A method for fabricating a high-reliability GaN power switching device
By employing high-density dielectric growth and gamma-ray irradiation damage repair techniques, combined with low-damage etching and surface passivation techniques, the interface state density of the AlGaN barrier layer is reduced, thus addressing the reliability gap in GaN HEMT devices, improving the dynamic characteristics and long-term electrical stress reliability of the devices, and achieving compatibility with silicon power switching devices.
Patent Information
- Application Number
- CN202611480905.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-17
Smart Images

Figure CN123124381A_ABST
Abstract
Description
Technical Field
[0001] This invention pertains to the fabrication of switching devices, specifically a method for preparing a highly reliable GaN power switching device. Background Technology
[0002] GaN-based high electron mobility transistors (HEMTs) have been widely used in fast charging power supplies, automotive on-board computers (OBCs), and data center power supplies due to their advantages such as high frequency, high voltage, low loss, and high power density. However, issues such as high interface state density, strong peak electric field, and dielectric breakdown under high electric fields result in a significant gap in reliability between GaN HEMT devices and silicon power switching devices, preventing GaN HEMT devices from completely replacing silicon power switching devices in application promotion. To reduce interface state density, research institutions have developed low-damage etching and surface passivation techniques that combine atomic layer etching (ALE) and atomic layer deposition (ALD) technologies, reducing surface damage caused by etching while obtaining high-quality interface states. For reducing peak electric field density, the main approach is to optimize the field plate structure. For dielectric breakdown under high fields, the primary solution is to increase the dielectric thickness. While combining one or more of these technologies has improved the reliability of GaN HEMT devices to an acceptable level for applications, a significant gap still exists compared to the reliability of commercially available silicon power devices. Summary of the Invention
[0003] Purpose of the invention: In order to overcome the shortcomings of the prior art, the purpose of this invention is to provide a method for fabricating a highly reliable GaN power switching device with low interface state density.
[0004] Technical solution: The present invention provides a method for fabricating a high-reliability GaN power switching device, comprising the following steps:
[0005] Step 1: The surface of the Si and SiC composite layer is mechanically polished and chemically etched.
[0006] Step 2: A p-type doped GaN high-resistivity buffer layer is grown on the surface of the material obtained in Step 1 by vapor phase epitaxy (MOCVD).
[0007] Step 3: On the p-type doped GaN high-resistivity buffer layer, an active layer is grown by vapor phase epitaxy (MOCVD). The active layer is an AlGaN / GaN heterojunction.
[0008] Step 4: On the active layer, a p-type GaN gate control layer is grown by vapor phase epitaxy (MOCVD). A SiN etching mask layer is grown by plasma-enhanced chemical vapor deposition. The photoresist outside the gate control layer is removed. The p-type GaN outside the gate control region is etched away by chlorine plasma. After etching, γ-ray irradiation is performed for repair.
[0009] Step 5: Remove the SiN etching mask layer on the surface of the product obtained in Step 4, and prepare an Al2O3 surface passivation layer on the surface of the product obtained in Step 4 using atomic layer deposition (ALD). Then, prepare a SiN withstand voltage enhancement layer on the surface of the Al2O3 surface passivation layer using low-pressure chemical vapor deposition (LPCVD).
[0010] Step 6: Etch the Al2O3 surface passivation layer and SiN withstand voltage enhancement layer, and prepare ohmic metal in the etched area using electron beam evaporation.
[0011] Step 7: Etch the SiN withstand voltage boosting layer and the Al2O3 surface passivation layer, and use electron beam evaporation to prepare the gate metal connected to the p-type GaN gate control layer in the etched area.
[0012] Furthermore, in step one, the Si and SiC composite layer is prepared by an activation bonding method using surface plasma treatment, with an activation vacuum degree ≤ 5 × 10⁻⁶. -6 Pa, the activation treatment Ar plasma power is 50~100W, the activation treatment time is 100~120s, the bonding pressure is 20~60KN, and the bonding time is 280~300s; after bonding, it is annealed at 1000~1100℃ for 50~60s to achieve atomic-level flatness.
[0013] Furthermore, in step two, the vapor phase epitaxial growth temperature is 1000~1200℃, p-type doping is performed using ferrocene or propane, the doping flow rate is 50~100 sccm, the thickness of the p-type doped GaN high-resistivity buffer layer is greater than 0.5 μm, and the doping concentration is 1E18~5E20 cm⁻¹. -3 .
