An anti-pilling, breathable athletic sock and method of knitting the same
By fixing the bottom layer and the relaxed knit structure together, the continuous elastomer expands laterally under foot pressure, transmitting strain and stretching the relaxed knit structure. This solves the problem that the breathability of sports socks does not change with foot pressure, achieving anti-pilling, durability and dynamic breathability.
Patent Information
- Application Number
- CN202611609747.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-19
- Publication Date
- 2026-11-20
AI Technical Summary
Existing sports socks have a breathable and abrasion-resistant structures that are spatially independent, and their breathability does not change with foot pressure. Furthermore, they do not utilize the elastic matching design between the elastomer and the knitted structure, making it impossible to simultaneously meet the needs for anti-pilling, durability, and dynamic breathability.
The base adhesive locking layer is fixedly connected to the relaxed braided structure. The continuous elastomer penetrates into the coil gap and is cured and anchored. The base adhesive locking layer transmits strain, causing the relaxed braided structure to stretch and expand, increasing the porosity and forming a mechanism of static flow guidance and dynamic air permeability.
It achieves good breathability under both static and dynamic conditions, while also being anti-pilling and durable. It improves breathability, has high structural stability, and the continuous elastomer surface grooves enhance heat dissipation.
Smart Images

Figure CN123126554A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of sock processing technology, specifically relating to an anti-pilling and breathable sports sock and its knitting method. Background Technology
[0002] During wear, the continuous friction between the sole and insole of athletic socks can easily cause pilling on the fabric surface; at the same time, the hot and humid air generated by the feet during exercise needs to be expelled in time. To enhance slip resistance and abrasion resistance, existing technologies typically incorporate a silicone layer or abrasion-resistant layer on the sole or heel of the sock.
[0003] CN209152389U discloses an anti-pilling, shock-absorbing, protective sports sock, comprising a cylindrical sock body. The instep of the sock body has an X-shaped elastic tightening zone, and triangular mesh fabric zones are provided on both sides of the elastic tightening zone. The mesh fabric zones have a perforated mesh structure. The heel and toe areas of the sock body are made of abrasion-resistant terry cloth. A breathable mesh with striped perforations can also be provided on the sole. This document achieves both breathability and abrasion resistance / shock absorption through a zoned physical isolation method: the instep is responsible for breathability and sweat wicking, while the sole is responsible for abrasion resistance and shock absorption, and the X-shaped elastic tightening zone is less prone to pilling.
[0004] However, the breathable and abrasion-resistant structures in this literature are spatially independent; the instep is breathable, while the sole is abrasion-resistant, with no structural coupling between them. Its breathable mesh has a fixed-size mesh structure, and its breathability does not change with foot pressure, making it passively breathable. Furthermore, this literature does not address the elastic matching design between the elastomer and the knitted structure, does not include a bottom locking layer to transfer elastic deformation, and does not utilize elastomer compression to drive fabric stretching and unfolding to dynamically change the porosity. Therefore, existing technology has not yet provided a sports sock that combines a continuous elastomer with a bottom locking layer, using a relaxed knitted structure as the elastomer fixing area and a tightly knitted structure as the gas channel, driving the relaxed area to stretch and unfold under foot pressure, thereby achieving anti-pilling, durability, and dynamic breathability.
[0005] In view of this, there is an urgent need for a simple structure, high reliability, and anti-pilling breathable sports sock that can maintain good breathability in both static and ground conditions, as well as its knitting method. Summary of the Invention
[0006] This invention provides an anti-pilling and breathable sports sock and its knitting method. The sock is fixedly connected to a relaxed knitting structure via a base adhesive locking layer. The base adhesive locking layer penetrates into the loop gaps and solidifies and anchors, shaping the relaxed knitting structure into a wrinkled form. When the foot is compressed, the elastomer expands laterally, and the base adhesive locking layer transmits strain, causing the relaxed knitting structure to stretch and unfold, increasing its porosity. This achieves both static airflow and dynamic breathability, balancing anti-pilling and durability, thus solving the problems mentioned in the background art.
