A superlubricant durable coating composition for puncturing medical instruments and its preparation method and application
By forming a self-layering coating on puncture medical devices and utilizing the combination mechanism of epoxy resin and silane coupling agent, the adhesion and interlayer bonding problems of existing coatings under high temperature and high pressure sterilization and long-term immersion environments are solved, achieving efficient and long-lasting lubrication performance and a simplified preparation process.
Patent Information
- Application Number
- CN202611324140.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-20
AI Technical Summary
The lubricating coatings of existing puncture medical devices have insufficient adhesion and poor interlayer bonding under moist heat sterilization and long-term liquid immersion conditions. Furthermore, the preparation process is complex, making it difficult to meet the stringent requirements of high-temperature and high-pressure sterilization and long-term immersion in anticoagulants.
A super-lubricating and durable coating composition is used to form a self-layered structure through a single dip coating. It utilizes the hydrogen bonding between epoxy resin and metal substrate and the covalent bonding between silane coupling agent, combining the dual mechanisms of chemical anchoring and physical binding to ensure strong adhesion between the coating and the substrate. Furthermore, the interpenetrating network structure formed by the gradient distribution of epoxy resin and organosilicon components improves the durability of lubrication performance.
It achieves stable puncture force under high temperature and high pressure sterilization and long-term anticoagulant immersion conditions, with a maximum puncture force ≤0.8 N, good lubrication performance, and a lubrication performance change rate ≤15%, meeting stringent usage requirements. Furthermore, the process is simplified and the cost is reduced.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of medical materials and surface treatment technology for medical devices, specifically relating to a super-lubricating and durable coating composition for puncture medical devices, its preparation method, and its application. This coating is particularly suitable for medical devices such as blood bags and blood collection needles that require long-term immersion in moist heat sterilization and anticoagulants. Background Technology
[0002] Medical puncture devices (such as blood collection needles, intravenous catheters, and injection needles) require repeated punctures of rubber stoppers or patient skin during use, thus placing high demands on their surface lubrication. Good lubrication can effectively reduce puncture resistance, alleviate patient pain, and minimize tissue damage. In actual clinical practice, injection needles often require puncturing the rubber stopper to extract the medication before puncturing the patient's skin; blood collection needles must undergo high-temperature, high-pressure, and moist heat sterilization (typically 115°C for 30 minutes) and are subject to reflux immersion in anticoagulants (such as sodium citrate or heparin solution) during use. These multiple stringent usage conditions pose an extremely serious challenge to the durability of the coating.
[0003] Currently, lubricating coatings used for puncture instruments can be mainly divided into the following two categories:
[0004] The first type is a single-layer silicone oil coating, with two representative schemes: one is to directly apply inert silicone oils such as dimethyl silicone oil to the instrument surface, relying on physical adsorption for adhesion; the other is to directly blend reactive and non-reactive silicone oils and then coat them into a film in one step. The former has a simple process and good initial lubrication, but the bonding force between the silicone oil and the substrate is extremely weak. After high-temperature, high-pressure, and moist heat sterilization and long-term immersion in anticoagulants, it is prone to migration, elution, or dissolution, leading to a rapid decline in lubrication performance. The latter attempts to improve adhesion by introducing reactive silicone oil and relying on chemical bonding, but it has obvious limitations in practical applications: high-activity silicone oil has poor storage stability, making it difficult to meet the shelf-life requirements of industrial production; while low-activity silicone oil has insufficient bonding efficiency with the substrate, resulting in limited improvement in adhesion. More importantly, this system lacks the support of a high-adhesion primer layer. Even if some reactive silicone oil bonds, it is difficult to form a dense cross-linked network, and non-reactive silicone oil is still prone to loss, failing to fundamentally solve the problem of insufficient lubrication durability.
[0005] The second type is a multi-layer composite coating consisting of epoxy resin primer and silicone oil topcoat. That is, epoxy resin primer is first applied to enhance the adhesion to the substrate, and then silicone topcoat is applied to give the surface lubrication properties. Although this solution improves the adhesion of the silicone oil layer to a certain extent, it still has the following defects: (1) The multi-layer coating process is complicated, the production efficiency is low, and the cost is high; (2) The primer and topcoat are only physically bonded, and interlayer peeling is prone to occur under humid heat sterilization and long-term immersion conditions; (3) The lubricating layer of the topcoat is still mainly physically adhered, and the improvement in durability is limited.
[0006] In summary, existing single-layer silicone oil coatings have failed to effectively solve the fundamental problem of insufficient adhesion, while two-layer coating systems are limited by bottlenecks such as weak interlayer bonding, complex processes, and high costs. Therefore, there is an urgent need to develop a new coating system that combines strong adhesion and long-lasting lubrication performance. Summary of the Invention
[0007] In view of this, the purpose of this invention is to address the technical problems of insufficient lubrication durability, poor interlayer bonding, and complex preparation process of existing lubricating coatings under moist heat sterilization and long-term liquid immersion environments, and to provide a self-layering super-lubricating durable coating that integrates the functions of a primer layer and a lubricating layer, as well as its preparation method. This coating achieves a spontaneous gradient structure on the surface of medical devices through a single dip coating process (advantages: single coating, one-step molding, no need for multiple layers, simple operation and high production efficiency). The bottom layer is enriched with epoxy resin to achieve a strong bond with the pretreated metal substrate (physical bonding: hydrogen bond adsorption; chemical bonding: Si-O-Fe covalent bonds formed by silane coupling agents). The middle layer (tiered gradient structure: epoxy resin and organosilicon components are continuously gradient distributed to eliminate interlayer interface defects and avoid peeling risks) and the surface layer is enriched with terminal epoxy reactive silicone oil and non-reactive silicone oil to provide a dual lubrication mechanism of chemical anchoring and physical supplementation. This ensures that the coating adheres firmly to the substrate while achieving ultra-low maximum puncture force and ultra-long lubrication life, meeting the stringent requirements of 115°C moist heat sterilization and long-term anticoagulant immersion.
[0008] To achieve this objective, the present invention adopts the following technical solution:
[0009] In a first aspect, the present invention provides a super-lubricating and durable coating composition for puncture medical devices, comprising, by weight, the following components:
[0010] 5-12 parts of bisphenol A type epoxy resin
[0011] 2-6 parts of epoxy-terminated reactive silicone oil
[0012] 2-5 parts of non-reactive silicone oil
[0013] 1-3 parts of silane coupling agent
[0014] 1-3 parts of polyetheramine curing agent
[0015] 70-88 parts of mixed solvent
[0016] The mixed solvents include propylene glycol methyl ether and butyl acetate.
[0017] Preferably, the mass ratio of propylene glycol methyl ether to butyl acetate is 1:1 to 2:1.
[0018] Preferably, the solid content of the super-lubricating and durable coating composition is 12-30%.
[0019] Preferably, the bisphenol A type epoxy resin is a liquid bisphenol A type epoxy resin with a degree of polymerization n<2, an epoxy equivalent of 180~200 g / eq, and a viscosity of 8000~16000 mPa·s at 25°C.
