PLLA / PCL / PLLA-b-PCL / BaSO4 composite material and application thereof in preparation of shape memory vascular stent

By incorporating PLLA-b-PCL block copolymer and BaSO₄ into the PLLA/PCL matrix, shape memory vascular stents were fabricated, solving the problems of PLLA/PCL interfacial compatibility and X-ray imaging. This resulted in high mechanical properties and image visualization of the stent, making it suitable for peripheral small-diameter vascular interventional therapy.

CN123127481APending Publication Date: 2026-11-20JIANGNAN UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611316644.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing biodegradable vascular stent materials, such as PLLA/PCL, have poor interfacial compatibility, resulting in insufficient mechanical properties and weak X-ray absorption capacity, making them difficult to visualize under imaging equipment and affecting stent positioning and degradation monitoring.

Method used

Shape memory vascular stents were fabricated using 3 wt% to 5 wt% of PLLA-b-PCL block copolymer and 10 wt% to 30 wt% of BaSO₄ in a PLLA/PCL matrix via 3D printing. The combination of PLLA-b-PCL improved interfacial compatibility, while BaSO₄ provided X-ray imaging capability.

Benefits of technology

It improves the flexibility, fatigue resistance, and X-ray imaging capability of the stent, enabling precise stent positioning and postoperative monitoring. It also has shape memory function, meeting the requirements of peripheral small-diameter vascular interventional therapy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123127481A_ABST
    Figure CN123127481A_ABST
Patent Text Reader

Abstract

The application discloses a PLLA / PCL / PLLA-b-PCL / BaSO4 composite material and application thereof in preparation of a shape memory vascular stent. By introducing a block copolymer as a compatibilizer, the interfacial compatibility and comprehensive mechanical properties of the PLLA / PCL blending system are improved. Meanwhile, barium sulfate (BaSO4) is added as an inorganic developing agent to endow the stent with good X-ray developing capacity, realize accurate positioning in operation and long-term image follow-up after operation, and provide a new technical scheme for interventional treatment of vascular diseases.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of implantable medical devices and biomedical materials technology, specifically relating to a PLLA / PCL / PLLA-b-PCL / BaSO4 composite material and its application in the preparation of shape memory vascular stents. Background Technology

[0002] Interventional stent implantation is an important method for treating peripheral vascular stenosis and occlusion. While traditional bare-metal stents (BMS) and drug-eluting stents (DES) can restore vascular patency, their permanent implantation can lead to decreased vascular compliance, chronic inflammation, late-stage thrombosis, and stent fracture. Biodegradable vascular stents (BVS), which gradually degrade and are absorbed after fulfilling their vascular support function, provide conditions for vascular tissue repair and functional recovery, and have therefore become an important research direction in the field of interventional vascular surgery in recent years.

[0003] Polylactic acid (PLLA) possesses excellent biocompatibility, biodegradability, and high mechanical strength, making it the most widely used biodegradable vascular stent material. However, PLLA exhibits poor toughness and brittleness, particularly prone to fatigue damage under prolonged bending and compressive loads in small-diameter peripheral vessels, affecting the long-term stability of the stent. Polycaprolactone (PCL) offers good flexibility and can be used to improve the toughness of PLLA; however, due to poor interfacial compatibility, direct blending of the two materials easily leads to phase separation, resulting in insufficient interfacial bonding and impacting the overall mechanical and processing properties of the material. Therefore, improving the compatibility of PLLA / PCL blends is a key issue in biodegradable vascular stent research. Furthermore, PLLA and PLLA / PCL polymers have weak X-ray absorption, making them difficult to visualize under digital subtraction angiography (DSA) and other imaging equipment. This leads to difficulties in stent placement during implantation and long-term imaging follow-up of stent position and degradation processes, limiting their clinical application.