[0007] To achieve the above objectives, the present invention provides the following technical solution: an anti-pilling and breathable sports sock, comprising a sock body, wherein a continuous elastomer is disposed on the outer surface of the sock body, the continuous elastomer being a continuous mesh and including multiple elastic ribs, with gas channels formed between adjacent elastic ribs; the knitting area of the sock body includes a loose knitting structure and a tightly knitting structure, the loose knitting structure corresponding to the fixed area of the continuous elastomer, and the coil length of the loose knitting structure being greater than the coil length of the tightly knitting structure, the tightly knitting structure corresponding to the gas channel area between the elastomers; the continuous elastomer is fixedly connected to the loose knitting structure through a base adhesive locking layer, the base adhesive locking layer partially penetrating into the coil gaps of the loose knitting structure and curing to form an adhesive anchor, shaping the loose knitting structure into a wrinkled and undulating form; the base adhesive locking layer is configured to transfer lateral strain to the loose knitting structure when the continuous elastomer expands laterally under pressure, causing the loose knitting structure to stretch and expand, increasing its porosity.
[0008] As a further option, the sock body includes a toe area, a forefoot area, an arch area, a heel area, and a leg area, with the continuous elastomer disposed at least on the outer surface of the sock sole in the forefoot area and the heel area, and covering the loose knit structure.
[0009] As a further option, a transition zone is provided between the tightly braided structure and the loosely braided structure, wherein the coil length of the transition zone gradually increases from the coil length of the tightly braided structure to the coil length of the loosely braided structure within 2 to 3 loop rows.
[0010] As a further option, the sock body adopts a layered knitting structure with a surface layer yarn and an inner bottom yarn. The surface layer yarn is an anti-pilling polyester filament, and the bottom yarn is a spandex-covered yarn. The tight knitting structure is a plain knit layered knitting structure. The loose knitting structure is a tuck-float composite structure, in which the bottom yarn is looped in each loop, the face yarn is looped in odd-numbered loops and tucked in even-numbered loops, and floats are formed at predetermined needle positions.
[0011] As a further option, the surface of the elastic ribs of the continuous elastomer is provided with unclosed surface grooves, which extend along the length direction and / or width direction of the sock body. Adjacent surface grooves are interconnected and communicate with the gas channels between the elastomers to form an open gas circulation network.
[0012] As a further option, phase change material microcapsules are incorporated into the continuous elastomer; and / or, the width of the gas channels between the elastomers varies in a gradient along the length of the sock, and the spacing between adjacent elastic ribs at the center of the arch area is greater than the spacing towards the two sides of the arch area; and / or, the hardness of the continuous elastomer in the forefoot area is greater than the hardness in the heel area.
[0013] A method for knitting anti-pilling and breathable sports socks as described in any of the above claims includes the following steps:
[0014] (1) Knitted sock body: The sock body is knitted on a computerized knitting machine using a single-sided weft knitting structure. A relaxed knitting structure is knitted in the area where a continuous elastic body is set in advance, and a tight knitting structure is knitted in the air channel area between the continuous elastic bodies. The loop length of the relaxed knitting structure is greater than the loop length of the tight knitting structure.
[0015] (2) Apply primer: Apply primer to the surface of the relaxed braided structure. The primer thickness is 0.03 to 0.08 mm. Pre-cur at 70 to 90°C for 3 to 8 minutes to form a primer locking layer. The primer partially penetrates into the coil gaps of the relaxed braided structure. After curing, it forms an adhesive anchor with the coil and shapes the relaxed braided structure into a wrinkled and undulating shape.
[0016] (3) Applying continuous elastomer: Apply continuous elastomer to the base adhesive locking layer using a computer-controlled multi-axis dispensing machine or multi-touch dispensing machine. The continuous elastomer is a continuous mesh and includes multiple elastic ribs. Gas channels are formed between adjacent elastic ribs. The continuous elastomer covers the loose weave structure, and the tightly weave structure is retained between adjacent elastic ribs as gas channels. (4) Curing and shaping: Cure the sock blank after applying the continuous elastomer at 90-110°C for 30-60 minutes, and then shape it at 120-140°C for 30-60 seconds.
[0017] As a further option, in step (1), 2 to 3 transition zones with loops are set between the tightly knitted structure and the loosely knitted structure, and the loop length of the transition zone gradually increases from the loop length of the tightly knitted structure to the loop length of the loosely knitted structure; and / or, the loosely knitted structure adopts a tuck-float composite structure: the base yarn is looped in each loop, the face yarn is looped in odd-numbered loops, tucked in even-numbered loops, and floats are formed at the positions of 3 consecutive needles in the second row.
[0018] As a further option, in step (3), an unclosed surface groove is imprinted on the surface of the elastic ribs of the continuous elastomer. The groove depth is 20% to 40% of the thickness of the continuous elastomer, and the width is 0.3 to 0.8 mm. The surface groove extends along the length and width of the sock and is interconnected with each other, and is also connected to the gas channel between the elastomers.