[0014] Furthermore, in step three, trimethylgallium and ammonia are used as precursors for vapor phase epitaxy growth, with a growth temperature of 1000~1050℃, a trimethylgallium flow rate of 30~1500 sccm, and an ammonia flow rate of 1~6 slm.
[0015] Furthermore, in step four, the p-type GaN gate control layer uses trimethylgallium and ammonia as precursors, with a growth temperature of 1000~1100℃, a trimethylgallium flow rate of 500~600 sccm, and an ammonia flow rate of 1~2 s. The Mg doping of the lmp-type GaN gate control layer uses magnesia-dicenocene with a flow rate of 330~1200 sccm.
[0016] Furthermore, in step four, after the p-type GaN gate control layer is grown, it undergoes post-annealing at 750~850℃ for 10~60 minutes in an N2 atmosphere.
[0017] Furthermore, in step four, the total dose of gamma ray irradiation repair is 1~3Mrad, and the dose rate is 50~300rad / s, which reduces surface etching damage.
[0018] Furthermore, in step five, the growth temperature of the Al2O3 surface passivation layer is 200~400℃, and the thickness is less than 100nm; the growth temperature of the SiN withstand voltage enhancement layer is 500~800℃, and the thickness is greater than 50nm. Preferably, the thickness of the Al2O3 surface passivation layer is 10~100nm, and the thickness of the SiN layer is 50~200nm.
[0019] Furthermore, in step six, the ohmic metal is one of several of Ti, Al, and Ti.
[0020] Furthermore, in step seven, the gate metal is one of Ti, Al, or Ti.
[0021] Fabrication principle: By combining high-density dielectric growth and γ-ray irradiation damage repair technology, the interface state density of the AlGaN barrier layer is reduced and the quality of the surface passivation layer is improved, thereby enhancing the reliability of the device. It can be applied to the research and production of GaN power switching devices.
[0022] Beneficial effects: Compared with the prior art, the present invention has the following significant features: low interface state density; high passivation medium density; high device dynamic characteristics and long-term electrical stress reliability; and compatibility with existing GaN power switching devices. Attached Figure Description
[0023] Figure 1 This is a schematic diagram of the structure of the product obtained in step S1 of the present invention;
[0024] Figure 2 This is a schematic diagram of the structure of the product obtained in step S2 of the present invention;
[0025] Figure 3 This is a schematic diagram of the structure of the product obtained in step S3 of the present invention;
[0026] Figure 4 This is a schematic diagram of the structure of the product obtained in step S4 of the present invention;
[0027] Figure 5 This is a schematic diagram of the structure of the product obtained in step S5 of the present invention;
[0028] Figure 6 This is a schematic diagram of the structure of the present invention. Detailed Implementation
[0029] Unless otherwise specified, all materials and reagents used in the following embodiments are commercially available. Experimental methods not specifically described in the embodiments are generally performed under standard conditions or as recommended by the manufacturer.
[0030] Example 1
[0031] A method for fabricating a high-reliability GaN power switching device includes the following steps:
[0032] S1, such as Figure 1 As shown, SiC was bonded on a clean Si substrate using an activation bonding process involving surface plasma treatment under high vacuum, forming a Si-SiC composite layer 1. The activation vacuum degree was 2 × 10⁻⁶. -6 The activation process involved an Ar plasma with a power of 100W and an activation time of 120s; a bonding pressure of 30kN and a bonding time of 300s; annealing at 1000℃ for 60s after bonding; and then mechanical polishing and chemical etching to ensure atomic-level flatness.
[0033] S2. Place the obtained Si and SiC composite layer 1 into an MOCVD apparatus. Using trimethylgallium, ammonia, and ferrocene as precursors, grow a p-type doped GaN high-resistivity buffer layer 2 at a temperature of 1050℃, a trimethylgallium flow rate of 500 sccm, an ammonia flow rate of 3 slm, and a ferrocene flow rate of 80 sccm to grow a 1 μm iron-doped GaN high-resistivity buffer layer with a doping concentration of 5E18cm⁻¹. -3 .
[0034] S3. Continue growing the active layer 3, i.e., the AlGaN / GaN heterojunction, in the MOCVD equipment. First, turn off the ferrocene source, maintain the temperature at 1050℃, the trimethylgallium flow rate at 500 sccm, and the ammonia flow rate at 2 slm to grow a 300nm GaN channel layer 31. Then, increase the temperature to 1000℃, turn on the trimethylaluminum source, the flow rate at 40 sccm, the trimethylgallium flow rate at 200 sccm, and the ammonia flow rate at 1.5 slm to grow a 15nm AlGaN barrier layer 32 with an Al atomic percentage of 12 at.