[0020] Preferably, the epoxy value of the terminal epoxy reactive silicone oil is 0.1~0.2 mol / 100 g, and the viscosity at 25°C is 300~1200 mPa·s.
[0021] Preferably, the non-reactive silicone oil is a linear polydimethylsiloxane with methyl ends, and a viscosity of 350~12500 mPa·s at 25°C.
[0022] Preferably, the polyetheramine curing agent has the general structural formula CH3CH(NH2)CH2[OCH2CH(CH3)] x NH2, wherein the degree of polymerization x is 2~3, and the viscosity at 25℃ is 3~10 mPa·s.
[0023] Preferably, the general structural formula of the silane coupling agent is (R 1 O)3Si-R 2 -O-CH2-CH-CH2, where R 1 It is methyl or ethyl, R 2 It is propylidene.
[0024] In a second aspect, the present invention provides a method for preparing the above-mentioned super-lubricating and durable coating composition for puncture medical devices, comprising the following steps:
[0025] Mix all components evenly according to the specified proportions to obtain the final product.
[0026] Thirdly, the present invention provides the application of the above-mentioned super-lubricating and durable coating composition for puncture medical devices in puncture medical devices. The puncture medical device is selected from blood collection needles, indwelling intravenous catheters, or injection needles.
[0027] Fourthly, the present invention provides a method of using the above-mentioned super-lubricating and durable coating composition for puncture medical devices, comprising the following steps:
[0028] S1: A solution of a coating composition is provided for cleaning puncture medical devices;
[0029] S2: Contact the cleaned puncture medical device with the solution of the coating composition;
[0030] S3: The puncture medical device obtained in step S2 is heated and cured to obtain a puncture medical device with a super-lubricated and durable coating on its surface.
[0031] Preferably, the cleaning process further includes an activation process, wherein the activation process employs plasma treatment.
[0032] Preferably, step S2 is as follows: immerse the cleaned puncture medical instrument in the solution of the coating composition at a speed of 80-120 mm / min, stay for 3-5 seconds, and then pull it up at a uniform speed of 80-120 mm / min.
[0033] Preferably, the temperature curing is performed according to the following procedure:
[0034] First stage: Pre-curing at 70~90℃ for 10~30 min;
[0035] Second stage: Curing at 100~120℃ for 20~40 min;
[0036] Third stage: Curing at 130~150℃ for 30~60 min.
[0037] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0038] (1) Ultra-long lubrication durability
[0039] This invention achieves permanent fixation of the lubricating components through a dual mechanism of chemical bonding anchoring with reactive silicone oil and physical binding with non-reactive silicone oil. Experiments show that after three cycles of moist heat sterilization at 115℃ for 30 min following the application of the lubricating coating to a 16 G blood bag collection needle, the maximum puncture force at the needle tip remains ≤0.8 N (according to the testing method in Appendix C of GB 15811-2025, the maximum puncture force at the needle tip should be less than 1.2 N). After immersion in an anticoagulant for 12 months, the change rate of the maximum puncture force at the needle tip is ≤15%, maintaining excellent lubrication performance. This significantly surpasses existing physically coated silicone oil layers and double-layer coated silicone oil layers (where the puncture force increases significantly after moist heat sterilization). In terms of long-term stability, it is superior to a single-layer hybrid coating of reactive and non-reactive silicone oil (where the change rate of puncture force is ≥20% after immersion in an anticoagulant for 12 months).
[0040] (2) Self-layered integrated structure
[0041] This invention utilizes surface tension differences, curing reaction kinetics, and solvent evaporation characteristics to enable the coating to spontaneously form a gradient structure of "epoxy-enriched underlayer + silicone oil-enriched surface layer" after a single dip-coating and curing process. This self-layering coating not only simplifies the process but also optimizes the surface properties of the coating, greatly improving the interfacial adhesion and service life of the coating.
[0042] (3) Strong substrate adhesion
[0043] The coating described in this invention has an epoxy resin enriched in the bottom layer, which binds to the hydroxyl groups (Fe-OH) on the metal surface through hydrogen bonding. At the same time, the silane coupling agent forms Si-O-Fe covalent bonds on the metal surface, chemically anchoring the coating to the substrate and providing strong adhesion.
[0044] (4) Excellent biocompatibility
[0045] All components in the coating composition are medical-grade materials. After curing, the coating surface is stable and can effectively prevent small molecules from migrating and precipitating out. It meets the requirements of ISO 10993 biocompatibility standard and is suitable for medical devices that come into direct contact with blood, such as blood bag collection needles and injection needles. Attached Figure Description
[0046] Figure 1 This is a schematic diagram of the layered curing process of the coating composition in this invention;
[0047] Figure 2 This is a curve showing the lubrication performance of the coating formed in Example 1.
[0048] Figure 3 This is a comparison diagram of the puncture force of the coatings in Example 1, Example 2, and Comparative Example 3. Detailed Implementation
[0049] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0050] This invention provides a super-lubricating and durable coating composition for puncture medical devices, comprising the following components in parts by weight:
[0051] 5-12 parts of bisphenol A type epoxy resin
[0052] 2-6 parts of epoxy-terminated reactive silicone oil
[0053] 2-5 parts of non-reactive silicone oil
[0054] 1-3 parts of silane coupling agent
[0055] 1-3 parts of polyetheramine curing agent
[0056] Mixed solvent 70-88 parts.
[0057] In this invention, the super-lubricating and durable coating composition comprises 5 to 12 parts by weight of bisphenol A type epoxy resin, such as 5 parts, 5.5 parts, 6 parts, 6.5 parts, 7 parts, 7.5 parts, 8 parts, 8.5 parts, 9 parts, 9.5 parts, 10 parts, 10.5 parts, 11 parts, 11.5 parts, or 12 parts.
[0058] In this invention, the structural formula of bisphenol A epoxy resin is represented as follows:
[0059] ;
[0060] Wherein, R1 is -C6H4-C(CH3)2-C6H4-, with a degree of polymerization n<2, and is a liquid bisphenol A type epoxy resin. The epoxy equivalent of the bisphenol A epoxy resin is 180~200 g / eq, such as 180 g / eq, 185 g / eq, 190 g / eq, 195 g / eq, or 200 g / eq, etc.; the viscosity at 25℃ is 8000~16000 mPa·s, such as 8000 mPa·s, 9000 mPa·s, 10000 mPa·s, 11000 mPa·s, 12000 mPa·s, 13000 mPa·s, 14000 mPa·s, 15000 mPa·s, or 16000 mPa·s, etc. In this invention, the low-polymerization-degree liquid epoxy resin has a high epoxy group content, which can provide sufficient chemical bonding sites for terminal epoxy group reactive silicone oil, and can be effectively diluted by mixed solvents to obtain a low-viscosity solution suitable for dip coating.
[0061] In this invention, the super-lubricating and durable coating composition comprises 2 to 6 parts by weight of terminal epoxy reactive silicone oil, such as 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, 5.5 parts, or 6 parts, etc.
