A method for deep oxidation-leaching tungsten extraction from waste cemented carbide powder

By employing processes such as segmented gradient heating oxygen-enriched oxidation roasting, atmospheric pressure alkaline leaching, and tailings sodium modification roasting, the problems of low tungsten recovery rate and poor purity of leaching solution in waste cemented carbide powder have been solved, achieving efficient and deep recovery and high-value utilization of tungsten resources.

CN123108328APending Publication Date: 2026-11-17GANNAN LABORATORY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611499424.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-24
Publication Date
2026-11-17

Smart Images

  • Figure CN123108328A_ABST
    Figure CN123108328A_ABST
Patent Text Reader

Abstract

This invention discloses a method for deep oxidation-leaching tungsten extraction from waste cemented carbide powder, relating to the field of rare metal recycling. Using tungsten / tungsten carbide-containing waste cemented carbide powder as raw material, the method includes the following steps: S1, raw material pretreatment; S2, segmented deep oxidation roasting; S3, atmospheric pressure alkaline leaching; S4, solid-liquid primary separation; S5, tailings sodium modification roasting; S6, secondary enhanced leaching; S7, tungsten resource integration and recycling. This invention achieves deep and complete oxidation of the tungsten component, solving the problem of oxidation residue. It employs a three-stage gradient heating oxygen-enriched oxidation roasting process, using a step-by-step reaction mode of low-temperature preheating dehydration and impurity removal, medium-temperature preliminary oxidation and bond breaking, and high-temperature shaping and complete oxidation. Combined with an oxygen-enriched atmosphere of ≥30%, it can gradually and thoroughly convert tungsten carbide and elemental tungsten in the waste cemented carbide powder into tungsten trioxide, while simultaneously fully oxidizing and decomposing the cobalt and nickel binder phases.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of rare metal recycling technology, specifically to a method for deep oxidation-leaching tungsten extraction from waste cemented carbide powder. Background Technology

[0002] Cemented carbide is a high-hardness, high-wear-resistant special alloy material prepared with tungsten carbide as the hard phase and cobalt or nickel as the binder phase. During the processing of cemented carbide tools, molds, and accessories, a large amount of grinding powder, waste scrap, and scrapped tools are generated. These materials contain high-grade tungsten resources and are secondary rare metal resources with great recycling value. Efficient recycling of waste cemented carbide powder can not only alleviate the shortage of primary tungsten ore resources and reduce the pressure of mining, but also reduce the production cost of tungsten products and realize the resource recycling of industrial solid waste.

[0003] Currently, the traditional single-stage oxidation roasting combined with single-stage alkaline leaching process is mostly used for tungsten extraction from waste cemented carbide powder. This process has certain drawbacks: First, the traditional single-stage high-temperature oxidation method has a fast heating rate and a single temperature zone, resulting in uneven oxidation of tungsten carbide and elemental tungsten inside the waste cemented carbide powder. This easily leads to problems such as excessive surface oxidation and incomplete internal oxidation, leaving a large amount of insoluble tungsten oxides and unreacted tungsten carbide residues in the tailings, resulting in a large loss of tungsten resources.

[0004] Second, traditional processes rely solely on a single alkaline leaching, which cannot effectively dissolve the insoluble tungsten components produced by incomplete oxidation. This results in high tungsten residue in the tailings and low overall tungsten recovery efficiency, with conventional processes typically achieving a comprehensive tungsten recovery rate of less than 93%.

[0005] Meanwhile, the existing solid-liquid separation method is simple, and the leachate is prone to carrying fine slag impurities, resulting in poor purity of tungsten-containing leachate, which makes subsequent purification and refining difficult and makes it hard to prepare high-purity ammonium paratungstate products.

[0006] Furthermore, traditional processes do not include a deep activation and recovery process for the residual tungsten resources in the leaching tailings. A large amount of valuable tungsten resources are discarded with the waste residue, resulting in extremely low resource utilization and insufficient solid waste resource utilization. This fails to meet the current industry development needs for efficient tungsten resource recovery, high-value utilization, and reduction of industrial solid waste.

[0007] To address this problem, we provide a method for deep oxidation-leaching tungsten extraction from waste cemented carbide powder. Summary of the Invention

[0008] To address one of the problems existing in the prior art, the present invention provides a method for deep oxidation-leaching tungsten extraction from waste cemented carbide powder, thereby achieving deep, efficient and high-value recovery of tungsten resources from waste cemented carbide.

