A high-strength, high-toughness sodium lignosulfonate composite gel, its preparation method and application
By constructing a PMAA/PEG-200/LS composite gel system, utilizing methacrylic acid and polyethylene glycol-200 to form a cross-linking network, and combining it with sodium lignosulfonate as a reinforcing agent, the problem of insufficient strength and toughness of traditional hydrogels was solved, realizing the preparation of high-strength and high-toughness sodium lignosulfonate composite gels, and expanding its application in flexible sensing and biomedical fields.
Patent Information
- Application Number
- CN202611291907.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-17
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer composite materials technology, specifically relating to a high-strength, high-toughness sodium lignosulfonate composite gel, its preparation method, and its application. Background Technology
[0002] Hydrogels, with their high water content and tunable mechanical properties resembling biological tissues, have demonstrated significant application value in flexible devices, biomedicine, and adsorption separation. However, the insufficient mechanical properties of traditional hydrogels have long remained unresolved; most materials exhibit low strength and poor toughness, making them prone to brittle fracture under stress and failing to meet practical application requirements. To address this bottleneck, existing modification strategies mainly include dual-network construction, nanofiller reinforcement, and supramolecular crosslinking, but these methods often involve complex processes, increased costs, and environmental impact. In recent years, utilizing natural polymers as reinforcing materials has become a new research direction. Lignin is widely available and rich in functional groups, especially its water-soluble derivative, sodium lignin sulfonate (LS), which contains numerous sulfonic acid groups and phenolic hydroxyl groups, possessing the potential to strengthen polymer networks through hydrogen bonding.
[0003] Therefore, developing a high-strength, high-toughness sodium lignosulfonate composite gel is of great significance for overcoming the shortcomings of traditional hydrogels in terms of mechanical properties, expanding their practical applications in fields such as flexible sensing and biomedicine, and promoting the green preparation of high-performance hydrogel materials. Summary of the Invention
[0004] To overcome the shortcomings and deficiencies of the existing technology, the primary objective of this invention is to provide a simple method for preparing a sodium lignosulfonate composite gel with both high strength and high toughness. This method constructs a PMAA / PEG-200 / LS composite gel system through rational molecular design. Methacrylic acid (MAA) and polyethylene glycol-200 (PEG-200) serve as comonomers, forming a cross-linked polymer network framework that provides the material with load-bearing capacity and structural integrity. Sodium lignosulfonate (LS), as a natural polymer reinforcing agent, has abundant sulfonic acid groups and phenolic hydroxyl groups that can form multiple hydrogen bonds with the polymer chains, endowing the gel with flexibility, energy dissipation capacity, and interfacial adhesion properties. Furthermore, the deep eutectic solvent system formed between MAA and PEG-200 through hydrogen bonding effectively enhances the gel's antifreeze and water-retention properties, broadening its application potential in complex environments.
[0005] Another objective of this invention is to provide a high-strength, high-toughness sodium lignosulfonate composite hydrogel prepared by the above-described preparation method.
[0006] Another object of the present invention is to provide the application of the above-mentioned high-strength and high-toughness sodium lignosulfonate composite hydrogel.
[0007] The objective of this invention is achieved through the following technical solution:
[0008] A method for preparing a high-strength, high-toughness sodium lignosulfonate composite gel, comprising the following steps:
[0009] (1) Stir methacrylic acid (MAA) and polyethylene glycol-200 (PEG-200) at room temperature for 40-60 min to form a uniform colorless and transparent liquid, and obtain a deep eutectic solution (PDES).
[0010] (2) Add pure water and sodium lignosulfonate to the deep eutectic solution obtained in step (1), and stir at 10-30℃ until completely dissolved; then add crosslinking agent and photoinitiator, stir evenly, and obtain gel prepolymer solution;
[0011] (3) The gel prepolymer obtained in step (2) is filled into the mold and polymerized by UV irradiation to obtain a high-strength and high-toughness sodium lignosulfonate composite gel, which is PMAA / PEG-200 / LS composite gel.
[0012] The ambient temperature in step (1) is 10-30℃; the stirring speed is 300-800 rpm.
[0013] The stirring time in step (1) is preferably 40 min.
[0014] The molar ratio of methacrylic acid to polyethylene glycol-200 in step (1) is 1:1.
