. Therefore, simplifying the preparation and composite process of solid-state electrolytes, improving production efficiency and product yield, reducing costs, and eliminating the influence of solvents on solid-state electrolytes are important challenges currently facing solid-state battery technology. Summary of the Invention

[0005] In view of the above analysis, and in view of the shortcomings of the prior art, the present invention aims to provide a solid electrolyte composite electrode forming method and forming device, which solves at least one of the following problems: difficulty in separating solid electrolyte from support carrier, complex process, low yield, difficulty in accurately adjusting film thickness and narrow film thickness range.

[0006] The objective of this invention is mainly achieved through the following technical solutions: This invention discloses a solid electrolyte composite electrode forming apparatus, including a first rolling mechanism; The first roller pressing mechanism includes multiple pressing rollers that are positioned close to each other without contact. Multiple pressure rollers have parallel axes and are arranged in a coplanar plane, and are arranged side by side along a direction perpendicular to their axes; adjacent pressure rollers are close to each other but do not contact each other, and rotate in different directions; Along the parallel arrangement direction of the pressure rollers in the first roller pressing mechanism, a first forming area is formed between the gaps of two adjacent pressure rollers at one end of the first roller pressing mechanism; the first forming area can compress and form a solid electrolyte to obtain a first solid electrolyte membrane; The gap between two adjacent pressure rollers at the other end of the first roller pressing mechanism forms a second forming area; the second forming area can press the first solid electrolyte membrane and the electrode sheet to form a single-sided solid electrolyte composite electrode sheet; the electrode sheet is a positive electrode sheet, a negative electrode sheet, a bipolar electrode sheet, a composite electrode sheet, or a self-supporting membrane sheet; The rotational linear speed of the multiple pressure rollers gradually increases from one end of the first forming area to the end where the second forming area is located.

[0007] One feasible solution is that, in the first roller pressing mechanism, the gap between the pressure rollers gradually decreases from the first forming area to the second forming area.

[0008] Preferably, the gap ratio between adjacent pressure rollers in the first roller pressing mechanism satisfies: 1.5~3:1 Another feasible solution is that, in the first roller pressing mechanism, from the first forming area to the second forming area, the gap between adjacent rollers first gradually increases and then gradually decreases.

[0009] Preferably, from the first molding area to the second molding area, all gaps are defined as first gap, second gap, ..., Nth gap, where the gap in the first molding area is the first gap and the gap in the second molding area is the Nth gap; the ratio of the first gap to the second gap satisfies: 0.8~0.9:1; the second gap, ..., Nth gap are arranged from the first molding area to the second molding area, and the ratio of two adjacent gaps satisfies: 1.5~5:1.

[0010] Preferably, the number of first roller pressing mechanisms is ≥3, and at least one set of adjacent pressing rollers is arranged between the first forming area and the second forming area.

[0011] Preferably, a second rolling mechanism is provided on the side of the second forming area away from the first forming area; the second rolling mechanism includes a plurality of close but non-contact pressure rollers.

[0012] Preferably, in the second roller pressing mechanism, the axes of the multiple pressure rollers are parallel and coplanar, and the multiple pressure rollers are arranged side by side along a direction perpendicular to their axes; adjacent pressure rollers rotate in different directions; At one end of the plane of multiple pressure rollers that is far from the second forming area, the gap between two adjacent pressure rollers forms a third forming area; the third forming area can compress the solid electrolyte to form a second solid electrolyte membrane. The second forming area can press the first solid electrolyte membrane, the second solid electrolyte membrane and the electrode sheet together to form an electrode sheet with double-layer solid electrolyte membranes on both sides; In the second roller pressing mechanism, the rotational linear velocity of multiple rollers gradually increases from one end of the third forming area to the end where the second forming area is located.

[0013] Preferably, the number of pressure rollers in the second roller pressing mechanism is ≥1, and at least one set of adjacent pressure rollers is arranged between the third forming area and the second forming area. Preferably, the first forming area is provided with a first feeding mechanism.

[0014] Preferably, the second forming area is provided with an unwinding mechanism on one side and a winding mechanism on the other side.

[0015] A method for forming a solid electrolyte composite electrode, using the above-mentioned forming apparatus, includes: rolling solid electrolyte powder raw material into a composite electrode by continuously passing it through a pressure roller with increasing rotation speed and rolling it with an electrode to obtain a solid electrolyte composite electrode.

[0016] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects: (1) The thin film of the present invention is transferred from powder film formation to composite by the surface support of the rolling mechanism throughout the entire process. It does not require self-support or additional support carrier, and there is no risk of tape breakage or composite defects. The traditional wet transfer process requires coating solid electrolyte onto support carriers such as PET, winding, transferring, tension adjustment, unwinding, and rolling transfer. The process is complicated and prone to tape breakage. In addition, the solid electrolyte adhering to the support carrier has difficulty in peeling off from the support carrier when it is rolled to the electrode, resulting in a decrease in yield. The total yield of the battery cell is >99.7%.

[0017] (2) In this invention, the gap between adjacent rollers in the first forming area gradually increases and then gradually decreases from the first forming area to the second forming area in the first roller pressing mechanism. This relieves tension and obtains better mechanical and electrical properties. The thickness of the solid electrolyte membrane can now be controlled within a wide range, achieving flexible adjustment of film thickness and compaction density over a wide range. This solves the problem that traditional wet processes are limited by the viscosity and surface tension of the slurry, making it difficult to accurately adjust the film thickness and resulting in a narrow film thickness range. This invention achieves better mechanical and electrical properties. The ionic conductivity of the solid electrolyte composite electrode is between 0.211 S / m and 0.736 S / m, preferably between 0.416 S / m and 0.736 S / m; the flow rate is between 10 m / min and 20 m / min; the porosity is between 9.6% and 14.1%; and the compaction density is between 1.42 and 1.60 g / cm³. 3 between.

[0018] (3) The process described in this invention eliminates the solvent evaporation step, and large-area baking equipment can be removed from the production line. While saving land costs, energy costs and raw material costs, it also eliminates the emission of toxic solvent gases in traditional production, and greatly improves the harm to the environment and health caused by production activities.

[0019] (4) The process and equipment described in this invention can realize integrated production from powder to composite. Compared with the traditional process of batching, homogenizing, coating, drying, winding and transfer printing, the process of this invention simplifies the production process and improves production efficiency; the total production efficiency of electrode sheets is between 10m / min and 20m / min.

[0020] (5) In the first roller pressing mechanism, the gap between adjacent rollers gradually increases and then gradually decreases from the first forming area to the second forming area. This relieves tension and obtains better mechanical and electrical properties. The thickness of the solid electrolyte membrane can be controlled within a wide range, and the film thickness and compaction density can be flexibly adjusted over a wide range. This solves the problem that the traditional wet process is limited by the viscosity and surface tension of the slurry, making it difficult to accurately adjust the film thickness and the film thickness range is narrow.

[0021] (6) No solvent is used in the entire preparation process described in this invention, which eliminates the negative impact of solvent on the performance of active materials and prevents side reactions between active materials and solvents. Attached Figure Description

[0022] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.

[0023] Figure 1 : Existing solid electrolyte preparation apparatus; Figure 2 : A schematic diagram of an integrated solid electrolyte film-forming composite six-roller device in one embodiment; Figure 3 : Schematic diagram of an integrated solid electrolyte film-forming composite six-roller device in another embodiment; Figure 4 Schematic diagram of positive electrode composite sheet structure; Figure 5 Schematic diagram of the negative electrode composite electrode structure; Figure 6 Schematic diagram of a single-sided composite internal parallel cell structure; Figure 7 Schematic diagram of the positive electrode structure; Figure 8 Schematic diagram of the negative electrode composite electrode structure; Figure 9 Schematic diagram of the internal parallel structure battery cell; Figure 10Schematic diagram of an integrated solid electrolyte film-forming composite ten-roller equipment; Figure 2a : A schematic diagram of an integrated solid electrolyte film-forming composite four-roller device in one embodiment; Figure 3a : Schematic diagram of an integrated solid electrolyte film-forming composite six-roller device in another embodiment; Figure 4a Schematic diagram of an integrated solid electrolyte film-forming composite ten-roller equipment; Figure 5a Schematic diagram of the positive electrode membrane structure; Figure 6a Schematic diagram of a double-sided composite negative electrode film structure; Figure 7a Schematic diagram of the internal parallel cell structure of the double-sided composite diaphragm; Figure 8a Schematic diagram of a single-sided composite negative electrode sheet; Figure 9a Schematic diagram of a bipolar double-sided composite membrane structure; Figure 10a Schematic diagram of the internal series cell structure of the bipolar composite diaphragm; Figure 11a Schematic diagram of a double-sided, double-layer electrolyte composite membrane structure; Figure 12a ; Schematic diagram of the internal battery cell structure of the double-layer electrolyte membrane.

[0024] Figure label: 100 - Electrode; 001 - Current collector; 002 - Positive electrode membrane; 003 - Negative electrode membrane; 600 - Solid electrolyte composite electrode; 601 - Positive solid electrolyte composite electrode; 602 - Negative solid electrolyte composite electrode; 601a - Positive electrode sheet; 602a - Double-sided composite negative electrode sheet; 603 - Single-sided composite negative electrode sheet; 604 - Double-sided composite bipolar membrane; 605 - Double-sided double-layer electrolyte composite membrane; 004 - Solid electrolyte membrane; 005 - Solid electrolyte membrane support substrate; 004a - Sulfide solid electrolyte membrane; 005a - Halide solid electrolyte membrane; 110 - First roller pressing mechanism; 120 - Second roller pressing mechanism; 011-First pressure roller; 012-Second pressure roller; 013-Third pressure roller; 014-Fourth pressure roller; 015-Fifth pressure roller; 016-Sixth pressure roller; 017-Seventh pressure roller; 018-Eighth pressure roller; 019-Ninth pressure roller; 020-Tenth pressure roller; 200 - Tension correction mechanism; 210 - First tension correction mechanism; 220 - Second tension correction mechanism; 300 - Unwinding mechanism; 400 - Rewinding mechanism; 510 - First feeding mechanism; 520 - Second feeding mechanism. Detailed Implementation

[0025] To make the technical problems solved, the technical solutions, and the beneficial effects of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.

[0026] On one hand, the present invention discloses a solid electrolyte composite electrode forming device, including: a first roller pressing mechanism 110, the first roller pressing mechanism 110 including a plurality of pressing rollers arranged close to each other without contact; Multiple pressure rollers have parallel axes and are arranged in a coplanar plane, and are arranged side by side along a direction perpendicular to their axes; adjacent pressure rollers are close to each other but do not contact each other, and rotate in different directions; Along the parallel arrangement direction of the pressure rollers in the first roller pressing mechanism 110, a first forming area is formed between the gaps of two adjacent pressure rollers at one end of the first roller pressing mechanism 110; the first forming area can press the solid electrolyte into shape to obtain a first solid electrolyte membrane. The gap between two adjacent pressure rollers at the other end of the first roller pressing mechanism 110 forms a second forming area; the second forming area can press the first solid electrolyte membrane and the electrode sheet together to obtain a single-sided solid electrolyte composite electrode sheet. The rotational linear speed of the multiple pressure rollers gradually increases from one end of the first forming area to the end where the second forming area is located.

