A cold heading die with DLC wear-resistant coating
By setting a nitriding hardening layer, a metal transition layer, and a gradient-designed wear-resistant coating on the mold substrate, the problem of weak adhesion between the DLC coating and the steel substrate is solved, thereby improving the wear resistance and service life of the mold.
Patent Information
- Application Number
- CN202611622852.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
Smart Images

Figure CN123102906A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of mold technology, specifically to a cold heading mold with a DLC wear-resistant coating. Background Technology
[0002] Cold heading is the mainstream processing technology for metal parts such as fasteners and standard parts. It relies on cold heading dies to apply pressure to metal blanks at room temperature to cause plastic deformation. During service, the inner wall of the cold heading die cavity must withstand high-frequency reciprocating impact loads and intense metal flow friction. The surface wear resistance and impact resistance directly determine the service life of the die and the forming quality of the parts.
[0003] Diamond-like carbon (DLC) coatings are increasingly being used in the surface strengthening of cold heading dies due to their high hardness, low coefficient of friction, and excellent wear resistance and friction reduction properties. However, existing DLC-coated cold heading dies still have the following technical problems: the coefficient of thermal expansion and elastic modulus of the DLC coating differ significantly from those of the steel substrate. When directly deposited on the surface of the die cavity, the interfacial bonding force between the film and the substrate is weak, and the coating is prone to early peeling under the high-frequency impact load of cold heading, thus failing to fully utilize its wear resistance advantages.
[0004] Therefore, improving the bonding strength between the DLC coating and the cold heading die substrate is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0005] The purpose of this invention is to provide a cold heading mold with a DLC wear-resistant coating to solve the problem that the DLC coating and the steel substrate have large differences in thermal expansion coefficient and elastic modulus, resulting in weak interfacial bonding when the coating is directly deposited on the surface of the mold cavity.
[0006] To achieve the above objectives, the present invention provides the following technical solution:
[0007] A cold heading die with a DLC wear-resistant coating includes a die substrate with a forming cavity. The die substrate has a nitriding hardening layer, a metal transition layer and a wear-resistant coating sequentially arranged towards the center of the cavity, with the surface of the inner wall of the forming cavity as the base. The wear-resistant coating is a chromium-doped diamond-like carbon coating. Along the direction from the metal transition layer to the surface of the wear-resistant coating, the chromium content continuously decreases and the sp³ hybrid carbon content continuously increases.
[0008] Preferably, the mold base is made of Cr12MoV cold work die steel with a hardness of 62~64HRC; the surface roughness Ra of the inner wall of the forming cavity of the mold base is ≤0.02μm.
[0009] Preferably, the thickness of the nitriding hardened layer is 0.15~0.2mm; the surface hardness of the nitriding hardened layer on the side facing the metal transition layer is 1050~1150HV, and the hardness decreases continuously from this surface toward the mold substrate.
[0010] Preferably, the metal transition layer is a pure chromium metal layer with a thickness of 100~200nm.
[0011] Preferably, along the direction from the metal transition layer to the surface of the wear-resistant coating, the atomic percentage of chromium in the wear-resistant coating continuously decreases from 15%~18% to 1%~3%, the proportion of sp³ hybrid carbon in the total carbon atoms of the wear-resistant coating continuously increases from 45%~50% to 75%~80%, and the microhardness of the wear-resistant coating continuously increases from 1400~1600HV to 2300~2500HV.
[0012] Preferably, the wear-resistant coating thickness of the step edge region of the forming cavity is 6~8μm, and the wear-resistant coating thickness of the remaining regions is 4~6μm. The step edge region is a region of 0.5~2mm on both sides of the edge line; the coating thickness between the step edge region and the remaining regions is continuously transitioned.
[0013] Compared with the prior art, the beneficial effects of the present invention are:
[0014] 1. Through the layered composite structure of nitriding hardening layer, metal transition layer and wear-resistant coating, a gradually transitioning property matching layer can be formed between steel substrate and diamond-like coating, which helps to alleviate the mismatch stress caused by the difference in thermal expansion coefficient and elastic modulus at the film-substrate interface, improve the bonding strength of the film-substrate interface, and reduce the possibility of early peeling of coating under cold heading impact load.