[0004] In summary, to meet the clinical needs of vascular interventional therapy, there is an urgent need to develop a 3D-printed biodegradable vascular stent that combines excellent mechanical properties, biodegradability, and imaging visualization capabilities. Summary of the Invention

[0005] The purpose of this section is to outline some aspects of embodiments of the present invention and to briefly describe some preferred embodiments. Simplifications or omissions may be made in this section, as well as in the abstract and title of this application, to avoid obscuring the purpose of these documents; however, such simplifications or omissions should not be construed as limiting the scope of the invention.

[0006] In view of the problems existing in the above and / or prior art, the present invention is proposed.

[0007] Therefore, the purpose of this invention is to overcome the shortcomings of the prior art and provide a PLLA / PCL / PLLA-b-PCL / BaSO4 composite material.

[0008] To solve the above-mentioned technical problems, the present invention provides the following technical solution: the composite material uses a PLLA / PCL system composed of L-polylactic acid and polycaprolactone as the matrix, and further includes, Compared to PLLA / PCL matrix, the block copolymer PLLA-b-PCL contains 3wt% to 5wt% of the matrix and BaSO4 contains 10wt% to 30wt% of the matrix.

[0009] As a preferred embodiment of the PLLA / PCL / PLLA-b-PCL / BaSO4 composite material of the present invention, wherein the mass ratio of L-polylactic acid to polycaprolactone is X:100-X, and X is 70-90.

[0010] As a preferred embodiment of the PLLA / PCL / PLLA-b-PCL / BaSO4 composite material of the present invention, the composite material is prepared by mixing the L-polylactic acid, polycaprolactone, block copolymer PLLA-b-PCL and BaSO4 composite material in an organic solvent, removing the organic solvent by evaporation, and then vacuum drying.

[0011] As a preferred embodiment of the PLLA / PCL / PLLA-b-PCL / BaSO4 composite material of the present invention, the stirring is carried out continuously at 200~500 r / min for 6~12 h.

[0012] As a preferred embodiment of the PLLA / PCL / PLLA-b-PCL / BaSO4 composite material of the present invention, the volatilization time is ≥24h.

[0013] As a preferred embodiment of the PLLA / PCL / PLLA-b-PCL / BaSO4 composite material of the present invention, the vacuum drying is performed by continuing vacuum drying in a vacuum oven at 30~40℃ for 24~48 h.

[0014] Another object of the present invention is to provide an application of PLLA / PCL / PLLA-b-PCL / BaSO4 composite material in the preparation of shape memory vascular stents.

[0015] To solve the above-mentioned technical problems, the present invention provides the following technical solution: The PLLA / PCL / PLLA-b-PCL / BaSO4 composite material is shredded into small particles of 3-5 mm in size and used as printing material. It is then melted in the heating chamber of a direct-write or fused deposition modeling 3D printing device and printed back and forth on a rotating receiving axis through a printing nozzle to form a vascular stent preform with an interwoven structure. The preform is then vacuum dried and shaped, and the shape memory vascular stent is obtained by removing it from the axis.

[0016] As a preferred embodiment of the application of the PLLA / PCL / PLLA-b-PCL / BaSO4 composite material described in this invention in the preparation of shape memory vascular stents, wherein the temperature of the heating chamber of the 3D printing equipment is 160~190℃.

[0017] As a preferred embodiment of the application of the PLLA / PCL / PLLA-b-PCL / BaSO4 composite material described in this invention in the preparation of shape memory vascular stents, wherein: the moving speed of the printing nozzle is 3~5 mm / s, and the rotational speed of the rotating receiving shaft is 20~40 r / min.

[0018] This is a preferred embodiment of the application of the PLLA / PCL / PLLA-b-PCL / BaSO4 composite material described in this invention in the preparation of shape memory vascular stents, wherein: the shape memory vascular stent is compressed to 50% strain at 65°C, cooled to 0°C while maintaining the strain, and then unloaded, and its shape fixation rate is measured to be ≥95% and its shape recovery rate is ≥94%.