[0027] During implementation, the first solid electrolyte membrane is formed by pressing and molding the first solid electrolyte in the first forming area. Under the action of the speed difference between adjacent pressure rollers in the first forming area, the first solid electrolyte membrane is separated from the low-speed pressure roller and transferred from the low-speed pressure roller to the high-speed pressure roller. Similarly, the electrode with the first solid electrolyte membrane attached in the second forming area is separated from the low-speed pressure roller and transferred from the low-speed pressure roller to the high-speed pressure roller under the action of the speed difference between adjacent pressure rollers in the second forming area. At the same time, the rotational linear speed of the adjacent pressure rollers on both sides of the second forming area is the same, so that the solid electrolyte membrane composite electrode prepared in the second forming area is pulled out from the second forming area.

[0028] Compared with existing technologies, due to the speed difference between adjacent pressure rollers, the solid electrolyte membrane can adhere to the roller surface of the higher-speed pressure roller for transfer after calendering and thinning. This avoids the traditional process of coating the PET film surface with solid electrolyte slurry, drying, winding, and then transferring it to the composite peeling mechanism. On the one hand, it solves the problem of solid electrolyte membrane peeling from the PET carrier when the solid electrolyte membrane is laminated with the electrode in the traditional process. On the other hand, it eliminates the intermediate transmission mechanism, tension control mechanism, and correction mechanism required when the solid electrolyte membrane is laminated with the electrode in the traditional process, greatly simplifying the equipment, reducing the floor area occupied by the equipment, and eliminating the risk of solid electrolyte membrane breakage during the transmission process.

[0029] Preferably, the first roller pressing mechanism 110 has ≥3 pressure rollers, and at least one set of adjacent pressure rollers is arranged between the first forming area and the second forming area. The adjacent pressure rollers are close to each other but do not contact each other, and rotate in different directions. The rotational linear speed of the adjacent pressure rollers gradually increases from the first forming area to one end of the second forming area.

[0030] During implementation, based on the sequentially arranged multiple pressure rollers, the rotational linear speed increases one by one, and the first solid electrolyte membrane formed in the first forming area can easily be transferred from the first forming area to the second forming area.

[0031] More preferably, the number of pressure rollers in the first roller pressing mechanism 110 is ≥4.

[0032] Specifically, the first forming area is provided with a first feeding mechanism 510.

[0033] During implementation, the first feeding mechanism 510 can feed material into the first forming area.

[0034] Preferably, the second forming area is provided with an unwinding mechanism 300 on one side and a winding mechanism 400 on the other side; The unwinding mechanism 300 unwinds the electrode sheet, and after it and the solid electrolyte membrane are formed in the second forming area, an electrode sheet with a single layer of solid electrolyte membrane is obtained.

[0035] Preferably, the roller spacing, roller surface temperature, rotation speed, and rotation direction of each first roller pressing mechanism 110 can be adjusted individually.

[0036] In one feasible implementation, in the first roller pressing mechanism, the gap between the pressure rollers gradually decreases from the first forming area to the second forming area, and the ratio of adjacent gaps satisfies: 1.5~5:1. Preferably, the ratio of adjacent gaps satisfies: 1.5~3:1.

[0037] Compared with existing technologies, when a single roll pass cannot meet the thinning requirements of the solid electrolyte membrane, pressure rollers can be added between the first forming area and the second forming area to increase the number of calendering and thinning passes, thereby enabling control of the solid electrolyte membrane thickness within a wide range.

[0038] Another feasible implementation involves the gap between adjacent pressure rollers gradually increasing and then gradually decreasing from the first forming area towards the second forming area. All gaps are defined as the first gap, the second gap, ..., the Nth gap, where the gap in the first forming area is the first gap, and the gap in the second forming area is the Nth gap. The ratio of the first gap to the second gap satisfies 0.8 to 0.9:1. The second gap, ..., the Nth gap are arranged from the first forming area towards the second forming area, and the ratio of two adjacent gaps satisfies 1.5 to 5:1.

[0039] During implementation, the second gap is larger than the first gap, which helps to alleviate tension and obtain better mechanical and electrical properties; the second gap, ..., the Nth gap decreases in sequence, which helps to transfer the first solid electrolyte membrane from the first forming region to the second forming region while realizing the calendering of the solid electrolyte membrane and achieving thickness control of the first solid electrolyte membrane.

[0040] Compared with existing technologies, this invention, through the gradual increase and then decrease of the gap between adjacent rollers in the first forming area towards the second forming area in the first roller pressing mechanism, alleviates tension and achieves better mechanical and electrical properties. It also allows for a wide range of control over the solid electrolyte membrane thickness, enabling flexible adjustment of film thickness and compaction density. This solves the problem of traditional wet processes being limited by slurry viscosity and surface tension, making precise film thickness adjustment difficult and resulting in a narrow film thickness range. The invention achieves better mechanical and electrical properties; the ionic conductivity of the solid electrolyte composite electrode is between 0.211 S / m and 0.736 S / m, preferably between 0.416 S / m and 0.736 S / m; the flow rate is between 10 m / min and 20 m / min; the porosity is between 9.6% and 14.1%; and the compaction density is between 1.42 and 1.60 g / cm³. 3 between.

[0041] Preferably, the temperature of the pressure rollers arranged sequentially from the first forming area to the second forming area in the first roller pressing mechanism gradually decreases, and the temperature range of the pressure rollers in the first roller pressing mechanism is 40℃~160℃; the temperature difference between two adjacent pressure rollers is 5℃~20℃.

[0042] It should be noted that the reasons for setting the temperature range of the pressure rollers and the temperature difference between adjacent pressure rollers are as follows: due to the different types and physical properties of the materials used, the morphology of the self-supporting diaphragm on the roller surface after processing varies considerably. Some materials severely stick to the rollers at high temperatures, affecting the normal winding of the electrode sheet. Therefore, it is necessary to reduce the electrode sheet viscosity by forming a film on a low-temperature roller during the initial processing stage. Furthermore, to meet the requirements of thermal bonding between the self-supporting diaphragm and the current collector in the subsequent stage, the roller surface temperature needs to be gradually increased until it reaches the thermal bonding temperature of the current collector. Some materials have poor processing performance and require high-temperature processing to increase the cohesion of the self-supporting film and improve the film strength. Excessive temperature can cause the current collector coating to melt and overflow; therefore, it is necessary to gradually cool the roller surface while simultaneously achieving high processability and thermal bonding.

[0043] For example, such as Figure 3 As shown, the first rolling mechanism 110 may include a first pressure roller 011, a second pressure roller 012, a third pressure roller 013, a fourth pressure roller 014, a fifth pressure roller 015, and a sixth pressure roller 016 arranged sequentially, with the rotational speeds of the first pressure roller 011, the second pressure roller 012, and the third pressure roller 013 increasing progressively. The gap between the first pressure roller 011 and the second pressure roller 012 forms a first forming region; the gap between the fifth pressure roller 015 and the sixth pressure roller 016 forms a second forming region; a tension buffer zone is formed between the second pressure roller 012 and the third pressure roller 013; and a calendering and thinning region is formed between the third pressure roller 013 and the fourth pressure roller 014, and between the fourth pressure roller 014 and the fifth pressure roller 015.

[0044] Preferably, a second rolling mechanism 120 is provided on the side of the second forming area away from the first forming area; The second roller pressing mechanism has multiple pressure rollers; the axes of the multiple pressure rollers are parallel and coplanar; the pressure rollers in adjacent first roller pressing mechanisms 110 and second roller pressing mechanisms 120 are close to each other but do not contact each other, and rotate in different directions; adjacent pressure rollers in the second roller pressing mechanism 120 are close to each other but do not contact each other, and rotate in different directions; the number of pressure rollers in the second roller pressing mechanism 120 is not less than 1. A second feeding mechanism is provided between two adjacent pressure rollers on the side of the second rolling mechanism away from the second forming area, and a third forming area is formed between the two adjacent pressure rollers; the second feeding mechanism can feed material into the third forming area and realize the solid electrolyte compression molding in the third forming area to obtain the second solid electrolyte membrane; In the second roller pressing mechanism, the rotational linear velocity of the multiple rollers gradually increases from the end where the second feeding mechanism is located to the end where the second forming area is located.

[0045] Preferably, the second roller pressing mechanism 120 has no fewer than two pressure rollers.

[0046] For example, such as Figure 4aAs shown, the second rolling mechanism may include a seventh roller 017, an eighth roller 018, a ninth roller 019, and a tenth roller 020 arranged sequentially, with the rotational speeds of the tenth roller 020, the ninth roller 019, the eighth roller 018, and the seventh roller 017 increasing progressively. The gap between the ninth roller 019 and the tenth roller 020 forms a third forming region; the spaces between the eighth roller 018 and the seventh roller 017, between the ninth roller 019 and the eighth roller 018, and between the tenth roller 020 and the ninth roller 019 form calendering and thinning regions.

[0047] In practice, the second solid electrolyte membrane is obtained by pressing and molding the second solid electrolyte in the third forming region. Under the action of the speed difference between adjacent pressure rollers in the third forming region, the second solid electrolyte membrane is separated from the low-speed pressure roller and transferred from the low-speed pressure roller to the high-speed pressure roller. Similarly, due to the speed difference between the pressure rollers in the adjacent first pressure roller mechanism 110 and second pressure roller mechanism 120 near the second forming region, the second solid electrolyte membrane can be separated from the low-speed pressure roller and transferred from the pressure roller in the low-speed second pressure roller mechanism 120 to the pressure roller in the high-speed first pressure roller mechanism 110, and then enter the second forming region to participate in the preparation of an electrode sheet with double-layer solid electrolyte membranes on both sides.

[0048] The electrode sheet with the solid electrolyte membrane is wound up by the winding mechanism 400 in the second forming area. The two pressure rollers used for lamination in the second forming area rotate at the same speed.

[0049] Preferably, the number of pressure rollers in the second roller pressing mechanism 120 is ≥1, at least one pressure roller is disposed between the third forming area and the second forming area, adjacent pressure rollers are close to each other but do not contact each other, and rotate in different directions, and the rotational linear velocity of adjacent pressure rollers in the second roller pressing mechanism 120 gradually increases from the third forming area to one end of the second forming area.

[0050] More preferably, the number of pressure rollers in the second roller pressing mechanism 120 is ≥3.

[0051] During implementation, the rotational linear velocity of the multiple pressure rollers arranged sequentially in the second roller pressing mechanism 120 gradually increases from one end of the third forming region to the second forming region, and the second solid electrolyte membrane formed in the third forming region can easily be transferred from the first forming region to the second forming region.

[0052] Preferably, in the second roller pressing mechanism, the gap between two adjacent rollers arranged sequentially from the third forming area to the second forming area first increases and then gradually decreases.