[0062] In this invention, the structural formula of the epoxy-terminated reactive silicone oil can be represented as follows:
[0063] ;
[0064] Wherein, R2 is a linking group, which is propylene (-CH2-CH2-CH2-) or a glycidyl ether group. The selected terminal epoxy reactive silicone oil has a viscosity of 300~1200 mPa·s at 25℃, such as 300 mPa·s, 400 mPa·s, 500 mPa·s, 600 mPa·s, 700 mPa·s, 800 mPa·s, 900 mPa·s, 1000 mPa·s, 1100 mPa·s, or 1200 mPa·s, etc.; the epoxy value is 0.1~0.2 mol / 100 g, such as 0.1 mol / 100 g, 0.11 mol / 100 g, 0.12 mol / 100 g, 0.13 mol / 100 g, 0.14 mol / 100 g, 0.15 mol / 100 g, 0.16 mol / 100 g, etc. The concentrations are 0.17 mol / 100 g, 0.18 mol / 100 g, 0.19 mol / 100 g, or 0.2 mol / 100 g, etc. In this invention, the epoxy-terminated reactive silicone oil can react with the polyetheramine curing agent through the epoxy groups at both ends, chemically bonding and anchoring it in the epoxy resin crosslinking network to provide durable lubrication.
[0065] In this invention, the super-lubricating and durable coating composition comprises 2 to 5 parts by weight of non-reactive silicone oil, such as 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, or 5 parts, etc.
[0066] In this invention, the non-reactive dimethyl silicone oil is a linear polydimethylsiloxane with methyl groups at both ends. Its molecular chain is composed of repeating dimethylsiloxane units, and it does not contain any active functional groups at either end. Its general structural formula is (CH3)3SiO-(Si(CH3)2O). n -Si(CH3)3, where the degree of polymerization n is 200~950, preferably 300~800, more preferably 400~600. In this invention, the viscosity of the non-reactive silicone oil at 25°C is 350~12500 mPa·s, such as 350 mPa·s, 500 mPa·s, 800 mPa·s, 1000 mPa·s, 3000 mPa·s, 5000 mPa·s, 8000 mPa·s, 10000 mPa·s, or 12500 mPa·s, etc.
[0067] In this invention, the super-lubricating and durable coating composition includes 1 to 3 parts of polyetheramine curing agent by weight, such as 1 part, 1.2 parts, 1.5 parts, 1.8 parts, 2 parts, 2.2 parts, 2.5 parts, 2.8 parts, or 3 parts, etc.
[0068] The preferred polyetheramine curing agent in this invention is an amino-terminated polyether with the general structural formula CH3CH(NH2)CH2[OCH2CH(CH3)]. x NH2, wherein the degree of polymerization X is 2~3, and the viscosity at 25℃ is 3~10 mPa·s, such as 3 mPa·s, 4 mPa·s, 5 mPa·s, 6 mPa·s, 7 mPa·s, 8 mPa·s, 9 mPa·s, or 10 mPa·s, etc. In this invention, the primary amino group of the polyether amine undergoes a ring-opening addition reaction with the epoxy groups of bisphenol A epoxy resin, terminal epoxy silicone oil, and silane coupling agent to form a three-dimensional cross-linked network. The good compatibility of polyether amine with epoxy resin and poor compatibility with organosilicon components is beneficial to the formation of a self-layered coating structure. Studies have shown that embedding polyether segments in the polyether amine molecular chain reduces the activity and polarity of the amine, and numerous literatures and commercial products have confirmed that it passes the ISO 10993 test.
[0069] The epoxy equivalents mentioned above were obtained by perchloric acid potentiometric titration (GB / T 4612-2008), and the viscosity was obtained by rotational viscometer determination (Chinese Pharmacopoeia 2025 Edition Viscosity Test Method III).
[0070] In this invention, the super-lubricating and durable coating composition includes 1 to 3 parts by weight of silane coupling agent, such as 1 part, 1.2 parts, 1.5 parts, 1.8 parts, 2 parts, 2.2 parts, 2.5 parts, 2.8 parts, or 3 parts, etc.
[0071] In this invention, the silane coupling agent, serving as the molecular bridge connecting the inorganic substrate and the organic coating, is an epoxy-based silane compound having the following general structural formula: (R 1 O)3Si-R 2 -O-CH2-CH-CH2, where R 1 It is methyl or ethyl, R 2 The silane coupling agent is propylene-based. Preferably, this invention uses γ-glycidyl etheroxypropyltrimethoxysilane: (CH3O)3Si-(CH2)3-O-CH2-CH-CH2. One end of the silane coupling agent contains a hydrolyzable methoxy group (-OCH3), which hydrolyzes to generate a silanol group (-Si-OH), which can undergo a condensation reaction with the hydroxyl groups (Fe-OH) on the surface of the metal substrate to form a Si-O-Fe covalent bond. The epoxy group at the other end can participate in the ring-opening addition reaction between the polyetheramine curing agent and the epoxy resin, thereby anchoring the entire coating to the metal surface through chemical bonds.
[0072] In this invention, the super-lubricating and durable coating composition comprises 70 to 88 parts by weight of mixed solvent, such as 70 parts, 72 parts, 75 parts, 78 parts, 80 parts, 82 parts, 85 parts or 88 parts, etc.
[0073] In this invention, the mixed solvent is a mixture of propylene glycol methyl ether and butyl acetate, with a mass ratio of 1:1 to 2:1, such as 1:1, 1.2:1, 1.5:1 or 2:1.
[0074] Among them, propylene glycol methyl ether has a boiling point of 120℃ and butyl acetate has a boiling point of 126℃, both being medium-boiling solvents. Their evaporation rates are similar but slightly different (butyl acetate evaporation rate 1.0, propylene glycol methyl ether 0.62~0.66), forming a gradient evaporation curve, providing sufficient time window for the self-stratification migration of the organosilicon components. Simultaneously, as a hydrogen bond acceptor solvent, propylene glycol methyl ether's hydroxyl groups can form reversible hydrogen bonds with the epoxy resin, effectively reducing the system viscosity and promoting the uniform dispersion of high-viscosity silicone oil.
[0075] In this invention, the solid content of the above-mentioned super-lubricating and durable coating composition is 12-30%, such as 12%, 15%, 18%, 20%, 22%, 25%, 28%, or 30%.
[0076] The present invention also provides a method for preparing the above-mentioned super-lubricating durable coating composition, comprising the following steps:
[0077] Mix all components evenly according to the specified proportions to obtain the final product.
[0078] In this invention, the mixing is preferably carried out under stirring conditions.
[0079] In some embodiments of the present invention, preferably under anhydrous conditions, bisphenol A type epoxy resin, terminal epoxy reactive silicone oil, non-reactive silicone oil, and silane coupling agent are added to a mixed solvent and stirred using a high-speed disperser at 1500-2500 rpm for 30-60 min, preferably at 1800-2000 rpm for 40-50 min, to ensure uniform dispersion of the components; then, polyetheramine curing agent calculated according to epoxy equivalents is added, stirred at low speed until homogeneous, and filtered to obtain a solution of the super-lubricating and durable coating composition.