[0019] Beneficial effects of this invention: (1) Using PLLA / PCL blend system as scaffold matrix, the flexibility and fatigue resistance of scaffold are improved while ensuring the biocompatibility and degradability of the material. By introducing PLLA-b-PCL block copolymer as compatibilizer, the interfacial compatibility of PLLA / PCL phases can be effectively improved, phase separation phenomenon can be reduced, and the tensile strength, elongation at break and radial support performance of the material can be improved. By adding nano barium sulfate (BaSO4) as inorganic contrast agent, while ensuring the comprehensive mechanical properties and degradation performance of the material, the scaffold is endowed with good X-ray imaging ability, which can realize precise intraoperative positioning and long-term postoperative imaging follow-up.

[0020] (2) The present invention uses additive manufacturing 4D printing technology to prepare vascular stents, which can realize precise control of stent structural parameters and personalized manufacturing, while reducing material waste.

[0021] (3) The PLLA / PCL / PLLA-b-PCL / BaSO4 composite system constructed in this invention has excellent mechanical properties, biodegradability, X-ray imaging properties, shape memory function and 4D printing molding properties, which can meet the requirements of peripheral small-diameter vascular interventional therapy for the comprehensive performance of vascular stents. Attached Figure Description

[0022] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. Wherein: Figure 1 This is a schematic diagram of the vascular stent structure prepared in Embodiment 1 of the present invention.

[0023] Figure 2 X-ray imaging results of the stent with different BaSO4 addition amounts.

[0024] Figure 3 Scanning electron microscope (SEM) images of composite materials with different PLLA-b-PCL addition amounts.

[0025] Figure 4 The radial compression performance test results are for the brackets prepared in Examples 1 to 3 and Comparative Examples 1, 3 to 4.

[0026] Figure 5 The results are the shape memory performance test results of the scaffold prepared in Example 1 of the present invention. Detailed Implementation

[0027] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the examples in the specification.

[0028] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.

[0029] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The phrase "in one embodiment" appearing in different places in this specification does not necessarily refer to the same embodiment, nor is it a single or selective embodiment that is mutually exclusive with other embodiments.

[0030] Unless otherwise specified, all raw materials used in this invention are commercially available in the art, wherein: Polylactic acid (PLLA) was purchased from Chengdu Nanding Medical Materials Co., Ltd., and the block copolymer (lactide-caprolactone copolymer, PLLA-b-PCL) was purchased from Xi'an Qiyue Biotechnology Co., Ltd., catalog number Q-0342521. Barium sulfate (BaSO4) was purchased from Leyan Reagent Co., Ltd., CAS number 727-43-7, product number 1042800. Dichloromethane (DCM) and polycaprolactone (PCL) were both purchased from Shanghai Titan Technology Co., Ltd. All raw materials except PLLA-b-PCL were dried at 35°C before use.

[0031] The experimental instruments used in this invention include: a field emission scanning electron microscope (FE-SEM, Sigma300, Carl Zeiss Co., Germany) for observing foam morphology; a universal testing machine (UTM2203, SanshiZongheng Technology Co., Ltd., China) for testing compression performance; a dynamic mechanical analyzer (DMA, Q800, TA Instruments, USA) for determining shape memory performance; a digital subtraction angiography system (DSA, Philips); and a four-axis bio-3D printer. The shape memory properties of the foam were evaluated using a dynamic mechanical analyzer (DMA) through thermomechanical cycling tests. The scaffolded samples were compressed to 50% strain at 65°C (Thigh), cooled to 0°C (Tlow) while maintaining the strain, and then unloaded. The shape retention rate (Rf) was measured. The support sample was subjected to a compression test using a universal testing machine at a compression rate of 5 mm / min. Example 1

[0032] This embodiment provides a method for preparing PLLA / PCL / PLLA-b-PCL / BaSO4 composite materials, specifically: 1) Weigh 10.0 g of polylactic acid (PLLA, Mw=600000 g / mol) and 4.3 g of polycaprolactone (PCL, Mw=50000 g / mol) as matrix materials, add 0.572 g of PLLA-b-PCL block copolymer (4wt% of the total mass of PLLA / PCL) and 4.29 g of nano-barium sulfate (BaSO4, 30 wt% of the total mass of PLLA / PCL), and add an amount of dichloromethane sufficient to dissolve each component. Place the resulting mixture in a magnetic stirrer and stir continuously at 300 r / min for 6 h to fully disperse PLLA, PCL, PLLA-b-PCL block copolymer and nano-barium sulfate to form a uniform premix.