[0019] As a further option, in step (3), phase change material microcapsules are mixed into the continuous elastomer. The phase change material microcapsules are paraffin microcapsules with a phase change temperature of 33°C, a particle size of 15-25 μm, and account for 18%-20% of the total mass of the continuous elastomer; and / or, Shore A60-A70 elastomer is applied to the forefoot area, and Shore A25-A40 elastomer is applied to the heel area; and / or, the width of the gas channel between the elastomers varies in a gradient along the length of the sock, the spacing between adjacent elastic ribs at the center of the arch area is 2.5 mm, and decreases to 1.2 mm towards the edges of the arch area.
[0020] Compared with the prior art, the beneficial effects of the present invention are:
[0021] 1. The continuous elastomer is fixedly connected to the relaxed braided structure through the base adhesive locking layer. The base adhesive penetrates into the coil gaps of the relaxed braided structure, and after curing, it forms an adhesive anchor and shapes the relaxed braided structure into a wrinkled and undulating shape.
[0022] 2. The fixed area of the elastomer features a relaxed woven structure, rather than a tightly woven one. When foot pressure compresses the continuous elastomer, it compresses and expands laterally. The base layer's locking layer transfers this lateral strain to the relaxed woven structure, causing it to stretch and expand, increasing porosity and improving air permeability. This dynamic air permeability mechanism does not rely on independent air tubes or sealed air chambers, ensuring high reliability.
[0023] 3. When the continuous elastomer expands laterally, it compresses the adjacent tightly braided structures. The tightly braided structure has short coil length, high density, and good dimensional stability. It can withstand compression without easily pilling or deformation, thus not affecting the overall durability.
[0024] 4. A tightly woven structure is set between adjacent parts of the continuous elastomer to serve as a gas channel, forming an open gas flow network between the continuous elastomers. In a static state, the gas channel can provide continuous airflow; in a grounded state, the relaxed woven structure stretches and unfolds, forming a dual heat dissipation mechanism of "static channel airflow + dynamic gap ventilation".
[0025] 5. The continuous elastomer can be a continuous mesh, including multiple elastic ribs. The intersections of the ribs are continuously and integrally formed, resulting in a stable structure that is not easily detached. The surface of the continuous elastomer can also be provided with unclosed surface grooves, connecting with gas channels between the elastomer and the surface, further enhancing heat dissipation. Attached Figure Description
[0026] The accompanying drawings, which are included to provide a further understanding of this application and form part of this application, illustrate exemplary embodiments and are used to explain this application, but do not constitute an undue limitation of this application. Obviously, the drawings described below are merely some embodiments of the present invention, and those skilled in the art can obtain other drawings based on these drawings without any creative effort.
[0027] In the attached diagram:
[0028] Figure 1 This is a schematic diagram of the overall structure of the sports socks of the present invention.
[0029] Figure 2 This is a schematic diagram of the knitting partition structure of the sock body according to the present invention.
[0030] Figure 3 This is a schematic diagram of a continuous elastomer with a relaxed braided structure.
[0031] Figure 4 This is a schematic diagram of the mechanical mechanism of dynamic air permeability regulation.
[0032] Figure 5 This is a schematic diagram of gas channels in the grooves on the surface of a continuous elastomer.
[0033] Figure 6 This is a schematic diagram of the knitting process for breathable sports socks.
[0034] Explanation of reference numerals in the attached figures:
[0035] 1-Sock body; 11-Toe area; 12-Forefoot area; 13-Arch area; 14-Heel area; 15-Cuff area; 2-Continuous elastomer; 21-Elastic ribs; 22-Gas channels between elastomers; 23-Lowering layer; 3-Tightly woven structure; 4-Loosely woven structure; 5-Transition area; 6-Surface grooves. Detailed Implementation
[0036] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0037] Example 1 - Basic Scheme
[0038] A pilling-resistant and breathable sports sock, using a single-sided weft knitting structure, is knitted on a computerized sock knitting machine (18 needles / inch).
[0039] (I) Overall Structural Design and Zonal Knitting of the Socks
[0040] like Figure 1 and Figure 2 As shown, the sock body (1) includes a toe area (11), a forefoot area (12), an arch area (13), a heel area (14), and a leg area (15). A continuous elastomer (2) is provided on the outer surface of the sock body (1). The continuous elastomer (2) is a continuous mesh shape, including multiple elastic ribs (21), and gas channels (22) are formed between adjacent elastic ribs (21). The continuous elastomer (2) is fixedly connected to the loose knit structure (4) of the sock body (1) through a bottom adhesive locking layer (23).
