Acoustic metamaterial aerogels obtained by nano-confined directional freezing and in-situ polymerization and their preparation methods
By employing nano-confined directional freezing and in-situ polymerization methods, a multi-level acoustic metamaterial aerogel was constructed, which solved the problem of insufficient low-frequency sound absorption of existing acoustic metamaterials in enclosed environments. This method achieves high-efficiency sound absorption and mechanical stability, making it suitable for enclosed environments.
Patent Information
- Application Number
- CN202611043691.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing acoustic metamaterials have insufficient low-frequency sound absorption performance in enclosed environments and are difficult to maintain stability under vibration, humidity or thermal stress conditions. Their high manufacturing difficulty limits their application in space-constrained environments.
By employing nano-confined directional freezing and in-situ polymerization, a hydrogel with a gradient pore structure is formed by mixing raw materials such as sodium alginate, acrylamide, and N,N-methylenebisacrylamide. The hydrogel is then immersed in calcium nitrate and aluminum nitrate solutions at low temperature to generate nano-hydrated calcium aluminosilicate, thus constructing a multi-level acoustic metamaterial aerogel.
It achieves broadband and efficient low-frequency sound absorption performance, possesses lightweight and high-strength mechanical properties, and has fire and water resistance capabilities, making it suitable for enclosed environments such as aircraft cabins and submarine compartments.
Smart Images

Figure CN123102248A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to an acoustic metamaterial aerogel that is nano-confined directional freezing and in-situ polymerization, belonging to the field of aerogel sound-absorbing materials technology. Background Technology
[0002] Noise pollution imposes a severe economic, environmental, and public health burden. Noise pollution in enclosed environments, particularly aircraft cabins, manned spacecraft, and submarine compartments, remains a long-standing challenge for achieving broadband, efficient sound absorption. Low-frequency sound waves have long wavelengths, far exceeding the thickness of traditional materials, thus requiring bulky absorbers or deep resonant cavities for effective attenuation. In recent years, the development of acoustic metamaterials has enabled subwavelength modulation of sound fields, achieving superior low-frequency sound absorption performance in ultrathin structures. However, most existing designs—especially those based on Helmholtz resonators and membranes—are limited by narrow operating bandwidth, single dissipation channels, sensitivity to geometric parameters, and poor mechanical robustness, resulting in severe performance degradation under vibration, humidity, or thermal stress conditions. Furthermore, the scalable, high-fidelity fabrication of these complex microstructures remains difficult, limiting their practical deployment and structural integration in space-constrained environments. Therefore, there is an urgent need to develop an acoustic metamaterial aerogel with strong sound absorption, high mechanical properties, fire resistance, water resistance, and the ability to be mass-produced. Summary of the Invention
[0003] Objectives of the invention: The first objective of this invention is to provide a method for preparing a high-strength acoustic metamaterial aerogel that is nano-confined, directionally frozen, and in-situ polymerized; the second objective of this invention is to provide a high-strength acoustic metamaterial aerogel material that is nano-confined, directionally frozen, and in-situ polymerized.
[0004] Technical solution: The preparation method of the acoustic metamaterial aerogel of the present invention includes the following steps:
[0005] Step 1: Mix sodium alginate aqueous solution, acrylamide, N,N-methylenebisacrylamide, tetramethylethylenediamine, ammonium persulfate, sodium silicate and foaming agent to prepare a foam-rich slurry;
[0006] Step 2: The slurry is placed in a vacuum environment for negative pressure treatment, causing it to expand in volume and form a gradient pore structure inside. Then the slurry is solidified in situ to obtain a hydrogel.
[0007] Step 3: Perform directional freezing treatment on the hydrogel obtained in Step 2, and after it freezes, obtain a frozen hydrogel.
[0008] Step 4: Under low temperature conditions, the frozen hydrogel obtained in Step 3 is immersed in a mixed solution composed of calcium nitrate, aluminum nitrate and ethanol-water to induce in-situ generation of nano-hydrated calcium aluminosilicate. Finally, after drying, the acoustic metamaterial aerogel is obtained.