[0033] 2) Pour the premixed liquid into a polytetrafluoroethylene mold and let it stand at room temperature for 24 h to allow the organic solvent to evaporate naturally. After evaporation, place the sample in a vacuum oven at 35℃ and continue to vacuum dry for 24 h to completely remove the residual organic solvent and obtain a uniform PLLA / PCL / PLLA-b-PCL / BaSO4 composite material.

[0034] 3) The obtained PLLA / PCL / PLLA-b-PCL / BaSO4 composite material was shredded into small particles of approximately 4 mm in size and added to the fused deposition modeling (FDM) 3D printer barrel as printing material. The mixture was preheated at 170 °C for 15-20 min before printing. The printer parameters were designed as follows: The nozzle diameter is 0.35mm, the layer height is 0.2mm, the barrel temperature is 170℃, the print head temperature is 185℃, the printing speed is 80mm / min, and the cylindrical rotating shaft with a diameter of 3mm is used for cylindrical printing.

[0035] The scaffold is designed with a rhomboid cell-like structure, such as Figure 1 As shown in (a), the length is 15.13 mm, the diameter is approximately 3.5 mm, the fiber angle is 60°, and the number of intersections is 4. The printed image is as follows. Figure 1 As shown in (b), after the scaffold is prepared, it is dried, sealed, and refrigerated, and designated as PC4-B. 30 .

[0036] A 90-day early degradation experiment was conducted on the stent of this embodiment. The results showed that the composite material could still maintain the core performance required for vascular stent use during the 90-day early degradation window. Example 2

[0037] The difference between this embodiment and Example 1 is that the amount of nano-barium sulfate in step 1) is adjusted to 1.43 g (accounting for 10 wt% of the total mass of PLLA / PCL). The remaining steps are the same as in Example 1, and the PLLA / PCL / PLLA-b-PCL / BaSO4 composite material of this embodiment is obtained, denoted as PC4-B. 10 . Example 3

[0038] The difference between this embodiment and Example 1 is that the amount of nano-barium sulfate in step 1) is adjusted to 2.86 g (accounting for 20 wt% of the total mass of PLLA / PCL). The remaining steps are the same as in Example 1, and the PLLA / PCL / PLLA-b-PCL / BaSO4 composite material of this embodiment is obtained, denoted as PC4-B. 20 . Comparative Example 1

[0039] The difference between this comparative example and Example 1 is that in step 1), PLLA-b-PCL block copolymer and nano-barium sulfate are not added. The remaining steps are the same as in Example 1, except that only the PLLA / PCL composite material is prepared, which is denoted as PC-Neat. Comparative Example 2

[0040] The difference between this comparative example and Example 1 is that nano-barium sulfate is not added in step 1), while the remaining steps are the same as in Example 1, and the PLLA / PCL composite material is prepared and denoted as PC4.