[0009] To achieve the above objectives, the present invention employs a method for deep oxidation-leaching tungsten extraction from waste cemented carbide powder, using tungsten / tungsten carbide-containing waste cemented carbide powder as raw material, comprising the following steps: S1. Raw material pretreatment: The waste cemented carbide powder is crushed, ground, sieved and impurity removed to remove lumpy particles, oil and mechanical impurities, and to obtain refined waste cemented carbide powder with uniform particle size. S2. Segmented deep oxidation roasting: The refined waste cemented carbide powder is placed in an oxidation roasting furnace and a segmented gradient heating oxidation roasting process is adopted to fully oxidize the tungsten carbide and elemental tungsten in the powder into tungsten trioxide, while oxidizing and decomposing the residual cobalt and nickel metal binder phase in the powder. S3. Atmospheric pressure alkaline leaching: The calcined product after oxidation and roasting is added to a strong alkaline leaching solution and leached by stirring at a constant temperature, so that tungsten trioxide reacts with the alkaline solution to generate soluble tungstate which enters the leaching solution, while retaining insoluble metal oxide residue. S4. Solid-liquid separation in one step: After leaching, filtration is performed to separate the solid tungsten-containing pure leachate and solid tailings containing unleached residual tungsten. S5. Sodium-modified roasting of tailings: collect tailings containing residual tungsten, add sodium-modification aids for mixing and preparation, and carry out medium-temperature sodium-modification roasting after uniform mixing to convert the insoluble tungsten oxides and incompletely oxidized tungsten carbide in the tailings into soluble sodium tungstate. S6. Secondary enhanced leaching: The clinker after sodium roasting is subjected to water leaching or dilute alkali leaching treatment again to dissolve all sodium tungstate components, and the filtration yields secondary tungsten-containing leachate and final inert waste residue. S7. Tungsten Resource Integration and Recycling: Merge the primary alkaline leaching solution and the secondary sodium leaching solution, and unify the subsequent purification and refining treatment to achieve efficient and deep recovery of tungsten resources from waste cemented carbide powder.

[0010] As a further optimization of the above scheme, in step S1, the particle size of the refined powder after sieving is controlled at 100 mesh to 300 mesh. The pretreatment process adopts hot air degreasing and oil removal, with a degreasing temperature of 120℃ to 150℃ and a degreasing time of 15 min to 30 min to remove cutting oil stains and dust impurities attached to the surface of the powder.

[0011] As a further optimization of the above scheme, in step S2, the segmented gradient heating oxidation calcination process specifically includes a low-temperature preheating section, a medium-temperature oxidation section, and a high-temperature shaping section. The low-temperature preheating section is heated to 250℃~350℃ and kept at that temperature for 20min~30min to remove residual moisture and trace organic matter. The intermediate-temperature oxidation section is at a temperature of 450℃~550℃ and held for 40min~60min to initially oxidize tungsten carbide. The high-temperature setting section is at a temperature of 600℃~700℃ and held for 50min~70min to achieve complete oxidation of tungsten and tungsten carbide into tungsten trioxide. Oxygen-enriched air is then introduced with an oxygen concentration ≥30%.

[0012] As a further optimization of the above scheme, in step S3, the strong alkali leaching solution is a sodium hydroxide solution with a mass concentration of 15% to 25%, the liquid-solid ratio of the leaching solution to the calcined product is 5:1 to 8:1, the leaching temperature is 85℃ to 95℃, the stirring rate is 250r / min to 400r / min, and the leaching time is 2h to 3h.

[0013] As a further optimization of the above scheme, in step S5, the sodium oxidizing agent is a compound sodium oxidizing agent of anhydrous sodium carbonate and sodium hydroxide, with a mass ratio of 4:1 to 6:1, and the amount of sodium oxidizing agent added is 15% to 25% of the mass of the tailings.

[0014] As a further optimization of the above scheme, in step S5, the sodium calcination temperature is 750℃~850℃, the calcination holding time is 60min~90min, and the heating rate is controlled at 5℃ / min~8℃ / min.

