Antibacterial and mildew-proof drying agent and preparation method thereof
By compounding antibacterial and antifungal agents onto the desiccant matrix and utilizing chemical cross-linking and grafting modification technologies, the problem of mold and bacteria easily growing in desiccants during use has been solved. This achieves uniform distribution and long-lasting sustained release of antibacterial and antifungal components, thereby improving the overall performance of the desiccant.
Patent Information
- Application Number
- CN202610986538.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-03
- Publication Date
- 2026-11-20
AI Technical Summary
Existing desiccants are prone to the growth of mold and bacteria after absorbing moisture, thus becoming a source of pollution. Furthermore, the antibacterial and anti-mold components are easily lost during use, resulting in insufficient long-term effectiveness.
By combining antibacterial and antifungal agents and using chemical crosslinking and grafting modification techniques to immobilize functional components onto the desiccant matrix in the form of chemical bonds, uniform distribution and long-lasting sustained release of antibacterial and antifungal components are achieved.
It significantly improves the overall antibacterial and antifungal properties and service life of the desiccant. The synergistic effect of the antibacterial agent and the antifungal agent enhances the antibacterial and antifungal effect, and the stability and slow-release properties of the functional components in the matrix are guaranteed.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of desiccant technology, and more specifically, to an antibacterial and antifungal desiccant and its preparation method. Background Technology
[0002] Desiccants are functional materials that adsorb moisture from the environment through physical or chemical means, and are widely used in moisture-proof packaging for food, pharmaceuticals, electronic products, and cultural relics. Traditional desiccants such as silica gel, montmorillonite, and calcium chloride, while possessing good moisture absorption properties, only slow down microbial growth by reducing ambient humidity; they do not inherently possess the ability to kill or inhibit microorganisms. In practical use, mold and bacteria can easily grow on the surface of desiccants after they absorb moisture, potentially becoming a source of contamination and causing secondary pollution to the packaged goods. Therefore, developing composite desiccants that combine drying and antibacterial / anti-mold properties has become a pressing technical challenge in this field.
[0003] Existing technologies also include the development of antibacterial desiccants. For example, Chinese patent CN105076228A discloses a bactericidal and mildew-proof desiccant for calligraphy and painting artworks, composed of ethylene-vinyl acetate copolymer, mineral silica desiccant powder, activated carbon, agarwood extract, iodopropynylcarbamate butyl ester, cinnamaldehyde, isothiazolinone, and other components. This desiccant combines multiple bactericidal and mildew-proof components with the desiccant carrier through simple physical mixing. Although it has a certain bactericidal and mildew-proof effect, the functional components and the desiccant matrix are only physically mixed, lacking chemical bonding. This results in the antibacterial and mildew-proof components being easily lost with moisture during use, leading to insufficient long-term effectiveness. Another example is Chinese patent CN103638785A, which discloses a mildew-proof desiccant prepared from components such as deoxidizers, nano-mildew inhibitors, type B silica gel, benzotriazole, type C silica gel, and silicone rubber. This desiccant physically mixes nano-antifungal agents with silica gel-based desiccants, relying on the synergistic effect between the components to achieve both antifungal and dehumidifying functions. However, this technical solution also lacks chemical bonding between the nano-antifungal agents and the silica gel matrix, making it difficult for the effective components of the antifungal agents to be stably immobilized in the desiccant structure. This results in an uncontrollable release rate of the antifungal components, affecting the long-term antifungal effect. Furthermore, none of the aforementioned existing technologies address the synergistic effect of combining antibacterial agents and antifungal agents, nor do they solve the problem of long-term immobilization of functional components in the desiccant matrix.
[0004] To address the shortcomings of the existing technology, this invention provides an antibacterial and antifungal desiccant and its preparation method. This invention combines an antibacterial agent and an antifungal agent, and utilizes chemical crosslinking and grafting modification techniques to immobilize the functional active ingredients onto the desiccant matrix in the form of chemical bonds. Simultaneously, process improvements achieve uniform distribution and long-lasting sustained release of the antibacterial and antifungal components, thereby significantly improving the overall antibacterial and antifungal performance and service life of the desiccant. Summary of the Invention
[0005] In view of this, in order to solve one of the above-mentioned technical problems, the present invention provides an antibacterial and antifungal desiccant and its preparation method, the specific technical solution of which is as follows: An antibacterial and antifungal desiccant, comprising the following raw materials in parts by weight: The matrix material consists of 50-80 parts, the composite antibacterial agent consists of 3-10 parts, the composite antifungal agent consists of 1-10 parts, the grafting monomer consists of 10-20 parts, the crosslinking agent consists of 1-5 parts, and the initiator consists of 0.03-1 parts.