[0015] The amount of sodium lignosulfonate used in step (2) is 1-3 wt% of the mass of methacrylic acid used in step (1); the amount of deep eutectic solution used in step (2) is 74.8-78.5 wt% of the gel prepolymer solution; the amount of pure water used is 18.15-23.04 wt% of the gel prepolymer solution; the amount of crosslinking agent used is 0.2-0.4 wt% of the mass of methacrylic acid; and the amount of initiator used is 4-6 wt% of the mass of methacrylic acid.
[0016] In step (2), the crosslinking agent is N,N'-methylenebisacrylamide (MBAA), and the initiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone (HMPP).
[0017] The UV irradiation-induced polymerization in step (3) is carried out under a 36W UV light source for 40 min.
[0018] The mold mentioned in step (3) is a circular or rectangular polytetrafluoroethylene mold. The thickness of the final composite gel is controlled by controlling the amount of gel prepolymer added to fill the mold.
[0019] A high-strength, high-toughness sodium lignosulfonate composite gel prepared by the above-described preparation method, wherein the composite gel comprises a polymer network skeleton formed by copolymerization of methacrylic acid and polyethylene glycol-200, and a sodium lignosulfonate reinforcing phase dispersed therein; the polymer network skeleton and sodium lignosulfonate form a three-dimensional cross-linked network structure through the synergistic effect of multiple hydrogen bonds and chemical cross-linking; the tensile strength of the composite gel is 1.0~1.5 MPa, and the elongation at break is 300%~450%.
[0020] The above-mentioned high-strength and high-toughness sodium lignosulfonate composite gel is used in the preparation of impact-resistant protective materials.
[0021] The above-mentioned high-strength and high-toughness sodium lignosulfonate composite gel is used in soft robot drive or structural components.
[0022] The present invention has the following advantages and beneficial effects compared with the prior art:
[0023] (1) This invention uses methacrylic acid (MAA) and polyethylene glycol-200 (PEG-200) as comonomers and constructs a chemical cross-linked network skeleton by UV-initiated free radical polymerization, which endows the hydrogel with excellent load-bearing capacity and structural integrity. At the same time, sodium lignosulfonate (LS) is introduced as a natural polymer reinforcing agent. The abundant sulfonic acid groups and phenolic hydroxyl groups in its molecule can form multiple hydrogen bonds with the carboxyl groups and ether bonds on the polymer chain to construct a physical cross-linked network. The chemical cross-linked network and the physical cross-linked network penetrate each other and reinforce each other. The resulting composite gel has a tensile strength of 1.03-1.48 MPa, an elongation at break of 430%, and a compressive strength of 5.71 MPa at 70% strain. It has excellent comprehensive mechanical properties with both high strength and high toughness, overcoming the technical problem that traditional hydrogels cannot balance strength and toughness.
[0024] (2) This invention utilizes sodium lignosulfonate (LS) as a green biomass enhancer, which is derived from a by-product of the papermaking industry. It is rich in raw materials, low in cost, and biodegradable. It avoids the problems of complex preparation processes, high costs, and potential environmental risks of traditional nanofillers such as carbon nanotubes and graphene. It conforms to the concept of green chemistry and sustainable development and significantly reduces the production cost of hydrogel materials. Attached Figure Description
[0025] Figure 1 Comparison photos of a prepolymer containing MAA, PEG-200, LS, MABAA, and HMPP before (A) and after (B) polymerization under UV irradiation.
[0026] Figure 2Tensile stress-strain curves at fracture for PMAA / PEG-200 / LS composite gels with different sodium lignosulfonate contents.
[0027] Figure 3 The stress curves (A) and dissipated energy versus peak stress curves (B) of the PMAA / PEG-200 / LS composite gel of the present invention under different compression amplitudes are shown.
[0028] Figure 4 The stress curve (A) of the PMAA / PEG-200 / LS composite gel of the present invention after 100 cycles of compression at 50% compression amplitude, and the dissipation energy and peak stress curve (B) after 100 cycles of compression at 50% compression amplitude.
[0029] Figure 5 These are photographs of the PMAA / PEG-200 / LS composite gel of the present invention under torsion (A) and biaxial tension (B), demonstrating its excellent flexibility.