[0053] Specifically, from the third molding area towards the second molding area, all gaps are defined as the N+M gap, the N+M-1 gap, ..., the Nth gap, where the gap in the third molding area is the N+M gap; the ratio of the N+M gap to the N+M-1 gap satisfies: 0.8~0.9:1; the N+M-1 gap, ..., the Nth gap are arranged from the third molding area towards the second molding area, and the ratio of two adjacent gaps satisfies: 1.5~5:1.

[0054] Preferably, the gap between each pressure roller, the roller surface temperature, the rotation speed, and the rotation direction can be adjusted individually.

[0055] Preferably, the gap between adjacent pressure rollers in the third forming area and the second forming area is smaller than the gap between rollers in the third forming area.

[0056] During implementation, the second solid electrolyte membrane can be calendered and formed simultaneously as it is transferred from the third forming region to the second forming region, thereby achieving thickness control of the second solid electrolyte membrane.

[0057] Compared with existing technologies, due to the speed difference between adjacent rollers in the first roller pressing mechanism 110 and the second roller pressing mechanism 120, the two solid electrolyte membranes are transferred from the first forming area and the third forming area to the second forming area while being calendered and thinned. Finally, they are formed in the second forming area to prepare a solid electrolyte composite electrode with a dual solid electrolyte membrane structure. This avoids the traditional process of coating the PET film surface with solid electrolyte slurry, drying it, winding it up, and then transferring it to the composite peeling mechanism. On the one hand, it solves the problem of solid electrolyte membrane peeling off from the PET carrier when the solid electrolyte membrane is laminated with the electrode in the traditional process. On the other hand, it eliminates the intermediate conduction mechanism, tension control mechanism, and correction mechanism required when the solid electrolyte membrane is laminated with the electrode in the traditional process, which greatly simplifies the equipment, reduces the floor area occupied by the equipment, and eliminates the risk of solid electrolyte membrane breakage during conduction.

[0058] Preferably, the temperature of the pressure rollers arranged sequentially from the third forming area to the second forming area in the second roller pressing mechanism gradually decreases, and the temperature range of the pressure rollers is 40℃~160℃; the temperature difference between two adjacent pressure rollers is 5℃~20℃.

[0059] It should be noted that the temperature range of the pressure rollers in the first roller pressing mechanism and the temperature difference between adjacent pressure rollers are set because the morphology of the self-supporting diaphragm on the roller surface varies greatly depending on the type and physical properties of the materials used. Some materials stick to the rollers severely at high temperatures, affecting the normal winding of the electrode sheet. Therefore, a low-temperature roller forming process is needed in the initial stage to reduce the electrode sheet viscosity. Furthermore, to meet the thermal bonding requirements between the self-supporting diaphragm and the current collector in the subsequent stage, the roller surface temperature needs to be gradually increased until it reaches the current collector thermal bonding temperature. Some materials have poor processing performance and require high-temperature processing to increase the cohesion of the self-supporting film and improve the film strength. Excessive temperature can cause the current collector coating to melt and overflow. Therefore, the roller surface needs to be gradually cooled while simultaneously achieving high processability and thermal bonding.

[0060] On the other hand, the present invention discloses a method for forming a solid electrolyte composite electrode using the above-mentioned solid electrolyte composite electrode forming device, comprising: rolling solid electrolyte powder raw material into a composite electrode by continuously passing it through a pressure roller with increasing rotation speed and rolling it with an electrode to obtain a solid electrolyte composite electrode.

[0061] In one feasible implementation, to prepare a composite electrode with a solid electrolyte on at least one side, the solid electrolyte composite electrode forming apparatus satisfies the following: a plurality of first rolling mechanisms 110 are sequentially labeled as: first pressure roller, second pressure roller, ..., Nth pressure roller from the first feeding mechanism 510 toward the second forming area, wherein a first feeding mechanism is provided between the first pressure roller and the second pressure roller to form a first forming area; and a second forming area is formed between the (N-1)th pressure roller and the Nth pressure roller. The linear velocity changes of the first pressure roller, the second pressure roller, ..., the Nth pressure roller satisfy the following: the speed ratio of adjacent rotating rollers is 1:(1.01~5), and the speed increases step by step from the first pressure roller to the Nth pressure roller... to ensure that the electrode sheet will not roll back due to too small a speed difference or detach from the roller surface due to too large a speed difference during transfer.

[0062] Another feasible implementation, in order to prepare a composite electrode with solid electrolytes on both sides, requires the solid electrolyte composite electrode forming device to satisfy all the features of the above implementation method as well as the following: multiple pressure rollers are sequentially labeled as: the Mth pressure roller, the (M-1)th pressure roller, ..., the (N+1)th pressure roller from one end of the third forming area to the end where the second forming area is located, where M ≥ N+1; a second feeding mechanism is provided between the Mth pressure roller and the (M-1)th pressure roller to form the third forming area; the formed second solid electrolyte membrane is transferred from the third forming area to the (N+1)th pressure roller, and then transferred to the Nth pressure roller via the (N+1)th pressure roller, and participates in the second forming area; The linear velocity of the Mth pressure roller, the M-1th pressure roller, ..., the N+1th pressure roller, and the Nth pressure roller changes in such a way that the linear velocity of the pressure roller increases progressively from the Mth pressure roller to the Nth pressure roller, and the speed ratio between two adjacent rollers is 1:(1.01~5).

[0063] Specifically, the solid electrolyte composite electrode forming method includes: The first solid electrolyte membrane is pressed and formed between the first pressure roller and the second pressure roller; The first solid electrolyte membrane is pressed into a film by the first pressure roller and the second pressure roller, and then transferred to the surface of the second pressure roller for further thinning.

[0064] The first solid electrolyte membrane is thinned by the second pressure roller and the (N-1)th pressure roller, and then transferred to the gap between the (N-1)th pressure roller and the Nth pressure roller on the surface of the (N-1)th pressure roller. The positive or negative electrode sheet to be composited is transmitted to the N-1 pressure roller and the Nth pressure roller through the unwinding mechanism 300, the correction mechanism and the tension control mechanism to be pressed and formed with the first solid electrolyte film, so that the electrode sheet is composited with the thinned first solid electrolyte film.

[0065] Preferably, the solid electrolyte composite electrode forming method further includes: The first solid electrolyte membrane is pressed and formed between the first pressure roller and the second pressure roller; The second solid electrolyte membrane is pressed into a film by the Mth pressure roller and the M-1th pressure roller, and then transferred to the surface of the M-1th pressure roller for further thinning.

[0066] The second solid electrolyte membrane is thinned by the M-1 pressure roller and the N pressure roller, and then transferred to the N-1 pressure roller and the gap between the N pressure roller on the surface of the N pressure roller. The composite positive or negative electrode sheet is transmitted to the N-1 pressure roller, the gap between the Nth pressure roller and the first solid electrolyte membrane and the second solid electrolyte membrane through the unwinding mechanism 300, the correction mechanism and the tension control mechanism to be pressed and formed, so that the electrode sheet is combined with the thinned first solid electrolyte membrane and the second solid electrolyte membrane to obtain a composite electrode sheet with solid electrolyte films on both sides.

[0067] Compared with existing technologies, the preparation process described in this invention does not use any solvents, thus eliminating the negative impact of solvents on the performance of active materials and preventing side reactions between active materials and solvents. The solvent evaporation step is eliminated, and large-area baking equipment can be removed from the production line. This saves on land costs, energy costs, and raw material costs while eliminating the emission of toxic solvent gases in traditional production, significantly reducing the environmental and health hazards of production activities.

[0068] Compared with existing technologies, the process and equipment described in this invention can realize integrated production from powder to composite. Compared with the traditional processes of ingredient preparation, homogenization, coating, drying, winding, and transfer printing, the process described in this invention simplifies the production process and improves production efficiency.

[0069] Compared with existing technologies, this invention allows for a wide range of flexible control over film thickness and compaction density by adjusting equipment parameters (such as differential speed ratio and roller gap). Traditional wet processes are limited by the viscosity and surface tension of the slurry, making it difficult to precisely adjust the film thickness and resulting in a narrow film thickness range.

[0070] Compared with existing technologies, the film of the present invention is transferred entirely by surface support of a roller pressing mechanism from powder film formation to lamination, without the need for self-support or additional support carriers, thus eliminating the risk of tape breakage and lamination defects. Traditional wet transfer printing processes require coating solid electrolytes onto support carriers such as PET, winding, transferring, tension adjustment, unwinding, and roller pressing, which is a complex process prone to tape breakage. Furthermore, the solid electrolytes adhering to the support carrier are difficult to peel off from the support carrier during roller pressing transfer to the electrodes, resulting in a reduced yield.

[0071] Thirdly, this invention discloses a solid electrolyte cell, such as... Figure 6 As shown, the cathode solid electrolyte composite electrode and the anode solid electrolyte composite electrode prepared above are stacked to prepare an internal series structure battery cell. The positive and negative electrodes are stacked and connected in series to improve the voltage of a single battery cell.

[0072] The present invention also discloses a test method for solid electrolyte composite electrode sheets and / or solid electrolyte composite cells, including constant current charge-discharge test, and capacity test of the battery under constant current conditions: charging with a constant current of 0.1C, resting for 5 minutes, and discharging with a constant current of 0.1C under constant current conditions.

[0073] Parameters such as thickness, areal density, compaction density, thickness uniformity, areal density uniformity, compaction uniformity, and ionic conductivity of the electrolyte film on the surface of the composite electrode were measured.

[0074] Example 1 This embodiment discloses a solid electrolyte composite electrode forming apparatus and forming method, such as Figure 2 As shown, the molding apparatus includes: The rotational speeds of the first pressure roller 011, the second pressure roller 012, and the third pressure roller 013 increase progressively, as do the rotational speeds of the sixth pressure roller 016, the fifth pressure roller 015, and the fourth pressure roller 014. The first pressure roller 011 and the sixth pressure roller 016 rotate at the same speed, as do the second pressure roller 012 and the fifth pressure roller 015, and the third pressure roller 130 and the fourth pressure roller 014 rotate at the same speed.

[0075] The forming method includes: adding the pre-fiberized powder into the first feeding mechanism 510 and the second feeding mechanism 520. The feeding mechanism adjusts the feeding speed according to the rotation speed of the pressure rollers and feeds the powder between the first pressure roller 011, the second pressure roller 012, the fifth pressure roller 015, and the sixth pressure roller 016.

[0076] The first solid electrolyte film is pressed and formed between the first pressure roller 011 and the second pressure roller 012. There is a speed difference between the two adjacent rollers, namely the first pressure roller 011 and the second pressure roller 012. When the powder passes through the rollers, the high shear force brought about by the speed difference rolls and stretches the solid electrolyte powder, pressing it into a film. The tensile resistance of the solid electrolyte after being sheared causes it to adhere to the surface of the second pressure roller 012 with a faster speed and be transferred.