[0009] In step one, the foaming agent is cocamidopropyl betaine. The viscosity of the foam-rich slurry is 1035~4894 mPas.
[0010] In step two, the relative vacuum degree during the negative pressure treatment is controlled at -0.07 to -0.08 MPa. Specifically, the slurry is placed in a vacuum chamber, and after a certain negative pressure is drawn, the gauge pressure on the vacuum chamber is -0.07 MPa to -0.08 MPa.
[0011] In step two, the diameter of the hydrogel pores gradually increases from the bottom to the top, with a pore diameter range of 25 μm to 250 μm.
[0012] In step three, the hydrogel is subjected to directional freezing treatment. After freezing, the frozen hydrogel is immersed in a mixed solution composed of calcium nitrate, aluminum nitrate and ethanol-water under low temperature conditions to induce the in-situ formation of nano-hydrated calcium aluminosilicate. Finally, after drying treatment, the acoustic metamaterial aerogel is obtained.
[0013] In step three, the directional freezing process involves placing a cold source on one side of the hydrogel to create a unidirectional temperature gradient, allowing the ice crystals of the hydrogel to grow orderly from one side to the other. Preferably, the cold source is liquid nitrogen.
[0014] In step four, the low-temperature condition is between -40°C and -45°C (-40°C to -45°C). Preferably, the frozen hydrogel is immersed in the mixed solution for at least 72 hours.
[0015] The present invention relates to an acoustic metamaterial aerogel derived from nano-confined directional freezing and in-situ polymerization. The sound-absorbing aerogel comprises sodium alginate, polyacrylamide, nano-hydrated calcium aluminosilicate, a foaming agent, and water.
[0016] The polyacrylamide is produced by in-situ polymerization of acrylamide, ammonium persulfate, N,N-methyleneacrylamide, and tetramethylethylenediamine. The nano-hydrated calcium aluminosilicate is generated by in-situ reaction of sodium silicate, calcium nitrate, and aluminum nitrate. The foaming agent is cocamidopropyl betaine. The pore structure is a gradient pore structure, with the pore size gradually increasing from bottom to top. The water is purified water.
[0017] This invention utilizes a nanoconfined cryogenic-assisted in-situ polymerization strategy to construct an acoustic metamaterial aerogel with a multi-level structure ranging from nanometers to micrometers to millimeters. Specifically, sodium alginate aqueous solution, acrylamide monomer, ammonium persulfate, N,N-methyleneacrylamide, tetramethylethylenediamine, sodium silicate, and cocamidopropyl betaine are uniformly mixed, and a macroscale gradient framework hydrogel is prepared through a vacuum-driven negative pressure-induced bubble growth mechanism. Subsequently, the directionally frozen hydrogel is immersed in an aqueous-ethanol solution containing calcium and aluminates, initiating the in-situ assembly of calcium aluminosilicate nanoparticles. Under nanoconfinement, calcium aluminosilicate nanoparticles nucleate and assemble along directional microchannels, while the nanoporous calcium aluminosilicate phase anchored on the pore walls induces an adsorption-desorption hysteresis effect, thereby generating an acoustic response similar to a resonant cavity and enhancing low-frequency sound absorption. This multi-level structure, with directional microchannels reinforced by strongly bonded calcium aluminosilicate nanoparticles, helps achieve efficient load transfer and structural integrity, while also promoting interfacial energy dissipation.
[0018] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:
[0019] (1) Excellent sound absorption performance: This invention constructs an acoustic metamaterial aerogel with a multi-level structure of nano-micro-millimeter through nano-confined directional freezing and in-situ polymerization. This structure has good acoustic impedance matching effect and multiple sound wave loss mechanisms. It exhibits excellent low-frequency sound absorption capability and broadband performance (noise reduction coefficient NRC = 0.85; sound absorption coefficient SAC = 1.00 at 550 Hz).