[0015] As a further optimization of the above scheme, in step S6, the secondary leaching adopts a constant temperature water leaching process, with a leaching temperature of 70℃~80℃, a liquid-solid ratio of 4:1~6:1, and a stirring leaching time of 1.5h~2.5h.

[0016] As a further optimization of the above scheme, in steps S4 and S6, the solid-liquid separation adopts a combination filtration method of plate and frame pressure filtration and microporous fine filtration, with a filter membrane pore size of 0.22μm to 0.45μm, to retain fine solid particles.

[0017] As a further optimization of the above scheme, the calcining furnace adopts low-frequency vibration conditions throughout the process, with a vibration frequency of 15Hz to 30Hz and an amplitude of 2mm to 5mm, so that the oxide layer on the surface of the powder continuously falls off, exposing the unoxidized tungsten alloy components in the core of the particles.

[0018] The present invention provides a method for deep oxidation-leaching tungsten extraction from waste cemented carbide powder, which has the following beneficial effects: This invention achieves deep and complete oxidation of tungsten components, solving the problem of residual oxidation. It adopts a three-stage gradient heating and oxygen-enriched oxidation roasting process, which uses a step-by-step reaction mode of low-temperature preheating dehydration and impurity removal, medium-temperature preliminary oxidation and bond breaking, and high-temperature shaping and complete oxidation. Combined with an oxygen-enriched atmosphere of ≥30%, it can gradually and thoroughly convert tungsten carbide and elemental tungsten in waste cemented carbide powder into tungsten trioxide, while fully oxidizing and decomposing the cobalt and nickel binder phases.

[0019] This invention improves the overall tungsten recovery rate by coupling secondary leaching with tailings sodium modification. The invention uses a sodium carbonate-sodium hydroxide compound sodium modification aid with a specific ratio for medium-temperature sodium modification roasting, which can completely activate the inert and insoluble tungsten components into soluble sodium tungstate. Then, the residual tungsten resources are completely dissolved through secondary enhanced leaching, so as to achieve maximum reduction of solid waste.

[0020] This invention uses a combined filtration and purification method to improve the purity of the leachate and realize the high-value utilization of tungsten resources. The two solid-liquid separations of this invention both adopt a combined filtration method of plate and frame pressure filtration and microporous fine filtration, which can retain fine solid residues, avoid impurities in the tungsten liquid, and improve the purity of the tungsten-containing leachate. After subsequent acid adjustment precipitation, ammonia refining and evaporation crystallization, high-purity ammonium paratungstate products can be stably prepared.

[0021] Specific embodiments of the present invention are disclosed in detail with reference to the following description and accompanying drawings, indicating how the principles of the present invention can be adopted. It should be understood that the embodiments of the present invention are not limited in scope as a result, and that the embodiments of the present invention include many changes, modifications and equivalents within the spirit and scope of the appended claims. Attached Figure Description

[0022] Figure 1 This is a flowchart illustrating the steps of the method for deep oxidation-leaching tungsten extraction from waste cemented carbide powder according to the present invention. Detailed Implementation

[0023] Please refer to the instruction manual appendix. Figure 1 This invention provides a technical solution: a method for deep oxidation-leaching tungsten extraction from waste cemented carbide powder. This invention solves the problems of incomplete oxidation, high residual refractory tungsten, low recovery rate, and poor product purity in traditional waste cemented carbide tungsten extraction processes by using segmented gradient deep oxidation roasting, atmospheric pressure quantitative alkaline leaching, tailings sodium modification roasting, and secondary enhanced leaching.

[0024] This invention uses waste cemented carbide powder containing tungsten and tungsten carbide as raw material. First, a raw material pretreatment process removes oil and mechanical impurities and standardizes the powder particle size, eliminating interference from impurities in the subsequent oxidation roasting process. Then, a segmented gradient temperature oxygen-enriched oxidation roasting process is used to complete dehydration and organic matter removal, preliminary oxidation, and deep shaping oxidation in stages, converting elemental tungsten and tungsten carbide in the raw material into tungsten trioxide, while simultaneously oxidizing and decomposing the cobalt and nickel metal binder phases in the raw material. Finally, a normal-pressure strong alkali leaching process is used to dissolve the tungsten trioxide. The process involves obtaining a primary tungsten-containing leachate. For the insoluble tungsten oxides and incompletely oxidized tungsten carbide components remaining in the primary leaching tailings, a compound sodium-modifying agent is used for medium-temperature sodium-modifying roasting to convert the insoluble tungsten components into soluble sodium tungstate. Finally, a secondary enhanced leaching process is used to extract all tungsten components from the tailings. The two tungsten-containing leachates are combined and then purified and refined to produce high-purity ammonium paratungstate. This process achieves tiered and deep recovery of tungsten resources throughout the entire process, reducing the amount of tungsten residue in waste residue and improving resource utilization and product added value.