[0015] 2. The wear-resistant coating adopts a continuous gradient design. The higher chromium doping content in the bottom layer can improve the bonding toughness between the coating and the metal transition layer. The higher sp³ hybrid carbon content in the surface layer can provide better wear resistance and friction reduction performance, which can balance the interfacial bonding reliability and surface wear resistance of the coating to a certain extent. At the same time, the hardness changes continuously along the depth direction, which helps to reduce stress concentration inside the coating and improve the impact resistance of the coating.
[0016] 3. The substrate adopts a heat treatment regime that is compatible with the nitriding process temperature, which helps to reduce the impact of the nitriding process on the substrate hardness, provides a more stable rigid support for the coating, and ensures the stable performance of the coating. Attached Figure Description
[0017] Figure 1 This is an axial sectional view of the entire invention;
[0018] Figure 2 For the present invention Figure 1 Enlarged view of point A in the middle.
[0019] In the figure: 1. Mold substrate; 2. Wear-resistant coating; 3. Nitrided hardening layer; 4. Metal transition layer. Detailed Implementation
[0020] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0021] Please see Figures 1 to 2 The present invention provides a technical solution.
[0022] A cold heading mold with DLC wear-resistant coating is provided. The cold heading mold has a circular integral structure, including a mold base 1. A through forming cavity is opened in the center of the mold base. The working surface of the forming cavity is treated with DLC coating. The coating surface is smooth and meets the requirements of low friction and anti-sticking.
[0023] During cold heading, the metal blank enters the forming cavity under the axial pressure of the punch. During the forming process, the closed air in the cavity is discharged to the outside through the exhaust groove designed on the end face.
[0024] Using the inner wall surface of the forming cavity as a base, a nitriding hardening layer 3, a metal transition layer 4, and a wear-resistant coating 2 are sequentially laminated in the direction of the center of the forming cavity.
[0025] The mold substrate 1 is made of Cr12MoV cold work die steel with a hardness of 62~64HRC. The inner wall of the forming cavity is polished with a surface roughness Ra≤0.02μm, which meets the requirements of a smooth substrate for DLC coating. In this embodiment, the mold substrate obtains the target hardness through a two-stage hardening process of high-temperature quenching and multiple high-temperature tempering: first, it is vacuum quenched at 1020~1050℃, and then tempered three times at 510~530℃. The tempering temperature is matched with the subsequent nitriding temperature to avoid the substrate softening during tempering. Finally, it is ensured that the hardness of the core of the substrate remains stable at 62~64HRC after nitriding.
[0026] The nitriding hardening layer 3 is a nitrogen diffusion layer formed on the inner wall of the cavity by ion nitriding process, with a thickness of 0.15~0.2mm. The surface hardness of the nitriding hardening layer 3 facing the metal transition layer 4 is 1050~1150HV, and the hardness decreases continuously from this surface towards the mold substrate 1. The function of this layer is to provide a high-hardness support substrate for the subsequent metal transition layer 4 and wear-resistant coating 2, to avoid the high-hardness wear-resistant coating from producing an eggshell effect due to insufficient substrate rigidity, and to prevent the coating from denting and peeling off under impact load. The continuous hardness gradient can alleviate interlayer stress concentration and improve the impact resistance of the film-base system.
[0027] The metal transition layer 4 is a pure chromium metal layer with a thickness of 100~200nm, deposited on the surface of the nitrided hardened layer 3 by magnetron sputtering. The function of the pure chromium transition layer is to compensate for the difference in physical properties: the coefficient of thermal expansion of the Cr12MoV steel substrate is approximately 11.5×10⁻ 6 At / ℃, the coefficient of thermal expansion of the diamond-like carbon coating is approximately 2~3×10⁻ 6 At ℃, the coefficient of thermal expansion of the pure chromium layer is approximately 8.2 × 10⁻ 6 / ℃, which can form a continuous transition of physical properties between the two, significantly reducing the thermal mismatch stress between the film layers. At the same time, metallic chromium has good bonding performance with the nitriding layer and the wear-resistant coating, which can greatly improve the film-substrate bonding force of the coating.