[0041] The knitting area of the sock body (1) is divided into two functional areas:
[0042] The first functional area is a relaxed weave structure (4), corresponding to the fixed area of the continuous elastomer (2). This area uses a larger coil length, making the fabric structure loose and having a larger stretch margin, and is shaped into a pleated shape by the base adhesive locking layer (23).
[0043] The second type of functional area is a tightly woven structure (3), which corresponds to the gas channel area between the continuous elastomers (2). This area uses a smaller coil length, which makes the fabric structure tight and dimensionally stable, able to withstand the compression when the continuous elastomers (2) expand laterally, and maintain anti-pilling performance.
[0044] The two functional areas are connected by a transition area (5). The coil length of the transition area (5) gradually increases from the coil length of the tightly braided structure (3) to the coil length of the loosely braided structure (4) within 2 to 3 coiled rows, so as to avoid the braiding tension fluctuation and structural stress concentration caused by the sudden change in coil length.
[0045] (II) Specific Design of the Knitting Structure of the Sock Body
[0046] The sock body (1) adopts a yarn-knitting structure with an outer layer yarn and an inner layer bottom yarn. The outer layer yarn is made of anti-pilling polyester filament (0.6 dtex single filament fineness, 48 filaments, 1000 twists / meter), and the bottom yarn is made of spandex-covered yarn (33 dtex spandex filament, 44 dtex outer nylon filament).
[0047] Knitting parameters for the tightly knitted structure (3): The loop length of the tightly knitted structure (3) in the forefoot area (12) is 5.0 mm, and the loop length of the tightly knitted structure (3) in the heel area (14) is 3.0 mm. The tightly knitted structure (3) adopts the knitting parameters of the dense knitting section. Each needle makes a loop in each looping column. The face yarn and the base yarn are fed in at the same time. The face yarn padding position is located outside the base yarn, forming a plain knitting structure. The face yarn tension is controlled at 5 cN, and the padding angle is 20°.
[0048] The weaving parameters of the relaxed weaving structure (4): In the predetermined fixed area of the continuous elastomer (2), the relaxed weaving structure (4) is adopted, and the loop length is 1.8 times that of the tightly woven structure (3). The loop length of the relaxed area in the forefoot area is about 9.0 mm, and the loop length of the relaxed area in the heel area is about 5.4 mm. The relaxed weaving structure (4) adopts a tuck-float composite structure: the base yarn is normally padded to form loops in each looping row to form a continuous basic skeleton; the face yarn is normally padded to form loops in odd-numbered looping rows, and in even-numbered looping rows, it is tucked to interlock with the old loops of the previous row; in the second row, the face yarn is not padded but padded with needle back yarn to form a float, and the float crosses 3 needles. Due to the large loop length and the intermittent weaving of the face yarn, the relaxed weaving structure (4) has obvious wrinkled undulations in its natural state.
[0049] The weaving parameters of the transition zone (5): Two to three transition zones (5) with loops arranged horizontally are set between the tightly woven structure (3) and the loosely woven structure (4). The coil length in the transition zone (5) gradually increases from the coil length of the tightly woven structure (3) to the coil length of the loosely woven structure (4) in an arithmetic sequence. For example, the coil lengths of the forefoot transition zone (5) are 5.8 mm, 6.6 mm, 7.4 mm, and 8.2 mm respectively.
[0050] (iii) Application of the base adhesive locking layer
[0051] like Figure 3 As shown, a base coat is applied to the relaxed knit structure (4) area of the sock body (1). An addition-curing liquid silicone rubber base coat is used, and the thickness is 0.05 mm. It is pre-cured at 80°C for 5 minutes. The base coat partially penetrates into the gaps between the coils of the relaxed knit structure (4), and after curing, it forms an adhesive anchor with the coils, while shaping the relaxed knit structure (4) into a wrinkled and undulating shape.
[0052] (iv) Application of continuous elastic body
[0053] The knitted sock blank is placed on the mold plate, and a continuous elastomer (2) is applied to the bottom adhesive locking layer (23) by a computer-controlled multi-axis dispensing machine. The continuous elastomer (2) is a continuous mesh shape, including multiple elastic ribs (21). The width of the elastic ribs (21) is 2.0 mm, the thickness is 1.2 mm, and the spacing between adjacent elastic ribs (21) is 2.0 mm. Shore A65 elastomer is applied to the forefoot area (12), and Shore A32 elastomer is applied to the heel area (14).