[0080] The present invention also provides the application of the above-mentioned super-lubricating and durable coating composition for puncture medical devices in puncture medical devices.
[0081] The puncture medical device is selected from blood bag collection needles, indwelling intravenous needles, or injection needles.
[0082] The present invention also provides a method of using a super-lubricating and durable coating composition for puncture medical devices, comprising the following steps:
[0083] S1: A solution of coating composition is provided; for cleaning puncture medical devices;
[0084] S2: Contact the cleaned puncture medical device with the solution of the coating composition;
[0085] S3: The puncture medical device obtained in step S2 is heated and cured to obtain a puncture medical device with a super-lubricated and durable coating on its surface.
[0086] According to the present invention, a solution of a coating composition is provided.
[0087] In some embodiments of the present invention, the cleaning process is as follows: the puncture medical device (such as a stainless steel blood collection needle) is ultrasonically cleaned in sequence with acetone and ethanol to remove surface oil.
[0088] In some preferred embodiments of the present invention, after cleaning, optionally, a low-temperature oxygen plasma treatment is performed to activate the metal surface.
[0089] Then, according to the present invention, the cleaned (or activated) puncture medical device is brought into contact with a solution of the coating composition.
[0090] In some embodiments of the present invention, the cleaned (or activated) puncture medical device is preferably immersed in the coating solution at a speed of 80-120 mm / min, preferably 90-100 mm / min, and held for 3-5 seconds (preferably 4 seconds) before being pulled up at a uniform speed of 80-120 mm / min, preferably 90-100 mm / min.
[0091] Then, according to the present invention, the puncture medical device obtained in step S2 is heated and cured to obtain a puncture medical device with a super-lubricated and durable coating on its surface.
[0092] In this invention, the temperature-curing process is preferably a stepped temperature-curing process: the first stage is pre-curing at 70~90℃ for 10~30 min to allow solvent evaporation and initial gelation of the system; the second stage is heating to 100~120℃ for 20~40 min to promote the crosslinking reaction between epoxy resin and polyetheramine and terminal epoxy silicone oil, and to drive the self-delamination behavior between components; the third stage is heating to 130~150℃ for 30~60 min to fully crosslink epoxy resin and polyetheramine and terminal epoxy silicone oil, and to complete the self-delamination process.
[0093] The above 70~90℃ can be 70℃, 75℃, 80℃, 85℃ or 90℃, etc.; the above 10~30 min can be 10 min, 15 min, 20 min, 25 min or 30 min, etc.
[0094] The above 100~120℃ can be 100℃, 105℃, 110℃, 115℃ or 120℃, etc., and the above 20~40 min can be 20 min, 25 min, 30 min, 35 min or 40 min, etc.
[0095] The above 130~150℃ can be 130℃, 135℃, 140℃, 145℃ or 150℃, etc.; the above 30~60 min can be 30 min, 35 min, 40 min, 45 min, 50 min, 55 min or 60 min, etc.
[0096] It is hereby explained that the key technical feature of the coating of the present invention is that, by adjusting the following parameters, the coating spontaneously forms a gradient layered structure during the curing process:
[0097] (1) Thermodynamic driving: The epoxy resin component has a high surface tension (about 40~45 mN / m) and strong polarity, and has good wettability to the metal substrate, and tends to accumulate at the substrate interface; the organosilicon component (terminated epoxy reactive silicone oil + non-reactive silicone oil) has a low surface tension (about 20~25 mN / m) and weak polarity, and tends to migrate to the coating surface to form a low surface energy lubricating layer.
[0098] (2) Curing reaction kinetics control: Polyetheramine was selected as the curing agent. It has good compatibility with epoxy resin but poor compatibility with organosilicon components, which promotes phase separation during the curing process. At the same time, the epoxy resin crosslinking reaction was carried out appropriately through the step-by-step temperature increase curing process. After the molecular weight increases, the compatibility with organosilicon components is further reduced, driving self-delamination.
[0099] (3) Solvent evaporation rate control: The gradient evaporation characteristics of propylene glycol methyl ether and butyl acetate maintain the fluidity of the system in the early stage after coating, providing a time window for self-separation. Subsequently, solvent evaporation promotes phase separation and fixation.
[0100] Research shows that the cured coating forms the following structure:
[0101] The bottom layer (close to the metal substrate) is enriched with epoxy resin, which binds to the hydroxyl groups (Fe-OH) on the metal surface through hydrogen bonding. At the same time, the silane coupling agent forms Si-O-Fe covalent bonds on the metal surface, chemically anchoring the coating to the substrate and providing strong adhesion. The middle layer (transition region) has a continuous gradient distribution of epoxy resin and organosilicon components, forming an interpenetrating network transition structure, eliminating interlayer interface defects and ensuring interlayer bonding. The top layer (outer surface of the coating) is enriched with terminal epoxy reactive silicone oil and non-reactive silicone oil. The terminal epoxy silicone oil is connected to the epoxy network through chemical bonds, while the non-reactive silicone oil is physically dispersed on the surface, forming a dual lubrication mechanism of chemical anchoring and physical replenishment.
[0102] To facilitate understanding of the technical solution of this invention, the reaction mechanism is explained as follows:
[0103] (1) Hydrolysis of silane coupling agents
[0104] The methoxy group (-OCH3) in the epoxy silane coupling agent molecule undergoes a hydrolysis reaction and is converted into a silanol group (-Si-OH).
[0105] (2) Condensation of silanol groups with metal surfaces
[0106] The silanol groups generated by hydrolysis undergo a dehydration condensation reaction with the hydroxyl groups (Fe-OH) on the surface of the stainless steel needle to form Si-O-Fe covalent bonds, which firmly anchor the silane coupling agent to the metal surface.
[0107] (3) Adhesion mechanism between epoxy resin and metal substrate
[0108] The hydroxyl groups on the bisphenol A type epoxy resin molecular chain form hydrogen bonds with the hydroxyl groups (Fe-OH) on the surface of the stainless steel needle, thus physically adsorbing the coating onto the metal surface.
[0109] (4) The primary amino group of polyetheramine undergoes a ring-opening addition reaction with the epoxy groups of bisphenol A epoxy resin, epoxy silane coupling agent, and terminal epoxy silicone oil:
[0110] Step 1: The primary amine reacts with an epoxy group to produce a secondary amine and a hydroxyl group;
[0111] ;
[0112] Step 2: The generated secondary amine continues to react with epoxy groups to generate tertiary amines;
[0113] .
[0114] Final result: A highly cross-linked three-dimensional network structure is formed, in which: bisphenol A epoxy resin provides a rigid skeleton and adhesion to metals; terminal epoxy reactive silicone oil is anchored in the network through chemical bonding, providing long-lasting lubrication; and non-reactive silicone oil is physically bound in the network voids, providing instant lubrication replenishment.