[0028] The wear-resistant coating 2 is a chromium-doped diamond-like carbon (Cr-DLC) coating. Along the direction from the metal transition layer 4 to the surface of the wear-resistant coating 2, the chromium content continuously decreases, while the sp³ hybrid carbon content continuously increases, forming a structure with a continuous gradient in composition and performance. The specific performance parameters correspond as follows:
[0029] The atomic percentage of chromium relative to the total number of atoms in the wear-resistant coating 2 decreases continuously from 15% to 18% near the metal transition layer 4 to 1% to 3% on the surface of the wear-resistant coating 2.
[0030] The percentage of sp³ hybrid carbon relative to the total number of carbon atoms in the wear-resistant coating 2 increases continuously from 45% to 50% on the side near the metal transition layer 4 to 75% to 80% on the surface of the wear-resistant coating 2.
[0031] Correspondingly, the microhardness of the wear-resistant coating 2 increases continuously from 1400~1600 HV near the metal transition layer 4 to 2300~2500 HV on the surface of the wear-resistant coating 2. The principle of this compositional gradient design is as follows: Chromium belongs to the transition metal group and catalyzes the formation of sp² hybrid carbon during the deposition of diamond-like carbon film. For the wear-resistant coating 2, the higher the chromium doping content, the higher the proportion of sp² hybrid carbon in the coating, the lower the hardness and the better the toughness. The lower the chromium doping content, the higher the proportion of sp³ hybrid carbon in the coating, the higher the hardness and the better the wear resistance. The bottom layer of the wear-resistant coating 2 near the metal transition layer 4 adopts a high chromium content design to ensure the bonding toughness between the wear-resistant coating 2 and the metal transition layer 4. The surface layer of the wear-resistant coating 2 adopts a low chromium and high sp³ hybrid carbon composition design, which can provide excellent wear resistance and friction reduction performance, ultimately achieving a balance between film bonding strength and wear resistance service life.
[0032] The thickness of the wear-resistant coating 2 varies in different functional areas of the forming cavity, and the thickness transitions smoothly and continuously between areas without abrupt changes. This distribution conforms to the deposition physics of PVD processes such as magnetron sputtering.
[0033] Step edge region: The region of 0.5~2mm on both sides of the edge of all the convex steps on the inner wall of the forming cavity. This type of convex edge structure has the deposition characteristics of being coated on both sides. Both adjacent step walls can receive the deposited particles. The deposition flux is naturally higher than that of the planar area. Therefore, the thickness of the wear-resistant coating 2 is naturally 6~8μm. For example, in the cold heading mold for anti-loosening teeth used in the forming of fastener heads, the region of 0.5~2mm on both sides of the edge of the convex tooth top surface of the anti-loosening tooth structure belongs to the above-mentioned step edge region.
[0034] Inner corner region: This refers to all concave corner regions on the inner wall of the forming cavity with a radius of ≤2mm. This type of concave corner structure has a shadow effect due to the obstruction of deposited particles, making it difficult for ionized particles to fully reach the inside of the concave corner. The deposition flux is naturally lower than that of the planar region, so the thickness of the wear-resistant coating 2 naturally forms 3~5μm. For example, the concave corner at the bottom of the tooth groove of the anti-loosening tooth structure in this embodiment belongs to the above-mentioned inner corner region.
[0035] Other planar areas: flat forming surfaces such as the inner conical surface of the forming cavity, the cylindrical forming strip surface, and the end face plane. The wear-resistant coating thickness in this area is 4~6μm.