[0006] Furthermore, the matrix material is at least one of starch-grafted sodium acrylate, sodium alginate, modified starch, and silica gel.
[0007] Furthermore, the composite antibacterial agent is obtained by compounding a modified antibacterial agent and ε-polylysine in a mass ratio of (0.1~1):(1~5).
[0008] Furthermore, the preparation method of the modified antibacterial agent is as follows: a. Zirconium phosphate was calcined, then added to an ethylenediamine solution, stirred, filtered, washed, and dried to obtain pretreated zirconium phosphate; b. Disperse the pretreated zirconium phosphate in deionized water, add cerium nitrate and silver nitrate, stir, filter, wash and dry to obtain the intercalated modified antibacterial agent; c. The intercalated modified antibacterial agent is added to a silane coupling agent solution, ultrasonically dispersed, stirred, filtered, washed, dried, and ground to obtain the modified antibacterial agent.
[0009] Further, in step a, the calcination treatment is carried out at 300~500℃ for 2~4h, and then added to an ethylenediamine solution with a mass percentage concentration of 5~15%, and stirred at a speed of 100~300r / min for 30~60min. After filtration, washing and drying, pretreated zirconium phosphate is obtained.
[0010] Furthermore, in step b, the mixture is stirred at 100-300 r / min for 1-3 hours at 60-90°C.
[0011] Further, in step c, the mixture is stirred at 100-200 r / min for 20-60 min at 50-80℃.
[0012] Furthermore, the composite antifungal agent is obtained by compounding isothiazolinone antifungal agents and cinnamaldehyde in a mass ratio of (2~3):(1~5).
[0013] Furthermore, the grafting monomer is at least one of acrylic acid, acrylamide, glycidyl methacrylate, and vinylpyrrolidone.
[0014] In addition, the present invention also provides a method for preparing an antibacterial and antifungal desiccant, the method comprising the following steps: The matrix material is added to the solvent and dispersed at a speed of 300-500 r / min for 30-60 min. Then, the grafted monomer, crosslinking agent and initiator are added and stirred at 100-300 r / min at 80-120℃ for 3-7 h. Then, the composite antibacterial agent and composite antifungal agent are added and stirred for another 1-3 h. The product is then washed, dried, pulverized and sieved to obtain the antibacterial and antifungal desiccant.
[0015] Compared with the prior art, the present invention has the following beneficial effects: 1. This invention significantly improves the antibacterial effect of desiccants by introducing modified antibacterial agents and ε-polylysine into the matrix material. The modified antibacterial agent is obtained by sequentially modifying zirconium phosphate through rare earth intercalation and silane surface modification. The pretreated zirconium phosphate increases the interlayer spacing, providing more loading space for cerium and silver ions. Silver ions, as the main antibacterial active centers, enter the interlayer through ion exchange, achieving a robust loading of the antibacterial components. Subsequently, surface modification is performed using a silane coupling agent. The silane coupling agent forms chemical grafts on the surface of the antibacterial agent, significantly improving its dispersibility, reducing aggregation, and imparting good organic compatibility, allowing it to better bind to the matrix material. This dual modification enables the slow release of antibacterial components, thus achieving long-lasting antibacterial effects. ε-polylysine, a natural broad-spectrum antibacterial agent, works synergistically with the modified antibacterial agent to significantly enhance the overall broad-spectrum antibacterial activity and efficiency of the desiccant.
[0016] 2. This invention combines isothiazolinone antifungal agents with cinnamaldehyde as an antifungal agent. Through target complementarity, it attacks and damages the cell membrane and disrupts cell metabolism, interfering with the energy metabolism pathway of the tricarboxylic acid cycle, thereby hindering the energy supply of the bacteria, inhibiting and killing mold, and further improving the antibacterial properties and antifungal effect of the desiccant.