[0054] A continuous elastomer (2) covers a relaxed knitted structure (4), with a tightly knitted structure (3) remaining between adjacent portions of the continuous elastomer (2) as a gas channel. The continuous elastomer (2) forms a continuous rather than discrete elastic network on the stocking body (1).
[0055] (v) Curing and shaping
[0056] The sock blank after applying the continuous elastomer (2) was cured at 100°C for 45 minutes. During the curing process, the base adhesive locking layer (23) formed an adhesive anchor with the coils of the relaxed knit structure (4). The setting temperature was 130°C and the setting time was 45 seconds.
[0057] (vi) Mechanical mechanism of dynamic air permeability regulation
[0058] like Figure 4 As shown, when the wearer is at rest, the continuous elastomer (2) is in its natural state, the relaxed weave structure (4) maintains its pleated shape, and the air permeability is approximately 75 mm / s. The gas channels (22) between the elastomers provide static airflow.
[0059] When the wearer walks or runs, the pressure generated by the foot striking the ground (0.3-0.6 MPa) causes the continuous elastomer (2) to undergo elastic compression deformation, with the compression amount being approximately 10%-20% of the height of the continuous elastomer. While the continuous elastomer (2) is compressed in the height direction, it expands laterally. The base adhesive locking layer (23) transfers the lateral strain to the relaxed braided structure (4), causing the relaxed braided structure (4) to be stretched and unfolded, the fold undulation shape to be flattened, the fabric porosity to increase, and the air permeability to approximately 190 mm / s. At the same time, the lateral expansion of the continuous elastomer (2) compresses the adjacent tightly braided structure (3). Due to the small coil length and high density, the tightly braided structure (3) only undergoes slight compression, without damaging the structure, ensuring anti-pilling and durability.
[0060] When the foot leaves the ground, the continuous elastomer (2) recovers its elasticity, and the relaxed woven structure (4) recovers its folded shape under the combined action of its own elastic recovery force and the constraint of the bottom adhesive locking layer (23), and the air permeability drops.
[0061] The performance parameters of the sports socks in this embodiment were tested and are as follows:
[0062] Performance indicators Test Standards Test Results Anti-pilling rating (tightly woven structure 3) GB / T4802.2 Martindale Method Level 4-5 Anti-pilling rating (relaxed weave structure 4) GB / T4802.2 Martindale Method Level 4 Air permeability (at rest) GB / T5453-1997 75mm / s Air permeability (under ground conditions, 0.5 MPa) GB / T5453-1997 190mm / s Breathability (arch area 13) GB / T5453-1997 320mm / s Base adhesive locking layer peel strength GB / T2790 ≥6N / cm Elastic recovery rate FZ / T70006-2004 ≥92% Peel strength retention rate after 50 water washes Enterprise Standards ≥75%
[0063] Example 2 – Surface Trench Reinforcement Scheme
[0064] like Figure 5 As shown, the difference from Example 1 is that an unclosed surface groove (6) is provided on the surface of the elastic ribs (21) of the continuous elastomer (2). The surface groove (6) is formed by embossing a convex rib structure on the mold plate. The groove depth is 30% of the thickness of the continuous elastomer (2), and the groove width is 0.5 mm. The surface groove (6) extends along the length and width of the sock body. Adjacent grooves are interconnected and communicate with the gas channel (22) between the elastomers to form an open gas flow network.
[0065] According to the test, the anti-pilling level of the arch area (13) in this embodiment is 4 to 5, the air permeability is 85 mm / s in the static state and 205 mm / s in the ground state. The static flow contribution of the surface groove (6) is about 10 mm / s.
[0066] Example 3 – Phase Transition Enhancement and Gradient Channel Scheme
[0067] The difference from Example 1 is that phase change material microcapsules (paraffin microcapsules, phase change temperature 33°C, particle size 15-25μm) are mixed into the continuous elastomer (2), and the microcapsules account for 20% of the total mass of the continuous elastomer. The mixing process is as follows: the phase change microcapsules are first premixed with component B by stirring at low speed, and then mixed with component A in the mixing head of the dispensing machine before application.
[0068] The width of the gas channel (22) between the elastomers varies in a gradient along the length of the sock: at the center of the arch area (13), the distance between adjacent elastic ribs (21) is 2.5 mm, and decreases to 1.2 mm towards the edges of the arch area (13).