[0025] It should be noted that in all embodiments of this invention, waste cemented carbide powder prepared from industrial waste cemented carbide scraps and grinding waste is selected as raw material. First, the raw material is refined using mechanical crushing and ultrafine grinding equipment. Then, it is sieved through a standard sieve to control the particle size of the refined waste cemented carbide powder after sieving to be 100 mesh to 300 mesh. The sieved powder is then sent to a hot air degreasing device for impurity removal and degreasing treatment. The degreasing temperature is controlled at 120℃ to 150℃, and the degreasing holding time is 15 minutes to 30 minutes. This removes cutting oil stains, dust, and trace organic impurities adhering to the surface of the powder. Removing the cutting oil stains and dust impurities adhering to the surface of the powder avoids impurities affecting the roasting and oxidation effect. Finally, a refined waste cemented carbide powder with uniform particle size, free of impurities and oil stains is obtained for later use.

[0026] Example 1 This embodiment provides a method for deep oxidation-leaching tungsten extraction from waste cemented carbide powder, including the following steps: S1. Raw material pretreatment: Industrial waste cemented carbide grinding powder is selected as raw material. After crushing and grinding, it is screened through a 100-mesh standard sieve to obtain refined powder with a particle size of 100 mesh. The refined powder is placed in a hot air degreasing furnace, and the degreasing temperature is set at 120℃. The degreasing is carried out at a constant temperature for 30 minutes to remove oil stains and mechanical impurities from the surface of the powder, so as to obtain clean and uniform refined waste cemented carbide powder and avoid impurities from affecting the subsequent roasting and oxidation effect.

[0027] S2. Segmented deep oxidation roasting: The refined powder obtained in step S1 is placed in an oxygen-enriched oxidation roasting furnace, and oxygen-enriched air with an oxygen concentration ≥30% is introduced. In this embodiment, the oxygen concentration is 30%. A three-stage gradient heating and roasting process is adopted: The first low-temperature preheating stage involves heating the material to 250°C and holding it at that temperature for 30 minutes to remove residual moisture and trace amounts of organic matter from the powder. The second stage is a medium-temperature oxidation stage, where the temperature is raised to 450℃ and held for 60 minutes to carry out a preliminary oxidation reaction on the tungsten carbide and elemental tungsten in the powder. The third stage, high-temperature shaping stage, involves heating to 600℃ and holding for 70 minutes to achieve complete oxidation of tungsten carbide and elemental tungsten, converting them all into tungsten trioxide. At the same time, it oxidizes and decomposes the cobalt and nickel binder metal components in the powder to obtain the oxidized roasted product.

[0028] During the segmented deep oxidation roasting process, the oxygen-enriched oxidation roasting furnace continuously vibrates at low frequency, causing the initial oxide layer formed on the surface of the powder particles to fall off and peel off in time, continuously exposing the unoxidized tungsten carbide and elemental tungsten core inside the particles. This avoids the dense oxide film on the surface from blocking the oxygen permeation channels, ensuring that the particles are fully oxidized step by step from the outside to the inside, and solving the problems of incomplete oxidation and residual tungsten carbide inside the particles that exist in single static roasting. The roasting furnace vibration frequency is 15Hz~30Hz, and the amplitude is 2mm~5mm. The three-stage gradient roasting process is continuously vibrated without interruption, keeping the powder in a slightly agitated and loose state, preventing the powder from caking and the oxide layer from accumulating and covering it.

[0029] S3. Atmospheric pressure alkaline leaching: Prepare a 15% (w / w) sodium hydroxide strong alkaline leaching solution. Add the oxidized roasted product to the strong alkaline leaching solution according to a liquid-to-solid ratio of 5:1 between the leaching solution and the roasted product. Set the leaching temperature to 85℃, the stirring speed to 250r / min, and leach at a constant temperature for 3 hours to allow the tungsten trioxide in the roasted product to react fully with the sodium hydroxide, generating soluble sodium tungstate which enters the leaching solution. The cobalt and nickel oxidation products remain in the solid slag as insoluble metal oxides, ensuring efficient leaching of tungsten trioxide.