[0017] 3. The matrix material used in this invention has excellent hygroscopicity and can undergo grafting and crosslinking reactions with grafted monomers, crosslinking agents, and initiators to form a stable three-dimensional network structure. Then, composite antibacterial agents and composite antifungal agents are added to continue the reaction, so that the antibacterial and antifungal components are evenly dispersed and chemically bonded to the desiccant matrix, giving the desiccant a significant antibacterial and antifungal effect. The entire process is mild and easy to operate, making it suitable for industrial production. Detailed Implementation
[0018] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to its embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the invention and do not limit the scope of protection of the invention.
[0019] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0020] An antibacterial and antifungal desiccant according to one embodiment of the present invention comprises the following raw materials in parts by weight: The matrix material consists of 50-80 parts, the composite antibacterial agent consists of 3-10 parts, the composite antifungal agent consists of 1-10 parts, the grafting monomer consists of 10-20 parts, the crosslinking agent consists of 1-5 parts, and the initiator consists of 0.03-1 parts.
[0021] In one embodiment, the matrix material is at least one of starch-grafted sodium acrylate, sodium alginate, modified starch, and silica gel.
[0022] In one embodiment, the composite antibacterial agent is obtained by compounding a modified antibacterial agent and ε-polylysine in a mass ratio of (0.1~1):(1~5).
[0023] In one embodiment, the modified antibacterial agent is prepared by: a. Zirconium phosphate was calcined, then added to an ethylenediamine solution, stirred, filtered, washed, and dried to obtain pretreated zirconium phosphate; b. Disperse the pretreated zirconium phosphate in deionized water, add cerium nitrate and silver nitrate, stir, filter, wash and dry to obtain the intercalated modified antibacterial agent; c. The intercalated modified antibacterial agent is added to a silane coupling agent solution, ultrasonically dispersed, stirred, filtered, washed, dried, and ground to obtain the modified antibacterial agent.
[0024] In one embodiment, in step a, the sample is calcined at 300-500°C for 2-4 hours, then added to an ethylenediamine solution with a mass percentage concentration of 5-15%, stirred at 100-300 r / min for 30-60 minutes, filtered, washed, and dried to obtain pretreated zirconium phosphate.
[0025] In one embodiment, in step a, the weight ratio of zirconium phosphate to ethylenediamine solution is (5~10):(20~50).
[0026] In one embodiment, in step b, the mixture is stirred at 100-300 r / min for 1-3 hours at 60-90°C.
[0027] In one embodiment, in step b, the weight ratio of the pretreated zirconium phosphate, deionized water, cerium nitrate, and silver nitrate is (5~10):(20~50):(0.01~3):(0.01~0.07).
[0028] In one embodiment, in step c, the mixture is stirred at 100-200 r / min for 20-60 min at 50-80°C.
[0029] In one embodiment, in step c, the weight ratio of the intercalation modified antibacterial agent to the silane coupling agent solution is (5~10):(20~30).
[0030] In one embodiment, the silane coupling solution is obtained by mixing a silane coupling agent, ethanol, and water in a volume ratio of (1~3):(50~70):(30~50).
[0031] In one embodiment, the silane coupling agent is at least one of γ-aminopropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, and γ-methacryloyloxypropyltrimethoxysilane.
[0032] In one embodiment, the composite antifungal agent is obtained by compounding isothiazolinone antifungal agents and cinnamaldehyde in a mass ratio of (2~3):(1~5).
[0033] In one embodiment, the grafting monomer is at least one of acrylic acid, acrylamide, glycidyl methacrylate, and vinylpyrrolidone.
[0034] In one embodiment, the crosslinking agent is at least one of trimethylolpropane triacrylate and polycarbodiimide.
[0035] In one embodiment, the initiator is at least one selected from ammonium persulfate, potassium persulfate, and azobisisobutyronitrile.
