A polymeric prosthetic heart valve and method of forming the same
By combining rotary drying and hanging drying, the problem of uneven leaflet thickness during the impregnation process of polymer artificial heart valves was solved, thereby improving the uniformity of valve thickness and service life.
Patent Information
- Application Number
- CN202611636340.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-22
- Publication Date
- 2026-11-20
Smart Images

Figure CN123126987A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of artificial heart valve technology, and in particular to a method for molding a polymer artificial heart valve and its application. Background Technology
[0002] Valvular heart disease is mainly caused by rheumatic fever or degenerative changes leading to valvular lesions, resulting in stenosis or insufficiency of the valves, affecting the unidirectional flow of blood and endangering the patient's life. With the accelerating aging of the population, the proportion of elderly patients with degenerative valvular heart disease is increasing year by year, becoming a significant challenge in the cardiovascular field. Currently, valvular heart disease can be treated with valve repair or valve replacement, with valve replacement being the more widely used treatment method. Therefore, the artificial heart valves used for replacement play a crucial role.
[0003] There are two main types of artificial heart valves on the market: mechanical valves and bioprosthetic valves. Mechanical valves use pyrolytic carbon as leaflets and have a long service life (over 50 years), but require implantation through invasive open-heart surgery and lifelong anticoagulation therapy, and they also produce opening and closing noise. Bioprosthetic valves use biological tissues such as porcine or bovine pericardium as leaflets, allowing for valve replacement through less invasive interventional procedures. Patients only need to take anticoagulants for 3-6 months post-surgery. However, biological tissues are susceptible to structural degradation, resulting in a shorter service life (10-20 years), making them unsuitable for younger patients. To address the shortcomings of these two types of artificial heart valves, the fabrication of artificial heart valves using polymers has become a new trend. Through the design of materials, structures, and processes, polymeric artificial heart valves can possess excellent durability, biostability, and blood compatibility, establishing hemodynamics and blood flow similar to human heart valves. This supports catheter-based interventions and surgical treatments, greatly benefiting clinical patients.
[0004] In the fabrication of polymer artificial heart valves, various molding methods can be employed, including dip coating, spray coating, injection molding, and thin-film casting. Among these, dip coating offers high efficiency and facilitates the creation of integrated valve structures. However, during the dip coating process, the polymer solution is affected by gravity, causing it to converge and flow along the direction of gravity. Furthermore, the irregular shapes of the three leaflets mean that even with additional rotation along the horizontal axis, the solution tends to flow and converge at the concave surface of the mold, affecting the uniformity of leaflet thickness and making it difficult to achieve the desired leaflet thickness distribution.
[0005] Therefore, it is necessary to design an improved method for molding polymer artificial heart valves to improve the uniformity of valve leaflet thickness, ensure stable valve opening and closing movements, and reduce the risk of valve failure. Summary of the Invention
[0006] To address the aforementioned technical problems, this invention provides a polymer artificial heart valve and its molding method. After dip coating, the artificial heart valve of this invention employs a two-step drying method combining rotary drying and suspension drying during the drying stage. This method not only solves the problem of polymer solution accumulating and flowing away in the direction of gravity, but also effectively removes excess solution accumulated in the concave structure of the mold. The final molded valve leaflet has a relatively uniform thickness, which is beneficial to improving its service life.
[0007] To achieve this objective, the present invention adopts the following technical solution: In a first aspect, the present invention provides a polymeric artificial heart valve, the polymeric artificial heart valve comprising a stent, three leaflets, and a suture edge; the stent comprises a stent body and a base, the stent body having an internal hollow structure, the bottom end of the stent body being circular, and the upper end having three arc-shaped segments evenly distributed along the circumference and curving towards the base; the base is provided with a circular through hole, the base being connected to the suture edge by a suture line, and the leaflets comprising a leaflet free edge, a leaflet ventral side, and a leaflet fixed edge, the leaflet fixed edge being connected to the arc-shaped segments of the stent body.
[0008] In this invention, the polymer artificial heart valve is hollow, allowing the mold to pass through and achieve a tight fit between the mold and the stent. Moreover, the structure is simple, the valve is clearly divided, and the thickness is uniform, which can greatly improve the lifespan of the heart valve.
[0009] In this invention, the leaflet fixing edge and the support body are connected by integral molding, with the support encased within the leaflet material to form a single unit. During dip coating, the solution fills the micropores of the arc-shaped segment of the support and its outer surface. After the solvent evaporates and the polymer solidifies, the support is firmly locked inside the material.