[0030] S4. Solid-liquid primary separation: After the leaching reaction is completed, a combination of plate and frame filter press and 0.45μm microporous fine filtration is used to separate solids and liquids, retain fine solid particles, avoid slag entrainment in tungsten liquid, improve the purity of leaching solution, and obtain a primary tungsten-containing leaching solution with high purity, as well as primary solid tailings containing residual insoluble tungsten components.

[0031] S5. Sodium-modified roasting of tailings: Collect the primary solid tailings obtained in step S4, and select anhydrous sodium carbonate and sodium hydroxide compound system as sodium-modification aid. The mass ratio of the two is 4:1, and the amount of sodium-modification aid added is 15% of the total mass of the primary tailings. This is suitable for the sodium-modification conversion reaction of insoluble tungsten components. After uniformly mixing the tailings and sodium-modification aid, the mixture is sent to a roasting furnace for sodium-modification roasting. The heating rate is controlled at 5℃ / min, and the temperature is raised to 750℃ and held at a constant temperature for 90 minutes to avoid local sintering and deactivation of tungsten components due to excessively rapid heating. This process converts the insoluble tungsten oxides and incompletely oxidized tungsten carbide in the tailings into soluble sodium tungstate.

[0032] S6. Secondary enhanced leaching: The sodium-calcined clinker obtained in step S5 is placed in a constant temperature water leaching device, the leaching temperature is controlled at 70℃, the liquid-solid ratio of the leaching solution to the clinker is 4:1, and the leaching is continuously stirred for 2.5 hours to efficiently dissolve the sodium tungstate generated by sodium-calcination. After leaching, a combination of plate and frame filter press and 0.45μm microporous fine filtration is used to separate the solid and liquid, avoiding the tungsten liquid from carrying slag, and obtaining a secondary tungsten-containing leaching solution and final inert waste residue.

[0033] S7. Tungsten Resource Integration and Recycling: Combine the primary tungsten-containing leachate obtained in step S4 with the secondary tungsten-containing leachate obtained in step S6, and process the mixed tungsten-containing leachate sequentially through a standardized process of acid precipitation, ammonia refining, and evaporation crystallization to prepare a high-purity ammonium paratungstate product, thereby realizing the high-value recycling and utilization of waste tungsten resources.

[0034] The process testing results of this embodiment show that the comprehensive tungsten recovery rate in waste cemented carbide powder is 98.6%, and the residual tungsten content in the final inert waste residue is 0.28%.

[0035] Example 2 This embodiment provides a method for deep oxidation-leaching tungsten extraction from waste cemented carbide powder, including the following steps: S1. Raw material pretreatment: Industrial waste cemented carbide scrap powder is selected as raw material. After crushing and fine grinding, it is screened through a 200-mesh standard sieve to obtain refined powder with a particle size of 200 mesh. The refined powder is placed in a hot air degreasing furnace, and the degreasing temperature is set at 135℃ for 22 minutes to remove cutting oil and dust impurities from the powder surface, thereby obtaining clean refined waste cemented carbide powder and eliminating the interference of impurities on roasting oxidation.

[0036] S2. Segmented deep oxidation roasting: The refined powder is placed in an oxygen-enriched oxidation roasting furnace and oxygen-enriched air with an oxygen concentration of 32% is introduced; the low-temperature preheating section is heated to 300℃ and held for 25 minutes to remove residual moisture and trace organic matter; the medium-temperature oxidation section is heated to 500℃ and held for 50 minutes to complete the initial oxidation of tungsten carbide; the high-temperature shaping section is heated to 650℃ and held for 60 minutes to achieve complete oxidation of tungsten and tungsten carbide into tungsten trioxide, and simultaneously oxidize and decompose the cobalt and nickel binder phases.