[0077] The first solid electrolyte membrane is pressed into a film by the first pressure roller 011 and the second pressure roller 012. The film is then transferred to the surface of the second pressure roller 012 and then transferred to the third pressure roller 013 for further thinning.

[0078] The first solid electrolyte membrane is thinned by the second pressure roller 012 and the third pressure roller 013, and then transferred on the surface of the third pressure roller 013 to the gap between the third pressure roller 013 and the fourth pressure roller 014.

[0079] The second solid electrolyte film is pressed and formed between the sixth pressure roller 016 and the fifth pressure roller 015. There is a speed difference between the two adjacent rollers, namely the sixth pressure roller 016 and the fifth pressure roller 015. When passing through the rollers, the high shear force brought about by the speed difference rolls the solid electrolyte powder to stretch it and press it into a film. The tensile resistance of the solid electrolyte after being sheared causes it to adhere to the surface of the faster fifth pressure roller 015 and be transferred.

[0080] The second solid electrolyte membrane is pressed into a film by the sixth pressure roller 016 and the fifth pressure roller 015. The film is then transferred to the surface of the fifth pressure roller 015 and then transferred to the area between the fifth pressure roller 015 and the fourth pressure roller 014 for further thinning.

[0081] The second solid electrolyte membrane is thinned by the fifth pressure roller 015 and the fourth pressure roller 014, and then transferred on the surface of the fourth pressure roller 014 to the gap between the third pressure roller 013 and the fourth pressure roller 014.

[0082] The composite positive or negative electrode sheet is transmitted to the space between the third pressure roller 013 and the fourth pressure roller 014 via the electrode sheet unwinding mechanism 300, the web-correcting mechanism, and the tension control mechanism 210. The two sides of the double-sided composite electrode sheet, along with the first and second sides of the solid electrolyte membrane, simultaneously pass through the gap between the third pressure roller 013 and the fourth pressure roller 014, thus bonding both sides of the electrode sheet with the thinned solid electrolyte membrane. After passing through the web-correcting and tension control mechanism 220, the composite electrode sheet is wound up by the solid electrolyte membrane composite electrode sheet winding mechanism 400.

[0083] The linear speeds of the first, second, ..., sixth pressure rollers vary in such a way that the ratio of the slower to the faster speeds of adjacent pressure rollers is 1:2, and the linear speeds of the third and fourth pressure rollers are the same.

[0084] The first and second solid electrolyte membranes are made of the same material, which is a halide solid electrolyte with an average particle size of 20 μm. The mixture of sulfide solid electrolyte powder and styrene block copolymer binder is a solid material with a mass ratio of 1:2.

[0085] In the first roller pressing mechanism, the ratio of the gap between the two rollers in the low-speed zone to the gap between the two rollers in the adjacent high-speed zone satisfies 2:1.

[0086] The surface temperatures of the first to sixth pressure rollers are controlled by a mold temperature controller, with the roller surface temperatures being 100℃, 110℃, 120℃, 120℃, 110℃, and 100℃ respectively.

[0087] The composite electrode sheets are stacked to prepare a battery cell. The structure of the positive electrode solid electrolyte composite electrode sheet 601 is as follows: Figure 4 As shown, the structure of the negative electrode solid electrolyte composite electrode 602 is as follows: Figure 5 As shown: Positive electrode membranes 002 are symmetrically distributed on both sides of current collector 001, or negative electrode membranes 003 are symmetrically distributed on both sides of current collector 001. Positive electrode membranes 002 or negative electrode membranes 003 are connected to current collector 001 and a solid electrolyte membrane 004 is provided on the opposite side.

[0088] Two negative solid electrolyte composite electrodes 602 and one positive solid electrolyte composite electrode 601 are stacked in the order of "negative → positive → negative" to prepare a battery cell. Figure 6 As shown.

[0089] Example 2 This embodiment discloses a solid electrolyte composite electrode forming apparatus and forming method, such as Figure 3 As shown, the molding apparatus includes: The first rolling mechanism 110 consists of a first roller 011, a second roller 012, a third roller 013, a fourth roller 014, a fifth roller 015, and a sixth roller 016 arranged sequentially. The rotational speeds of the first roller 011, the second roller 012, the third roller 013, the fourth roller 014, and the fifth roller 015 increase progressively. The gap between the first roller 011 and the second roller 012 forms a first forming area; the gap between the fifth roller 015 and the sixth roller 016 forms a second forming area; and the areas between the second roller 012 and the third roller 013, between the third roller 013 and the fourth roller 014, and between the fourth roller 014 and the fifth roller 015 form calendering and thinning areas.

[0090] The forming method includes: pressing a first solid electrolyte membrane between a first pressure roller and a second pressure roller; The first type of solid electrolyte membrane is pressed into a film by the first and second pressure rollers, and then transferred to the surface of the second pressure roller for further thinning between the second and fifth pressure rollers.

[0091] The first type of solid electrolyte membrane is thinned by the second and fifth pressure rollers and then transferred on the surface of the fifth pressure roller to the gap between the fifth and sixth pressure rollers. The electrode 100 is transmitted through the electrode unwinding mechanism 300 and the first tension correction mechanism 210 to the fifth and sixth pressure rollers to be pressed and formed with the first solid electrolyte membrane. After the electrode is combined with the thinned first solid electrolyte membrane, it is transmitted through the second tension correction mechanism 22 to the solid electrolyte membrane composite electrode winding mechanism 400 for collection.

[0092] The linear speeds of the first, second, ..., fifth pressure rollers vary such that the ratio of the rotational speeds of the slower and faster rollers of adjacent pressure rollers is 1:1.5, and the linear speed of the sixth pressure roller is the same as that of the fourth pressure roller.

[0093] The ratio of the gap between the two pressure rollers in the low-speed zone to the gap between the two pressure rollers in the adjacent high-speed zone satisfies the condition: 1.5:1.

[0094] The first solid electrolyte membrane is a halide solid electrolyte with an average particle size of 30~40μm; the sulfide solid electrolyte powder and the styrene block copolymer binder are mixed solid materials with a mass ratio of 1:2.

[0095] The surface temperatures of the first to sixth pressure rollers are controlled by a mold temperature controller, with roller surface temperatures of 160℃, 150℃, 140℃, 130℃, 122℃, and 120℃ respectively.

[0096] The composite electrode sheets are stacked to prepare a battery cell. The structure of the positive electrode solid electrolyte composite electrode sheet 601 is as follows: Figure 7 As shown, symmetrically distributed positive electrode films 002 are located on both sides of the current collector 001; the structure of the negative electrode solid electrolyte composite electrode 602 is as follows. Figure 8 As shown: A negative electrode membrane 003 is symmetrically distributed on both sides of the current collector 001. The negative electrode membrane 003 is connected to the current collector 001 and a solid electrolyte membrane 004 is provided on the opposite side.

[0097] Two negative solid electrolyte composite electrodes 602 and one positive solid electrolyte composite electrode 601 are stacked in the order of "negative → positive → negative" to prepare a battery cell. Figure 9 As shown.

[0098] Example 3 This embodiment discloses a solid electrolyte composite electrode forming apparatus and forming method, such as Figure 10 As shown, the molding apparatus includes: The first rolling mechanism 110 consists of a first rolling roller 011, a second rolling roller 012, a third rolling roller 013, a fourth rolling roller 014, and a fifth rolling roller 015 arranged sequentially. The rotational speeds of the first rolling roller 011, the second rolling roller 012, and the third rolling roller 013 increase progressively. The gap between the first rolling roller 011 and the second rolling roller 012 forms a first forming area; the areas between the second rolling roller 012 and the third rolling roller 013, between the third rolling roller 013 and the fourth rolling roller 014, and between the fourth rolling roller 014 and the fifth rolling roller 015 form calendering and thinning areas.

[0099] The second rolling mechanism consists of a sixth roller 016, a seventh roller 017, an eighth roller 018, a ninth roller 019, and a tenth roller 020 arranged sequentially. The rotational speeds of the tenth roller 011, the ninth roller 019, the eighth roller 018, and the seventh roller 017 increase progressively. The gap between the ninth roller 019 and the tenth roller 020 forms a third forming area; the areas between the eighth roller 018 and the seventh roller 017, between the ninth roller 019 and the eighth roller 018, and between the tenth roller 020 and the ninth roller 019 form calendering and thinning areas.

[0100] The gap between the fifth pressure roller 015 and the sixth pressure roller 016 forms a second forming area; Molding methods include: The pre-fiberized powder is fed into the first feeding mechanism 510 and the second feeding mechanism 520. The feeding mechanism adjusts the feeding speed according to the rotation speed of the pressure rollers and feeds the powder between the first pressure roller 011, the second pressure roller 012, the ninth pressure roller 019, and the tenth pressure roller 020.

[0101] The first solid electrolyte film is pressed and formed between the first pressure roller 011 and the second pressure roller 012. There is a speed difference between the two adjacent rollers, namely the first pressure roller 011 and the second pressure roller 012. When the powder passes through the rollers, the high shear force brought about by the speed difference rolls and stretches the solid electrolyte powder, pressing it into a film. The tensile resistance of the solid electrolyte after being sheared causes it to adhere to the surface of the second pressure roller 012 with a faster speed and be transferred.

[0102] The first solid electrolyte membrane is pressed into a film by the first pressure roller 011 and the second pressure roller 012. The membrane is then transferred to the surface of the second pressure roller 012 and then transferred to the gap between the second pressure roller 012 and the fifth pressure roller 015 for further thinning treatment before reaching the gap between the fifth pressure roller 015 and the sixth pressure roller 016.

[0103] The second solid electrolyte film is pressed and formed between the ninth pressure roller 019 and the tenth pressure roller 020. There is a speed difference between the two adjacent rollers, namely the ninth pressure roller 019 and the tenth pressure roller 020. When passing through the rollers, the high shear force brought about by the speed difference rolls the solid electrolyte powder to stretch it and press it into a film. The tensile resistance of the solid electrolyte after being sheared causes it to adhere to the surface of the faster-rotating ninth pressure roller 019 and be transferred.

[0104] The second solid electrolyte membrane is pressed into a film by the ninth pressure roller 019 and the tenth pressure roller 020. The film is then transferred to the surface of the ninth pressure roller 019 and conducted between the ninth pressure roller 019 and the eighth pressure roller 018 for further thinning.

[0105] The second solid electrolyte membrane is thinned by the ninth pressure roller 019 to the sixth pressure roller 016, and then transferred on the surface of the sixth pressure roller 016 to the gap between the fifth pressure roller 015 and the sixth pressure roller 016.

[0106] The electrode sheet to be laminated is transmitted to the space between the fifth pressure roller 015 and the sixth pressure roller 016 via the electrode sheet unwinding mechanism 300, the web-correcting mechanism, and the tension control mechanism 210. Both sides of the electrode sheet and the first and second solid electrolyte films simultaneously pass through the gap between the fifth pressure roller 015 and the sixth pressure roller 016, thus laminating both sides of the electrode sheet with the two thinned solid electrolyte films. After passing through the web-correcting and tension control mechanism 220, the laminated electrode sheet is wound up by the solid electrolyte film laminated electrode sheet winding mechanism 400.