[0041] Figure 2 X-ray imaging of the scaffold with different BaSO4 addition amounts. Figure 2 (a) is a quantitative graph of the imaging intensity of the scaffold. Figure 2 (b) is a DSA photograph. It can be seen that the stents prepared in Examples 1 to 3 containing barium sulfate all have good development effect. The structure of the stent can be clearly seen under DSA. However, the PC4 stent in Comparative Example 2 without barium sulfate has no development effect under DSA. Comparative Example 3

[0042] The difference between this comparative example and Example 1 is that in step 1), no nano-barium sulfate is added, and the amount of PLLA-b-PCL block copolymer added is adjusted to 0.429 g (accounting for 3 wt% of the total mass of PLLA / PCL). The remaining steps are the same as in Example 1. The PLLA / PCL / PLLA-b-PCL composite material is prepared and denoted as PC3. Comparative Example 4

[0043] The difference between this comparative example and Example 1 is that in step 1), no nano-barium sulfate is added, and the amount of PLLA-b-PCL block copolymer added is adjusted to 0.715g (accounting for 5 wt% of the total mass of PLLA / PCL). The remaining steps are the same as in Example 1. The PLLA / PCL / PLLA-b-PCL composite material is prepared and denoted as PC5.

[0044] Figure 3 The images show the scanning electron microscope (SEM) morphology of the composite materials with different amounts of PLLA-b-PCL added in Comparative Examples 1 to 4 without BaSO4. It can be seen that the samples without compatibilizer exhibit a typical "island structure," with weak interfacial bonding between PLLA and PCL and obvious phase separation. With the introduction of PLLA-b-PCL, the dispersed phase size gradually decreases, and the interface contour becomes blurred. Among these, sample PC4 shows the most continuous two-phase interface, significantly refined particle size, and near-complete disappearance of interfacial voids. Comparative Example 5

[0045] The difference between this comparative example and Example 1 is that the amount of nano-barium sulfate in step 1) is adjusted to 5.72 g (accounting for 40 wt% of the total mass of PLLA / PCL). The remaining steps are the same as in Example 1, and the PLLA / PCL / PLLA-b-PCL / BaSO4 composite material of this example is obtained, denoted as PC4-B. 40 .

[0046] Figure 4 The radial compression performance test results of the stents prepared in Examples 1-3 and Comparative Examples 1, 3-5 show that the radial stiffness of the PC-Neat stent at 50% compressive strain is 78.66 mN / mm, and that of the PC4-B stent is... 30 The value of the stent under the same strain increased to 384.16 mN / mm, and the radial strength increased by about 5 times, showing the significant reinforcing effect of compatibilizer and barium sulfate on the blend system. However, the results showed that the mechanical properties began to decline when the content of BaSO4 was further increased to 40 wt%.

[0047] Figure 5 The results are the shape memory performance test results of the scaffold prepared in Embodiment 1 of the present invention. Figure 5 (a) shows the fixation rate (Rf) and recovery rate (Rr) of the stent. It can be seen that Rf is higher than 95% and Rr is higher than 94%. Figure 5 (b) is a physical image of the scaffold's shape memory fixation-deformation-recovery process. The scaffold remains structurally stable during the shape memory process, and its shape after recovery is not significantly different from the initial shape, demonstrating excellent shape memory performance. The shape memory performance test results of other embodiments are comparable to those of Embodiment 1.

[0048] Furthermore, to improve the interfacial compatibility between polylactic acid (PLA) and polycaprolactone (PCL) blends, this invention also explored the use of polypropylene glycol diglycidyl ether (PPGDGE) and cashew nut shell powder (CD) as compatibilizers. PPGDGE can undergo ring-opening reactions with the carboxyl or hydroxyl groups at the ends of the polyester chain through epoxy groups, achieving chain extension or branching, thereby improving the interfacial bonding between PLA and PCL. CD can form a bridging structure at the interface between the two phases through esterification and free radical polymerization, thereby reducing the degree of phase separation. However, after participating in the reaction, PPGDGE and CD may remain inside the material as unreacted small molecules, oligomers, or reaction byproducts. During the long-term contact and gradual degradation of the stent with blood and vascular tissue, these substances may have a potential impact on the local cellular microenvironment. In contrast, the molecular chain of PLLA-b-PCL itself is composed of PLLA and PCL segments, exhibiting higher structural relevance in the application of vascular stent bulk materials.