[0036] This thickness distribution is also matched to the wear characteristics of cold heading dies: the convex edge of the anti-loosening tooth is the part with the strongest metal flow shear and the most severe adhesive wear, and the thickest coating corresponds to the highest wear resistance requirement; the corner inside the tooth groove is the impact stress concentration area, and appropriate thinning can reduce the internal stress of the coating and avoid impact peeling; the planar area adopts the industry-standard optimal thickness, taking into account both wear resistance and impact stability.
[0037] Specific mold manufacturing process: In this embodiment, a cold heading mold is prepared through a complete process including substrate heat treatment, ultra-precision polishing, ion nitriding, and magnetron sputtering deposition. The specific steps are as follows:
[0038] Step 1: Mold base preparation and pretreatment: Blanking and rough machining: Select Cr12MoV cold work die steel bar, and after forging and annealing, rough machine the outer shape, inner hole and anti-loosening tooth cavity, leaving a 0.3~0.5mm finishing allowance on each side;
[0039] Quenching heat treatment: The rough-machined matrix is placed in a vacuum heat treatment furnace and heated to 1030℃ at a rate of 8~10℃ / min. After holding at this temperature for 30min, it is oil quenched and then subjected to three high-temperature tempering processes at a tempering temperature of 520℃. Each tempering process is held for 2 hours and then air-cooled. The final matrix hardness reaches 62~64HRC.
[0040] Precision polishing: The inner wall surface of the forming cavity is precision polished. This can be done using a step-by-step diamond polishing process: sequentially using 800#, 1200#, 2000#, and 5000# diamond polishing pastes; or using an abrasive fluid polishing process. After polishing, the surface roughness Ra of the inner wall of the forming cavity is ≤0.02μm, which meets the smoothness requirements of the coating substrate.
[0041] Cleaning: After polishing, the mold is placed in acetone and anhydrous ethanol for ultrasonic cleaning for 15 minutes each. After removal, it is dried with nitrogen and placed in the special fixture of the coating machine.
[0042] Step 2: Ion nitriding to prepare the nitriding hardened layer: Place the mold substrate 1 into the ion nitriding furnace and perform the following process: evacuate the furnace until the pressure inside the furnace is ≤1Pa, introduce a mixed gas of ammonia and hydrogen with a volume ratio of NH3:H2=1:2, and adjust the pressure inside the furnace to maintain at 300~500Pa.
[0043] Ion nitriding was performed by heating to 520℃ at a rate of 5℃ / min and holding at that temperature for 9 hours.
[0044] After nitriding, the mold substrate is cooled to below 100°C in the furnace and then removed from the furnace to obtain a mold base with a nitrided hardened layer.
[0045] After this step is completed, the thickness of the nitrided hardened layer 3 on the inner wall of the forming cavity is 0.15~0.2mm, the surface hardness of the nitrided hardened layer 3 on the side facing the metal transition layer 4 is 1050~1150HV, and the hardness decreases continuously from this surface towards the mold substrate 1; the nitrided hardened layer 3 is evenly and continuously distributed along the inner wall of the forming cavity.
[0046] Step 3: Magnetron sputtering deposition of metal transition layer 4 and gradient wear-resistant coating 2
[0047] The nitrided mold substrate 1 is placed into the vacuum chamber of an unbalanced magnetron sputtering coating machine, and co-sputtering deposition is performed using a 99.99% pure chromium target and a 99.99% pure graphite target. The specific process steps are as follows:
[0048] Background vacuuming: Turn on the vacuum molecular pump unit to evacuate the coating chamber to a vacuum level of 8×10⁻⁻⁻⁶. 4 Below Pa;
[0049] Argon ion bombardment cleaning: High-purity argon gas is introduced into the chamber, the working pressure of the chamber is adjusted to 0.4 Pa, the substrate bias power supply is turned on, the bias value is set to -800 V and the duty cycle is 80%, and the inner wall surface of the forming cavity is etched and cleaned with argon ions for 15 min; the oxide film and adsorbed impurities on the inner wall surface of the forming cavity are removed by ion sputtering, and the inner wall surface of the forming cavity is simultaneously cleaned and activated;
[0050] Depositing a pure chromium metal transition layer: Maintain the argon gas pressure in the forming chamber at 0.4 Pa, turn on the DC power supply of the chromium target, set the target current to 10 A, adjust the substrate bias voltage to -150 V, and deposit for 15 min to form a pure chromium metal transition layer with a thickness of about 150 nm on the surface of the nitrided hardened layer.