[0107] The linear speeds of the first, second, ..., tenth pressure rollers vary in such a way that the ratio of the slower to the faster speeds of adjacent pressure rollers is 1:3, and the linear speed of the sixth pressure roller is the same as that of the fifth pressure roller.

[0108] In the first roller pressing mechanism, the ratio of the gap between the two rollers in the low-speed zone to the gap between the two rollers in the adjacent high-speed zone satisfies 2:1.

[0109] In the second roller pressing mechanism, the ratio of the gap between the two rollers in the low-speed zone to the gap between the two rollers in the adjacent high-speed zone satisfies 2:1.

[0110] The surface temperatures of the first to tenth pressure rollers are controlled by a mold temperature controller, and their roller surface temperatures are 100℃, 105℃, 110℃, 115℃, 120℃, 120℃, 130℃, 140℃, 150℃, and 160℃ respectively.

[0111] The first and second solid electrolyte membranes are made of the same material, namely sulfide solid electrolyte with an average particle size of 40~50μm; the sulfide solid electrolyte powder and styrene block copolymer binder are mixed in a 1:1 mass ratio as a solid material.

[0112] The composite electrode sheets are stacked to prepare a battery cell. The structure of the positive electrode solid electrolyte composite electrode sheet 601 is as follows: Figure 7 As shown, symmetrically distributed positive electrode films 002 are located on both sides of the current collector 001; the structure of the negative electrode solid electrolyte composite electrode 602 is as follows. Figure 8 As shown: A negative electrode membrane 003 is symmetrically distributed on both sides of the current collector 001. The negative electrode membrane 003 is connected to the current collector 001 and a solid electrolyte membrane 004 is provided on the opposite side.

[0113] Two negative solid electrolyte composite electrodes 602 and one positive solid electrolyte composite electrode 601 are stacked in the order of "negative → positive → negative" to prepare a battery cell. Figure 9 As shown.

[0114] Example 4 This embodiment discloses a solid electrolyte composite electrode forming apparatus and forming method, such as Figure 2a As shown, the molding apparatus includes: The rotational speeds of the first pressure roller 011 and the second pressure roller 012 increase progressively, as do the rotational speeds of the fourth pressure roller 014 and the third pressure roller 013. The first pressure roller 011 and the fourth pressure roller 014 rotate at the same speed, as do the second pressure roller 012 and the third pressure roller 013.

[0115] The forming method includes: adding the pre-fiberized powder to the first feeding mechanism 510 and the second feeding mechanism 520. The feeding mechanism adjusts the feeding speed according to the rotation speed of the pressure rollers and feeds the powder between the first pressure roller 011, the second pressure roller 012, the third pressure roller 013, and the fourth pressure roller 014.

[0116] The first solid electrolyte membrane is formed by pressing between the first pressure roller 011 and the second pressure roller 012. There is a speed difference between the two adjacent rollers, namely the first pressure roller 011 and the second pressure roller 012. When the powder passes through the rollers, the high shear force brought about by the speed difference rolls and stretches the solid electrolyte powder to form a membrane. The tensile resistance of the solid electrolyte after being sheared causes it to adhere to the surface of the second pressure roller 012 with a faster speed and be transferred.

[0117] The first solid electrolyte membrane is transferred from the surface of the second pressure roller 012 to the gap between the second pressure roller 012 and the third pressure roller 013.

[0118] The second solid electrolyte membrane is pressed and formed between the fourth pressure roller 014 and the third pressure roller 013. There is a speed difference between the two adjacent rollers, namely the fourth pressure roller 014 and the third pressure roller 013. When passing through the rollers, the high shear force brought about by the speed difference rolls the solid electrolyte powder to stretch it and press it into a membrane. The tensile resistance of the solid electrolyte after being sheared causes it to adhere to the surface of the faster-rotating third pressure roller 013 and be transferred.

[0119] The second solid electrolyte membrane is transferred from the surface of the third pressure roller 013 to the gap between the third pressure roller 013 and the second pressure roller 012.

[0120] The solid electrolyte composite electrode 600 is transmitted through the unwinding mechanism 300, the web-correcting mechanism, and the tension control mechanism 210 to the space between the third pressure roller 013 and the second pressure roller 012. The two sides of the double-sided composite film, along with the first and second solid electrolyte films, pass through the gap between the third pressure roller 013 and the second pressure roller 012 simultaneously, so that both sides of the film are composited with the solid electrolyte film. After passing through the web-correcting and tension control mechanism 220, the winding mechanism 400 winds up the composite electrode to obtain a film with a double-sided symmetrical composite of solid electrolyte films.

[0121] The linear speeds of the first, second, ..., fourth pressure rollers vary in such a way that the ratio of the rotational speeds of the slower and faster rollers of adjacent pressure rollers is 1:2, and the linear speeds of the second and third pressure rollers are the same.

[0122] The first and second solid electrolyte membranes are made of the same raw materials, namely sulfide solid electrolytes with an average particle size of 10~30μm. The sulfide solid electrolyte powder and PTFE binder are mixed at a mass ratio of 98:2 to obtain solid powder.

[0123] The ratio of the gap between the two pressure rollers in the low-speed zone of the first roller pressing mechanism to the gap between the two pressure rollers in the adjacent high-speed zone satisfies 5:1.

[0124] The surface temperatures of the first to sixth pressure rollers are controlled by a mold temperature controller, with the roller surface temperatures being 100℃, 110℃, 120℃, 120℃, 110℃, and 100℃ respectively.

[0125] The composite electrode sheets are stacked to prepare a battery cell. The structure of the positive electrode 601a is as follows: Figure 5a As shown, the structure of the double-sided composite negative electrode 602a is as follows: Figure 6a As shown: Positive electrode membranes 002 are symmetrically distributed on both sides of current collector 001, or negative electrode membranes 003 are symmetrically distributed on both sides of current collector 001, and solid electrolyte membranes 004 are symmetrically distributed on both sides of negative electrode membranes.

[0126] A battery cell is prepared by stacking positive electrode 601a and double-sided composite negative electrode 602a in an alternating sequence, as shown in the example. Figure 7a As shown.

[0127] Conversely, the same effect can be achieved by combining the solid electrolyte membrane 004 with both sides of the positive electrode 601a, and by stacking the solid electrolyte membrane with the positive electrode and the negative electrode in an alternating order.

[0128] Example 5 This embodiment discloses a solid electrolyte composite electrode forming apparatus and forming method, such as Figure 3aAs shown, the molding apparatus includes: The first roller pressing mechanism 110 consists of a first roller 011, a second roller 012, a third roller 013, a fourth roller 014, a fifth roller 015, and a sixth roller 016 arranged sequentially. The rotational speeds of the first roller 011, the second roller 012, the third roller 013, the fourth roller 014, and the fifth roller 015 increase progressively. The gap between the first roller 011 and the second roller 012 forms a first forming area; the gap between the fifth roller 015 and the sixth roller 016 forms a second forming area; the calendering and thinning areas are formed between the third roller 013 and the fourth roller 014, and between the fourth roller 014 and the fifth roller 015; and a tension buffer zone is formed between the second roller 012 and the third roller 013.

[0129] The forming method includes: pressing a first solid electrolyte membrane between a first pressure roller and a second pressure roller; The first solid electrolyte membrane is pressed into a film by the first and second pressure rollers, and then transferred to the surface of the second pressure roller for further thinning between the second and fifth pressure rollers.

[0130] The first solid electrolyte membrane is thinned by the second and fifth pressure rollers and transferred on the surface of the fifth pressure roller to the gap between the fifth and sixth pressure rollers; The electrode 100 is transmitted through the unwinding mechanism 300 and the first tension correction mechanism 210 to the fifth pressure roller and the sixth pressure roller to be pressed together with the first solid electrolyte film. After the electrode 100 is combined with the thinned first solid electrolyte film, it is transmitted through the second tension correction mechanism 220 to the winding mechanism 400 for collection.

[0131] The linear speeds of the first, second, ..., fifth pressure rollers change in accordance with the following conditions: the ratio of the rotational speeds of the slower and faster rollers of adjacent pressure rollers is 1:1.5, and the linear speed of the sixth pressure roller (016) is the same as that of the fifth pressure roller (015).

[0132] The ratio of the gap between the first pressure roller 011 and the second pressure roller 012 to the gap between the second pressure roller 012 and the third pressure roller 013 is 0.8:1, which is used to release the diaphragm rebound and improve the uniformity of the diaphragm. Subsequently, the gap between each pressure roller decreases step by step along the direction of the sixth pressure roller, and the ratio of two adjacent gaps satisfies: 1.5:1.

[0133] The first solid electrolyte membrane is a sulfide solid electrolyte with an average particle size of 10~30μm; the sulfide solid electrolyte powder and PTFE binder are mixed at a mass ratio of 97:3 to obtain a solid powder.

[0134] The surface temperatures of the first to sixth pressure rollers are controlled by a mold temperature controller, with roller surface temperatures of 160℃, 150℃, 140℃, 130℃, 122℃, and 120℃ respectively.

[0135] The composite electrode sheets are stacked to prepare a battery cell. The structure of the composite electrode sheet 603 is as follows: Figure 8a As shown, negative electrode membranes 003 are symmetrically distributed on both sides of the current collector 001; the negative electrode membranes 003 are connected to the current collector 001 and a sulfide solid electrolyte membrane 004a is provided on the opposite side.

[0136] Example 6 This embodiment discloses a solid electrolyte composite electrode forming apparatus and forming method, such as Figure 4a As shown, the molding apparatus includes: The first rolling mechanism 110 consists of a first pressure roller 011, a second pressure roller 012, a third pressure roller 013, a fourth pressure roller 014, and a fifth pressure roller 015 arranged sequentially, with their rotational speeds increasing progressively. The gap between the first pressure roller 011 and the second pressure roller 012 forms a first forming area; the gap between the third pressure roller 013 and the fourth pressure roller 014, and the gap between the fourth pressure roller 014 and the fifth pressure roller 015, form a calendering and thinning area; and the gap between the second pressure roller 012 and the third pressure roller 013 forms a tension buffer zone.

[0137] The second rolling mechanism consists of a sixth roller 016, a seventh roller 017, an eighth roller 018, a ninth roller 019, and a tenth roller 020 arranged sequentially. The rotational speeds of the tenth roller 020, the ninth roller 019, the eighth roller 018, the seventh roller 017, and the sixth roller 016 increase progressively. The gap between the ninth roller 019 and the tenth roller 020 forms a third forming area; the areas between the seventh roller 017 and the sixth roller 018, and between the eighth roller 018 and the seventh roller 017, form calendering and thinning areas; and the area between the ninth roller 019 and the eighth roller 018 forms a tension buffer zone.