[0030] Figure 6 This is a photo demonstrating the load-bearing capacity of the PMAA / PEG-200 / LS composite gel of the present invention. The gel can stably lift a 1 kg weight.
[0031] Figure 7 These are photographs illustrating the puncture resistance (A) and cut resistance (B) properties of the PMAA / PEG-200 / LS composite gel of this invention. Detailed Implementation
[0032] The following specific embodiments further illustrate the content of the present invention, but should not be construed as limiting the present invention.
[0033] The preparation process of the high-strength and high-toughness sodium lignosulfonate composite gel in the following examples follows the steps below:
[0034] Step 1: Mix methacrylic acid (MAA) and polyethylene glycol-200 (PEG-200) at a molar ratio of 1:1, and stir at 300-800 rpm for 40-60 min at room temperature (10-30℃) to prepare a transparent and colorless deep eutectic solution.
[0035] Step 2: Add pure water and sodium lignosulfonate to the deep eutectic solution obtained in step (1), and stir at 10-30℃ until completely dissolved; then add crosslinking agent N,N'-methylenebisacrylamide and photoinitiator 2-hydroxy-2-methyl-1-phenyl-1-propanone, and stir evenly to obtain a gel prepolymer solution; the sodium lignosulfonate accounts for 1-3 wt% of the polymeric monomer MAA; the amount of the deep eutectic solution is 74.8-78.5 wt% of the gel prepolymer solution; the amount of pure water is 18.15-23.04 wt% of the gel prepolymer solution; the amount of crosslinking agent is 0.2-0.4 wt% of the polymeric monomer MAA; the amount of initiator is 4-6 wt% of the polymeric monomer MAA.
[0036] Step 3: Fill the obtained gel prepolymer solution into a circular or rectangular polytetrafluoroethylene mold. Control the thickness of the final hydrogel by controlling the amount of gel prepolymer solution added. Induce polymerization under 36W ultraviolet light source to obtain a high-strength and high-toughness sodium lignosulfonate composite gel, namely PMAA-PEG-200-LS composite gel.
[0037] Example 1
[0038] This embodiment provides a method for preparing a high-strength, high-toughness sodium lignosulfonate (PMAA / PEG-200 / LS) composite gel, comprising the following steps:
[0039] (1) Mix methacrylic acid (1.75 g) and polyethylene glycol-200 (2 g) at room temperature at a speed of 600 rpm for 40 min to form a uniform colorless liquid, and a clear and transparent PDES solution can be obtained.
[0040] (2) Add pure water (1 g) and sodium lignosulfonate (the amount of sodium lignosulfonate is three: 0 g, 0.0175 g or 0.0525 g, which correspond to 0 wt%, 1 wt% or 3 wt% of the mass of methacrylic acid, respectively) to the PDES solution (3.75 g) obtained in step (1), and stir at 25°C until completely dissolved; then add 0.005 g of crosslinking agent N,N'-methylenebisacrylamide and 0.1 g of initiator 2-hydroxy-2-methyl-1-phenyl-1-propanone, and stir at 600 rpm until homogeneous to obtain gel prepolymer solution;
[0041] (3) The prepolymer solution in the vial was irradiated with a 36W UV lamp for 40 minutes to obtain sodium lignosulfonate composite gel (PMAA / PEG-200 / LS composite gel). Depending on the amount of sodium lignosulfonate added in step (2), the different PMAA / PEG-200 / LS composite gels were labeled as PMAA / PEG-200 / LS-0, PMAA / PEG-200 / LS-1 and PMAA / PEG-200 / LS-3 composite gels, respectively.
[0042] Experimental results: Taking the PMAA / PEG-200 / LS-1 composite gel prepared in step (3) as an example, its macroscopic morphology before and after polymerization was observed. Figure 1 These are photographs of the gel prepolymer obtained in step (2) and the composite gel obtained after UV curing in step (3), where A is the prepolymer before UV curing and B is the composite gel after UV curing. Figure 1 It can be seen that before UV curing ( Figure 1 (A), the prepolymer is a flowable liquid; after UV curing ( Figure 1 The prepolymer (B) transforms into a non-flowing, internally homogeneous, and transparent solid gel, with no liquid residue precipitating out during the curing process. These macroscopic changes indicate that methacrylic acid (MAA), polyethylene glycol-200 (PEG-200), and sodium lignosulfonate (LS) have successfully undergone copolymerization.