[0035] S4. After AlGaN growth, turn off the trimethylaluminum source, adjust the temperature to 1050℃, adjust the trimethylgallium flow rate to 500 sccm, the ammonia flow rate to 2 slm, turn on the magnesia-dicenocene source, and set the flow rate to 600 sccm. Epitaxially grow a 120nm Mg-doped p-type GaN gate layer 4 with a Mg concentration of 3E19cm⁻¹. -3After the p-type GaN gate control layer 4 was grown, it underwent a post-annealing treatment at 800℃ for 10 minutes in an N2 atmosphere. Then, a 200nm SiN etching mask layer 5 was grown using PECVD with 7220 photoresist. The photoresist outside the gate control layer area was removed through coating and development. SiN was then etched using fluorine plasma at an SF6 flow rate of 15 sccm, an etching power of 150 W, and an etching time of 50 s. The photoresist was removed using acetone-ethanol. Using the remaining SiN etching mask layer 5 as a mask, p-type GaN outside the gate control region was etched using chlorine plasma at a chlorine flow rate of 20 sccm, a power of 10 W, and an etching time of 140 sec. After etching, the area was irradiated with gamma rays at a total dose of 1 Mrad and a dose rate of 100 rad / s to reduce surface etching damage. Figure 2 and Figure 3 As shown.
[0036] S5. Remove the SiN etching mask layer 5 from the surface of the product obtained in step S4 using a 1:5 volume ratio ammonium fluoride aqueous solution. Prepare a 20nm Al2O3 surface passivation layer 6 on the surface of the product obtained in step S4 using ALD at a growth temperature of 300℃ and a growth time of 400s. Prepare a 100nm SiN pressure-boosting layer 7 using low-pressure chemical vapor deposition at a temperature of 600℃, a pressure of 1E-4Pa, and a time of 20min. Figure 4 As shown.
[0037] S6. Using 7908 photoresist, the source and drain electrode positions are defined through coating and development. The SiN withstand voltage enhancement layer 7 is etched using RIE (SF6 flow rate 15 sccm, etching power 150 W, etching time 30 s). The Al2O3 surface passivation layer 6 is etched using ICP (Inductively Coupled Plasma) with a Cl2 flow rate of 20 sccm, etching power 100 W, etching time 50 s. Ti / Al / Ti = 10nm / 100nm / 20nm ohmic metal 8 is evaporated using electron beam evaporation. Then, the source and drain electrodes are formed by ultrasonic lift-off in acetone and ethanol. Annealing is performed at 600℃ for 60 s. Figure 5 As shown.
[0038] S7. Using 7908 photoresist, the gate electrode positions are defined through coating and development. The SiN withstand voltage enhancement layer 7 is etched using RIE at an SF6 flow rate of 15 sccm, an etching power of 150 W, and an etching time of 30 s. The Al2O3 surface passivation layer 6 is etched using ICP at a Cl2 flow rate of 20 sccm, an etching power of 100 W, and an etching time of 50 s. The Ti / Ni / Al gate metal 9 (5nm / 20nm / 100nm) is evaporated using an electron beam, followed by ultrasonic lift-off in acetone and ethanol to form the gate electrode. The electrode is then heat-treated in air at 200°C for 1 hour. Figure 6 As shown.
[0039] Example 2
[0040] A method for fabricating a high-reliability GaN power switching device includes the following steps:
[0041] S1. SiC is bonded on a clean Si substrate using an activation bonding process involving surface plasma treatment under high vacuum to form a Si-SiC composite layer 1. The activation vacuum degree is 5 × 10⁻⁶. -6 The activation process involved 50W of physical Ar plasma and 100s of activation time; a bonding pressure of 20kN and a bonding time of 280s; followed by annealing at 1100℃ for 50s after bonding; and then mechanical polishing and chemical etching to ensure atomic-level flatness.
[0042] S2. Place the obtained Si and SiC composite layer 1 into an MOCVD apparatus. Using trimethylgallium, ammonia, and ferrocene as precursors, grow a p-type doped GaN high-resistivity buffer layer 2 at a temperature of 1000℃, a trimethylgallium flow rate of 500 sccm, an ammonia flow rate of 3 slm, and a ferrocene flow rate of 50 sccm to grow a 0.6 μm iron-doped GaN high-resistivity buffer layer with a doping concentration of 1E18cm⁻¹. -3 .