[0036] In addition, the present invention also provides a method for preparing an antibacterial and antifungal desiccant, the method comprising the following steps: The matrix material is added to the solvent and dispersed at a speed of 300-500 r / min for 30-60 min. Then, the grafted monomer, crosslinking agent and initiator are added and stirred at 100-300 r / min at 80-120℃ for 3-7 h. Then, the composite antibacterial agent and composite antifungal agent are added and stirred for another 1-3 h. The product is then washed, dried, pulverized and sieved to obtain the antibacterial and antifungal desiccant.
[0037] In one embodiment, the solvent is obtained by mixing ethanol and water in a volume ratio of (1~6):(1~9).
[0038] In one embodiment, the weight ratio of the substrate material to the solvent is (50~80):(100~200).
[0039] The above-mentioned scheme optimizes the raw materials for desiccant preparation, introduces composite antibacterial agents and composite antifungal agents to achieve synergistic effects, resulting in highly efficient, broad-spectrum, and long-lasting antibacterial and antifungal effects. Simultaneously, the matrix material ensures excellent moisture absorption and retention properties, enabling it to undergo grafting and cross-linking reactions with grafted monomers, cross-linking agents, and initiators to form a stable three-dimensional network structure. Further addition of composite antibacterial agents and composite antifungal agents allows for continued reaction, ensuring uniform dispersion and chemical bonding of the antibacterial and antifungal components within the desiccant matrix. This imparts significant antibacterial and antifungal effects to the desiccant, and the cross-linked grafted desiccant also exhibits excellent moisture absorption.
[0040] The implementation schemes of the present invention will now be described in detail with reference to specific embodiments.
[0041] Example 1: Preparation of modified antibacterial agents: a. According to the weight, 10 parts of zirconium phosphate were calcined at 450℃ for 3 hours, and then added to 50 parts of ethylenediamine solution with a mass percentage concentration of 8%. The mixture was stirred at 100 r / min for 45 minutes, filtered, washed and dried to obtain pretreated zirconium phosphate. b. Disperse 8 parts of pretreated zirconium phosphate in 30 parts of deionized water by weight, add 1 part of cerium nitrate and 0.01 parts of silver nitrate, stir at 100 r / min for 2 h at 65 °C, filter, wash and dry to obtain intercalation modified antibacterial agent. c. By weight, 8 parts of the intercalation-modified antibacterial agent were added to 30 parts of a silane coupling agent solution (a mixture of γ-aminopropyltriethoxysilane, ethanol, and water in a volume ratio of 1:60:40), ultrasonically dispersed, and stirred at 100 r / min for 30 min at 75 °C. The mixture was then filtered, washed, dried, and ground to obtain the modified antibacterial agent.
[0042] Preparation of antibacterial and antifungal desiccant: By weight, 60 parts of starch-grafted sodium acrylate were added to 100 parts of solvent (ethanol and water mixed in a volume ratio of 1:1) and dispersed at 300 r / min for 40 min. Then, 10 parts of glycidyl methacrylate, 2 parts of trimethylolpropane triacrylate and 0.05 parts of ammonium persulfate were added. The mixture was stirred at 100 r / min for 5 h at 90 °C. Then, 5 parts of composite antibacterial agent (obtained by compounding modified antibacterial agent and ε-polylysine in a mass ratio of 1:4) and 3 parts of composite antifungal agent (obtained by compounding isothiazolinone antifungal agent and cinnamaldehyde in a mass ratio of 2:3) were added and stirred for another 2 h. The product was then washed, dried, pulverized and sieved to obtain an antibacterial and antifungal desiccant.
[0043] Example 2: Preparation of modified antibacterial agents: a. According to the weight, 10 parts of zirconium phosphate were calcined at 500℃ for 3 hours, and then added to 50 parts of ethylenediamine solution with a mass percentage concentration of 10%. The mixture was stirred at 100 r / min for 45 minutes, filtered, washed and dried to obtain pretreated zirconium phosphate. b. Disperse 9 parts of pretreated zirconium phosphate in 30 parts of deionized water by weight, add 1 part of cerium nitrate and 0.02 parts of silver nitrate, stir at 100 r / min for 2 h at 65 °C, filter, wash and dry to obtain intercalation modified antibacterial agent. c. By weight, 8 parts of the intercalation-modified antibacterial agent were added to 30 parts of a silane coupling agent solution (a mixture of γ-aminopropyltriethoxysilane, ethanol, and water in a volume ratio of 1:60:40), ultrasonically dispersed, and stirred at 100 r / min for 35 min at 80 °C. The mixture was then filtered, washed, dried, and ground to obtain the modified antibacterial agent.