[0043] Example 2
[0044] This embodiment provides a method for evaluating the fracture tensile strength of PMAA / PEG-200 / LS composite gel, following these steps:
[0045] The tensile properties at fracture of the three PMAA / PEG-200 / LS composite gels obtained in Example 1 were tested using a universal testing machine. The two ends of the composite gel were neatly clamped on the tensile testing machine, the tensile speed was set to 50 mm / min, and the stress-strain curves were recorded in real time until the composite gel fractured.
[0046] Experimental results: such as Figure 2As shown, among the three PMAA / PEG-200 / LS composite gels prepared in Example 1, the tensile strength of PMAA / PEG-200 / LS-0 composite gel was 1.45 MPa, and the elongation at break was 299.47%; the tensile strength of PMAA / PEG-200 / LS-1 composite gel was 1.03 MPa, and the elongation at break was 430.04%; and the tensile strength of PMAA / PEG-200 / LS-3 composite gel was 1.33 MPa, and the elongation at break was 376.01%. These results indicate that the introduction of an appropriate amount of sodium lignosulfonate can significantly improve the elongation at break of the composite gel, but excessive addition (3 wt% of the mass of methacrylic acid) leads to a decrease in tensile strength, indicating that there is an optimal addition amount. In this example, the material exhibits the best toughness when the sodium lignosulfonate addition amount is 1 wt% of the mass of methacrylic acid.
[0047] Example 3
[0048] This embodiment provides a method for evaluating the performance of PMAA / PEG-200 / LS composite gel under different compression amplitudes, including the following steps:
[0049] Step A: The steps are exactly the same as those in Example 1 for preparing the PMAA / PEG-200 / LS-1 composite gel, and a cylindrical PMAA / PEG-200 / LS composite gel with a diameter of (20 mm) × thickness of (3 mm) is obtained.
[0050] Step B: The obtained composite gel was subjected to compression performance tests at different amplitudes using a universal testing machine. A bubble-free, well-formed cylindrical composite gel sample was placed flat at the center of the testing platform. The compression speed was set to 100 mm / min, and the compressive strains were set to 10%, 20%, 30%, 40%, 50%, 60%, and 70% of the initial thickness, respectively. The compressive strain-stress curves were recorded in real time. The dissipated energy and peak stress at each compressive strain were calculated by integrating the area of the stress-strain curves.
[0051] Experimental results: such as Figure 3 As shown in Figures A and B, the peak stresses of the PMAA / PEG-200 / LS composite gel at compression amplitudes of 10%, 20%, 30%, 40%, 50%, 60%, and 70% are 0.0919 MPa, 0.2354 MPa, 0.4573 MPa, 0.8192 MPa, 1.5035 MPa, 2.8621 MPa, and 5.7078 MPa, respectively, with a dissipated energy of 0.37429 MJ / m. 3 1.44276 MJ / m 3 3.53222 MJ / m 3 7.27249 MJ / m3 14.57773 MJ / m 3 28.43837 MJ / m 3 and 53.84459 MJ / m 3 The above results show that the peak stress and dissipated energy of the PMAA / PEG-200 / LS composite gel prepared in this invention increase significantly with increasing compressive strain, exhibiting excellent compressive mechanical properties and energy dissipation capacity. This indicates that the composite gel can effectively absorb and dissipate external energy when subjected to large deformation compression, and has the potential to be used as an impact-resistant buffer material.
[0052] Example 4
[0053] This embodiment provides a method for evaluating the cyclic compression performance of PMAA / PEG-200 / LS composite gel under constant compression amplitude, including the following steps:
[0054] Step A: The steps are exactly the same as those in Example 1 for preparing the PMAA / PEG-200 / LS-1 composite gel, and a cylindrical PMAA / PEG-200 / LS composite gel with a diameter of (20 mm) × thickness of (3 mm) is obtained.
[0055] Step B: The cyclic compression performance of the obtained composite gel was tested using a universal testing machine. A bubble-free, well-formed cylindrical composite gel sample was placed flat at the center of the testing platform. The compression speed was set to 100 mm / min, and the compressive strain to 50% of the initial thickness. 100 cycles of loading-unloading were performed, and the compressive strain-stress curve was recorded in real time. The dissipated energy and peak stress for each cycle were calculated by integrating the area of the stress-strain curve. Five parallel experiments were performed on each group of samples, and the average value was taken.