[0010] Preferably, the vertical height of the bracket is 20-25 mm. This 20-25 mm can be, for example, 20 mm, 21 mm, 22 mm, 23 mm, 24 mm, or 25 mm.
[0011] Preferably, the arc segment is tangent to the horizontal line, and the endpoint plane of the arc segment is tangent to the vertical axis of the valve center.
[0012] Preferably, the diameter of the support body is 18-22 mm. The 18-22 mm can be, for example, 18 mm, 19 mm, 20 mm, 21 mm, or 22 mm.
[0013] Preferably, the thickness of the support body is 0.5-1 mm. The 0.5-1 mm can be, for example, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, or 1 mm.
[0014] Preferably, the material of the support body includes any one or a combination of at least two of polyetheretherketone, stainless steel, nickel-titanium alloy, cobalt-chromium alloy or polytetrafluoroethylene.
[0015] Preferably, the outer diameter of the suture edge is 40-44 mm, and the inner diameter is the same as the diameter of the support body. The 40-44 mm can be, for example, 40 mm, 41 mm, 42 mm, 43 mm, or 44 mm.
[0016] Preferably, the thickness of the stitched edge is 1-3 mm. The 1-3 mm can be, for example, 1 mm, 1.5 mm, 2 mm, 2.5 mm, or 3 mm.
[0017] Preferably, the material of the sewn edge includes any one or a combination of at least two of polyester, polytetrafluoroethylene, or polyurethane.
[0018] Preferably, the stitched edge extends radially outward from the bottom end of the support body.
[0019] Preferably, the number of circular through holes is 24-33. The number 24-33 can be, for example, 24, 27, 30, or 33.
[0020] Preferably, the diameter of the circular through hole is 0.4-0.8 mm. The 0.4-0.8 mm can be, for example, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, or 0.8 mm.
[0021] Preferably, the suture thread connects the suture edge and the base through a circular through-hole.
[0022] Preferably, the suture connection method includes backstitching and / or straight stitching.
[0023] Preferably, the material of the suture includes any one or a combination of at least two of polyester, polytetrafluoroethylene, or polyethylene.
[0024] Preferably, the base is made of any one or a combination of at least two of the following materials: polyetheretherketone, stainless steel, nickel-titanium alloy, cobalt-chromium alloy, or polytetrafluoroethylene.
[0025] Preferably, the base includes a ring structure.
[0026] Preferably, the inner diameter of the base is 19-24 mm and the outer diameter is 29-34 mm. The 19-24 mm can be, for example, 19 mm, 20 mm, 21 mm, 22 mm, 23 mm, or 24 mm. The 29-34 mm can be, for example, 29 mm, 30 mm, 31 mm, 32 mm, 33 mm, or 34 mm.
[0027] Preferably, the ratio of the vertical height of the leaflet to the outer radius of the base is 1:(1-1.4). The (1-1.4) can be, for example, 1, 1.1, 1.2, 1.3 or 1.4, etc.
[0028] Preferably, the angle between the fixed edge of the leaflet and the central axis of the valve is 15°-25°. The 15°-25° can be, for example, 15°, 16°, 17°, 18°, 19°, 20°, 21°, 22°, 23°, 24° or 25°, etc.
[0029] Preferably, the ratio of the free edge of the leaflet to the outer radius of the base is 1:(1.98-2.04). The (1.98-2.04) can be, for example, 1.98, 1.99, 2.00, 2.01, 2.02, 2.03, or 2.04, etc.
[0030] Preferably, the free edge of the leaflet is arc-shaped.
[0031] Preferably, the radius of the arc is 5π / 9-7π / 9. The 5π / 9-7π / 9 can be, for example, 5π / 9, 6π / 9, or 7π / 9, etc.
[0032] Preferably, the material of the leaflet includes any one or a combination of at least two of the following: polyether polyurethane, polyester polyurethane, polysiloxane polyurethane, polyisobutylene elastomer, polystyrene elastomer, or fiber-reinforced polymer material.
[0033] Preferably, the fiber type in the fiber-reinforced polymer material includes any one or a combination of at least two of polyester fibers, polytetrafluoroethylene fibers, or polyurethane fibers.