[0044] Preparation of antibacterial and antifungal desiccant: By weight, 60 parts of starch-grafted sodium acrylate were added to 100 parts of solvent (ethanol and water mixed in a volume ratio of 1:1) and dispersed at 300 r / min for 40 min. Then, 12 parts of glycidyl methacrylate, 2 parts of trimethylolpropane triacrylate and 0.06 parts of ammonium persulfate were added. The mixture was stirred at 100 r / min for 5 h at 95 °C. Then, 4 parts of composite antibacterial agent (obtained by compounding modified antibacterial agent and ε-polylysine in a mass ratio of 1:4) and 4 parts of composite antifungal agent (obtained by compounding isothiazolinone antifungal agent and cinnamaldehyde in a mass ratio of 3:2) were added and stirred for another 2 h. The product was then washed, dried, pulverized and sieved to obtain an antibacterial and antifungal desiccant.
[0045] Example 3: Preparation of modified antibacterial agents: a. According to the weight, 10 parts of zirconium phosphate were calcined at 500℃ for 3h, and then added to 50 parts of ethylenediamine solution with a mass percentage concentration of 12%. The mixture was stirred at 100r / min for 45min, filtered, washed and dried to obtain pretreated zirconium phosphate. b. Disperse 9 parts of pretreated zirconium phosphate in 30 parts of deionized water by weight, add 1 part of cerium nitrate and 0.02 parts of silver nitrate, stir at 100 r / min for 2 h at 70 °C, filter, wash and dry to obtain intercalation modified antibacterial agent. c. By weight, 8 parts of the intercalation-modified antibacterial agent were added to 30 parts of a silane coupling agent solution (a mixture of γ-aminopropyltriethoxysilane, ethanol, and water in a volume ratio of 1:60:40), ultrasonically dispersed, and stirred at 100 r / min for 35 min at 80 °C. The mixture was then filtered, washed, dried, and ground to obtain the modified antibacterial agent.
[0046] Preparation of antibacterial and antifungal desiccant: By weight, 60 parts of starch-grafted sodium acrylate were added to 100 parts of solvent (ethanol and water mixed in a volume ratio of 1:1) and dispersed at 300 r / min for 40 min. Then, 11 parts of glycidyl methacrylate, 3 parts of trimethylolpropane triacrylate and 0.06 parts of ammonium persulfate were added. The mixture was stirred at 100 r / min for 5 h at 95 °C. Then, 6 parts of composite antibacterial agent (obtained by compounding modified antibacterial agent and ε-polylysine in a mass ratio of 1:4) and 2 parts of composite antifungal agent (obtained by compounding isothiazolinone antifungal agent and cinnamaldehyde in a mass ratio of 3:2) were added and stirred for another 2 h. The product was then washed, dried, pulverized and sieved to obtain an antibacterial and antifungal desiccant.
[0047] Comparative Example 1: The difference between Comparative Example 1 and Example 3 is that the preparation method of the modified antibacterial agent in Comparative Example 1 is different, while the rest is the same as in Example 3. The preparation method of the antibacterial agent in Comparative Example 1 is as follows: a. Disperse 10 parts by weight of zirconium phosphate in 30 parts by weight of deionized water, then add 0.02 parts by weight of silver nitrate, stir at 100 r / min for 2 h at 75 °C, filter, wash and dry to obtain intercalation modified antibacterial agent; b. By weight, 8 parts of the intercalation-modified antibacterial agent were added to 30 parts of a silane coupling agent solution (a mixture of γ-aminopropyltriethoxysilane, ethanol, and water in a volume ratio of 1:60:40), ultrasonically dispersed, and stirred at 100 r / min for 35 min at 80 °C. The mixture was then filtered, washed, dried, and ground to obtain the modified antibacterial agent.