[0020] (2) Lightweight and high strength: The preparation method of this invention utilizes a nano-confined strategy to generate nano-sized hydrated calcium aluminosilicate through in-situ polymerization on the pore walls of aerogel. This structure utilizes the chemical bonding between nano-inorganic particles and organic matter to produce extremely high mechanical properties while maintaining its lightweight structure, exhibiting low density (approximately 50 mg / cm³), high compressive strength (approximately 1.88 MPa), and high toughness (approximately 959 kJ / m³).
[0021] (3) Fire resistance and water resistance: The aerogel of the present invention contains a large amount of hydrated calcium aluminosilicate inorganic material, which undergoes a ceramic transformation when exposed to high temperatures, providing good fire resistance. In addition, these inorganic materials enhance the waterproof performance of the material. Attached Figure Description
[0022] Figure 1 This invention relates to the gradient structure morphology control process of acoustic metamaterial aerogel;
[0023] Figure 2The acoustic metamaterial aerogel 1-2 of the present invention is used for sound absorption testing. 1 refers to the first microphone, 2 refers to the second microphone, Pi refers to the incident sound wave, pr refers to the reflected sound wave, x1 refers to the distance from the first microphone to the sample, and x2 refers to the distance from the second microphone to the sample.
[0024] Figure 3 This is a diagram illustrating the sound absorption mechanism of the acoustic metamaterial aerogel of the present invention.
[0025] Figure 4 This is a pore structure distribution diagram of the acoustic metamaterial aerogel of the present invention. Detailed Implementation
[0026] The technical solution of the present invention will be further described below with reference to the accompanying drawings.
[0027] Example 1
[0028] This embodiment provides a sodium alginate-polyacrylamide aerogel with a gradient anisotropic structure grown in a confined space of hydrated calcium aluminosilicate. The specific steps are as follows:
[0029] Step 1: Foam-rich slurry: 10g of 2% sodium alginate aqueous solution, 2g of acrylamide monomer, 70mg of ammonium persulfate, 20mg of N,N-methyleneacrylamide, 100μl of tetramethylethylenediamine, 10g of sodium silicate, and 1g of cocamidopropyl betaine. Mix the above ingredients thoroughly and stir at high speed to form a foam-rich slurry with a viscosity of 1035 mPas.
[0030] Step 2, Gradient Framework Hydrogel: The slurry is poured into a mold with a copper plate at the bottom and polytetrafluoroethylene (PTFE) around the edges. It is then placed in a vacuum dish, and a negative pressure of approximately 0.08 MPa is applied, causing the slurry volume to expand to about three times its original size. The resulting gradient pore size ranges from approximately 25 micrometers to 250 micrometers from bottom to top. After in-situ solidification, the slurry is removed to obtain the hydrogel.
[0031] Step 3, Directional Freezing: Place the above hydrogel into a mold with a copper plate at the bottom and acrylic around the edges, place it in a foam box, with liquid nitrogen at -196℃ at the bottom of the box and the mold on top, and perform directional freezing to obtain a frozen hydrogel.
[0032] Step 4: In-situ polymerization: Simultaneously prepare a 1M solution of calcium nitrate and aluminum nitrate in ethanol-water, with a water-to-ethanol volume ratio of 1:1, and place it in a freezer at -40°C. Immerse the frozen hydrogel in the low-temperature solution for approximately 72 hours. After removal, dry it in a 40°C oven to form aerogel A.
[0033] Example 2
[0034] This embodiment provides a sodium alginate-polyacrylamide aerogel with a gradient anisotropic structure grown in a confined space of hydrated calcium aluminosilicate; the negative pressure in step two is 0.07 MPa; the remaining preparation conditions are the same as in Example 1.
[0035] Example 3
[0036] This embodiment provides a sodium alginate-polyacrylamide aerogel with a gradient anisotropic structure grown in a confined space of hydrated calcium aluminosilicate; the concentration of the sodium alginate aqueous solution in step one is 3%, and the viscosity of the final slurry is 2876 mPas; the remaining preparation conditions are the same as in Example 1.