[0138] The gap between the fifth pressure roller 015 and the sixth pressure roller 016 forms a second forming area; Molding methods include: The pre-fiberized powder is fed into the first feeding mechanism 510 and the second feeding mechanism 520. The feeding mechanism adjusts the feeding speed according to the rotation speed of the pressure rollers and feeds the powder between the first pressure roller 011, the second pressure roller 012, the ninth pressure roller 019, and the tenth pressure roller 020.

[0139] The first solid electrolyte membrane is formed by pressing between the first pressure roller 011 and the second pressure roller 012. There is a speed difference between the two adjacent rollers, namely the first pressure roller 011 and the second pressure roller 012. When the powder passes through the rollers, the high shear force brought about by the speed difference rolls and stretches the solid electrolyte powder to form a membrane. The tensile resistance of the solid electrolyte after being sheared causes it to adhere to the surface of the second pressure roller 012 with a faster speed and be transferred.

[0140] The first solid electrolyte membrane is pressed into a film by the first pressure roller 011 and the second pressure roller 012. The membrane is then transferred to the surface of the second pressure roller 012 and then transferred to the gap between the second pressure roller 012 and the fifth pressure roller 015 for further thinning treatment before reaching the gap between the fifth pressure roller 015 and the sixth pressure roller 016.

[0141] The second solid electrolyte membrane is pressed and formed between the ninth pressure roller 019 and the tenth pressure roller 020. There is a speed difference between the two adjacent rollers, namely the ninth pressure roller 019 and the tenth pressure roller 020. When passing through the rollers, the high shear force brought about by the speed difference rolls the solid electrolyte powder to stretch it and press it into a membrane. The tensile resistance of the solid electrolyte after being sheared causes it to adhere to the surface of the faster-rotating ninth pressure roller 019 and be transferred.

[0142] The second solid electrolyte membrane is pressed into a film by the ninth pressure roller 019 and the tenth pressure roller 020. The membrane is then transferred to the surface of the ninth pressure roller 019 and conducted between the ninth pressure roller 019 and the eighth pressure roller 018 for further thinning.

[0143] The second solid electrolyte membrane is thinned by the ninth pressure roller 019 to the sixth pressure roller 016, and then transferred on the surface of the sixth pressure roller 016 to the gap between the fifth pressure roller 015 and the sixth pressure roller 016.

[0144] The membrane to be laminated is transmitted through the unwinding mechanism 300, the web-correcting mechanism, and the tension control mechanism 210 to the space between the fifth pressure roller 015 and the sixth pressure roller 016. The membrane and the first and second solid electrolyte membranes pass through the gap between the fifth pressure roller 015 and the sixth pressure roller 016 simultaneously, so that both sides of the membrane are laminated with the two thinned solid electrolyte films. After passing through the web-correcting and tension control mechanism 220, the laminated membrane is wound up by the winding mechanism 400.

[0145] The linear speeds of the first, second, ..., tenth pressure rollers vary in such a way that the ratio of the slower to the faster speeds of adjacent pressure rollers is 1:3, and the linear speed of the sixth pressure roller is the same as that of the fifth pressure roller.

[0146] The ratio of the gap between the first pressure roller 011 and the second pressure roller 012 to the gap between the second pressure roller 012 and the third pressure roller 013 is 0.8:1. The ratio of the gap between the tenth pressure roller 020 and the ninth pressure roller 019 to the gap between the ninth pressure roller 019 and the eighth pressure roller 018 is 0.8:1. This is to release the diaphragm rebound and improve the uniformity of the diaphragm. Subsequently, the gap between each pressure roller decreases step by step along the direction of the sixth pressure roller, and the ratio of two adjacent gaps satisfies 2:1.

[0147] The surface temperatures of the first to tenth pressure rollers are controlled by a mold temperature controller, and their roller surface temperatures are 100℃, 105℃, 110℃, 115℃, 120℃, 120℃, 130℃, 140℃, 150℃, and 160℃ respectively.

[0148] The first and second solid electrolyte membranes are made of different raw materials, namely sulfide solid electrolyte and halide solid electrolyte, respectively. The average particle size of the sulfide solid electrolyte is 10~30μm, and the average particle size of the halide solid electrolyte is 3~4μm. The solid electrolyte powder and PTFE binder are mixed at a mass ratio of 98.5:1.5 to obtain solid powder.

[0149] A battery cell is fabricated by combining a bipolar membrane with two electrolyte membranes and then stacking the composite electrode sheets. The structure of the double-sided composite bipolar membrane 604 is as follows: Figure 9a As shown, a positive electrode membrane 002 and a negative electrode membrane 003 are distributed on both sides of the current collector 001, respectively; the positive electrode membrane 002 is composite with a sulfide solid electrolyte membrane 004a, and the negative electrode membrane 003 is composite with a halide solid electrolyte membrane 005a.

[0150] A battery cell is prepared by stacking double-sided composite bipolar diaphragms 604 in sequence. Figure 10a The internal string structure of the battery cell is shown.

[0151] Example 7 This embodiment discloses a solid electrolyte composite electrode forming apparatus and forming method, such as Figure 4a As shown, the molding apparatus includes: The first roller pressing mechanism 110 consists of a first roller 011, a second roller 012, a third roller 013, a fourth roller 014, and a fifth roller 015 arranged sequentially, with their rotational speeds increasing progressively. The gap between the first roller 011 and the second roller 012 forms a first forming area; the gap between the third roller 013 and the fourth roller 014, and the gap between the fourth roller 014 and the fifth roller 015, forms a calendering and thinning area; and the gap between the second roller 012 and the third roller 013 forms a tension buffer area.

[0152] The second rolling mechanism consists of a sixth roller 016, a seventh roller 017, an eighth roller 018, a ninth roller 019, and a tenth roller 020 arranged sequentially. The rotational speeds of the tenth roller 020, the ninth roller 019, the eighth roller 018, the seventh roller 017, and the sixth roller 016 increase progressively. The gap between the ninth roller 019 and the tenth roller 020 forms a third forming area; the calendering and thinning areas are formed between the seventh roller 017 and the eighth roller 018, and between the eighth roller 018 and the seventh roller 017; and the tension buffer area is formed between the ninth roller 019 and the eighth roller 018.

[0153] The gap between the fifth pressure roller 015 and the sixth pressure roller 016 forms a second forming area; Molding methods include: The pre-fiberized powder is fed into the first feeding mechanism 510 and the second feeding mechanism 520. The feeding mechanism adjusts the feeding speed according to the rotation speed of the pressure rollers and feeds the powder between the first pressure roller 011, the second pressure roller 012, the ninth pressure roller 019, and the tenth pressure roller 020.

[0154] The first solid electrolyte membrane is formed by pressing between the first pressure roller 011 and the second pressure roller 012. There is a speed difference between the two adjacent rollers, namely the first pressure roller 011 and the second pressure roller 012. When the powder passes through the rollers, the high shear force brought about by the speed difference rolls and stretches the solid electrolyte powder to form a membrane. The tensile resistance of the solid electrolyte after being sheared causes it to adhere to the surface of the second pressure roller 012 with a faster speed and be transferred.

[0155] The first solid electrolyte membrane is pressed into a film by the first pressure roller 011 and the second pressure roller 012. The membrane is then transferred to the surface of the second pressure roller 012 and then transferred to the gap between the second pressure roller 012 and the fifth pressure roller 015 for further thinning treatment before reaching the gap between the fifth pressure roller 015 and the sixth pressure roller 016.

[0156] The second solid electrolyte membrane is pressed and formed between the ninth pressure roller 019 and the tenth pressure roller 020. There is a speed difference between the two adjacent rollers, namely the ninth pressure roller 019 and the tenth pressure roller 020. When passing through the rollers, the high shear force brought about by the speed difference rolls the solid electrolyte powder to stretch it and press it into a membrane. The tensile resistance of the solid electrolyte after being sheared causes it to adhere to the surface of the faster-rotating ninth pressure roller 019 and be transferred.

[0157] The second solid electrolyte membrane is pressed into a film by the ninth pressure roller 019 and the tenth pressure roller 020. The membrane is then transferred to the surface of the ninth pressure roller 019 and conducted between the ninth pressure roller 019 and the eighth pressure roller 018 for further thinning.

[0158] The second solid electrolyte membrane is thinned by the ninth pressure roller 019 to the sixth pressure roller 016, and then transferred on the surface of the sixth pressure roller 016 to the gap between the fifth pressure roller 015 and the sixth pressure roller 016.

[0159] The membrane to be laminated is transmitted through the unwinding mechanism 300, the web-correcting mechanism, and the tension control mechanism 210 to the space between the fifth pressure roller 015 and the sixth pressure roller 016. The membrane and the first and second solid electrolyte membranes pass through the gap between the fifth pressure roller 015 and the sixth pressure roller 016 simultaneously, so that both sides of the membrane are laminated with the thinned solid electrolyte film. After passing through the web-correcting and tension control mechanism 220, the laminated membrane is wound up by the winding mechanism 400 to obtain a double-sided single-layer solid electrolyte composite membrane.

[0160] Repeat the above steps to add the pre-fiberized powder to the first feeding mechanism 510 and the second feeding mechanism 520. The feeding mechanism adjusts the feeding speed according to the rotation speed of the pressure rollers to feed the powder between the first pressure roller 011, the second pressure roller 012, the ninth pressure roller 019, and the tenth pressure roller 020 to obtain the first and second solid electrolyte membranes.

[0161] The first and second solid electrolyte membranes, after being formed and thinned, are transferred between the fifth pressure roller 015 and the sixth pressure roller 016. The double-sided single-layer solid electrolyte composite film is then transmitted between the fifth pressure roller 015 and the sixth pressure roller 016 via the unwinding mechanism 300, the web-correcting mechanism, and the tension control mechanism 210. Both sides of the film, along with the first and second solid electrolyte membranes, pass through the gap between the fifth pressure roller 015 and the sixth pressure roller 016 simultaneously, thus bonding both sides of the film with the thinned solid electrolyte film. After passing through the web-correcting and tension control mechanism 220, the composite film is wound up by the winding mechanism 400 to obtain a double-sided double-layer solid electrolyte composite film.

[0162] The linear speeds of the first, second, ..., tenth pressure rollers vary in such a way that the ratio of the slower to the faster speeds of adjacent pressure rollers is 1:3, and the linear speed of the sixth pressure roller is the same as that of the fifth pressure roller.

[0163] The ratio of the gap between the first pressure roller 011 and the second pressure roller 012 to the gap between the second pressure roller 012 and the third pressure roller 013 is 0.8:1. The ratio of the gap between the tenth pressure roller 020 and the ninth pressure roller 019 to the gap between the ninth pressure roller 019 and the eighth pressure roller 018 is 0.8:1. This is to release the diaphragm rebound and improve the uniformity of the diaphragm. Subsequently, the gap between each pressure roller decreases step by step along the direction of the sixth pressure roller, and the ratio of two adjacent gaps satisfies 2:1.

[0164] The surface temperatures of the first to tenth pressure rollers are controlled by a mold temperature controller, and their roller surface temperatures are 100℃, 105℃, 110℃, 115℃, 120℃, 120℃, 130℃, 140℃, 150℃, and 160℃ respectively.