[0048] Comparative Example 2: The difference between Comparative Example 2 and Example 3 is that the preparation method of the modified antibacterial agent in Comparative Example 2 is different, while the rest is the same as in Example 3; The preparation method of the antibacterial agent in Comparative Example 2 is as follows: a. According to the weight, 10 parts of zirconium phosphate were calcined at 500℃ for 3h, and then added to 50 parts of ethylenediamine solution with a mass percentage concentration of 12%. The mixture was stirred at 100r / min for 45min, filtered, washed and dried to obtain pretreated zirconium phosphate. b. Disperse 9 parts of pretreated zirconium phosphate in 30 parts of deionized water by weight, add 1 part of cerium nitrate and 0.02 parts of silver nitrate, stir at 100 r / min for 2 h at 70 °C, filter, wash and dry to obtain intercalation modified antibacterial agent.
[0049] Comparative Example 3: The difference between Comparative Example 3 and Example 3 is that Comparative Example 3 uses a single ε-polylysine to replace the composite antibacterial agent, that is, no modified antibacterial agent is added.
[0050] Comparative Example 4: The difference between Comparative Example 4 and Example 3 is that the composite antifungal agent in Comparative Example 4 is a single isothiazolinone antifungal agent, that is, no cinnamaldehyde is added, while the rest is the same as in Example 3.
[0051] Comparative Example 5: The difference between Comparative Example 5 and Example 3 is that the composite antifungal agent in Comparative Example 5 is a single cinnamaldehyde, that is, no isothiazolinone antifungal agent is added, while the rest is the same as in Example 3.
[0052] Comparative Example 6: The difference between Comparative Example 6 and Example 3 is that no composite antifungal agent was added in Comparative Example 6, but otherwise it is the same as Example 3.
[0053] Comparative Example 7: Compared with Example 3, Comparative Example 7 differs in that the desiccant in Comparative Example 7 is prepared as follows: 60 parts by weight of starch-grafted sodium acrylate are added to 100 parts by weight of solvent (ethanol and water mixed in a volume ratio of 1:1), followed by 5 parts by weight of composite antibacterial agent (obtained by compounding modified antibacterial agent and ε-polylysine in a mass ratio of 1:4) and 3 parts by weight of composite antifungal agent (obtained by compounding isothiazolinone antifungal agent and cinnamaldehyde in a mass ratio of 2:3). The mixture is stirred at 300 r / min for 5 h, then dried, pulverized, and sieved to obtain the desiccant.
[0054] The desiccant samples prepared in Examples 1-3 and the desiccant samples prepared in Comparative Examples 1-7 were subjected to performance tests.
[0055] 1. Antibacterial performance test: The desiccant samples from Examples 1-3 and Comparative Examples 1-7 were pulverized and passed through a 100-mesh sieve. 1.0 g of each sample was weighed and placed in a 250 mL Erlenmeyer flask. Then, 70 mL of PBS and 5 mL of test bacterial solution (diluted with sterile phosphate-buffered saline (PBS) to a concentration of (1.0-3.0) × 10⁻⁶) were added respectively. 5 The test bacterial solution (CFU / mL) was used to completely submerge the sample. The Erlenmeyer flask was placed in a constant temperature shaking incubator and incubated at (24±1)℃ with shaking at 150 r / min for 24 h. After shaking incubation, 1 mL of the culture solution was serially diluted with PBS. 0.1 mL of the appropriate dilution was spread onto a nutrient agar plate and incubated at (37±1)℃ for 24 h, followed by viable cell counting. A blank control group without the sample was also included. Antibacterial rate % = (AB) / A × 100%, where A is the viable cell count (CFU / mL) of the blank control group and B is the viable cell count (CFU / mL) of the sample group. The results are shown in Table 1.
[0056] 2. Anti-mold test: The desiccant samples of Examples 1-3 and Comparative Examples 1-7 were pulverized and passed through a 100-mesh sieve. 2.0g of each sample was evenly spread in a sterile petri dish; a concentration of (1.0~5.0)×10⁻⁶ was selected. 6 A CFU / mL suspension of Aspergillus niger spores was sprayed evenly onto the surface of the desiccant sample using a sprayer. The petri dishes were then placed in a constant temperature and humidity incubator and cultured in the dark for 28 days at a temperature of (28±2)℃ and a relative humidity of ≥90%. The grades were assessed according to the standards in Table 2, and the results are shown in Table 3.