[0069] According to the test, the anti-pilling level of the arch area (13) in this embodiment is 4 to 5, the air permeability is 70 mm / s in the static state and 235 mm / s in the ground state.
[0070] Example 4 – Comprehensive Optimization Scheme
[0071] The difference from Example 1 is as follows:
[0072] Sock body knitting parameters: The loop length of the tight knitting structure (3) in the heel area (14) is 3.0 mm, and the loop length of the loose knitting structure (4) is 5.4 mm; the loop length of the tight knitting structure (3) in the forefoot area (12) is 5.0 mm, and the loop length of the loose knitting structure (4) is 9.0 mm.
[0073] Continuous elastomer (2): The elastomer hardness of the forefoot area (12) is Shore A68, and the elastomer hardness of the heel area (14) is Shore A30. The width of the elastic rib (21) is 2.2mm, the thickness is 1.3mm, and the spacing between adjacent elastic ribs (21) is 2.0mm.
[0074] Base adhesive locking layer (23): thickness is 0.06mm.
[0075] Surface groove (6): The groove depth is 25% of the thickness of the continuous elastomer (2), and the groove width is 0.6 mm.
[0076] Phase change material microcapsules: Paraffin microcapsules are mixed into continuous elastomer (2), the phase change temperature is 33℃, and the microcapsules account for 18% of the total mass of the continuous elastomer.
[0077] According to the test, the anti-pilling level of the arch area (13) in this embodiment is 4 to 5, the air permeability is 90 mm / s when stationary, the air permeability is 265 mm / s when on the ground, and the peel strength of the bottom rubber locking layer is ≥6 N / cm.
[0078] Comparative Example 1 – No-Base Adhesive Locking Solution
[0079] The difference from Example 1 is that the continuous elastomer (2) is directly bonded to the tightly woven structure (3), and the loosely woven structure (4) does not have a base adhesive locking layer (23).
[0080] Test results: Static air permeability was 70 mm / s, and ground air permeability was 120 mm / s. This comparative example shows that the base layer locking layer (23) plays a key role in transferring the lateral expansion of the continuous elastomer (2) to the relaxed woven structure (4) for dynamic air permeability.
[0081] Comparative Example 2 – Elastomer Coverage of Dense Region Scheme
[0082] The difference from Example 1 is that the continuous elastomer (2) covers the tightly woven structure (3), and the loosely woven structure (4) is exposed.
[0083] Test results: The static air permeability was 65 mm / s, and the ground air permeability was 100 mm / s. This comparative example shows that choosing a relaxed weave structure (4) in the fixed area of the elastomer is more conducive to dynamic air permeability.
[0084] Comparative Example 3 – Continuous Elastomer Full Coverage Channelless Solution
[0085] The difference from Example 1 is that the continuous elastomer (2) continuously covers the entire bottom of the sock, and no gas channel (22) is provided between the elastomers.
[0086] Test results: The static air permeability was 55 mm / s, and the ground air permeability was 110 mm / s. This comparative example shows that the gas channels (22) between the elastomers play an important role in both static air conduction and dynamic air permeability.
[0087] Comparative Example 4 – Discrete Elastomer Scheme
[0088] The difference from Example 1 is that discrete silicone units are used instead of continuous elastomer (2), and there is no continuous gas channel between adjacent silicone units.
[0089] Test results: The static air permeability was 60 mm / s, and the ground air permeability was 170 mm / s. This comparative example shows that the combination of the continuous elastomer (2) and the gas channel (22) between the elastomers can improve the static air permeability.
[0090] Performance Summary Comparison Table
[0091] project Static air permeability (mm / s) Ground permeability (mm / s) Peel strength (N / cm) Peel strength retention rate after 50 water washes Anti-pilling grade Example 1 75 190 ≥6 ≥75% Level 4-5 Example 2 85 205 ≥6 ≥75% Level 4-5 Example 3 70 235 ≥6 ≥75% Level 4-5 Example 4 90 265 ≥6 ≥75% Level 4-5 Comparative Example 1 70 120 ≥6 ≥75% Level 4-5 Comparative Example 2 65 100 ≥6 ≥75% Level 4-5 Comparative Example 3 55 110 ≥6 ≥75% Level 4-5 Comparative Example 4 60 170 ≥5 ≥70% Level 4
[0092] .
[0093] like Figure 6 As shown, the anti-pilling and breathable sports socks of the present invention can be prepared by the following knitting method, wherein the surface groove embossing in step (3) is an optional step.