[0165] The inner and outer solid electrolyte membranes are made of different materials, namely sulfide solid electrolyte and halide solid electrolyte. The average particle size of the sulfide solid electrolyte is 10~30μm, and the average particle size of the halide solid electrolyte is 3~4μm. The solid electrolyte powder and PTFE binder are mixed at a mass ratio of 98:2 to obtain solid powder.

[0166] After two composite processes, a symmetrical double-sided, double-layer solid electrolyte composite membrane structure 605 is obtained, as shown below. Figure 11a As shown, a battery cell is fabricated by alternately stacking the composite double-sided double-layer electrolyte membrane 605 and the positive electrode 601a, as shown. Figure 12a The battery cell is shown in the figure.

[0167] Example 8 This comparative example discloses an existing apparatus and method for preparing solid electrolyte composite electrodes. The preparation method differs from that in Example 6 in that: The gap between each pressure roller decreases progressively along the direction of the sixth pressure roller, and the ratio of any two adjacent gaps satisfies 2:1.

[0168] like Figure 4a As shown, the molding apparatus includes: The first rolling mechanism 110 consists of a first pressure roller 011, a second pressure roller 012, a third pressure roller 013, a fourth pressure roller 014, and a fifth pressure roller 015 arranged sequentially, with the rotational speed increasing progressively. The gap between the first pressure roller 011 and the second pressure roller 012 forms a first forming area; the gaps between the second pressure roller 012 and the third pressure roller 013, the third pressure roller 013 and the fourth pressure roller 014, and the fourth pressure roller 014 and the fifth pressure roller 015 form a calendering and thinning area.

[0169] The second rolling mechanism consists of a sixth roller 016, a seventh roller 017, an eighth roller 018, a ninth roller 019, and a tenth roller 020 arranged sequentially. The rotational speeds of the tenth roller 020, the ninth roller 019, the eighth roller 018, the seventh roller 017, and the sixth roller 016 increase progressively. The gap between the ninth roller 019 and the tenth roller 020 forms a third forming area. The areas between the ninth roller 019 and the eighth roller 018, the eighth roller 018 and the seventh roller 017, and the seventh roller 017 and the sixth roller 016 form calendering and thinning areas.

[0170] The gap between the fifth pressure roller 015 and the sixth pressure roller 016 forms a second forming area; Molding methods include: The pre-fiberized powder is fed into the first feeding mechanism 510 and the second feeding mechanism 520. The feeding mechanism adjusts the feeding speed according to the rotation speed of the pressure rollers and feeds the powder between the first pressure roller 011, the second pressure roller 012, the ninth pressure roller 019, and the tenth pressure roller 020.

[0171] The first solid electrolyte membrane is formed by pressing between the first pressure roller 011 and the second pressure roller 012. There is a speed difference between the two adjacent rollers, namely the first pressure roller 011 and the second pressure roller 012. When the powder passes through the rollers, the high shear force brought about by the speed difference rolls and stretches the solid electrolyte powder to form a membrane. The tensile resistance of the solid electrolyte after being sheared causes it to adhere to the surface of the second pressure roller 012 with a faster speed and be transferred.

[0172] The first solid electrolyte membrane is pressed into a film by the first pressure roller 011 and the second pressure roller 012. The membrane is then transferred to the surface of the second pressure roller 012 and then transferred to the gap between the second pressure roller 012 and the fifth pressure roller 015 for further thinning treatment before reaching the gap between the fifth pressure roller 015 and the sixth pressure roller 016.

[0173] The second solid electrolyte membrane is pressed and formed between the ninth pressure roller 019 and the tenth pressure roller 020. There is a speed difference between the two adjacent rollers, namely the ninth pressure roller 019 and the tenth pressure roller 020. When passing through the rollers, the high shear force brought about by the speed difference rolls the solid electrolyte powder to stretch it and press it into a membrane. The tensile resistance of the solid electrolyte after being sheared causes it to adhere to the surface of the faster-rotating ninth pressure roller 019 and be transferred.

[0174] The second solid electrolyte membrane is pressed into a film by the ninth pressure roller 019 and the tenth pressure roller 020. The membrane is then transferred to the surface of the ninth pressure roller 019 and conducted between the ninth pressure roller 019 and the eighth pressure roller 018 for further thinning.

[0175] The second solid electrolyte membrane is thinned by the ninth pressure roller 019 to the sixth pressure roller 016, and then transferred on the surface of the sixth pressure roller 016 to the gap between the fifth pressure roller 015 and the sixth pressure roller 016.

[0176] The membrane to be laminated is transmitted through the unwinding mechanism 300, the web-correcting mechanism, and the tension control mechanism 210 to the space between the fifth pressure roller 015 and the sixth pressure roller 016. The membrane and the first and second solid electrolyte membranes pass through the gap between the fifth pressure roller 015 and the sixth pressure roller 016 simultaneously, so that both sides of the membrane are laminated with the two thinned solid electrolyte films. After passing through the web-correcting and tension control mechanism 220, the laminated membrane is wound up by the winding mechanism 400.

[0177] The linear speeds of the first, second, ..., tenth pressure rollers vary in such a way that the ratio of the slower to the faster speeds of adjacent pressure rollers is 1:3, and the linear speed of the sixth pressure roller is the same as that of the fifth pressure roller.

[0178] Within the first roller pressing mechanism, the ratio of the gap between the first roller 011 and the second roller 012 to the gap between the second roller 012 and the third roller 013 is 2:1. The gaps between subsequent rollers decrease progressively along the direction of the sixth roller, and the ratio of two adjacent gaps satisfies 2:1. Within the second roller pressing mechanism, the ratio of the gap between the tenth roller 020 and the ninth roller 019 to the gap between the ninth roller 019 and the eighth roller 018 is 2:1. The gaps between subsequent rollers decrease progressively along the direction of the sixth roller, and the ratio of two adjacent gaps satisfies 2:1.

[0179] The surface temperatures of the first to tenth pressure rollers are controlled by a mold temperature controller, and their roller surface temperatures are 100℃, 105℃, 110℃, 115℃, 120℃, 120℃, 130℃, 140℃, 150℃, and 160℃ respectively.

[0180] The first and second solid electrolyte membranes are made of different raw materials, namely sulfide solid electrolyte and halide solid electrolyte, respectively. The average particle size of the sulfide solid electrolyte is 10~30μm, and the average particle size of the halide solid electrolyte is 3~4μm. The solid electrolyte powder and PTFE binder are mixed at a mass ratio of 98.5:1.5 to obtain solid powder.

[0181] A battery cell is fabricated by combining a bipolar membrane with two electrolyte membranes and then stacking the composite electrode sheets. The structure of the bipolar solid electrolyte electrode sheet 605 is as follows: Figure 9 As shown, a positive electrode membrane 002 and a negative electrode membrane 003 are distributed on both sides of the current collector 001, respectively; the positive electrode membrane 002 is combined with a solid electrolyte membrane 004, and the negative electrode membrane 003 is combined with a solid electrolyte membrane 005.

[0182] A battery cell is prepared by stacking bipolar solid electrolyte electrodes 605 in sequence. Figure 10 The internal string structure of the battery cell is shown.

[0183] Comparative Example 1 This comparative example discloses an existing apparatus and method for preparing solid electrolyte composite electrodes, the preparation method being as follows: Figure 1 As shown, it includes: S1: Mix the sulfide solid electrolyte powder with the styrene block copolymer binder, add xylene as a solvent, and homogenize the mixture using a dual planetary mixer. S2: Coat the well-stirred solid electrolyte slurry onto the surface of the PET support carrier; S3: Transfer the PET film to the drying workshop for high-temperature baking and drying.

[0184] S4: The dried PET film coated with solid electrolyte membrane 004 is wound up and transferred to the laminating mechanism.

[0185] S5: A PET film coated with a solid electrolyte membrane 004 is roll-pressed with an electrode 100 (composed of a current collector 001 and an external positive electrode membrane 002 or negative electrode membrane 003), with the side of the PET film coated with the solid electrolyte facing the electrode. After passing through the roll, the PET substrate is removed to peel the solid electrolyte from the PET film. This method produces a film as shown in the image. Figure 6a The double-sided composite negative electrode sheet 602a is shown.

[0186] Comparative Example 2 This comparative example discloses an existing apparatus and method for preparing solid electrolyte composite electrodes, the preparation method being as follows: Figure 1 As shown, it includes: S1: Mix the sulfide solid electrolyte powder with the SBR binder, add xylene as a solvent, and homogenize the mixture using a dual planetary mixer. S2: Coat the well-stirred solid electrolyte slurry onto the surface of the PET support carrier; S3: Transfer the PET film to the drying workshop for high-temperature baking and drying.

[0187] S4: The dried PET film coated with sulfide solid electrolyte membrane 004a is wound up and transferred to the laminating mechanism.

[0188] S5: A PET film coated with a sulfide solid electrolyte membrane 004a is roll-pressed with an electrode 100 (composed of a current collector 001 and an external positive electrode membrane 002 or negative electrode membrane 003), with the side of the PET coated with the solid electrolyte facing the electrode. After passing through the roll, the PET substrate is removed to peel the solid electrolyte from the PET film, resulting in a membrane as shown. Figure 8a The single-sided composite negative electrode sheet 603 is shown.

[0189] Comparative Example 3 This comparative example discloses an existing apparatus and method for preparing solid electrolyte composite electrodes, the preparation method being as follows: Figure 1 As shown, it includes: S1: Sulfide solid electrolyte powder is mixed with SBR binder, xylene is added as solvent, and homogenization is performed using a double planetary mixer to obtain sulfide electrolyte slurry; Halogen solid electrolyte powder is mixed with SBR binder, xylene is added as solvent, and homogenization is performed using a double planetary mixer to obtain halide electrolyte slurry. S2: Coat the well-stirred solid electrolyte slurry onto the surfaces of two rolls of PET support carrier respectively; S3: Transfer the PET film to the drying workshop for high-temperature baking and drying.

[0190] S4: The two rolls of PET film, which are dried and coated with sulfide solid electrolyte membrane 004a and halide solid electrolyte membrane 005a respectively, are wound up and transferred to the laminating mechanism.

[0191] S5: A PET film coated with a sulfide solid electrolyte membrane 004a and a halide solid electrolyte membrane 005a is roll-pressed with an electrode 100 (composed of a current collector 001 and an external positive electrode membrane 002 or a negative electrode membrane 003). The side of the PET film coated with the solid electrolyte faces the electrode. The sulfide solid electrolyte membrane 004a is bonded to the positive electrode membrane 002, and the halide solid electrolyte membrane 005a is bonded to the negative electrode membrane 003. After passing through the roll, the PET substrate is removed to peel the solid electrolyte from the PET film. This method produces a film as shown in the image. Figure 9a The double-sided composite bipolar membrane 604 is shown.