[0037] Example 4
[0038] This embodiment provides a sodium alginate-polyacrylamide aerogel with a gradient anisotropic structure grown in a confined space of hydrated calcium aluminosilicate; the concentration of the sodium alginate aqueous solution in step one is 4%, and the viscosity of the final slurry is 3629 mPas; the remaining preparation conditions are the same as in Example 1.
[0039] Example 5
[0040] This embodiment provides a sodium alginate-polyacrylamide aerogel with a gradient anisotropic structure grown in a confined space of hydrated calcium aluminosilicate; the concentration of the sodium alginate aqueous solution in step one is 5%, and the viscosity of the final slurry is 4894 mPas; the remaining preparation conditions are the same as in Example 1.
[0041] Comparative Example 1
[0042] This comparative example provides an aerogel with a gradient isotropic structure, which differs from Example 1 in that it does not perform the "directional freezing" step. The specific steps of this comparative example are as follows:
[0043] Step 1: Foam-rich slurry: 10g of 2% sodium alginate aqueous solution, 2g of acrylamide monomer, 70mg of ammonium persulfate, 20mg of N,N-methyleneacrylamide, 100μl of tetramethylethylenediamine, 10g of sodium silicate, and 1g of cocamidopropyl betaine. Mix the above ingredients thoroughly and stir at high speed to form a foam-rich slurry with a viscosity of 1035 mPas.
[0044] Step 2, Gradient Framework Hydrogel: The slurry is poured into a mold with a copper plate at the bottom and polytetrafluoroethylene (PTFE) around the edges. It is then placed in a vacuum dish, and a negative pressure of approximately 0.08 MPa is applied, causing the slurry volume to expand to about three times its original size. The resulting gradient pore size ranges from approximately 25 micrometers to 250 micrometers from bottom to top. After in-situ solidification, the slurry is removed to obtain the hydrogel.
[0045] Step 3, In-situ Polymerization: The gel is then placed in a -40°C freezer for freezing. Simultaneously, a 1M solution of calcium nitrate and aluminum nitrate in ethanol and water (1:1 volume ratio) is prepared and placed in the -40°C freezer. The frozen hydrogel is then immersed in the low-temperature solution for approximately 72 hours. After removal, it is dried in a 40°C oven to form aerogel B.
[0046] Comparative Example 2
[0047] This comparative example provides a homogeneous aerogel, which differs from Example 1 in that it does not perform the "gradient framework hydrogel" step. The specific steps of this comparative example are as follows:
[0048] Step 1: Foam-rich slurry: 10g of 2% sodium alginate aqueous solution, 2g of acrylamide monomer, 70mg of ammonium persulfate, 20mg of N,N-methyleneacrylamide, 100μl of tetramethylethylenediamine, 10g of sodium silicate, and 1g of cocamidopropyl betaine. Mix the above ingredients thoroughly and stir at high speed to form a foam-rich slurry with a viscosity of 1035 mPas.
[0049] Step 2, Directional Freezing: Place the above slurry into a mold with a copper plate at the bottom and acrylic around the edges, then place it in a foam box. The bottom of the box is filled with liquid nitrogen at -196℃, and the top is the mold, for directional freezing.
[0050] Step 3: In-situ polymerization: Simultaneously prepare a 1M solution of calcium nitrate and aluminum nitrate in ethanol-water, with a water-to-ethanol volume ratio of 1:1, and place it in a freezer at -40°C. Immerse the frozen hydrogel in the low-temperature solution for approximately 72 hours. After removal, dry it in a 40°C oven to form aerogel C.