[0057] 3. Hygroscopicity Test: The desiccant samples of Examples 1-3 and Comparative Examples 1-7 were dried in a forced-air drying oven at (105±2)℃ until constant weight, and the mass m0 after drying was recorded. The dried samples were then placed in a constant temperature and humidity chamber at (25±1)℃ and (90±2)% relative humidity. The samples were weighed every 24 hours until the weight difference between two consecutive weighings did not exceed 0.01g, at which point hygroscopic equilibrium was reached, and the mass m1 after equilibrium was recorded. Hygroscopic rate % = (m1-m0) / m0 × 100%. The results are shown in Table 4 below.
[0058] Table 1: Results of Antibacterial Performance Tests
[0059] Table 2: Mildew Resistance Rating Assessment
[0060] Table 3: Results of Anti-mildew Performance Test
[0061] Table 4: Moisture Absorption Performance Results
[0062] Analysis of the data in Tables 1, 3, and 4 shows that the present invention immobilizes the composite antibacterial agent and composite antifungal agent onto the matrix material in the form of chemical bonds through a grafting crosslinking reaction. Furthermore, rare earth / silver ion intercalation modification and silane surface modification are used to synergistically improve the dispersibility and compatibility of the antibacterial agent, resulting in a desiccant with excellent broad-spectrum antibacterial properties. Compared to Example 3, the preparation method of the modified antibacterial agent in Comparative Example 1 is different (it does not include the calcination pretreatment of zirconium phosphate and the ethylenediamine intercalation step, and it does not introduce cerium nitrate for rare earth modification; it only directly performs silver ion loading and silane coupling agent surface treatment). Due to the lack of calcination layer expansion and ethylenediamine pre-intercalation, the interlayer spacing of zirconium phosphate cannot be effectively increased, the silver ion loading is limited and unevenly distributed; at the same time, the lack of synergistic antibacterial effect of cerium ions results in antibacterial activity and antifungal effect that are inferior to those of Example 3. The preparation method of the modified antibacterial agent in Comparative Example 2 was different (no silane coupling agent surface modification was performed after intercalation modification; the untreated intercalated modified antibacterial agent was used directly). Due to the lack of organosilane modification on the surface of the antibacterial agent, its dispersibility in the matrix was poor, it was prone to agglomeration, and its chemical bonding ability with the matrix material was weakened, resulting in antibacterial performance and antifungal effect that were not as good as in Example 3. In Comparative Example 3, a single ε-polylysine was used to replace the composite antibacterial agent (no modified antibacterial agent was added). Due to the lack of silver / cerium-supported zirconium phosphate modified by intercalation and silane, the system lacked long-lasting and sustained-release inorganic antibacterial active centers, relying only on the antibacterial effect of ε-polylysine. This resulted in an antibacterial rate and antifungal effect that were not as good as in Example 3, indicating that the synergy between the modified antibacterial agent and ε-polylysine helps to improve the efficacy of broad-spectrum antibacterial and auxiliary antifungal effects. In Comparative Example 4, the compound antifungal agent was a single isothiazolinone antifungal agent (without cinnamaldehyde). Due to the lack of complementary targets of cinnamaldehyde (cinnamaldehyde can attack the cell membrane and interfere with energy metabolism, while isothiazolinones mainly inhibit enzyme activity), the single antifungal agent resulted in insufficient antifungal effect, indicating that the addition of cinnamaldehyde helps to improve the overall antibacterial and antifungal synergy. In Comparative Example 5, the compound antifungal agent was a single cinnamaldehyde (without isothiazolinone antifungal agent). Due to the lack of the strong inhibitory effect of isothiazolinones on the fungal enzyme system, the natural antibacterial activity of single cinnamaldehyde failed to exert a better antifungal effect, and it also affected the antibacterial rate.