[0034] Preferably, the thickness of the leaflet is 100-500 μm; more preferably, it is 120-360 μm. The 100-500 μm thickness can be, for example, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm, 400 μm, 450 μm, or 500 μm. The 120-360 μm thickness can be, for example, 120 μm, 140 μm, 160 μm, 180 μm, 200 μm, 220 μm, 240 μm, 260 μm, 280 μm, 300 μm, 320 μm, 340 μm, or 360 μm, etc.
[0035] In a second aspect, the present invention provides a molding method for the polymer artificial heart valve described in the first aspect, the method comprising: (1) preheating and keeping the polymer solution warm after vacuum degassing; (2) assembling the mold from the bottom end of the polymer artificial heart valve stent to obtain the assembly, keeping the bottom end of the stent on top, and uniformly immersing it in the polymer solution obtained in step (1) in a vertical state, and letting it stand when the polymer solution has submerged the leaflet position; (3) after completing step (2) and resting, resetting the assembly and installing it onto the chuck of the rotating device, and rotating it around the horizontal axis in a self-rotating manner for drying; (4) after completing step (3) and rotating it for drying, hanging the stent with the bottom end facing upwards; (5) after completing step (4) and hanging it for drying, cutting the free edge of the leaflet, using suture thread through the suture hole to connect the suture edge and the stent base; the mold is a cylindrical structure, and the end of the cylinder that fits with the stent has a curve with the same shape as the arc segment.
[0036] The molding method of this invention first involves rotary drying. The mold is quickly turned horizontally and rotated, which effectively prevents the polymer solution from continuing to flow towards the solution outlet (opposite to the base, i.e., the direction of the petals) after dipping, thus preventing solution loss. Sufficient solution remains on the mold and gradually redistributes on the surface as the mold rotates. By setting appropriate drying temperature, rotation speed, and drying time, the solution can move on the mold at a suitable flow rate, which helps improve the thickness uniformity of the petals along the line connecting the center points, i.e., improves the thickness uniformity of the upper and lower parts of the petals.
[0037] The operating principle of suspension drying lies in the fact that, due to the irregular shape of the leaflets and their concave structure, the corresponding mold also possesses this structure. When the mold is adjusted to a horizontal position to begin the first stage of rotary drying, although the solution redistributes as the mold rotates, it cannot prevent the objective tendency for some edge solution to converge there. After the first stage of rotary drying ends, the solution flow at the leaflet edge points weakens, while the solvent in the concave structure areas has not yet fully escaped and remains more fluid. This means that there is too much solution in the concave structure areas of the mold. Direct and complete drying would result in a larger thickness at the center point compared to the edge points. At this point, the mold and support are rotated so that the solution outlet is facing downwards, and the second stage of suspension drying begins. By setting appropriate drying temperature and time, the solution achieves suitable viscosity and flow rate due to moderate solvent evaporation. Excess solution at the concave structure diffuses in the direction of gravity in the form of droplets, which can appropriately compensate for the solution lost by accumulating at the edge points towards the concave structure. Furthermore, it ensures that before the valve is completely dry, excess solution flows sufficiently outside the free edge curve of the leaflet, i.e., into the area where the leaflet tip should be cut, avoiding wrinkles in the leaflet area. As a result, both the edge and center points of the leaflet have relatively uniform thickness, improving the overall thickness uniformity of the valve.
[0038] Preferably, the preheating and heat preservation temperature is 20-30℃. This 20-30℃ can be, for example, 20℃, 22℃, 24℃, 26℃, 28℃, or 30℃.
[0039] Preferably, the mold is made of any one or a combination of at least two of polytetrafluoroethylene, stainless steel, or aluminum alloy.
[0040] Preferably, in step (2), the immersion speed is 50-200 mm / min. The 50-200 mm / min can be, for example, 50 mm / min, 100 mm / min, 150 mm / min or 200 mm / min.
[0041] Preferably, in step (2), the settling time is 1-3 minutes. The 1-3 minutes can be, for example, 1 minute, 1.5 minutes, 2 minutes, 2.5 minutes, or 3 minutes.
[0042] Preferably, the reset speed is 100-600 mm / min. The 100-600 mm / min can be, for example, 100 mm / min, 200 mm / min, 300 mm / min, 400 mm / min, 500 mm / min, or 600 mm / min.