[0115] To further illustrate the present invention, the following embodiments provide a detailed description. Unless otherwise specified, all experimental materials used in the following embodiments of the present invention are commercially available products.
[0116] Example 1
[0117] 1. Preparation of coating composition
[0118] Weigh each component according to the following parts by weight:
[0119] Bisphenol A type epoxy resin (E-51, epoxy equivalent 190 g / eq, viscosity at 25℃ 12000 mPa·s, n≈0.2): 8 parts;
[0120] Epoxy-terminated reactive silicone oil (viscosity 800 mPa·s, 25℃, epoxy value 0.15 mol / 100 g): 5 parts;
[0121] Non-reactive dimethyl silicone oil (viscosity 12500 mPa·s, 25℃): 3 parts;
[0122] The polyetheramine curing agent (D-230, average molecular weight 220, amine value approximately 8.5 meq / g), calculated based on epoxy equivalent, has an active hydrogen equivalent of approximately 60 g / eq. After the formation of the layered structure, the polyetheramine curing agent has good compatibility with bisphenol A epoxy resin and is mainly distributed at the bottom of the coating. Therefore, the dosage is mainly calculated based on the bisphenol A epoxy equivalent. The dosage = 8 × (60 / 190) ≈ 2.52 parts, and 3 parts are actually used.
[0123] Silane coupling agent (KH-560): 1 part;
[0124] Propylene glycol methyl ether: 40 parts;
[0125] Butyl acetate: 40 parts;
[0126] Preparation steps:
[0127] Under anhydrous conditions, 8 parts of E-51 epoxy resin, 5 parts of terminal epoxy reactive silicone oil, 3 parts of non-reactive dimethyl silicone oil, and 1 part of silane coupling agent were added to 80 parts of mixed solvent (propylene glycol methyl ether: butyl acetate = 1:1). The mixture was stirred at 2000 rpm for 30 min using a high-speed disperser to ensure uniform dispersion of all components. Subsequently, 3 parts of polyetheramine curing agent were added, and the mixture was stirred at 500 rpm for 10 min. After thorough mixing, the solution was filtered through a 200-mesh filter to obtain the coating solution. The viscosity of this solution at 25°C was 40–60 mPa·s, and the solid content was approximately 20%.
[0128] 2. Substrate Pretreatment
[0129] Take a 304 stainless steel blood collection needle (blood bag collection needle, needle outer diameter 1.6 mm, length 38 mm), immerse it in acetone and anhydrous ethanol in sequence, and ultrasonically clean each for 10 min (ultrasonic power 200 W, frequency 40 kHz). After taking it out, blow it dry with nitrogen gas, and then place it in a low-temperature oxygen plasma treatment instrument (power 100 W, oxygen flow rate 50 mL / min) for 3 min to activate the metal surface.
[0130] 3. Dip coating and curing
[0131] The pretreated blood collection needle was vertically immersed in the above coating solution to a depth of 30 mm, held for 3 seconds, and then pulled out at a uniform speed of 100 mm / min. The coated needle was then placed in a forced-air drying oven and cured according to the following stepped temperature increase procedure. A schematic diagram of the coating self-delamination curing process is shown below. Figure 1 As shown:
[0132] First stage: Pre-curing at 80℃ for 20 min (to allow solvent to evaporate and the system to initially gel);
[0133] Second stage: Curing at 120℃ for 30 min (to promote cross-linking reaction and self-delamination);
[0134] Third stage: Curing at 150℃ for 30 min (complete cross-linking, fixing gradient structure);
[0135] After curing, the needles are naturally cooled to room temperature to obtain a super-lubricating and durable coating on the surface.
[0136] 4. Performance Testing
[0137] (1) Lubrication performance test
[0138] Referring to GB 15811-2025 standard (Appendix C Test Method for Needle Tip Puncture Force and Resistance), the maximum puncture force of the blood collection needle was determined using an injection needle puncture force tester. Test conditions: The test needle was inserted into a specific test material at a constant speed. The test material was polyurethane with a Shore hardness of (85±10) HA, a nominal thickness of (0.40±0.05) mm, and a puncture speed of 100 mm / min.
[0139] Results: The initial maximum puncture force was 0.68 ± 0.01 N, and the detection curve is shown below. Figure 2 .
[0140] (2) Lubrication performance test after moist heat sterilization
[0141] The coated blood collection needles were placed in an autoclave and sterilized at 115°C and 0.13 MPa for 30 minutes, repeated three times. After each sterilization, the needles were removed and the maximum puncture force at the needle tip was measured using the method described above.
[0142] result:
[0143] Maximum puncture force (mean ± standard deviation) for sterilization cycles (N)
[0144] 0 times 0.68±0.01
[0145] 0.70±0.01 per time
[0146] 2 times 0.72±0.01
[0147] 3 times 0.76±0.01.
[0148] (3) Lubrication performance test after long-term immersion in anticoagulant
[0149] After initial sterilization, the coated blood collection needles were completely immersed in a sodium citrate anticoagulant solution and placed in a 37°C constant temperature incubator for 1 month, 3 months, 6 months, and 12 months, respectively. Samples were taken out for testing at each time point.
[0150] result:
[0151] Maximum puncture force over time (mean ± standard deviation) N
[0152] The value was 0.70 ± 0.01 after one sterilization.
[0153] 0.72±0.01 per month
[0154] 3 months 0.73±0.01
[0155] 6 months 0.76±0.01
[0156] 12 months 0.79±0.01.
[0157] Example 2
[0158] 1. Preparation of coating composition
[0159] Weigh each component according to the following parts by weight:
[0160] Bisphenol A type epoxy resin (NPEL-128, epoxy equivalent 185 g / eq, viscosity at 25℃ 14000 mPa·s): 8 parts;
[0161] Epoxy-terminated reactive silicone oil (viscosity 1200 mPa·s, 25℃, epoxy value 0.1 mol / 100 g): 6 parts;
[0162] Non-reactive dimethyl silicone oil (viscosity 1000 mPa·s, 25℃): 4 parts;
[0163] Polyetheramine curing agent (D-230, average molecular weight 220, amine value approximately 8.5 meq / g): calculated based on epoxy equivalent, active hydrogen equivalent approximately 60 g / eq, dosage = 8 × (60 / 185) ≈ 2.59 parts, actual dosage is 3 parts;
[0164] Silane coupling agent (KH-560): 1 part;
[0165] Propylene glycol methyl ether: 52 parts;
[0166] Butyl acetate: 26 parts;
[0167] Preparation steps:
[0168] Under anhydrous conditions, 8 parts of NPEL-128 epoxy resin, 6 parts of terminal epoxy reactive silicone oil, 4 parts of non-reactive dimethyl silicone oil, and 1 part of silane coupling agent were added to 78 parts of mixed solvent (propylene glycol methyl ether: butyl acetate = 2:1). The mixture was stirred at 2000 rpm for 30 min using a high-speed disperser to ensure uniform dispersion of all components. Subsequently, 3 parts of polyetheramine curing agent were added, and the mixture was stirred at a low speed of 500 rpm for 10 min. After thorough mixing, the mixture was filtered through a 200-mesh filter to obtain the coating solution. The viscosity of this solution at 25°C was 30–50 mPa·s, and the solid content was approximately 22%.