[0051] Comparative Example 3
[0052] This comparative example provides a homogeneous aerogel, which differs from Example 1 in that it does not perform the "gradient framework hydrogel" and "directional freezing" steps. The specific steps of this comparative example are as follows:
[0053] Step 1: Foam-rich slurry: 10g of 2% sodium alginate aqueous solution, 2g of acrylamide monomer, 70mg of ammonium persulfate, 20mg of N,N-methyleneacrylamide, 100μl of tetramethylethylenediamine, 10g of sodium silicate, and 1g of cocamidopropyl betaine. Mix the above ingredients thoroughly and stir at high speed to form a foam-rich slurry with a viscosity of 1035 mPas.
[0054] Step 2: In-situ polymerization: The slurry is poured into a mold with a copper plate at the bottom and polytetrafluoroethylene (PTFE) surrounding it. After in-situ curing, it is removed and placed in a -40°C freezer. Simultaneously, a 1M solution of calcium nitrate and aluminum nitrate in ethanol-water (1:1 volume ratio) is prepared and placed in a -40°C freezer. The frozen hydrogel is then immersed in the low-temperature solution for approximately 72 hours. After removal, it is dried in a 40°C oven to form aerogel D.
[0055] Comparative Example 4
[0056] This comparative example provides a sodium alginate-polyacrylamide aerogel with a gradient anisotropic structure. The difference between this and Example 1 is that the "in-situ polymerization" step is omitted. The specific steps of this comparative example are as follows:
[0057] Step 1: Foam-rich slurry: 10g of 2% sodium alginate aqueous solution, 2g of acrylamide monomer, 70mg of ammonium persulfate, 20mg of N,N-methyleneacrylamide, 100μl of tetramethylethylenediamine, and 1g of cocamidopropyl betaine. Mix the above ingredients thoroughly and stir at high speed to form a foam-rich slurry with a viscosity of 1035 mPas.
[0058] Step 2, Gradient Framework Hydrogel: The slurry is poured into a mold with a copper plate at the bottom and polytetrafluoroethylene (PTFE) around the edges. It is then placed in a vacuum dish, and a negative pressure of approximately 0.08 MPa is applied, causing the slurry volume to expand to about three times its original size. The resulting gradient pore size ranges from approximately 25 micrometers to 250 micrometers from bottom to top. After in-situ solidification, the slurry is removed to obtain the hydrogel.
[0059] Step 3, Directional Freezing: Place the hydrogel into a mold with a copper bottom and acrylic sides, then place it in a foam box. The bottom of the box is filled with liquid nitrogen at -196℃, and the top is the mold, for directional freezing. Afterward, place it in a freeze dryer for freeze drying to form aerogel E.
[0060] Comparative Example 5
[0061] This comparative example provides a homogeneous aerogel, which differs from Example 1 in that it does not perform the "gradient framework hydrogel" and "in-situ polymerization" steps. The specific steps of this comparative example are as follows:
[0062] Step 1: Foam-rich slurry: 10g of 2% sodium alginate aqueous solution, 2g of acrylamide monomer, 70mg of ammonium persulfate, 20mg of N,N-methyleneacrylamide, 100μl of tetramethylethylenediamine, and 1g of cocamidopropyl betaine. Mix the above ingredients thoroughly and stir at high speed to form a foam-rich slurry with a viscosity of 1035 mPas.
[0063] Step 2, Directional Freezing: After solidifying in situ, the hydrogel is removed and placed into a mold with a copper bottom and acrylic sides. This mold is then placed in a foam box with liquid nitrogen at -196°C at the bottom and the mold on top for directional freezing. Afterward, it is freeze-dried in a freeze dryer to form aerogel F.
[0064] Comparative Example 6
[0065] This comparative example provides an aerogel, which differs from Example 1 in that the negative pressure during aerogel preparation is 0.01 MPa and the viscosity is 78 mPas. The specific steps of this comparative example are as follows:
[0066] Step 1: Foam-rich slurry: 10g of 0.1% sodium alginate aqueous solution, 2g of acrylamide monomer, 70mg of ammonium persulfate, 20mg of N,N-methyleneacrylamide, 100μl of tetramethylethylenediamine, 10g of sodium silicate, and 1g of cocamidopropyl betaine. Mix the above ingredients thoroughly and stir at high speed to form a foam-rich slurry with a viscosity of 78 mPas.