[0043] Preferably, in step (3), the rotary drying temperature is 25-40℃, the time is 45-90 min, and the rotation speed is 50-120 rpm. The 25-40℃ can be, for example, 25℃, 26℃, 28℃, 30℃, 32℃, 34℃, 36℃, 38℃, or 40℃. The 45-120 min can be, for example, 45 min, 50 min, 55 min, 60 min, 65 min, 70 min, 75 min, 80 min, 85 min, or 90 min. The 50-120 rpm can be, for example, 50 rpm, 60 rpm, 70 rpm, 80 rpm, 90 rpm, 100 rpm, 110 rpm, or 120 rpm.
[0044] Preferably, in step (4), the hanging drying temperature is 50-60℃ and the time is 300-720 min. The 50-60℃ can be, for example, 50℃, 52℃, 54℃, 56℃, 58℃, or 60℃. The 300-720 min can be, for example, 300 min, 350 min, 400 min, 450 min, 500 min, 550 min, 600 min, 650 min, 700 min, or 720 min.
[0045] Compared with the prior art, the present invention has at least the following beneficial effects: The polymer artificial heart valve and its molding method provided by this invention innovatively combine two drying methods—rotary drying and suspension drying—in the drying film-forming process after dip coating. By adjusting the parameters of these two stages, it is possible to ensure that the valve achieves a certain expected thickness while improving the overall thickness uniformity of the valve, which is beneficial for valve opening and closing stability, achieving good hydrodynamics, and improving the service life of the valve. Attached Figure Description
[0046] Figure 1 This is a schematic diagram of the overall model of a polymer artificial heart valve.
[0047] Figure 2 This is a schematic diagram of a polymer artificial heart valve leaflet model.
[0048] Figure 3 This is a schematic diagram showing the connection between a polymer artificial heart valve mold and a stent.
[0049] Figure 4 This is a flowchart illustrating the molding process of a polymer artificial heart valve.
[0050] Figure 5 This is a schematic diagram of the main edge points of the leaflet of a polymer artificial heart valve.
[0051] Figure 6 This is a schematic diagram showing the main center points of the leaflets of a polymer artificial heart valve.
[0052] Among them, 1-polymer artificial heart valve, 11-valve stent, 12-valve leaflet, 13-valve suture edge, 21-free edge of leaflet, 22-lower abdomen of leaflet, 23-fixed edge of leaflet, 31-circular through hole, 32-mold, 41-left anterior edge point of leaflet, 42-right anterior edge point of leaflet, 43-left edge point of middle leaflet, 44-right edge point of middle leaflet, 45-bottom edge point of leaflet, 51-center point of anterior leaflet, 52-center point of middle leaflet. Detailed Implementation
[0053] The technical solution of the present invention will be further described below with reference to the accompanying drawings and specific embodiments. However, the following embodiments are merely simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention is determined by the claims.
[0054] Example 1 The polymeric artificial heart valve in this embodiment The polymeric artificial heart valve in this embodiment is as follows: Figure 1 As shown, the artificial heart valve includes a stent, leaflets, and suture edges. The stent comprises a stent body and a base. The base extends radially outward from the bottom of the stent body, with an outer diameter of 31.5 mm. The thickness of the suture edges is 1.5 mm. Thirty circular through-holes, each with a diameter of 0.5 mm, are arranged around the base. The stent is connected to the suture edges via sutures through these circular through-holes using a backstitch. The base has a ring structure with an inner diameter of 21.5 mm and an outer diameter of 31.5 mm.
[0055] The stent body has a hollow internal structure. The bottom of the stent body is circular with an inner diameter of 20 mm. The upper end consists of three evenly distributed, curved segments that bend towards the base, tangent to the horizontal line. The endpoints of the curved segments are tangent to the vertical axis of the valve center. The stent body is connected to the fixed edge of the valve leaflet. The vertical height of the stent is 22 mm, the inner diameter of the stent body is 20 mm, and the thickness is 0.75 mm.
[0056] The structure of the petals is as follows Figure 2 As shown, the leaflet includes the free side, the ventral side, and the fixed side. The ratio of the vertical height of the leaflet to the outer radius of the base is 1:1.2, the angle between the fixed side of the leaflet and the central axis of the valve is 20°, the ratio of the free side of the leaflet to the outer radius of the base is 1:2, and the radian of the free side of the leaflet is 2π / 3.
[0057] The support structure is made of polyetheretherketone, the seam edges are made of polyester, the sutures are made of polyester, and the leaflets are made of polyether polyurethane.