[0037] During the segmented deep oxidation roasting process, the oxygen-enriched oxidation roasting furnace continuously vibrates at low frequency, causing the initial oxide layer formed on the surface of the powder particles to fall off and peel off in time, continuously exposing the unoxidized tungsten carbide and elemental tungsten core inside the particles. This avoids the dense oxide film on the surface from blocking the oxygen permeation channels, ensuring that the particles are fully oxidized step by step from the outside to the inside, and solving the problems of incomplete oxidation and residual tungsten carbide inside the particles that exist in single static roasting. The roasting furnace vibration frequency is 15Hz~30Hz, and the amplitude is 2mm~5mm. The three-stage gradient roasting process is continuously vibrated without interruption, keeping the powder in a slightly agitated and loose state, preventing the powder from caking and the oxide layer from accumulating and covering it.

[0038] S3. Atmospheric pressure alkaline leaching: Prepare a strong alkaline leaching solution with a mass concentration of 20% sodium hydroxide, control the liquid-solid ratio of the leaching solution to the calcined product to be 6.5:1, the leaching temperature to be 90℃, the stirring speed to be 320r / min, and leach at a constant temperature for 2.5 hours to ensure that tungsten trioxide is efficiently dissolved and converted into sodium tungstate.

[0039] S4. Solid-liquid primary separation: After leaching, a combination of plate and frame filter press and 0.33μm microporous fine filtration process is used to separate the solids, retain fine solid particles, avoid slag entrainment, and obtain pure primary tungsten-containing leachate and tailings containing residual tungsten solids.

[0040] S5. Sodium-modified roasting of tailings: Collect primary solid tailings and use a compound sodium-modification aid with anhydrous sodium carbonate and sodium hydroxide in a mass ratio of 5:1. The amount of aid added is 20% of the mass of tailings and is suitable for the conversion of insoluble tungsten components. After uniformly mixing and preparing the material, control the heating rate to 6.5℃ / min, raise the temperature to 800℃, and keep it at a constant temperature for 75 minutes to avoid local sintering and coating, and complete the sodium-modification conversion of insoluble tungsten components in the tailings to generate soluble sodium tungstate.

[0041] S6. Secondary enhanced leaching: A constant temperature water leaching process is adopted, with the leaching temperature set at 75℃, the liquid-to-solid ratio at 5:1, and the stirring leaching time at 2 hours. After the sodium tungstate component is fully dissolved, it is separated by plate and frame filter press combined with 0.33μm micropore fine filtration to obtain secondary tungsten-containing leachate and final inert waste residue.

[0042] S7. Tungsten Resource Integration and Recycling: Combining two tungsten-containing leachates, high-purity ammonium paratungstate is prepared through acid precipitation, ammonia refining, and evaporation crystallization processes to achieve high-value recovery of tungsten resources.

[0043] The process testing results of this embodiment show that the comprehensive tungsten recovery rate in waste cemented carbide powder is 99.1%, and the residual tungsten content in the final inert waste residue is 0.21%.

[0044] Example 3 This embodiment provides a method for deep oxidation-leaching tungsten extraction from waste cemented carbide powder, including the following steps: S1. Raw material pretreatment: Select waste cemented carbide tool crushed and ground powder as raw material, and after fine treatment, screen it with a 300-mesh standard sieve to obtain refined powder with a particle size of 300 mesh; hot air degreasing temperature is 150℃, and degreasing is kept at 15 minutes to remove oil and mechanical impurities from the surface of the powder to obtain refined raw material powder, ensuring the roasting oxidation effect.

[0045] S2. Segmented deep oxidation roasting: The refined powder is placed in an oxygen-enriched roasting furnace and oxygen-enriched air with an oxygen concentration of 35% is introduced; the low-temperature preheating section is 350℃ and held for 20 minutes to remove impurities and moisture; the medium-temperature oxidation section is 550℃ and held for 40 minutes to initially oxidize the tungsten carbide components; the high-temperature shaping section is 700℃ and held for 50 minutes to completely oxidize the tungsten-based components into tungsten trioxide and decompose the cobalt and nickel metal binder phases.

[0046] During the segmented deep oxidation roasting process, the oxygen-enriched oxidation roasting furnace continuously vibrates at low frequency, causing the initial oxide layer formed on the surface of the powder particles to fall off and peel off in time, continuously exposing the unoxidized tungsten carbide and elemental tungsten core inside the particles. This avoids the dense oxide film on the surface from blocking the oxygen permeation channels, ensuring that the particles are fully oxidized step by step from the outside to the inside, and solving the problems of incomplete oxidation and residual tungsten carbide inside the particles that exist in single static roasting. The roasting furnace vibration frequency is 15Hz~30Hz, and the amplitude is 2mm~5mm. The three-stage gradient roasting process is continuously vibrated without interruption, keeping the powder in a slightly agitated and loose state, preventing the powder from caking and the oxide layer from accumulating and covering it.