[0067] Step 2, Gradient Framework Hydrogel: The slurry is poured into a mold with a copper plate at the bottom and polytetrafluoroethylene (PTFE) around the edges. It is then placed in a vacuum dish, and a negative pressure of approximately 0.01 MPa is applied, causing the slurry volume to expand to about three times its original size. The resulting pores have a diameter of approximately 100 micrometers from bottom to top. After in-situ solidification, the slurry is removed to obtain the hydrogel.
[0068] Step 3: Directional Freezing: Place the hydrogel into a mold with a copper bottom and acrylic sides, then place it in a foam box. The bottom of the box is filled with liquid nitrogen at -196℃, and the top is the mold, for directional freezing. Simultaneously, prepare a 1M solution of calcium nitrate and aluminum nitrate in ethanol-water (1:1 volume ratio) and place it in a -40℃ freezer. Immerse the frozen hydrogel in the low-temperature solution for approximately 72 hours. After removal, dry it in a 40℃ oven to form an aerogel.
[0069] Comparative Example 7
[0070] The difference between this comparative example and Example 1 is that the negative pressure is 0.01 MPa and the viscosity is 22472 mPas. The specific steps of this comparative example are as follows:
[0071] Step 1: Foam-rich slurry: 10g of 5% sodium alginate aqueous solution, 2g of acrylamide monomer, 70mg of ammonium persulfate, 20mg of N,N-methyleneacrylamide, 100μl of tetramethylethylenediamine, 10g of sodium silicate, and 1g of cocamidopropyl betaine. Mix the above ingredients thoroughly and stir at high speed to form a foam-rich slurry with a viscosity of 22472 mPas.
[0072] Step 2, Gradient Framework Hydrogel: The slurry is poured into a mold with a copper plate at the bottom and polytetrafluoroethylene (PTFE) around the edges. It is then placed in a vacuum dish, and a negative pressure of approximately 0.01 MPa is applied, causing the slurry volume to expand to about three times its original size. The resulting pores have a diameter of approximately 25 micrometers from bottom to top. After in-situ solidification, the slurry is removed to obtain the hydrogel.
[0073] Step 3, Directional Freezing: Place the above hydrogel into a mold with a copper plate at the bottom and acrylic around the edges, place it in a foam box, with liquid nitrogen at -196℃ at the bottom of the box and the mold on top, and perform directional freezing to obtain a frozen hydrogel.
[0074] Step 4: In-situ polymerization: Simultaneously prepare a 1M solution of calcium nitrate and aluminum nitrate in ethanol-water, with a water-to-ethanol volume ratio of 1:1, and place it in a freezer at -40°C. Immerse the frozen hydrogel in the low-temperature solution for approximately 72 hours. After removal, dry it in a 40°C oven to form an aerogel.
[0075] Comparative Example 8
[0076] The difference between this comparative example and Example 1 is that the negative pressure is 0.1 MPa and the viscosity is 22472 mPas. The specific steps of this comparative example are as follows:
[0077] Step 1: Foam-rich slurry: 10g of 5% sodium alginate aqueous solution, 2g of acrylamide monomer, 70mg of ammonium persulfate, 20mg of N,N-methyleneacrylamide, 100μl of tetramethylethylenediamine, 10g of sodium silicate, and 1g of cocamidopropyl betaine. Mix the above ingredients thoroughly and stir at high speed to form a foam-rich slurry with a viscosity of 22472 mPas.
[0078] Step 2, Gradient Framework Hydrogel: The slurry is poured into a mold with a copper plate at the bottom and polytetrafluoroethylene (PTFE) around the edges. It is then placed in a vacuum dish, and a negative pressure of approximately 0.1 MPa is applied, causing the slurry volume to expand to about three times its original size. The resulting gradient pore size ranges from approximately 100-500 micrometers from bottom to top. After in-situ solidification, the slurry is removed to obtain the hydrogel.