[0058] Preparation Example 1 This preparation example demonstrates the fabrication of a polymeric artificial heart valve. (1) Preparation of polymer solution Prepare a 25wt% polyether polyurethane solution, perform vacuum degassing on the solution, and then preheat and maintain the temperature at 25℃.
[0059] (2) Assemblies In this preparation example, the polymeric artificial heart valve of Example 1 was prepared. First, the stent and cylindrical mold were cleaned. Then, the mold was inserted from the bottom of the stent. The side of the mold that fits against the stent has a curve identical to the arc segment shape. This curve extends towards the solution outflow end (in the opposite direction to the base, i.e., the leaflet direction is the outflow end), forming a recessed mold surface to achieve a tight fit. Figure 3 As shown.
[0060] (3) Dipping With the bottom of the mold and support facing up and the leaflet facing down, immerse the mold and support in the polymer solution at a vertical speed of 100 mm / min. Once the polymer solution has submerged the leaflet, let it stand for 1 minute.
[0061] (4) First stage rotary drying After the dip coating is completed, the mold is reset at a speed of 100 mm / min. The mold is quickly removed and its clamping end (the end of the mold that is not attached to the support) is installed on the chuck of the rotating device. The first stage of rotational drying begins in the form of rotation around the horizontal axis at a speed of 90 rpm, a drying temperature of 30℃, and a drying time of 90 min.
[0062] (5) Second stage of hanging drying After completing the first stage of rotary drying, the mold and support are turned so that the solution outlet is facing down, and the second stage of hanging drying begins. The drying temperature is 50℃ and the drying time is 390 min to obtain the formed valve.
[0063] (6) Cutting After hanging to dry, trim the free edges of the leaflets, and use sutures to connect the sutured edges to the support base through the suture holes. Specific preparation steps are as follows: Figure 4 As shown.
[0064] Preparation Example 2 This preparation example is for the preparation of a polymeric artificial heart valve. The difference between this example and preparation example 1 is that the drying time in step (4) is 120 min and the drying time in step (5) is 420 min. The rest are the same as preparation example 1.
[0065] Preparation Example 3 This preparation example is for the preparation of a polymeric artificial heart valve. The difference between this example and preparation example 1 is that the drying time in step (4) is 60 min and the drying time in step (5) is 360 min. The rest are the same as preparation example 1.
[0066] Preparation Example 4 This preparation example is for the preparation of a polymeric artificial heart valve. The difference between this example and preparation example 1 is that the drying time in step (4) is 150 min and the drying time in step (5) is 480 min. The rest are the same as preparation example 1.
[0067] Comparative Preparation Example 1 This comparative example demonstrates the preparation of a polymeric artificial heart valve. The difference between this example and Example 1 is that the drying method used is suspension drying. The specific preparation method is as follows: Steps (1) to (3) are the same as in Preparation Example 1. Step (4) involves resetting the device at a speed of 600 mm / min after the dip coating is completed, and continuing to hang it for drying while keeping the solution outlet end facing down. The drying temperature is 50°C and the drying time is 300 min to obtain the molded valve. The rest is the same as in Preparation Example 1.
[0068] Comparative Preparation Example 2 This comparative example demonstrates the preparation of a polymeric artificial heart valve. The difference between this example and Example 1 is that the drying method used is rotary drying. The specific preparation method is as follows: Steps (1) to (3) are the same as in Preparation Example 1. Step (4) is to reset the mold at a speed of 100 mm / min after the dip coating is completed, quickly remove the mold and install its clamping end on the chuck of the rotating device, and start to rotate and dry around the horizontal axis in the form of rotation. The rotation speed is 90 rpm, the drying temperature is 30℃, and the drying time is 540 min to obtain the molded valve.
[0069] Test Example 1 Test Example 1 describes the detection of leaflet thickness in a fabricated polymeric artificial heart valve. The main edge points and center points of the leaflets are as follows: Figure 5 and Figure 6 As shown in the figure, in this test example, the thickness of the valve was measured at seven points: the left anterior edge, the right anterior edge, the left middle edge, the right middle edge, the bottom edge, the center of the front edge, and the center of the middle edge of each valve preparation example. The average thickness of the anterior edge, middle edge, bottom edge, anterior center, and middle center points was taken. The specific results are shown in Table 1.