[0169] 2. Substrate Pretreatment
[0170] Same as Example 1.
[0171] 3. Dip coating and curing
[0172] Same as Example 1.
[0173] 4. Performance Testing
[0174] (1) Lubrication performance test
[0175] The test conditions were the same as in Example 1. Result: The initial maximum puncture force was 0.71 ± 0.01 N.
[0176] (2) Lubrication performance test after moist heat sterilization
[0177] The test conditions are the same as in Example 1.
[0178] result:
[0179] Maximum puncture force (mean ± standard deviation) for sterilization cycles (N)
[0180] 0 times 0.71±0.01
[0181] 0.72±0.01 per time
[0182] 2 times 0.73±0.01
[0183] 3 times 0.75±0.01.
[0184] (3) Lubrication performance test after long-term immersion in anticoagulant
[0185] The test conditions are the same as in Example 1.
[0186] result:
[0187] Maximum puncture force over time (mean ± standard deviation) N
[0188] The value was 0.72 ± 0.01 after one sterilization.
[0189] 0.73±0.01 per month
[0190] 3 months 0.74±0.01
[0191] 6 months 0.76±0.01
[0192] 12 months 0.78±0.01.
[0193] In Example 2, because a low-viscosity non-reactive dimethyl silicone oil of 1000 mPa·s (25°C) was used, the initial lubricity was slightly reduced. However, the increased solvent gradient and the easier dispersion of the low-viscosity silicone oil resulted in a slight improvement in coating adhesion compared to Example 1. A comparison of the puncture force with Example 1 is shown below. Figure 3 .
[0194] Example 3
[0195] 1. Preparation of coating composition
[0196] Weigh each component according to the following parts by weight:
[0197] Bisphenol A type epoxy resin (E-51, epoxy equivalent 190 g / eq, viscosity at 25℃ 12000 mPa·s, n≈0.2): 5 parts;
[0198] Epoxy-terminated reactive silicone oil (viscosity 800 mPa·s, 25℃, epoxy value 0.15 mol / 100g): 2 parts;
[0199] Non-reactive dimethyl silicone oil (viscosity 12500 mPa·s, 25℃): 2 parts;
[0200] Silane coupling agent (KH-560): 1 part;
[0201] Polyetheramine curing agent (D-230, active hydrogen equivalent approximately 60 g / eq): Dosage calculated based on epoxy equivalent = 5 × (60 / 190) ≈ 1.58 parts, actual dosage is 2 parts;
[0202] Mixed solvent: 44 parts propylene glycol methyl ether, 44 parts butyl acetate (solid content ≈ 12%).
[0203] Preparation steps:
[0204] Under anhydrous conditions, 5 parts of E-51 epoxy resin, 2 parts of terminal epoxy reactive silicone oil, 2 parts of non-reactive dimethyl silicone oil, and 1 part of silane coupling agent were added to 88 parts of mixed solvent (propylene glycol methyl ether: butyl acetate = 1:1). The mixture was stirred at 2000 rpm for 30 min until homogeneous. Then, 2 parts of polyetheramine curing agent D-230 were added, and the mixture was stirred at 500 rpm for 10 min. The mixture was then filtered through a 200-mesh screen to obtain the coating solution. The viscosity at 25℃ was approximately 15~25 mPa·s.
[0205] 2. Substrate Pretreatment
[0206] Same as Example 1.
[0207] 3. Dip coating and curing
[0208] Same as Example 1.
[0209] 4. Performance Testing
[0210] (1) Lubrication performance test (same conditions as in Example 1)
[0211] Initial maximum puncture force: 0.75±0.02 N.
[0212] (2) Lubrication performance after moist heat sterilization
[0213] Maximum puncture force (mean ± standard deviation) for sterilization cycles (N)
[0214] 0 times 0.75±0.02
[0215] 0.77±0.02 per time
[0216] 2 times 0.78±0.02
[0217] 3 times 0.80±0.02.
[0218] (3) Lubricating performance of anticoagulant after long-term immersion (immersion after one sterilization)
[0219] Maximum puncture force over time (mean ± standard deviation) N
[0220] 0.77±0.02 after one sterilization.
[0221] 0.79±0.02 after 1 month
[0222] 3 months 0.82±0.03
[0223] 6 months 0.85±0.03
[0224] 12 months 0.87±0.04.
[0225] Results analysis:
[0226] In this embodiment, the contents of epoxy resin, reactive silicone oil, and total solids are all taken at the lower limit of the range, resulting in a low crosslinking network density and weak chemical anchoring and physical binding ability for the silicone oil. The maximum puncture force of 0.87 N is still lower than the national standard (puncture force ≤ 1.2 N), but the puncture force under various conditions is significantly greater than that of Example 1 with appropriate contents.
[0227] Example 4
[0228] 1. Preparation of coating composition
[0229] Weigh each component according to the following parts by weight:
[0230] Bisphenol A type epoxy resin (E-51, epoxy equivalent 190 g / eq, viscosity at 25℃ 12000 mPa·s, n≈0.2): 12 parts;
[0231] Epoxy-terminated reactive silicone oil (viscosity 800 mPa·s, 25℃, epoxy value 0.15 mol / 100g): 6 parts;
[0232] Non-reactive dimethyl silicone oil (viscosity 12500 mPa·s, 25℃): 5 parts;
[0233] Silane coupling agent (KH-560): 3 parts;
[0234] Polyetheramine curing agent (D-230, active hydrogen equivalent approximately 60 g / eq): Dosage calculated based on epoxy equivalent = 12 × (60 / 190) ≈ 3.78 parts, actual dosage is 4 parts;
[0235] Mixed solvent: 35 parts propylene glycol methyl ether, 35 parts butyl acetate (total solvent 70 parts, making solid content ≈30%).
[0236] Preparation steps:
[0237] Under anhydrous conditions, 12 parts of E-51 epoxy resin, 6 parts of terminal epoxy reactive silicone oil, 5 parts of non-reactive dimethyl silicone oil, and 3 parts of silane coupling agent KH-560 were added to 70 parts of mixed solvent (propylene glycol methyl ether: butyl acetate = 1:1). The mixture was stirred at 2000 rpm for 40 min using a high-speed disperser (due to the high viscosity of the resin, stirring was prolonged to ensure complete dissolution and dispersion). Subsequently, 4 parts of polyetheramine curing agent D-230 were added, and the mixture was stirred at 500 rpm for 10 min. The solution was then filtered through a 200-mesh sieve to obtain the coating solution. The viscosity at 25℃ was approximately 100~150 mPa·s, and the solid content was approximately 30%.