[0051] Deposition of gradient wear-resistant coating: The intermediate frequency power supply of the graphite target is kept constant at 20kW, and the DC current of the chromium target is reduced linearly and uniformly, so that the chromium target current is reduced from 12A to 1A within 150min; at the same time, the substrate bias voltage is gradually and linearly adjusted from -150V to -200V; the argon gas pressure in the chamber is kept stable at 0.4Pa during the deposition process; during the deposition process, the mold substrate 1 rotates uniformly at a speed of 2r / min.
[0052] Cooling and unloading: After deposition, turn off all target power and substrate bias power, continue to introduce argon gas into the chamber to maintain the pressure inside the furnace, and after the mold cools down to below 60°C with the furnace, break the vacuum and take out the finished mold.
[0053] Specific numerical example: This example is a die used for cold heading of the anti-loosening teeth of an M3 screw head. The specific parameters of each structure and coating are as follows:
[0054] Mold base: Made of Cr12MoV cold work die steel, after vacuum quenching at 1030℃ and three high-temperature tempering treatments at 520℃, the base hardness is 63HRC; the inner wall of the forming cavity is precision polished, and the surface roughness Ra is 0.012μm.
[0055] Nitriding hardening layer: The thickness of nitriding hardening layer 3 is 0.18 mm; the surface hardness of the side of nitriding hardening layer 3 facing the metal transition layer 4 is 1100 HV, and the hardness decreases continuously from this surface towards the mold substrate.
[0056] Metal transition layer: a pure chromium metal layer with a thickness of 150nm;
[0057] Wear-resistant coating: Along the direction from the side near the metal transition layer 4 towards the surface of the wear-resistant coating 2, the atomic percentage of chromium relative to the total number of atoms in the wear-resistant coating continuously decreases from 16at% to 2at%, and the proportion of sp³ hybrid carbon relative to the total number of carbon atoms in the wear-resistant coating continuously increases from 48% to 77%; correspondingly, the microhardness of the wear-resistant coating continuously increases from 1500HV near the metal transition layer 4 to 2400HV on the surface.
[0058] Coating thickness distribution: In the convex step edge area, corresponding to a 1mm range on both sides of the top edge of the convex tooth of the anti-loosening tooth in this embodiment, the wear-resistant coating thickness is 7.2μm; in the concave corner area, corresponding to the concave corner at the bottom of the tooth groove of the anti-loosening tooth in this embodiment, the wear-resistant coating thickness is 4.2μm; in the remaining planar areas, corresponding to the flat inner walls of the cavity such as the inner conical surface and cylindrical surface, the wear-resistant coating thickness is 5.1μm; the wear-resistant coating thickness between each area is smoothly and continuously transitioned.
[0059] To quantitatively verify the service performance of the cold heading die in this embodiment, three sets of control samples were set up for comparative testing under the same production conditions. The test conditions and results are as follows:
[0060] Test conditions: Processing equipment: six-station high-speed cold heading machine, slide stroke 120 times / minute;
[0061] Workpiece to be machined: ML35 cold heading steel wire, finished product is M3 nominal diameter 8.8 grade screw, original hardness of workpiece ≤HRB90;
[0062] Lubrication conditions: Extreme pressure cold heading oil is used, with a viscosity of 68 mm² / s at 40°C and a sulfur-based extreme pressure additive content of 8%.
[0063] Test environment: ambient temperature workshop environment, mold without additional forced cooling.
[0064] Comparative sample setup: Three groups of control samples were set up, with three molds in each group for testing. The results were averaged. The substrate material, heat treatment process, cavity size, and surface roughness of all samples were consistent with those in this embodiment, with only the surface treatment method differing.