[0079] Step 3, Directional Freezing: Place the above hydrogel into a mold with a copper plate at the bottom and acrylic around the edges, place it in a foam box, with liquid nitrogen at -196℃ at the bottom of the box and the mold on top, and perform directional freezing to obtain a frozen hydrogel.
[0080] Step 4: In-situ polymerization: Simultaneously prepare a 1M solution of calcium nitrate and aluminum nitrate in ethanol-water, with a water-to-ethanol volume ratio of 1:1, and place it in a freezer at -40°C. Immerse the frozen hydrogel in the low-temperature solution for approximately 72 hours. After removal, dry it in a 40°C oven to form an aerogel.
[0081] Comparative Example 9
[0082] The difference between this comparative example and Example 1 is that the negative pressure is 0.1 MPa and the viscosity is 78 mPas. The specific steps of this comparative example are as follows:
[0083] Step 1: Foam-rich slurry: 10g of 0.1% sodium alginate aqueous solution, 2g of acrylamide monomer, 70mg of ammonium persulfate, 20mg of N,N-methyleneacrylamide, 100μl of tetramethylethylenediamine, 10g of sodium silicate, and 1g of cocamidopropyl betaine. Mix the above ingredients thoroughly and stir at high speed to form a foam-rich slurry with a viscosity of 78 mPas.
[0084] Step 2, Gradient Framework Hydrogel: The slurry is poured into a mold with a copper plate at the bottom and polytetrafluoroethylene (PTFE) around the edges. It is then placed in a vacuum dish, and a negative pressure of approximately 0.1 MPa is applied, causing the slurry volume to expand to about three times its original size. The resulting pores have a diameter of approximately 500 micrometers from bottom to top. After in-situ solidification, the slurry is removed to obtain the hydrogel.
[0085] Step 3, Directional Freezing: Place the above hydrogel into a mold with a copper plate at the bottom and acrylic around the edges, place it in a foam box, with liquid nitrogen at -196℃ at the bottom of the box and the mold on top, and perform directional freezing to obtain a frozen hydrogel.
[0086] Step 4: In-situ polymerization: Simultaneously prepare a 1M solution of calcium nitrate and aluminum nitrate in ethanol-water, with a water-to-ethanol volume ratio of 1:1, and place it in a freezer at -40°C. Immerse the frozen hydrogel in the low-temperature solution for approximately 72 hours. After removal, dry it in a 40°C oven to form an aerogel.
[0087] Example 3 Performance Testing
[0088] (1) Acoustic performance testing
[0089] Utilize Figure 2 The acoustic impedance tubes shown were used to test the sound absorption performance of the aerogels obtained in Examples 1-5 and Comparative Examples 1-9. The test results show that the aerogels in Comparative Examples 6-9 have poor sound absorption performance, confirming that slurry viscosity and expansion negative pressure have a significant impact on the sound absorption performance of the aerogels. Specifically, when the slurry viscosity is below 1035 mPas or above 4894 mPas, and the expansion negative pressure is below 0.01 MPa or above 0.1 MPa, the sound absorption performance of the prepared aerogels decreases significantly.
[0090] according to Figure 1When the negative pressure is high and the slurry viscosity is low, the bubbles are large and no gradient structure is observed (Comparative Example 9); when the slurry viscosity is high, a gradient structure is observed, but the overall pore size is large, which is not conducive to sound absorption (Comparative Example 8). When the negative pressure is low and the slurry viscosity is low, the bubbles are small and no gradient structure is observed (Comparative Example 6); when the slurry viscosity is high, the bubbles are still small and no gradient structure is observed (Comparative Example 7). Therefore, sound absorption tests were not conducted on Comparative Examples 6-9. Using 4 cm thick samples, the sound absorption coefficient of the cement-based sound-absorbing material was tested. The sound absorption performance of the material was represented by the average sound absorption coefficient (NRC). The higher the NRC value, the better the sound absorption capacity of the material. The results are shown in Table 1.