[0094] (1) Knitted sock body
[0095] The sock body is knitted on a computerized sock knitting machine using a single-sided weft knitting structure. A relaxed knitting structure is knitted in a predetermined fixed area of the continuous elastomer, and a tight knitting structure is knitted in the gas channel area between the continuous elastomers. Two to three transition zones with loops arranged horizontally are set between the tight knitting structure and the relaxed knitting structure. The loop length in the transition zone gradually increases from the loop length of the tight knitting structure to the loop length of the relaxed knitting structure.
[0096] (2) Apply primer
[0097] A primer with a thickness of 0.03–0.08 mm is applied to the surface of the relaxed braided structure and pre-cured at 70–90°C for 3–8 minutes to form a primer locking layer. The primer partially penetrates into the gaps between the coils of the relaxed braided structure, and after curing, it forms an adhesive anchor with the coils, shaping the relaxed braided structure into a wrinkled and undulating form.
[0098] (3) Applying a continuous elastomer
[0099] A continuous elastomer is applied to the base coat locking layer using a computer-controlled multi-axis dispensing machine. The continuous elastomer is a continuous mesh structure, comprising multiple elastic ribs with a width of 1.5–4.0 mm, a thickness of 0.8–1.5 mm, and a spacing of 1.0–3.0 mm between adjacent ribs. Shore A60–A70 elastomer is applied to the forefoot area, and Shore A25–A40 elastomer is applied to the heel area. The continuous elastomer covers a loosely woven structure, while a tightly woven structure is maintained between the ribs to serve as air channels.
[0100] Optionally, unclosed surface grooves are imprinted on the surface of the continuous elastomer. The groove depth is 20% to 40% of the elastomer thickness and the width is 0.3 to 0.8 mm. The surface grooves extend along the length and width of the sock and are interconnected, forming an open gas flow network together with the gas channels between the elastomers.
[0101] (4) Curing and shaping
[0102] The sock blank after applying the continuous elastomer is cured at 90-110℃ for 30-60 minutes, and then set at 120-140℃ for 30-60 seconds to allow the bottom adhesive locking layer to form a stable bond with the relaxed knitting structure coils. The continuous elastomer completes cross-linking and setting, resulting in anti-pilling and breathable sports socks.
[0103] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A pilling-resistant and breathable sports sock, comprising a sock body (1), characterized in that, The outer surface of the sock body (1) is provided with a continuous elastic body (2), which is a continuous mesh and includes multiple elastic ribs (21). An inter-elastic gas channel (22) is formed between adjacent elastic ribs (21). The knitting area of the sock body (1) includes a loose knitting structure (4) and a tight knitting structure (3). The loose knitting structure (4) corresponds to the fixed area of the continuous elastic body (2), and the coil length of the loose knitting structure (4) is greater than the coil length of the tight knitting structure (3). The tight knitting structure (3) corresponds to the fixed area of the continuous elastic body (2). Gas channel (22) region between elastomers; the continuous elastomer (2) is fixedly connected to the relaxed braided structure (4) through the base adhesive locking layer (23), the base adhesive locking layer (23) partially penetrates into the coil gap of the relaxed braided structure (4) and solidifies to form an adhesive anchor, shaping the relaxed braided structure (4) into a wrinkled and undulating shape; the base adhesive locking layer (23) is configured to transfer the lateral strain to the relaxed braided structure (4) when the continuous elastomer (2) is compressed and expands laterally, so that the relaxed braided structure (4) stretches and expands, and the porosity increases.
2. The anti-pilling and breathable sports socks according to claim 1, characterized in that, The sock body (1) includes a toe area (11), a forefoot area (12), an arch area (13), a heel area (14), and a leg area (15). The continuous elastomer (2) is provided on the outer surface of the sock bottom of the forefoot area (12) and the heel area (14) and covers the loose knit structure (4).
3. The anti-pilling and breathable sports socks according to claim 1, characterized in that, A transition zone (5) is provided between the tightly braided structure (3) and the loosely braided structure (4). The coil length of the transition zone (5) gradually increases from the coil length of the tightly braided structure (3) to the coil length of the loosely braided structure (4) within 2 to 3 looped rows.
4. The anti-pilling and breathable sports socks according to claim 1, characterized in that, The sock body (1) adopts a yarn-padded knitting structure of surface layer yarn and inner bottom yarn. The surface layer yarn is anti-pilling polyester filament, and the bottom yarn is spandex-covered yarn. The tight knitting structure (3) is a plain knit yarn-padded structure. The loose knitting structure (4) is a tuck-float composite structure. The bottom yarn is looped in each loop, the face yarn is looped in odd-numbered loops and tucked in even-numbered loops, and floats are formed at predetermined needle positions.