[0070] Table 1
[0071] The results above show that: (1) By comparing Preparation Example 1 and Preparation Example 2, it can be seen that in Preparation Example 2, the average thickness of any leaflet of the valve is 297±57μm, and the average thicknesses of the front center point and the middle center point are 427±50μm and 400±58μm, respectively. This indicates that the longer the rotary drying time, the more solution remains in the concave structure of the leaflet. After drying, the solvent overflows, resulting in a larger thickness at the center point, i.e., a greater hardness, which is not conducive to the full opening of the leaflet. At the same time, the amount of solution flowing down during hanging drying is small, and the overall average thickness of the valve increases.
[0072] (2) By comparing Preparation Example 1 and Preparation Example 3, it can be seen that in Preparation Example 3, the average thickness of any leaflet of the valve is 265±11μm, and the average thicknesses of the front center point and the middle center point are 360±87μm and 347±6μm, respectively. The shorter the rotary drying time, the less solution remains in the concave structure of the leaflet, and the less the solvent overflows after drying, resulting in a smaller thickness at the center point. However, the amount of solution that flows off during hanging drying is greater, and the overall average thickness of the valve is reduced.
[0073] (3) By comparing preparation examples 1, 2, and 3 with preparation example 4, it can be seen that in preparation example 4, the average thickness of any leaflet of the valve is 321±84μm, and the average thickness of the front center point and the middle center point is 415±21μm and 425±64μm, respectively. This indicates that if the rotation drying time is too long, too much solution will remain in the concave structure of the leaflet, and more solvent will evaporate in the rotation state, resulting in increased solution viscosity and slower flow rate. After switching to suspension drying, it is more difficult to flow down and distribute evenly, and the average thickness and thickness difference of the leaflet will increase. In particular, the thickness of the middle center point is too large, which is extremely unfavorable for the valve to open fully.
[0074] (4) By comparing Preparation Example 1 with Comparative Preparation Example 1, it can be seen that in Comparative Preparation Example 1, the average thickness of any leaflet of the valve is 54±3μm. The results show that if only the hanging drying method is used, even if the reset speed is increased to 600 mm / min, the average thickness of any leaflet of the valve is still very thin, and none of them reach 100μm. That is, the solution is excessively lost due to gravity, and only a small amount of polymer solution adheres to the mold and the support. The valve cannot achieve the expected thickness target.
[0075] (5) By comparing Preparation Example 1 with Comparative Preparation Example 2, it can be seen that in Comparative Preparation Example 2, the average thickness of any leaflet of the valve is 319±99μm, and its average thickness and corresponding standard deviation are greater than the results of each example. It can be seen from the results that if only the rotary drying method is used, the average thickness of the leaflet will increase. This is mainly because too much solution accumulates at the concave structure of the mold, and this part of the solution cannot be evenly distributed on the mold, thus affecting the overall thickness uniformity of the valve.
[0076] During the dip-coating process with the polymer solution, regardless of whether the solution outlet is always at the top or bottom, the solution may be lost due to gravity, or it may easily lead to uneven thickness of the upper and lower parts of the leaflet after drying. Specifically, there are significant thickness differences between the three types of points: the front edge points 41 and 42 and the points near their connection, the middle edge points 43 and 44 and the points near their connection, and the bottom edge point 45. Changing to a rotational drying method along the horizontal axis can improve this unevenness to some extent. However, because the shape of the leaflet itself is irregular, during the mold rotation, the solution initially attached to the edge points of the leaflet tends to flow into the concave structure positions. That is, the points near the front edge points 41 and 43 and the points near their connection, the points near the front edge points 42 and 44 and the points near their connection, and the points near the front center point 51 and the middle center point 52 and the points near their connection, resulting in larger thickness at these points. The bottom edge point 45, which is farther from the concave structure, shows the least change. The molding method designed in this invention, in particular, the methods of preparation examples 1 and 3, can achieve good results. In the drying film formation process, a drying method of first rotating and then hanging drying is introduced, and the parameters of the two stages are controlled. The average thickness of any leaflet of the obtained valve is between 120-360 μm.
[0077] In summary, the artificial heart valve of the present invention, after being dip-coated, uses a two-step drying method combining rotary drying and hanging drying, which not only solves the problem of polymer solution accumulating and flowing away in the direction of gravity, but also effectively removes excess solution accumulated in the concave structure of the mold. The final formed valve leaflet has a relatively uniform thickness, which is beneficial to improving its service life.
[0078] The applicant declares that the above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.