[0056] Experimental results: such as Figure 4As shown in Figures A and B, after 100 cycles of compression at 50% constant compressive strain, the dissipated energy of the PMAA / PEG-200 / LS-1 composite gel at the 2nd, 10th, 20th, 40th, 60th, 80th, and 100th cycles are 12.3583 MJ / m³, 9.9879 MJ / m³, 9.2723 MJ / m³, 8.6183 MJ / m³, 8.2487 MJ / m³, 7.9582 MJ / m³, and 7.7587 MJ / m³, respectively, with corresponding peak stresses of 1.14 MPa, 1.08 MPa, 1.05 MPa, 1.03 MPa, 1.01 MPa, 0.997 MPa, and 0.984 MPa. The above results show that the PMAA / PEG-200 / LS composite gel prepared in this invention maintains a high level of peak stress and dissipated energy during 100 cycles of compression, decreasing by only about 13.7% and 37.2% respectively, exhibiting good fatigue resistance and structural stability. This indicates that it can still maintain stable energy dissipation capacity under large deformation cyclic loading conditions and can be used as a long-term effective buffer and protective material.
[0057] Example 5
[0058] This embodiment provides a method for evaluating the flexibility of PMAA / PEG-200 / LS composite gel. It includes the following steps:
[0059] The PMAA / PEG-200 / LS composite gel was prepared using the same method as the PMAA / PEG-200 / LS-1 composite gel in Example 1. The gel measured 20 mm (length) × 10 mm (width) × 2 mm (thickness) and underwent torsion and biaxial stretching operations. A gel strip was rotated 720° in opposite directions at both ends and stretched, its surface condition was observed and photographed. Subsequently, two gels were interlaced perpendicularly, and the four edges of the sample were held in place by hand. Tensile forces in opposite directions were applied simultaneously in the horizontal and vertical directions, and the deformation of the gel under the cross-stress was observed and photographed.
[0060] Experimental results: such as Figure 5 As shown in A and B, the PMAA / PEG-200 / LS composite gel, after being twisted 720° and stretched, has a smooth surface without cracks and retains its structural integrity. Figure 5 The A-grade gel strips exhibit excellent flexibility and torsional resistance; in the biaxial tensile test, the two perpendicularly intersecting gel strips did not tear or separate at the intersection under four-way tensile force. Figure 5The result (B) indicates that the composite gel can maintain structural integrity under complex multi-directional stress conditions, exhibiting excellent tear resistance and omnidirectional toughness. This superior flexibility is attributed to the excellent mobility of the polymer network provided by the flexible segments of PEG-200, and the reversible breakage and reconstruction of the multiple hydrogen bonds of sodium lignosulfonate during deformation, effectively dissipating strain energy and thus synergistically enhancing the gel's resistance to deformation damage.
[0061] Example 6
[0062] This embodiment provides a method for evaluating the load-bearing performance of PMAA / PEG-200 / LS composite gel, including the following steps:
[0063] The procedure was exactly the same as that for preparing the PMAA / PEG-200 / LS-1 composite gel in Example 1, resulting in a PMAA / PEG-200 / LS composite gel with dimensions of length (20 mm) × width (10 mm) × thickness (2 mm). The gel sample was fixed at both ends, and a 1 kg weight was suspended in the middle of the gel. The deformation and fracture of the composite gel sample during the load-bearing process were observed and recorded by photograph.
[0064] Experimental results: such as Figure 6 As shown, the PMAA / PEG-200 / LS composite gel can stably suspend a 1 kg weight, and the gel maintains its structural integrity without significant creep. These results demonstrate that the composite gel prepared in this invention possesses excellent mechanical strength and load-bearing capacity.
[0065] Example 7
[0066] This embodiment provides a method for evaluating the puncture and cut resistance properties of PMAA / PEG-200 / LS composite gel, including the following steps:
[0067] Puncture resistance test: The PMAA / PEG-200 / LS composite gel was prepared using the same method as the PMAA / PEG-200 / LS-1 composite gel in Example 1 (diameter 20 mm × thickness 3 mm), and placed flat on the stage. A 1000 µL pipette tip (tip outer diameter approximately 1.0 mm) was taken, and the tip was vertically aligned with the center of the gel. The ends of the gel were held in place by hand, and the pipette tip was pressed vertically downwards to puncture the center of the gel. The deformation and breakage of the gel during the puncture process were observed and recorded.