[0063] In Comparative Example 6, no composite antifungal agent was added. Although the composite antibacterial agent was effective against bacteria, its overall inhibitory effect on mold was not as good as in Example 3. Furthermore, the antibacterial effect decreased, indicating that the composite antifungal agent not only had a mildew-preventing effect but also had a synergistic effect in maintaining overall antibacterial performance. In Comparative Example 7, the desiccant was prepared using a different method (no grafting cross-linking reaction was performed; the matrix material was directly physically mixed with the composite antibacterial agent and composite antifungal agent, without forming chemical bonds). Because the antibacterial agent and antifungal agent were only physically dispersed in the matrix in a free state, the chemical bonding effect was weak. Functional components were easily lost with moisture migration, and the matrix material did not form a three-dimensional network structure, failing to effectively encapsulate and slowly release active components. This resulted in a significant decrease in the antibacterial rate and a significant reduction in the moisture absorption rate. This demonstrates that the grafting cross-linking chemical bonding process is a core technical means to simultaneously ensure high moisture absorption capacity, long-lasting antibacterial effect, and durable mildew prevention.
[0064] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0065] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.
Claims
1. An antibacterial and antifungal desiccant, characterized in that, The antibacterial and antifungal desiccant comprises the following raw materials in parts by weight: The matrix material consists of 50-80 parts, the composite antibacterial agent consists of 3-10 parts, the composite antifungal agent consists of 1-10 parts, the grafting monomer consists of 10-20 parts, the crosslinking agent consists of 1-5 parts, and the initiator consists of 0.03-1 parts.
2. The antibacterial and antifungal desiccant according to claim 1, characterized in that, The matrix material is at least one of starch-grafted sodium acrylate, sodium alginate, modified starch, and silica gel.
3. The antibacterial and antifungal desiccant according to claim 1, characterized in that, The composite antibacterial agent is obtained by compounding a modified antibacterial agent and ε-polylysine in a mass ratio of (0.1~1):(1~5).
4. The antibacterial and antifungal desiccant according to claim 3, characterized in that, The modified antibacterial agent is prepared by: a. Zirconium phosphate was calcined, then added to an ethylenediamine solution, stirred, filtered, washed, and dried to obtain pretreated zirconium phosphate; b. Disperse the pretreated zirconium phosphate in deionized water, add cerium nitrate and silver nitrate, stir, filter, wash and dry to obtain the intercalated modified antibacterial agent; c. The intercalated modified antibacterial agent is added to a silane coupling agent solution, ultrasonically dispersed, stirred, filtered, washed, dried, and ground to obtain the modified antibacterial agent.
5. The antibacterial and antifungal desiccant according to claim 4, characterized in that, In step a, the sample is calcined at 300-500℃ for 2-4 hours, then added to an ethylenediamine solution with a mass percentage concentration of 5-15%, and stirred at a speed of 100-300 r / min for 30-60 minutes. After filtration, washing, and drying, pretreated zirconium phosphate is obtained.
6. The antibacterial and antifungal desiccant according to claim 1, characterized in that, In step b, the mixture is stirred at 100-300 r / min for 1-3 hours at 60-90℃.
7. The antibacterial and antifungal desiccant according to claim 1, characterized in that, In step c, the mixture is stirred at 100-200 r / min for 20-60 min at 50-80℃.
8. The antibacterial and antifungal desiccant according to claim 1, characterized in that, The composite antifungal agent is obtained by compounding isothiazolinone antifungal agents and cinnamaldehyde in a mass ratio of (2~3):(1~5).
9. The antibacterial and antifungal desiccant according to claim 1, characterized in that, The grafting monomer is at least one of acrylic acid, acrylamide, glycidyl methacrylate, and vinylpyrrolidone.
10. A method for preparing an antibacterial and antifungal desiccant, characterized in that, The preparation method is used to prepare the antibacterial and antifungal desiccant according to any one of claims 1 to 9, and the preparation method includes the following steps: The matrix material is added to the solvent and dispersed at a speed of 300-500 r / min for 30-60 min. Then, the grafted monomer, crosslinking agent and initiator are added and stirred at 100-300 r / min at 80-120℃ for 3-7 h. Then, the composite antibacterial agent and composite antifungal agent are added and stirred for another 1-3 h. The product is then washed, dried, pulverized and sieved to obtain the antibacterial and antifungal desiccant.
Citation Information
Patent Citations
Drying agent with mildew-proof effect and preparation method thereof
CN103638785A
Bactericidal, mould-proof and drying agent for calligraphy and painting artworks
CN105076228A