[0192] Comparative Example 4 This comparative example discloses an existing apparatus and method for preparing solid electrolyte composite electrodes, the preparation method being as follows: Figure 1 As shown, it includes: S1: Sulfide solid electrolyte powder is mixed with SBR binder, xylene is added as solvent, and homogenization is performed using a double planetary mixer to obtain sulfide electrolyte slurry; Halogen solid electrolyte powder is mixed with SBR binder, xylene is added as solvent, and homogenization is performed using a double planetary mixer to obtain halide electrolyte slurry. S2: Coat the well-stirred solid electrolyte slurry onto the surfaces of two rolls of PET support carrier respectively; S3: Transfer the PET film to the drying workshop for high-temperature baking and drying.

[0193] S4: The two rolls of PET film, which are dried and coated with sulfide solid electrolyte membrane 004a and halide solid electrolyte membrane 005a respectively, are wound up and transferred to the laminating mechanism.

[0194] S5: A PET film coated with a sulfide solid electrolyte membrane 004a and a halide solid electrolyte membrane 005a is sequentially rolled and laminated with an electrode 100 (composed of a current collector 001 and an external positive electrode membrane 002 or a negative electrode membrane 003). The side of the PET coated with the solid electrolyte faces the electrode. The sulfide solid electrolyte membrane 004a is bonded to the electrode 100. After passing through the roll, the PET substrate is removed to peel the solid electrolyte from the PET film, resulting in an electrode film with a double-sided single-layer sulfide solid electrolyte membrane 004a composite. Subsequently, the halide solid electrolyte membrane 005a is bonded to the electrode film with the double-sided sulfide solid electrolyte membrane 004a composite. After passing through the roll, the PET substrate is removed to peel the solid electrolyte from the PET film. Figure 11a This method was used to prepare a composite electrode 605 with double-sided double-layer solid electrolyte.

[0195] The ionic conductivity of the solid electrolyte composite electrode sheets prepared in the examples and comparative examples was detected using existing testing methods. The overall assessment is that the thickness uniformity, areal density uniformity, and compaction uniformity are good or above, and the ionic conductivity is > S / m10. -2 The quality is good.

[0196] The specific test results are as follows: Table 1. Qualitative and semi-quantitative detection data from the examples and comparative examples.

[0197] As can be seen from the above, the solid electrolyte composite electrode prepared by the device and method of the present invention has significantly better performance uniformity, ionic conductivity and yield than the prior art.

[0198] The solid electrolyte composite electrode sheets prepared in the examples and comparative examples were tested for production efficiency, compaction density, porosity, and yield using sampling methods in the prior art.

[0199] The ionic conductivity of the electro-solid electrolyte composite electrodes prepared in the examples and comparative examples was tested using existing testing methods, as follows: Select the membrane sample to be tested and a 10 mm ion-blocking electrode; Place the ion-blocking electrode, the membrane to be tested, and the ion-blocking electrode into the pressure sleeve of the mold battery in sequence. Apply pressure to ensure good contact between the ion-blocking electrode and the membrane to be tested. The applied pressure is 200~400MPa, the pressure holding time is not less than 30s, and the battery is left to stand for not less than 1h. The sample was tested using an electrochemical workstation with an EIS module, amplitude 5mV, frequency 10MHz~0.01Hz.

[0200] The specific test results are as follows: Table 2 Quantitative detection data of electrode sheets in the examples and comparative examples

[0201] As can be seen from the above, the total production efficiency of the electrode sheets in the embodiments of the present invention is between 10 m / min and 20 m / min; the porosity is between 9.6% and 14.1%; and the compaction density is between 1.42 and 1.60 g / cm³. 3 The electrode ionic conductivity is between 0.211 S / m and 0.736 S / m, preferably between 0.416 S / m and 0.736 S / m.

[0202] Comparative Example 1 uses the most basic wet transfer printing process, resulting in low production efficiency (15 m / min), mainly limited by the coating drying speed and the unwinding and rewinding operations of the PET carrier. The high porosity (17.1%) is due to the loose electrolyte structure after wet film formation, making it difficult to achieve sufficient densification during roll lamination. The low compaction density (1.28 g / cm³) further confirms the problem of film looseness. The yield rate is only 73%, mainly because the solid electrolyte film is difficult to separate from the PET carrier, easily leading to tape breakage or incomplete localized separation. The low ionic conductivity (1.43 mS / cm) is related to the obstructed ion transport path caused by high porosity and uneven binder distribution.

[0203] Comparative Example 2 prepared a single-sided composite electrode with the same production efficiency as Comparative Example 1 (15 m / min). The porosity further increased to 20.7%, the highest among all comparative examples, indicating that the pressure conditions on the membrane during single-sided composite may not be as uniform as those during double-sided symmetrical composite. The compaction density increased slightly (1.37 g / cm³), but was still much lower than that of the example. The yield was slightly higher than that of Comparative Example 1 (75%), possibly because the single-sided composite process is relatively simple and the risk of peeling is slightly lower. Notably, the ionic conductivity reached 3.45 mS / cm, the highest among all comparative examples. This may be because the mechanical stretching or calendering of the electrolyte membrane during single-sided composite is relatively mild, maintaining good ion channel continuity; however, the excessively high porosity still limited its further improvement. Comparative Example 3, using two different solid electrolytes, required the preparation of two separate coated films and simultaneous lamination, making the process more complex and reducing production efficiency to 11 m / min. The porosity (15.9%) was between Comparative Examples 1 and 2, but the compaction density (1.31 g / cm³) was lower, possibly due to differences in the particle size of the two electrolyte powders (sulfides 10–30 μm, halides 3–4 μm), leading to different mixing and packing efficiencies. The yield rate dropped significantly to 64%, the lowest among all comparative examples. The main reasons include: the different peeling characteristics of the two electrolytes with the PET carrier, requiring simultaneous peeling, which exponentially increases the risk of failure; and the high precision required for bipolar lamination, where deviations easily lead to defects. The ionic conductivity was only 1.18 mS / cm, close to the level of Comparative Example 1, possibly due to interfacial resistance between the two electrolyte layers, coupled with their respective high internal porosity.

[0204] Comparative Example 4 employed two independent compounding and peeling operations, resulting in the most complex process and the lowest production efficiency (only 6 m / min). Its porosity (15.4%) was similar to Comparative Example 3, while its compaction density (1.33 g / cm³) was slightly higher but still relatively low. The yield rate was only 62%, the lowest among all comparative examples. This was due to the need for two PET carrier peeling operations, each carrying the risk of tape breakage or incomplete peeling; and the extremely high alignment requirements for the two compounding operations, with accumulated deviations easily leading to unqualified final products. The ionic conductivity dropped to 0.95 mS / cm, the lowest among all comparative examples and embodiments. This is because the double-layer structure introduces an interface between the two electrolyte layers, coupled with the high porosity of each layer due to the wet process, and the potential for poor interlayer bonding due to the two rolling operations, all contributing to a significant increase in ion transport resistance.

[0205] As can be seen from the above, the solid electrolyte composite electrode prepared by the device and method of the present invention has significantly better production efficiency, porosity, compaction density, ionic conductivity and yield than the prior art.

[0206] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.

Claims

1. A solid electrolyte composite electrode forming device, characterized in that, include: First roller pressing mechanism; The first roller pressing mechanism includes multiple pressing rollers that are positioned close to each other without contact. Multiple pressure rollers have parallel axes and are arranged in a coplanar plane, and are arranged side by side along a direction perpendicular to their axes; adjacent pressure rollers are close to each other but do not contact each other, and rotate in different directions; Along the parallel arrangement direction of the pressure rollers in the first roller pressing mechanism, a first forming area is formed between the gaps of two adjacent pressure rollers at one end of the first roller pressing mechanism; the first forming area can compress and form a solid electrolyte to obtain a first solid electrolyte membrane; The gap between two adjacent pressure rollers at the other end of the first roller pressing mechanism forms a second forming area; the second forming area can press the first solid electrolyte membrane and the electrode sheet to form a single-sided solid electrolyte composite electrode sheet; the electrode sheet is a positive electrode sheet, a negative electrode sheet, a bipolar electrode sheet, a composite electrode sheet, or a self-supporting membrane sheet; The rotational linear speed of the multiple pressure rollers gradually increases from one end of the first forming area to the end where the second forming area is located.

2. The solid electrolyte composite electrode forming apparatus according to claim 1, characterized in that, In the first roller pressing mechanism, the gap between the rollers gradually decreases from the first forming area to the second forming area.

3. The solid electrolyte composite electrode forming apparatus according to claim 2, characterized in that, The gap ratio between adjacent pressure rollers in the first roller pressing mechanism satisfies: 1.5~3:

1.

4. The solid electrolyte composite electrode forming apparatus according to claim 1, characterized in that, In the first roller pressing mechanism, from the first forming area to the second forming area, the gap between adjacent rollers first gradually increases and then gradually decreases.

5. The solid electrolyte composite electrode forming apparatus according to claim 4, characterized in that, From the first molding area to the second molding area, all gaps are defined as first gap, second gap, ..., Nth gap, where the gap in the first molding area is the first gap and the gap in the second molding area is the Nth gap; the ratio of the first gap to the second gap satisfies: 0.8~0.99:1; the second gap, ..., Nth gap are arranged from the first molding area to the second molding area, and the ratio of two adjacent gaps satisfies: 1.5~5:

1.

6. The solid electrolyte composite electrode forming apparatus according to claim 3 or 5, characterized in that, The first roller pressing mechanism has ≥3 pressure rollers, and at least one set of adjacent pressure rollers is arranged between the first forming area and the second forming area.

7. The solid electrolyte composite electrode forming apparatus according to claim 6, characterized in that, A second forming area is provided on the side away from the first forming area, and the second forming area includes a plurality of pressure rollers that are close to each other but do not contact each other.

8. The solid electrolyte composite electrode forming apparatus according to claim 7, characterized in that, In the second roller pressing mechanism, the axes of multiple rollers are parallel and coplanar, and the multiple rollers are arranged side by side along a direction perpendicular to their axes, with adjacent rollers rotating in different directions; At one end of the plane of multiple pressure rollers that is far from the second forming area, the gap between two adjacent pressure rollers forms a third forming area; the third forming area can compress the solid electrolyte to form a second solid electrolyte membrane. The second forming area can press the first solid electrolyte membrane, the second solid electrolyte membrane and the electrode sheet together to form an electrode sheet with double-layer solid electrolyte membranes on both sides; In the second roller pressing mechanism, the rotational linear speed of multiple pressing rollers gradually increases from one end of the third forming area to the end where the second forming area is located.

9. The solid electrolyte composite electrode forming apparatus according to claim 8, characterized in that, In the second roller pressing mechanism, the number of pressure rollers is ≥1, and at least one set of adjacent pressure rollers is arranged between the third forming area and the second forming area.

10. A method for forming a solid electrolyte composite electrode, characterized in that, Using the molding apparatus according to any one of claims 1-9, the process includes: rolling solid electrolyte powder raw material into a composite electrode by continuously passing it through a pressure roller with increasing rotation speed and then rolling it with an electrode sheet to obtain a solid electrolyte composite electrode sheet.