[0238] 2. Substrate Pretreatment
[0239] Same as Example 1.
[0240] 3. Dip coating and curing
[0241] Same as Example 1
[0242] 4. Performance Testing
[0243] (1) Lubrication performance test
[0244] Initial maximum puncture force: 0.74±0.01 N.
[0245] (2) Lubrication performance after moist heat sterilization
[0246] Maximum puncture force (mean ± standard deviation) for sterilization cycles (N)
[0247] 0 times 0.74±0.01
[0248] 0.75±0.01 per time
[0249] 2 times 0.77±0.01
[0250] 3 times 0.79±0.02.
[0251] (3) Lubricating performance of anticoagulant after long-term immersion (immersion after one sterilization)
[0252] Maximum puncture force over time (mean ± standard deviation) N
[0253] 0.75±0.01 after one sterilization.
[0254] 0.77±0.01 per month
[0255] 3 months 0.81±0.02
[0256] 6 months 0.83±0.02
[0257] 12 months 0.86±0.03.
[0258] Results analysis:
[0259] In this embodiment, with epoxy resin, reactive silicone oil, and total solids content all close to the upper limit of the present invention, a high-viscosity non-reactive silicone oil of 12500 mPa·s was selected. The high system viscosity hindered the uniform migration of the silicone oil, and some silicone oil aggregated during puncture, increasing the puncture force. Although the maximum puncture force of 0.86 N was still lower than the national standard (puncture force ≤ 1.2 N), the puncture force performance under various conditions was actually worse than in Example 1 with medium content. This indicates that higher amounts of reactive silicone oil and epoxy resin are not necessarily better; the synergy of the components and the migration-anchoring balance of the silicone oil are key to this invention.
[0260] Comparative Example 1 (Non-reactive silicone oil)
[0261] 1. Coating composition
[0262] Bisphenol A type epoxy resin (E-51): 8 parts;
[0263] Non-reactive dimethyl silicone oil (viscosity 12500 mPa·s): 6 parts;
[0264] Polyetheramine D-230: 4 parts;
[0265] Silane coupling agent (KH-560): 2 parts;
[0266] Propylene glycol methyl ether: butyl acetate = 1:1:80 parts; without terminal epoxy reactive silicone oil.
[0267] 2. Preparation and Testing
[0268] Same as Example 1.
[0269] 3. Performance Test Results
[0270] Test item: Maximum puncture force (mean ± standard deviation) N
[0271] Initial maximum puncture force: 0.78 ± 0.01 N
[0272] After three cycles of moist heat sterilization, the maximum puncture force was 1.26 ± 0.05 N (due to lubrication failure).
[0273] The results showed that, lacking the chemical anchoring effect of reactive silicone oil, the dimethyl silicone oil, which was only physically blended, was lost in large quantities after three cycles of wet heat sterilization, resulting in a rapid decline in lubrication performance to below the national standard requirement (1.2 N).
[0274] Comparative Example 2 (Physical coating with pure dimethyl silicone oil)
[0275] 1. Coating composition
[0276] Dimethyl silicone oil (viscosity 12500 mPa·s): 5 parts;
[0277] Hexamethyldisiloxane: 95 parts; free of epoxy resin, reactive silicone oil, curing agent and silane coupling agent.
[0278] 2. Preparation and Testing
[0279] Dimethyl silicone oil was dissolved in hexamethyldisiloxane, stirred evenly, and then coated onto the surface of the blood collection needle using the same process. The remaining tests were the same as in Example 1.
[0280] 3. Performance Test Results
[0281] Test item: Maximum puncture force (mean ± standard deviation) N
[0282] Initial maximum puncture force: 0.85 ± 0.02 N
[0283] After three rounds of moist heat sterilization, the maximum puncture force was 1.42 ± 0.05 N (lubrication was basically lost).
[0284] The results showed that the pure silicone oil physical coating layer had almost no resistance to damp heat sterilization and immersion, and could not meet the long-term lubrication requirements of medical devices.
[0285] Comparative Example 3 (Reactive silicone oil + non-reactive silicone oil coating)
[0286] 1. Coating composition
[0287] 6 parts of epoxy-terminated reactive silicone oil (viscosity 800 mPa·s, 25℃);
[0288] Dimethyl silicone oil (viscosity 1000 mPa·s, 25℃): 3 parts;
[0289] Hexamethyldisiloxane: 91 parts; free of epoxy resin, silane coupling agent and curing agent.
[0290] 2. Preparation and Testing
[0291] Under anhydrous conditions, 6 parts of terminal epoxy reactive silicone oil and 3 parts of dimethyl silicone oil were added to 91 parts of hexamethyldisiloxane. The mixture was stirred at 2000 rpm for 10 min using a high-speed disperser to ensure uniform dispersion of the components. After thorough mixing, a coating solution was obtained.
[0292] 3. Performance Test Results
[0293] Test item: Maximum puncture force (mean ± standard deviation) N
[0294] Initial maximum puncture force: 0.72 ± 0.01 N
[0295] The maximum puncture force after three cycles of moist heat sterilization was 1.06 ± 0.02 N.
[0296] After soaking in the anticoagulant for 12 months, the energy level was 1.34 ± 0.05 N (lubrication was basically lost).
[0297] The results showed that the initial lubrication performance was better after adding epoxy-terminated reactive silicone oil, and the resistance to moist heat sterilization was improved compared with Comparative Example 2. However, the epoxy value of the epoxy-terminated silicone oil was low, and the puncture force of the coating increased significantly under moist heat sterilization conditions, making it more difficult to withstand long-term anticoagulant immersion. A comparison of the puncture force with Examples 1 and 2 is shown in [reference needed]. Figure 3 .
[0298] Comparative Example 4 (Solid epoxy resin, n>2)
[0299] 1. Coating composition
[0300] Bisphenol A type epoxy resin (E-20, solid, epoxy equivalent 500 g / eq, n≈2~3): 10 parts;
[0301] Terminal epoxy-based silicone oil (same as in Example 1): 6 parts;
[0302] Dimethyl silicone oil: 4 parts;
[0303] Polyetheramine D-230: Approximately 2 parts are required based on epoxy equivalent;
[0304] Silane coupling agent (KH-560): 1 part;
[0305] Propylene glycol methyl ether: butyl acetate = 1:1:76 parts;
[0306] 2. Preparation attempt
[0307] When E-20 epoxy resin was added to the mixed solvent, it failed to dissolve after stirring at room temperature for 30 minutes. It required heating to 60°C and stirring for 1 hour to partially dissolve, resulting in a cloudy solution. Adding other components failed to form a transparent, homogeneous solution. During dip coating, the coating was uneven, with particulate precipitates appearing, preventing the formation of a continuous coating; therefore, subsequent performance testing was not conducted.
[0308] This comparative example illustrates that solid or semi-solid epoxy resins with a degree of polymerization n≥2 have poor solubility in the solvent system of this invention and are not suitable for dip coating processes.