[0049] In addition, this invention has also attempted to use elemental iodine or iodine-containing organic compounds as contrast agents. However, these contrast agents still have certain limitations in practical applications. When using elemental iodine as a contrast agent, it is easily affected by factors such as material composition, dosage, and dispersion state. When the iodine content is low, the contrast of the vascular stent under imaging equipment is insufficient, making it difficult to clearly identify the stent outline, stent position, and stent release state. On the other hand, increasing the amount of iodine added has an adverse effect on the processing performance, mechanical properties, and structural stability of the stent material. When using iodine-containing organic compounds such as 2,3,5-triiodobenzoic acid as a contrast agent, these compounds have a high iodine content, which can improve the X-ray visualization performance of the material to a certain extent. However, there are shortcomings in the biosafety of using them as contrast agents for vascular stents in the long term.

[0050] Therefore, existing contrast agents and compatibilizers suffer from a trade-off between imaging performance and biocompatibility, exhibiting potential cytotoxicity and insufficient biocompatibility. This application utilizes the synergistic effect of PLLA-b-PCL compatibilizer and barium sulfate contrast agent as a vascular stent imaging material that combines excellent X-ray imaging performance, good dispersion stability, and biocompatibility. This is of great significance for improving the imaging visualization level of intraoperative stent positioning, release status observation, and postoperative follow-up.

[0051] In summary, this invention develops a biodegradable composite material possessing high mechanical properties, X-ray imaging capabilities, and shape memory properties, which can be used to prepare novel 3D-printed biodegradable vascular stents. This composite material uses poly-L-lactic acid (PLLA) and polycaprolactone (PCL) as the matrix, improves the interfacial bonding between the two phases by introducing a PLLA-b-PCL block copolymer as a compatibilizer, and adds nano-barium sulfate as an X-ray imaging agent. Simultaneously, the material exhibits shape memory properties, providing a new technical solution for the design and clinical application of biodegradable vascular stents. Based on the composition and performance characteristics of this composite material, it has the following advantages: (1) Compatibilizer enhances interfacial bonding and improves the radial support performance of the stent. This invention uses a PLLA-b-PCL block copolymer as a compatibilizer. On one hand, it effectively improves the interfacial compatibility between the PLLA and PCL phases, promoting the formation of a stable and homogeneous composite system, reducing phase separation, and increasing interfacial bonding strength. On the other hand, it improves the dispersion of nano-BaSO4 within the polymer matrix and inhibits the aggregation of inorganic fillers. The resulting scaffold exhibits higher radial support and superior mechanical stability, effectively resisting vascular retraction while maintaining the normal vascular lumen diameter, thus providing reliable mechanical support for diseased vessels.

[0052] (2) The contrast agent gives the stent excellent X-ray imaging function, enabling precise intraoperative positioning. By introducing nano-barium sulfate as an X-ray contrast agent into the composite material, and ensuring good dispersion with a compatibilizer, 10-30 wt% BaSO4 not only provides X-ray imaging but also acts as a reinforcing filler, significantly improving the radial support of the stent. The introduction of BaSO4 significantly enhances the stent's X-ray absorption capacity, resulting in excellent imaging performance under medical imaging equipment such as DSA. During the procedure, surgeons can observe the stent's position, deployment, and apposition to the vessel wall in real time, improving the accuracy and safety of stent implantation. It also facilitates postoperative follow-up monitoring of stent degradation and vascular recovery.

[0053] (3) Shape memory performance provides a new scaffold deployment method and improves implantation safety. The composite material prepared in this invention possesses excellent shape memory properties, allowing it to be pre-processed into a compressed state and maintain a temporary shape. After implantation into the diseased blood vessel, external thermal stimulation triggers the material to return to its preset shape, achieving autonomous stent deployment and wall-adhering support. Compared to traditional deployment methods relying on balloon dilation or self-expanding metal stents, this invention provides a novel stent deployment scheme based on the shape memory effect, which can reduce mechanical damage to the vascular wall during implantation, improve stent deployment uniformity and wall-adhering effect, and is beneficial for complex lesions and minimally invasive interventional treatments.