5. The anti-pilling and breathable sports socks according to claim 1, characterized in that, The surface of the elastic ribs (21) of the continuous elastomer (2) is provided with unclosed surface grooves (6), which extend along the length direction and / or width direction of the sock body. Adjacent surface grooves (6) are interconnected and connected to the gas channel (22) between the elastomers to form an open gas flow network.
6. The anti-pilling and breathable sports socks according to claim 2, characterized in that, Phase change material microcapsules are mixed into the continuous elastomer (2); and / or, the width of the gas channel (22) between the elastomers varies in a gradient along the length of the sock, and the distance between adjacent elastic ribs (21) at the center of the arch area (13) is greater than the distance towards the two sides of the arch area (13); and / or, the hardness of the continuous elastomer (2) in the forefoot area (12) is greater than the hardness in the heel area (14).
7. A knitting method for anti-pilling and breathable sports socks as described in any one of claims 1 to 6, characterized in that, Includes the following steps: (1) Knitted sock body: The sock body (1) is knitted on a computer knitting sock machine using a single-sided weft knitting structure. A relaxed knitting structure (4) is knitted in the area where a continuous elastic body (2) is set in advance, and a tight knitting structure (3) is knitted in the gas channel area between the continuous elastic bodies (2). The loop length of the relaxed knitting structure (4) is greater than the loop length of the tight knitting structure (3). (2) Apply primer: Apply primer to the surface of the relaxed braided structure (4). The primer thickness is 0.03 to 0.08 mm. Pre-cur at 70 to 90°C for 3 to 8 minutes to form a primer locking layer (23). The primer partially penetrates into the coil gap of the relaxed braided structure (4). After curing, it forms an adhesive anchor with the coil and shapes the relaxed braided structure (4) into a wrinkled and undulating shape. (3) Applying a continuous elastomer: Using a computer-controlled multi-axis dispensing machine or a multi-touch dispensing machine, apply a continuous elastomer (2) to the base adhesive locking layer (23). The continuous elastomer (2) is a continuous mesh and includes multiple elastic ribs (21). Gas channels (22) are formed between adjacent elastic ribs (21). The continuous elastomer (2) covers the relaxed braided structure (4). The tightly braided structure (3) is retained between adjacent elastic ribs (21) as a gas channel. (4) Curing and shaping: The sock blank after applying continuous elastomer (2) is cured at 90-110℃ for 30-60 minutes, and then shaped at 120-140℃ for 30-60 seconds.
8. The knitting method for an anti-pilling and breathable sports sock according to claim 7, characterized in that, In step (1), 2 to 3 transition zones (5) with loops are set between the tightly knitted structure (3) and the loosely knitted structure (4). The loop length of the transition zone (5) gradually increases from the loop length of the tightly knitted structure (3) to the loop length of the loosely knitted structure (4). And / or, the loosely knitted structure (4) adopts a tuck-float composite structure: the base yarn is looped in each loop, the face yarn is looped in odd-numbered loops and tucked in even-numbered loops, and floats are formed at the positions of 3 consecutive needles in the second row.
9. The knitting method for an anti-pilling and breathable sports sock according to claim 7, characterized in that, In step (3), an unclosed surface groove (6) is imprinted on the surface of the elastic rib (21) of the continuous elastomer (2). The groove depth is 20% to 40% of the thickness of the continuous elastomer (2) and the width is 0.3 to 0.8 mm. The surface groove (6) extends along the length direction and width direction of the sock and is interconnected with each other, and is connected to the gas channel (22) between the elastomers.
10. A knitting method for anti-pilling and breathable sports socks according to claim 7, characterized in that, In step (3), phase change material microcapsules are mixed into the continuous elastomer (2). The phase change material microcapsules are paraffin microcapsules with a phase change temperature of 33°C and a particle size of 15-25 μm, accounting for 18%-20% of the total mass of the continuous elastomer (2); and / or, Shore A60-A70 elastomer is applied to the forefoot area (12), and Shore A25-A40 elastomer is applied to the heel area (14); and / or, the width of the gas channel (22) between the elastomers varies in gradient along the length of the sock, the distance between adjacent elastic ribs (21) at the center of the arch area (13) is 2.5 mm, and decreases to 1.2 mm towards the edges of the arch area (13).
Citation Information
Patent Citations
Anti-pilling shock-absorbing protective sports socks
CN209152389U