[0309] Comparative Example 5 (Single solvent: Propylene glycol methyl ether only)
[0310] 1. Coating composition
[0311] The components and weight parts are the same as in Example 1, the only difference being that the mixed solvent is replaced with a single solvent: propylene glycol methyl ether: 80 parts, butyl acetate: 0 parts.
[0312] 2. Preparation and Testing
[0313] The preparation steps, substrate pretreatment, dip coating, and curing processes were the same as in Example 1. During the preparation of the mixed solution, it was observed that the solubility parameters of the system changed due to the lack of butyl acetate, and the dispersion uniformity of the terminal epoxy silicone oil and non-reactive silicone oil was slightly poor, requiring a longer stirring time. The dip coating and curing processes were the same as in Example 1.
[0314] 3. Performance Test Results
[0315] Test item: Maximum puncture force (mean ± standard deviation) N
[0316] The initial dynamic maximum puncture force was 0.72 ± 0.02 N.
[0317] After three cycles of moist heat sterilization, the maximum puncture force was 0.85 ± 0.03 N.
[0318] The anticoagulant concentration was 0.96±0.05 after 12 months of long-term soaking.
[0319] The results show that when using propylene glycol methyl ether as a single solvent, the lack of a gradient volatilization profile with butyl acetate resulted in insufficient self-stratification driving force during the curing process, leading to insufficient enrichment and uneven distribution of surface silicone oil. After moist heat sterilization and long-term immersion, the silicone oil that was not sufficiently anchored or physically bound was more prone to loss, resulting in significantly inferior lubrication durability compared to Example 1. This demonstrates that the specific mixed solvent formulation and its gradient volatilization characteristics of the present invention are one of the key technical features for achieving excellent self-stratification structure and long-lasting lubrication performance.
[0320] Comparative Example 6 (Single solvent: using only butyl acetate)
[0321] 1. Coating composition
[0322] The components and weight parts are the same as in Example 1, the only difference being that the mixed solvent is replaced with a single solvent: propylene glycol methyl ether: 0 parts, butyl acetate: 80 parts.
[0323] 2. Preparation and Testing
[0324] The preparation steps, substrate pretreatment, dip coating, and curing processes were the same as in Example 1. During the preparation of the mixed solution, it was observed that because butyl acetate has a weaker hydrogen bond accepting ability than propylene glycol methyl ether, its ability to dissolve and disperse high-viscosity silicone oil is insufficient, resulting in a small amount of high-viscosity silicone oil deposited at the bottom of the solution.
[0325] 3. Performance Test Results
[0326] Test item: Maximum puncture force (mean ± standard deviation) N
[0327] The initial dynamic maximum puncture force was 0.72 ± 0.03 N.
[0328] The maximum puncture force after three cycles of moist heat sterilization was 1.05 ± 0.02 N.
[0329] After soaking in the anticoagulant for 12 months, the concentration was 1.28 ± 0.05 N (lubrication was basically lost).
[0330] The results show that when using butyl acetate as a single solvent, on the one hand, the solvent evaporates too quickly, causing a rapid increase in system viscosity, which prevents the organosilicon components from migrating to the surface, resulting in poor self-stratification. On the other hand, the solvent's dissolving power for the resin components is insufficient, affecting the final crosslinking density and uniformity of the coating. This leads to poor initial lubrication performance, and a significant decrease in performance after sterilization and immersion. This comparative example further demonstrates the indispensability of the mixed solvent system of the present invention in controlling the self-stratification process and ensuring the overall performance of the coating.
[0331] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A super-lubricating and durable coating composition for puncture medical devices, characterized in that, Based on parts by weight, it includes the following components: 5-12 parts of bisphenol A type epoxy resin 2-6 parts of epoxy-terminated reactive silicone oil 2-5 parts of non-reactive silicone oil 1-3 parts of silane coupling agent 1-3 parts of polyetheramine curing agent 70-88 parts of mixed solvent The mixed solvents include propylene glycol methyl ether and butyl acetate.
2. The super-lubricating and durable coating composition for puncture medical devices according to claim 1, characterized in that, The mass ratio of propylene glycol methyl ether to butyl acetate is 1:1 to 2:1; The solid content of the super-lubricating and durable coating composition is 12-30%.
3. The super-lubricating and durable coating composition for puncture medical devices according to claim 1 or 2, characterized in that, The bisphenol A type epoxy resin is a liquid bisphenol A type epoxy resin with a degree of polymerization n<2, an epoxy equivalent of 180~200 g / eq, and a viscosity of 8000~16000 mPa·s at 25℃.
4. The super-lubricating and durable coating composition for puncture medical devices according to any one of claims 1 to 3, characterized in that, The epoxy value of the terminal epoxy reactive silicone oil is 0.1~0.2 mol / 100 g, and the viscosity at 25℃ is 300~1200 mPa·s; The non-reactive silicone oil is a linear polydimethylsiloxane with methyl ends, and its viscosity at 25°C is 350~12500 mPa·s.
5. The super-lubricating and durable coating composition for puncture medical devices according to any one of claims 1 to 4, characterized in that, The general structural formula of the polyetheramine curing agent is CH3CH(NH2)CH2[OCH2CH(CH3)]. x NH2, wherein the degree of polymerization x is 2~3, and the viscosity at 25℃ is 3~10 mPa·s; The general structural formula of the silane coupling agent is (R 1 O)3Si-R 2 -O-CH2-CH-CH2, where R 1 It is methyl or ethyl, R 2 It is propylidene.
6. A method for preparing a super-lubricating and durable coating composition for puncture medical devices as described in any one of claims 1 to 5, characterized in that, Includes the following steps: Mix all components evenly according to the specified proportions to obtain the final product.
7. The application of the super-lubricating and durable coating composition for puncture medical devices according to any one of claims 1 to 5, or the super-lubricating and durable coating composition for puncture medical devices prepared according to the preparation method according to claim 6, in puncture medical devices; The puncture medical device is selected from blood bag collection needles, indwelling intravenous needles, or injection needles.
8. A method of using a super-lubricating, durable coating composition for puncture medical devices as described in any one of claims 1 to 5, characterized in that, Includes the following steps: S1: A solution of coating composition is provided; for cleaning puncture medical devices; S2: Contact the cleaned puncture medical device with the solution of the coating composition; S3: The puncture medical device obtained in step S2 is heated and cured to obtain a puncture medical device with a super-lubricated and durable coating on its surface.
9. The method of use according to claim 8, characterized in that, The cleaning process is followed by an activation process, which is performed using plasma treatment. Step S2 is as follows: Immerse the cleaned puncture medical instrument in the solution of the coating composition at a speed of 80-120 mm / min, stay for 3-5 seconds, and then pull it up at a uniform speed of 80-120 mm / min.
10. The method of use according to claim 8 or 9, characterized in that, The temperature curing process is carried out according to the following procedure: First stage: Pre-curing at 70~90℃ for 10~30 min; Second stage: Curing at 100~120℃ for 20~40 min; Third stage: Curing at 130~150℃ for 30~60 min.