[0043] S3. Continue growing the active layer 3, i.e., the AlGaN / GaN heterojunction, in the MOCVD equipment. First, turn off the ferrocene source, maintain the temperature at 1050℃, the trimethylgallium flow rate at 500 sccm, and the ammonia flow rate at 2 slm to grow a 300nm GaN channel layer 31. Then, increase the temperature to 1000℃, turn on the trimethylaluminum source, the flow rate at 30 sccm, the trimethylgallium flow rate at 200 sccm, and the ammonia flow rate at 1 slm to grow a 15nm AlGaN barrier layer 32 with an Al atomic percentage of 12 at.
[0044] S4. After AlGaN growth, turn off the trimethylaluminum source, adjust the temperature to 1050℃, adjust the trimethylgallium flow rate to 600 sccm, the ammonia flow rate to 1 slm, turn on the magnesia-dicenocene source with a flow rate of 330 sccm, and epitaxially grow a 120nm Mg-doped p-type GaN gate layer 4 with a Mg concentration of 3E19cm⁻¹. -3After the p-type GaN gate control layer 4 was grown, it underwent post-annealing at 790℃ for 20 minutes in an N2 atmosphere. Then, a 200nm SiN etching mask layer 5 was grown using PECVD with 7220 photoresist. The photoresist outside the gate control layer area was removed through coating and development. SiN was then etched using fluorine plasma at an SF6 flow rate of 15 sccm, an etching power of 150 W, and an etching time of 50 s. The photoresist was removed using acetone-ethanol. Using the remaining SiN etching mask layer 5 as a mask, p-type GaN outside the gate control region was etched using chlorine plasma at a chlorine flow rate of 20 sccm, a power of 10 W, and an etching time of 140 sec. After etching, the surface was irradiated with gamma rays at a total dose of 3 Mrad and a dose rate of 50 rad / s to reduce surface etching damage.
[0045] S5. Remove the SiN etching mask layer 5 from the surface of the product obtained in step S4 using an ammonium fluoride aqueous solution with a volume ratio of 1:5. Prepare a 10nm Al2O3 surface passivation layer 6 on the surface using ALD at a growth temperature of 200℃ and a growth time of 200s. Prepare a 50nm SiN pressure-resistant enhancement layer 7 using low-pressure chemical vapor deposition at a temperature of 500℃, a pressure of 1E-4Pa, and a time of 15min.
[0046] S6. Using 7908 photoresist, the positions of the source and drain electrodes are defined by coating and developing. The SiN withstand voltage enhancement layer 7 is etched by RIE with an SF6 flow rate of 15 sccm, an etching power of 120 W, and an etching time of 20 s. The Al2O3 surface passivation layer 6 is etched by ICP with a Cl2 flow rate of 20 sccm, an etching power of 100 W, and an etching time of 30 s. The Ti / Al / Ti=10nm / 100nm / 20nm ohmic metal 8 is evaporated by electron beam. Then, the source and drain electrodes are formed by ultrasonic stripping in acetone and ethanol. The electrodes are annealed at 600℃ for 60 s.
[0047] S7. Using 7908 photoresist, the gate electrode position is defined by coating and developing. The SiN withstand voltage enhancement layer 7 is etched by RIE with an SF6 flow rate of 15 sccm, an etching power of 120 W, and an etching time of 20 s. The Al2O3 surface passivation layer 6 is etched by ICP with a Cl2 flow rate of 20 sccm, an etching power of 100 W, and an etching time of 30 s. The gate metal 9 with Ti / Ni / Al = 5nm / 20nm / 100nm is evaporated by electron beam evaporation. Then, the gate electrode is formed by ultrasonic stripping in acetone and ethanol. The gate electrode is then heat-treated in air at 200°C for 1 hour.
[0048] Example 3
[0049] A method for fabricating a high-reliability GaN power switching device includes the following steps:
[0050] S1. SiC is bonded on a clean Si substrate using an activation bonding process involving surface plasma treatment under high vacuum to form a Si-SiC composite layer 1. The activation vacuum degree is 3 × 10⁻⁶. -6 The activation process involved a physical Ar plasma power of 70W and an activation time of 110s; a bonding pressure of 60kN and a bonding time of 290s; followed by annealing at 1050℃ for 55s after bonding; and then mechanical polishing and chemical etching to ensure atomic-level flatness.