Claims
1. A polymeric artificial heart valve, characterized in that, The polymer artificial heart valve includes a stent, three leaflets, and suture edges; The support includes a support body and a base. The support body has an internal hollow structure. The bottom of the support body is circular, and the top has three arc-shaped segments that are evenly distributed along the circumference and curve toward the base. The base is provided with a circular through hole, and the base is connected to the suture edge by a suture line. The leaflet includes a leaflet free edge, a leaflet ventral side, and a leaflet fixed edge. The leaflet fixed edge is connected to the arc segment of the support body.
2. The polymeric artificial heart valve according to claim 1, characterized in that, The vertical height of the bracket is 20-25 mm; The arc-shaped segment is tangent to the horizontal line, and the endpoint plane of the arc-shaped segment is tangent to the vertical axis of the valve center; The diameter of the support body is 18-22 mm; The thickness of the support body is 0.5-1 mm; The support is made of any one or a combination of at least two of the following materials: polyetheretherketone, stainless steel, nickel-titanium alloy, cobalt-chromium alloy, or polytetrafluoroethylene.
3. The polymeric artificial heart valve according to claim 1, characterized in that, The outer diameter of the suture edge is 40-44 mm, and the inner diameter is the same as the diameter of the support body; The thickness of the stitched edge is 1-3 mm; The material of the stitched edge includes any one or a combination of at least two of polyester, polytetrafluoroethylene, or polyurethane.
4. The polymeric artificial heart valve according to claim 1, characterized in that, The suture edge is located radially outward along the bottom end of the support body; The number of circular through holes is 24-33; The diameter of the circular through hole is 0.4-0.8 mm; The suture thread connects the suture edge and the base through a circular through-hole; The suture connection method includes backstitch and / or straight stitch; The material of the suture includes any one or a combination of at least two of polyester, polytetrafluoroethylene, or polyethylene. The base includes a ring structure; The base has an inner diameter of 19-24 mm and an outer diameter of 29-34 mm.
5. The polymeric artificial heart valve according to claim 1, characterized in that, The ratio of the vertical height of the leaflet to the outer radius of the base is 1:(1-1.4); The angle between the fixed edge of the leaflet and the central axis of the valve is 15°-25°; The ratio of the free edge of the leaflet to the outer radius of the base is 1:(1.98-2.04); The material of the leaflet includes any one or a combination of at least two of the following: polyether polyurethane, polyester polyurethane, polysiloxane polyurethane, polyisobutylene elastomer, polystyrene elastomer, or fiber-reinforced polymer material. The fiber-reinforced polymer material contains any one or a combination of at least two of polyester fibers, polytetrafluoroethylene fibers, or polyurethane fibers. The thickness of the leaflets is 100-500 μm.
6. The method for molding the polymer artificial heart valve according to claim 1, characterized in that, The method includes: (1) After vacuum degassing the polymer solution, preheat and keep it at a constant temperature; (2) Assemble the mold from the bottom of the polymer artificial heart valve stent to obtain the assembly. Keep the bottom of the stent on top and immerse it vertically and uniformly into the polymer solution obtained in step (1). When the polymer solution covers the leaflet position, let it stand. (3) After completing step (2), reset the assembly and install it onto the chuck of the rotating device. The assembly will then rotate around the horizontal axis to dry. (4) After completing step (3) of rotational drying, hang the support with the bottom end facing upwards for drying; (5) After completing step (4) and hanging to dry, cut off the free edge of the leaflet, use suture thread to pass through the suture hole, and connect the suture edge to the support base; The mold is a cylindrical structure, and the end of the cylinder that fits into the support has a curve that is the same shape as the arc segment.
7. The method for molding a polymer artificial heart valve according to claim 6, characterized in that, In step (1), the preheating and heat preservation temperature is 20-30℃; The mold is made of any one or a combination of at least two of the following materials: polytetrafluoroethylene, stainless steel, or aluminum alloy.
8. The method for molding a polymer artificial heart valve according to claim 6, characterized in that, In step (2), the immersion speed is 50-200 mm / min; In step (2), the settling time is 1-3 minutes.
9. The method for molding a polymer artificial heart valve according to claim 6, characterized in that, In step (3), the reset speed is 100-600 mm / min; In step (3), the temperature of the rotary drying is 25-40℃, the time is 45-90 min, and the rotation speed is 50-120 rpm.
10. The method for molding a polymer artificial heart valve according to claim 6, characterized in that, In step (4), the hanging drying temperature is 50-60℃ and the time is 300-720 min.