[0054] Furthermore, this invention utilizes a PLLA / PCL biodegradable system as the scaffold matrix, which gradually degrades and is absorbed after completing its vascular repair function, avoiding the chronic inflammation and long-term complications associated with permanent implants. Combined with 4D printing technology, it also allows for personalized manufacturing based on the patient's vascular size and lesion characteristics, improving stent size matching and therapeutic efficacy.

[0055] In summary, this invention achieves comprehensive improvements in radial support performance, intraoperative visualization, and novel deployment methods for biodegradable vascular stents through the synergistic effect of three key technologies: compatibilizer enhancement, imaging function imparting, and shape memory regulation. It provides a new material system and technical path for the research and development and clinical application of next-generation intelligent biodegradable vascular stents.

[0056] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.

Claims

1. A PLLA / PCL / PLLA-b-PCL / BaSO4 composite material, characterized in that: The composite material uses a PLLA / PCL system composed of L-polylactic acid and polycaprolactone as the matrix, and also includes, Compared to PLLA / PCL matrix, the block copolymer PLLA-b-PCL contains 3wt% to 5wt% of the matrix and BaSO4 contains 10wt% to 30wt% of the matrix.

2. The PLLA / PCL / PLLA-b-PCL / BaSO4 composite material as described in claim 1, characterized in that: The mass ratio of L-polylactic acid to polycaprolactone is X:100-X, where X is 70-90.

3. The PLLA / PCL / PLLA-b-PCL / BaSO4 composite material as described in claim 1, characterized in that: The composite material is prepared by mixing the L-polylactic acid, polycaprolactone, block copolymer PLLA-b-PCL and BaSO4 composite material in an organic solvent, removing the organic solvent by evaporation, and then vacuum drying.

4. The PLLA / PCL / PLLA-b-PCL / BaSO4 composite material as described in claim 3, characterized in that: The stirring is performed continuously at 200~500 r / min for 6~12 h.

5. The PLLA / PCL / PLLA-b-PCL / BaSO4 composite material as described in claim 3, characterized in that: Evaporation time ≥ 24h.

6. The PLLA / PCL / PLLA-b-PCL / BaSO4 composite material as described in claim 3, characterized in that: The vacuum drying process involves continuing vacuum drying in a vacuum oven at 30-40°C for 24-48 hours.

7. The application of the PLLA / PCL / PLLA-b-PCL / BaSO4 composite material as described in any one of claims 1 to 6 in the preparation of shape memory vascular stents, characterized in that: include, The PLLA / PCL / PLLA-b-PCL / BaSO4 composite material is shredded into small particles of 3-5 mm in size and used as printing material. It is then melted in the heating chamber of a direct-write or fused deposition modeling 3D printing device and printed back and forth on a rotating receiving axis through a printing nozzle to form a vascular stent preform with an interwoven structure. The preform is then vacuum dried and shaped, and the shape memory vascular stent is obtained by removing it from the axis.

8. The application of the PLLA / PCL / PLLA-b-PCL / BaSO4 composite material as described in claim 7 in the fabrication of shape memory vascular stents, characterized in that: The temperature of the heating chamber of the 3D printing equipment is 160~190℃.

9. The application of the PLLA / PCL / PLLA-b-PCL / BaSO4 composite material as described in claim 7 in the fabrication of shape memory vascular stents, characterized in that: The moving speed of the printing nozzle is 3 to 5 mm / s, and the rotational speed of the rotating receiving shaft is 20 to 40 r / min.

10. The application of the PLLA / PCL / PLLA-b-PCL / BaSO4 composite material as described in claim 7 in the fabrication of shape memory vascular stents, characterized in that: The shape memory vascular stent was compressed to 50% strain at 65°C, cooled to 0°C while maintaining the strain, and then unloaded. Its shape fixation rate was measured to be ≥95%, and its shape recovery rate was ≥94%.