[0051] S2. Place the obtained Si and SiC composite layer 1 into an MOCVD apparatus. Using trimethylgallium, ammonia, and ferrocene as precursors, grow a p-type doped GaN high-resistivity buffer layer 2 at a temperature of 1200℃, a trimethylgallium flow rate of 500 sccm, an ammonia flow rate of 3 slm, and a ferrocene flow rate of 120 sccm to grow a 2 μm iron-doped GaN high-resistivity buffer layer with a doping concentration of 5E20cm⁻¹. -3 .
[0052] S3. Continue growing the active layer 3, i.e., the AlGaN / GaN heterojunction, in the MOCVD equipment. First, turn off the ferrocene source, maintain the temperature at 1050℃, the trimethylgallium flow rate at 500 sccm, and the ammonia flow rate at 2 slm to grow a 300nm GaN channel layer 31. Then, increase the temperature to 1020℃, turn on the trimethylaluminum source, the flow rate at 60 sccm, the trimethylgallium flow rate at 200 sccm, and the ammonia flow rate at 6 slm to grow a 15nm AlGaN barrier layer 32 with an Al atomic percentage of 14 at.
[0053] S4. After growing AlGaN, turn off the trimethylaluminum source, adjust the temperature to 1050℃, adjust the trimethylgallium flow rate to 550 sccm, and the ammonia flow rate to 1.5 slm. Turn on the magnesia-dicenocene source with a flow rate of 800 sccm. Epitaxially grow a 120 nm Mg-doped p-type GaN gate layer 4 with a Mg concentration of 4E19cm⁻¹. -3After the p-type GaN gate control layer 4 was grown, it underwent a post-annealing treatment at 800℃ for 10 minutes in an N2 atmosphere. Then, a 200nm SiN etching mask layer 5 was grown using PECVD with 7220 photoresist. The photoresist outside the gate control layer area was removed through coating and development. SiN was then etched using fluorine plasma at an SF6 flow rate of 15 sccm, an etching power of 150 W, and an etching time of 50 s. The photoresist was removed using acetone-ethanol. Using the remaining SiN etching mask layer 5 as a mask, p-type GaN outside the gate control region was etched using chlorine plasma at a chlorine flow rate of 20 sccm, a power of 10 W, and an etching time of 140 sec. After etching, the surface was irradiated with gamma rays at a total dose of 2 Mrad and a dose rate of 300 rad / s to reduce surface etching damage.
[0054] S5. The SiN etching mask layer 5 on the surface of the product obtained in step S4 is removed by using an ammonium fluoride aqueous solution with a volume ratio of 1:5. An 80 nm Al2O3 surface passivation layer 6 is prepared on the surface by ALD at a growth temperature of 400℃ and a growth time of 1600 s. A 200 nm SiN pressure-resistant enhancement layer 7 is prepared by low-pressure chemical vapor deposition at a temperature of 800℃, a pressure of 1E-4 Pa, and a time of 40 min.
[0055] S6. Using 7908 photoresist, the positions of the source and drain electrodes are defined by coating and developing. The SiN withstand voltage enhancement layer 7 is etched by RIE with an SF6 flow rate of 15 sccm, an etching power of 150 W, and an etching time of 70 s. The Al2O3 surface passivation layer 6 is etched by ICP with a Cl2 flow rate of 20 sccm, an etching power of 180 W, and an etching time of 300 s. The Ti / Al / Ti=10nm / 100nm / 20nm ohmic metal 8 is evaporated by electron beam. Then, the source and drain electrodes are formed by ultrasonic stripping in acetone and ethanol. The electrodes are annealed at 600℃ for 60 s.
[0056] S7. Using 7908 photoresist, the gate electrode positions are defined by coating and developing. The SiN withstand voltage enhancement layer 7 is etched using RIE with an SF6 flow rate of 15 sccm, an etching power of 150 W, and an etching time of 70 s. The Al2O3 surface passivation layer 6 is etched using ICP with a Cl2 flow rate of 20 sccm, an etching power of 180 W, and an etching time of 300 s. The gate metal 9 with a Ti / Ni / Al ratio of 5nm / 20nm / 100nm is evaporated using an electron beam. Then, the gate electrode is formed by ultrasonic stripping in acetone and ethanol. The gate electrode is then heat-treated in air at 200°C for 1 hour.