[0047] S3. Atmospheric pressure alkaline leaching: Prepare a sodium hydroxide leaching solution with a mass concentration of 25%, a liquid-to-solid ratio of 8:1, a leaching temperature of 95℃, a stirring rate of 400r / min, and constant temperature leaching for 2 hours to allow tungsten trioxide to completely react with the alkaline solution and dissolve.

[0048] S4. Solid-liquid primary separation: Plate and frame filter press combined with 0.22μm microporous fine filtration is used to maximize the retention of fine slag materials and obtain high-purity primary tungsten-containing leachate and residual tungsten tailings.

[0049] S5. Sodium-modified roasting of tailings: A compound sodium-modification aid with anhydrous sodium carbonate and sodium hydroxide in a mass ratio of 6:1 is added to the tailings, and the amount of the aid added is 25% of the mass of the tailings. After mixing and forming the material, the heating rate is 8℃ / min, the roasting temperature is 850℃, and the temperature is kept constant for 60 minutes to avoid rapid heating and sintering, so as to complete the sodium-modification conversion of the insoluble tungsten components.

[0050] S6. Secondary enhanced leaching: water leaching temperature 80℃, liquid-solid ratio 6:1, stirring leaching for 1.5 hours to efficiently dissolve all sodium tungstate; after leaching, a combined filtration process is used to separate the tungsten-containing leachate and the final waste residue.

[0051] S7. Tungsten Resource Integration and Recycling: Combine the two leaching solutions, purify and refine them, and then evaporate and crystallize them to prepare high-purity ammonium paratungstate, thus completing the deep recycling of tungsten resources.

[0052] The process testing results of this embodiment show that the comprehensive tungsten recovery rate in waste cemented carbide powder is 98.8%, and the residual tungsten content in the final inert waste residue is 0.25%.

[0053] Comparative Example 1 The traditional waste cemented carbide tungsten extraction process is adopted, which only uses a single high-temperature oxidation roasting and a single alkaline leaching, without segmented gradient oxidation and tailings sodium modification secondary leaching process. Other parameters such as raw material pretreatment, leaching temperature, liquid-solid ratio and stirring rate are the same as in Example 2.

[0054] Test results: The traditional process has a tungsten recovery rate of only 92.3%, and the residual tungsten content in the final waste residue is as high as 1.15%, resulting in serious waste of tungsten resources and a recovery efficiency far lower than that of the process of this invention.

[0055] In summary, the comprehensive recovery rate of tungsten in the waste cemented carbide powder of this invention is ≥98.5%, and the residual tungsten content in the final waste residue is ≤0.3%. The tungsten-containing mixed solution generated by the primary alkaline leaching and secondary sodium leaching can be stably prepared into high-purity ammonium paratungstate through acid precipitation, ammonia refining and evaporation crystallization processes, thereby realizing the high-value and circular recycling of waste tungsten resources.

Claims

1. A method for deep oxidation-leaching of tungsten from waste hard metal powder, characterized in that, Using tungsten / tungsten carbide-containing waste cemented carbide powder as raw material, the process includes the following steps: S1. Raw material pretreatment: The waste cemented carbide powder is crushed, ground, sieved and impurity removed to remove lumpy particles, oil and mechanical impurities, and to obtain refined waste cemented carbide powder with uniform particle size. S2. Segmented deep oxidation roasting: The refined waste cemented carbide powder is placed in an oxidation roasting furnace and a segmented gradient heating oxidation roasting process is adopted to fully oxidize the tungsten carbide and elemental tungsten in the powder into tungsten trioxide, while oxidizing and decomposing the residual cobalt and nickel metal binder phase in the powder. S3. Atmospheric pressure alkaline leaching: The calcined product after oxidation and roasting is added to a strong alkaline leaching solution and leached by stirring at a constant temperature, so that tungsten trioxide reacts with the alkaline solution to generate soluble tungstate which enters the leaching solution, while retaining insoluble metal oxide residue. S4. Solid-liquid separation in one step: After leaching, filtration is performed to separate the solid tungsten-containing pure leachate and solid tailings containing unleached residual tungsten. S5. Sodium-modified roasting of tailings: collect tailings containing residual tungsten, add sodium-modification aids for mixing and preparation, and carry out medium-temperature sodium-modification roasting after uniform mixing to convert the insoluble tungsten oxides and incompletely oxidized tungsten carbide in the tailings into soluble sodium tungstate. S6. Secondary enhanced leaching: The clinker after sodium roasting is subjected to water leaching or dilute alkali leaching treatment again to dissolve all sodium tungstate components, and the filtration yields secondary tungsten-containing leachate and final inert waste residue. S7. Tungsten Resource Integration and Recycling: Merge the primary alkaline leaching solution and the secondary sodium leaching solution, and unify the subsequent purification and refining treatment to achieve efficient and deep recovery of tungsten resources from waste cemented carbide powder.