[0068] Cut resistance test: Take gel samples of the same size, use a cutter to make a single cut on the gel surface with a vertical pressure of about 2 N, with a cut length of 10 mm, and observe the cut morphology and integrity of the gel after cutting.
[0069] Result: As Figure 7As shown in Figures A and B, when the PMAA / PEG-200 / LS-1 composite gel is vertically punctured by a pipette tip, only a local indentation occurs at the puncture site, and the gel remains intact without crack propagation or rupture. After the pipette tip is removed, the puncture hole closes rapidly. When cut by a cutting blade, the gel only deforms along the cutting direction without cracking or penetrating fracture. This indicates that the composite gel prepared in this invention has excellent puncture and cutting resistance and can effectively resist puncture damage from sharp objects.
[0070] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations and simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.
Claims
1. A method for preparing a high-strength high-toughness sodium lignosulfonate composite gel, characterized by Follow these steps: (1) Stir methacrylic acid and polyethylene glycol-200 at room temperature for 40-60 min to form a uniform, colorless, and transparent liquid, thus obtaining a deep eutectic solution; (2) Add pure water and sodium lignosulfonate to the deep eutectic solution obtained in step (1), and stir at 10-30℃ until completely dissolved; then add crosslinking agent and photoinitiator, stir evenly, and obtain gel prepolymer solution; (3) The gel prepolymer obtained in step (2) is filled into the mold and polymerized by UV irradiation to obtain a high-strength and high-toughness sodium lignosulfonate composite gel.
2. A process for the preparation of a high strength high toughness sodium lignosulfonate composite gel as claimed in claim 1, wherein: The ambient temperature in step (1) is 10-30℃; the stirring speed is 300-800 rpm.
3. A process for the preparation of a high strength high toughness sodium lignosulfonate composite gel as claimed in claim 1, wherein: The molar ratio of methacrylic acid to polyethylene glycol-200 in step (1) is 1:
1.
4. The method for preparing a high-strength, high-toughness sodium lignosulfonate composite gel according to claim 1, characterized in that: The amount of sodium lignosulfonate used in step (2) is 1-3 wt% of the mass of methacrylic acid used in step (1); the amount of deep eutectic solution used in step (2) is 74.8-78.5 wt% of the gel prepolymer solution; the amount of pure water used is 18.15-23.04 wt% of the gel prepolymer solution; the amount of crosslinking agent used is 0.2-0.4 wt% of the mass of methacrylic acid; and the amount of initiator used is 4-6 wt% of the mass of methacrylic acid.
5. The method for preparing a high-strength, high-toughness sodium lignosulfonate composite gel according to claim 1, characterized in that: In step (2), the crosslinking agent is N,N'-methylenebisacrylamide, and the initiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone.
6. The method for preparing a high-strength, high-toughness sodium lignosulfonate composite gel according to claim 1, characterized in that: The UV irradiation-induced polymerization in step (3) is carried out under a 36W UV light source for 40 min.
7. The method for preparing a high-strength, high-toughness sodium lignosulfonate composite gel according to claim 1, characterized in that: The mold mentioned in step (3) is a circular or rectangular polytetrafluoroethylene mold. The thickness of the final composite gel is controlled by controlling the amount of gel prepolymer added to fill the mold.
8. A high-strength, high-toughness sodium lignosulfonate composite gel prepared by the preparation method according to any one of claims 1-7, characterized in that: The composite gel comprises a polymer network skeleton formed by copolymerization of methacrylic acid and polyethylene glycol-200, and a sodium lignosulfonate reinforcing phase dispersed therein; the polymer network skeleton and sodium lignosulfonate form a three-dimensional cross-linked network structure through the synergistic effect of multiple hydrogen bonds and chemical cross-linking; the tensile strength of the composite gel is 1.0~1.5 MPa, and the elongation at break is 300%~450%.
9. The application of the high-strength, high-toughness sodium lignosulfonate composite gel according to claim 8 in the preparation of impact-resistant protective materials.