Claims
1. A method for fabricating a high-reliability GaN power switching device, characterized in that, Includes the following steps: Step 1: The surface of the Si and SiC composite layer (1) is mechanically polished and chemically etched. Step 2: A p-type doped GaN high-resistivity buffer layer is grown on the surface of the material obtained in Step 1 by vapor phase epitaxy (2). Step 3: A vapor phase epitaxial growth of an active layer (3) is performed on a p-type doped GaN high-resistivity buffer layer (2), wherein the active layer (3) is an AlGaN / GaN heterojunction; Step 4: A p-type GaN gate control layer (4) is grown on the active layer (3) by vapor phase epitaxy. A SiN etching mask layer (5) is grown by plasma-enhanced chemical vapor deposition. The photoresist outside the gate control layer is removed. The p-type GaN outside the gate control region is etched away by chlorine plasma. After etching, γ-ray irradiation is performed for repair. Step 5: Remove the SiN etching mask layer (5) on the surface of the product obtained in Step 4, and prepare an Al2O3 surface passivation layer (6) on the surface of the product obtained in Step 4 using atomic layer deposition. Then, prepare a SiN withstand voltage enhancement layer (7) on the surface of the Al2O3 surface passivation layer (6) using low-pressure chemical vapor deposition. Step 6: Etch the Al2O3 surface passivation layer (6) and the SiN withstand voltage enhancement layer (7), and prepare ohmic metal (8) in the etched area using electron beam evaporation. Step 7: Etch the SiN withstand voltage boosting layer (7) and the Al2O3 surface passivation layer (6), and use electron beam evaporation to prepare the gate metal (9) connected to the p-type GaN gate control layer (4) in the etched area.
2. The method for fabricating a high-reliability GaN power switching device according to claim 1, characterized in that: In step one, the Si and SiC composite layer (1) is prepared by an activation bonding method through surface plasma treatment, with an activation vacuum degree ≤ 5 × 10⁻⁶. -6 Pa, the activation treatment Ar plasma power is 50~100W, the activation treatment time is 100~120s, the bonding pressure is 20~60kN, and the bonding time is 280~300s; after bonding, annealing is carried out at 1000~1100℃ for 50~60s.
3. The method for fabricating a high-reliability GaN power switching device according to claim 1, characterized in that: In step two, the vapor phase epitaxial growth temperature is 1000~1200℃, ferrocene or propane is used for p-type doping, the doping flow rate is 50~100 sccm, the thickness of the p-type doped GaN high-resistivity buffer layer (2) is greater than 0.5 μm, and the doping concentration is 1E18~5E20 cm⁻¹. -3 .
4. The method for fabricating a high-reliability GaN power switching device according to claim 1, characterized in that: In step three, trimethylgallium and ammonia are used as precursors for vapor phase epitaxy growth. The growth temperature is 1000~1050℃, the trimethylgallium flow rate is 30~1500 sccm, and the ammonia flow rate is 1~6 slm.
5. The method for fabricating a high-reliability GaN power switching device according to claim 1, characterized in that: In step four, the p-type GaN gate control layer (4) uses trimethylgallium and ammonia as precursors, with a growth temperature of 1000~1100℃, a trimethylgallium flow rate of 500~600 sccm, and an ammonia flow rate of 1~2 slm. The Mg doping of the p-type GaN gate control layer (4) uses magnesia-dicenocene with a flow rate of 330~1200 sccm.
6. The method for fabricating a high-reliability GaN power switching device according to claim 1, characterized in that: In step four, after the p-type GaN gate control layer (4) is grown, it is subjected to post-annealing treatment at 750~850℃ for 10~60 minutes in N2 atmosphere.
7. The method for fabricating a high-reliability GaN power switching device according to claim 1, characterized in that: In step four, the total dose of gamma ray irradiation repair is 1~3Mrad, and the dose rate is 50~300rad / s.
8. The method for fabricating a high-reliability GaN power switching device according to claim 1, characterized in that: In step five, the growth temperature of the Al2O3 surface passivation layer (6) is 200~400℃ and the thickness is less than 100nm; the growth temperature of the SiN withstand voltage enhancement layer (7) is 500~800℃ and the thickness is greater than 50nm.
9. The method for fabricating a high-reliability GaN power switching device according to claim 1, characterized in that: In step six, the ohmic metal (8) is one of the following: Ti, Al, and Ti.
10. The method for fabricating a high-reliability GaN power switching device according to claim 1, characterized in that: In step seven, the gate metal (9) is one of the following: Ti, Al, and Ti.