[0065] Control group 1 (ordinary nitriding group): only ion nitriding treatment was performed, without metal transition layer and wear-resistant coating;
[0066] Control group 2 (uniform DLC group): treated with ion nitriding, 150nm pure chromium transition layer, and uniform Cr-DLC coating, with chromium atom ratio of 8at%, sp³ hybrid carbon ratio of 60%, and average coating thickness of 5μm;
[0067] Experimental group (invention scheme): Gradient composition, differential thickness Cr-DLC coating cold heading mold of this embodiment.
[0068] Failure criteria: The mold is deemed to have failed and the counting will stop if any of the following conditions are met: adhesive tearing, plastic deformation or coating peeling occurs on the working surface of the cavity, with the cumulative area accounting for 5% or more of the total working surface area.
[0069] Test Results and Analysis: After continuous production testing, the average failure life of each group of molds is as follows:
[0070] Control group 1 (ordinary nitriding group): The average failure life was 112,000 pieces, and the failure modes were mainly adhesive wear on the cavity surface and plastic deformation of the tooth edges;
[0071] Control group 2 (uniform DLC group): The average failure life was 227,000 units, and the failure mode was mainly early flaking of the coating in the toothed area, followed by rapid wear of the substrate;
[0072] Test group (the present invention scheme): The average failure life is 368,000 pieces, and the failure mode is progressive abrasive wear on the cavity surface, with no large-area coating peeling.
[0073] The comparison shows that the service life of the cold heading mold in this embodiment is about 3.3 times that of the ordinary nitriding mold and about 1.6 times that of the uniform composition DLC coating mold, which is consistent with the expected performance improvement effect. The main reason is that the gradient composition structure alleviates the stress concentration inside the coating and at the film-substrate interface, avoids early peeling under impact load, and achieves a significant improvement in mold life.
[0074] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A cold heading die with a DLC wear-resistant coating, comprising a die base, wherein the die base has a forming cavity, characterized in that: Using the surface of the inner wall of the forming cavity of the mold substrate as the base, a nitriding hardening layer, a metal transition layer and a wear-resistant coating are sequentially provided in the direction towards the center of the cavity; the wear-resistant coating is a chromium-doped diamond-like coating, and along the direction from the metal transition layer to the surface of the wear-resistant coating, the chromium content continuously decreases and the sp³ hybrid carbon content continuously increases.
2. The cold heading die with DLC wear-resistant coating according to claim 1, characterized in that: The mold base is made of Cr12MoV cold work die steel with a hardness of 62~64HRC; the surface roughness Ra of the inner wall of the forming cavity of the mold base is ≤0.02μm.
3. The cold heading die with DLC wear-resistant coating according to claim 1, characterized in that: The thickness of the nitrided hardening layer is 0.15~0.2mm; the surface hardness of the nitrided hardening layer facing the metal transition layer is 1050~1150HV, and the hardness decreases continuously from this surface towards the mold substrate.
4. The cold heading die with DLC wear-resistant coating according to claim 1, characterized in that: The metal transition layer is a pure chromium metal layer with a thickness of 100~200nm.
5. A cold heading die with a DLC wear-resistant coating according to claim 1, characterized in that: Along the direction from the metal transition layer to the surface of the wear-resistant coating, the atomic percentage of chromium in the wear-resistant coating continuously decreases from 15%~18% to 1%~3%, the proportion of sp³ hybrid carbon in the total carbon atoms of the wear-resistant coating continuously increases from 45%~50% to 75%~80%, and the microhardness of the wear-resistant coating continuously increases from 1400~1600HV to 2300~2500HV.
6. The cold heading die with DLC wear-resistant coating according to claim 1, characterized in that: The wear-resistant coating thickness in the step edge area of the forming cavity is 6~8μm, and the wear-resistant coating thickness in the remaining areas is 4~6μm. The step edge area is a region of 0.5~2mm on both sides of the edge line; the coating thickness between the step edge area and the remaining areas is continuously transitioned.