[0091] (2) Compressive strength test
[0092] The aerogels obtained in the examples and comparative examples were subjected to compressive strength tests, and the results are shown in Table 1.
[0093] Table 1. Results of average sound absorption coefficient (NRC) and compressive strength of the sound-absorbing materials in Example 1 and Comparative Examples 1-5
[0094] serial number Average sound absorption coefficient (NRC) Compressive strength (MPa) A 0.85 1.9 B 0.69 1.4 C 0.51 1.1 D 0.46 0.9 E 0.44 0.3 F 0.38 0.2
[0095] As shown in Table 1, sodium alginate-polyacrylamide aerogel with a gradient anisotropic structure exhibits the best sound absorption performance and compressive strength. Analysis reveals that its multi-scale hierarchical structure integrates gradient macropores, oriented micropore walls, and uniformly distributed nanoporous CASH (carbon dioxide). Figure 4 This forms an anisotropic skeleton with unprecedented strength (~1.88 MPa). This structure achieves broadband sound absorption (NRC = 0.85 in the 50–6300 Hz range) and near-perfect sound absorption performance at low frequencies (SAC = 1.00 at 550 Hz). Figure 3 This is due to the resonant energy dissipation induced by the in-situ formation of CASH nanoparticles attached to the walls of microscale pores.
Claims
1. A method for preparing an acoustic metamaterial aerogel, characterized in that, Includes the following steps: Step 1: Mix sodium alginate aqueous solution, acrylamide, N,N-methylenebisacrylamide, tetramethylethylenediamine, ammonium persulfate, sodium silicate and foaming agent to prepare a foam-rich slurry; Step 2: The slurry is placed in a vacuum environment for negative pressure treatment, causing it to expand in volume and form a gradient pore structure inside. Then the slurry is solidified in situ to obtain a hydrogel. Step 3: Perform directional freezing treatment on the hydrogel obtained in Step 2, and after it freezes, obtain a frozen hydrogel. Step 4: Under low temperature conditions, the frozen hydrogel obtained in Step 3 is immersed in a mixed solution composed of calcium nitrate, aluminum nitrate and ethanol-water to induce in-situ generation of nano-hydrated calcium aluminosilicate. Finally, after drying, the acoustic metamaterial aerogel is obtained.
2. The method for preparing acoustic metamaterial aerogel according to claim 1, characterized in that, In step one, the foaming agent is cocamidopropyl betaine.
3. The method for preparing acoustic metamaterial aerogel according to claim 1, characterized in that, In step one, the viscosity of the foam-rich slurry is 1035~4894 mPas.
4. The method for preparing acoustic metamaterial aerogel according to claim 1, characterized in that, In step two, the vacuum level is controlled at -0.07 to -0.08 MPa during the negative pressure treatment.
5. The method for preparing acoustic metamaterial aerogel according to claim 1, characterized in that, In step two, the diameter of the hydrogel pores gradually increases from the bottom to the top, with a pore diameter range of 25 μm to 250 μm.
6. The method for preparing acoustic metamaterial aerogel according to claim 1, characterized in that, In step three, the directional freezing treatment method is as follows: a cold source is set on one side of the hydrogel to form a temperature gradient in one direction, so that the ice crystals of the hydrogel grow in an orderly manner from one side to the other.
7. The method for preparing acoustic metamaterial aerogel according to claim 6, characterized in that, In step three, the cold source is liquid nitrogen.
8. The method for preparing acoustic metamaterial aerogel according to claim 1, characterized in that, In step four, the temperature of the low-temperature condition is between -40°C and -45°C.
9. The method for preparing acoustic metamaterial aerogel according to claim 1, characterized in that, In step four, the cryogel is soaked in the mixed solution for at least 72 hours.
10. An acoustic metamaterial aerogel prepared by the preparation method according to any one of claims 1-9, which is nano-confined directional freezing and in-situ polymerization.