2. A method for deep oxidation-leaching of tungsten from waste hard metal powder according to claim 1, characterized in that: In step S1, the particle size of the refined powder after sieving is controlled between 100 mesh and 300 mesh. The pretreatment process uses hot air degreasing and oil removal, with a degreasing temperature of 120℃ to 150℃ and a degreasing time of 15 min to 30 min to remove cutting oil stains and dust impurities adhering to the surface of the powder.

3. A method for deep oxidation-leaching of tungsten from waste hard metal powder according to claim 1, characterized in that: In step S2, the segmented gradient heating oxidation calcination process specifically includes a low-temperature preheating section, a medium-temperature oxidation section, and a high-temperature shaping section; The low-temperature preheating section is heated to 250℃~350℃ and kept at that temperature for 20min~30min to remove residual moisture and trace organic matter. The intermediate-temperature oxidation section is at a temperature of 450℃~550℃ and held for 40min~60min to initially oxidize tungsten carbide. The high-temperature setting section is at a temperature of 600℃~700℃ and held for 50min~70min to achieve complete oxidation of tungsten and tungsten carbide into tungsten trioxide. Oxygen-enriched air is then introduced with an oxygen concentration ≥30%.

4. A process for deep oxidation-leaching of tungsten from spent carbide according to claim 1, characterized in that: In step S3, the strong alkali leaching solution is a sodium hydroxide solution with a mass concentration of 15% to 25%, the liquid-solid ratio of the leaching solution to the calcined product is 5:1 to 8:1, the leaching temperature is 85℃ to 95℃, the stirring rate is 250r / min to 400r / min, and the leaching time is 2h to 3h.

5. A process for deep oxidation-leaching of tungsten from spent carbide according to claim 1, characterized in that: In step S5, the sodium oxidizing agent is a compound sodium oxidizing agent of anhydrous sodium carbonate and sodium hydroxide, with a mass ratio of 4:1 to 6:1, and the amount of sodium oxidizing agent added is 15% to 25% of the mass of the tailings.

6. A process for deep oxidation-leaching of tungsten from spent carbide according to claim 1, characterized in that: In step S5, the sodium calcination temperature is 750℃~850℃, the calcination holding time is 60min~90min, and the heating rate is controlled at 5℃ / min~8℃ / min.

7. A process for deep oxidation-leaching of tungsten from spent carbide according to claim 1, characterized in that: In step S6, the secondary leaching adopts a constant temperature water leaching process with a leaching temperature of 70℃~80℃, a liquid-solid ratio of 4:1~6:1, and a stirring leaching time of 1.5h~2.5h.

8. A process for deep oxidation-leaching of tungsten from spent carbide according to claim 1, characterized in that: In steps S4 and S6, the solid-liquid separation adopts a combination filtration method of plate and frame pressure filtration and microporous fine filtration, with a filter membrane pore size of 0.22μm to 0.45μm, which retains fine solid particles.

9. A process for deep oxidation-leaching of tungsten from spent carbide according to claim 1, characterized in that: The roasting furnace operates under low-frequency vibration throughout the process, with a vibration frequency of 15Hz to 30Hz and an amplitude of 2mm to 5mm, which causes the oxide layer on the surface of the powder to continuously peel off, exposing the unoxidized tungsten alloy components in the core of the particles.