A system and method for producing trimanganese tetraoxide based on cyclic pre-oxidation

By stripping the oxide film through a circulating pre-oxidation production system and enhancing gas-liquid mass transfer, the problem of low reaction efficiency in the preparation of manganese tetroxide is solved, achieving efficient, low-cost, and low-pollution preparation of manganese tetroxide, which meets the requirements of battery materials.

CN123127918APending Publication Date: 2026-11-20ZHONGYE-CHANGTIAN INT ENG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611618164.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-19
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing technologies have low reaction efficiency in the preparation of manganese tetroxide, the oxide film blocks the reaction rate, traditional methods have high energy consumption and serious pollution, low oxygen utilization or introduce impurity ions.

Method used

A circulating pre-oxidation production system is adopted. Through slurry circulation between the pre-oxidation reactor and the deep oxidation reactor, the oxide film is peeled off by the abrasive mechanism and the stirring mechanism, the gas-liquid mass transfer is enhanced, and oxygen is dispersed from the hollow rotating shaft and the grinding wheel, and the unreacted oxygen is reused.

Benefits of technology

It significantly improves reaction conversion rate and oxygen utilization rate, reduces production costs, prepares high-purity manganese tetroxide, meets battery material requirements, and the process is green and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123127918A_ABST
    Figure CN123127918A_ABST
Patent Text Reader

Abstract

The application discloses a system and method for producing trimanganese tetraoxide based on cyclic pre-oxidation, and a segmented reaction system is constructed through a pre-oxidation reactor and a deep oxidation reactor. Part of the return slurry can be continuously recycled and ground in the pre-oxidation stage, the oxide film generated on the surface of the manganese metal particles can be continuously stripped, and the fresh manganese metal reaction surface is continuously exposed, so that the reaction stagnation caused by surface passivation is effectively avoided, the conversion rate of the manganese metal is improved, and the reaction period is shortened. Meanwhile, the hollow grinding wheel is used for axial gas supply, the gas is sheared and dispersed into the slurry by the rotation of the grinding wheel, and the gas-liquid-solid three-phase mass transfer efficiency is further improved. In addition, the unreacted residual gas is introduced into the deep oxidation reactor for cascade utilization, the total oxygen consumption utilization rate is improved, the prepared trimanganese tetraoxide product has high purity and low impurity content, and can meet the use requirements in the field of battery materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the preparation of battery-grade manganese tetroxide, specifically to a system and method for producing manganese tetroxide based on cyclic pre-oxidation, belonging to the field of battery material preparation technology. Background Technology

[0002] Manganese tetroxide (Mn3O4) is a key raw material for preparing high-performance manganese-zinc ferrite soft magnetic materials and lithium-ion battery cathode materials (such as lithium manganese oxide and lithium manganese iron phosphate). Currently, the industrial preparation of manganese tetroxide mainly employs the calcination method of metallic manganese powder and the liquid-phase precipitation method of manganese salts. However, the calcination method usually requires a long reaction time at high temperatures, resulting in huge energy consumption and severe dust pollution; the liquid-phase precipitation method requires raw materials such as manganese sulfate and liquid alkali, and generates a large amount of wastewater containing impurities such as sodium sulfate during the reaction process, making subsequent impurity removal and washing processes cumbersome and posing a significant environmental burden.

[0003] In contrast, wet oxidation using manganese flakes (or powder) in an ammonium salt medium is a low-cost, low-pollution, and environmentally friendly approach. However, this approach faces several challenges in practical engineering: First, the dense oxide film formed on the surface of the manganese flakes during the reaction in aqueous solution blocks the contact between the internal manganese and oxygen, resulting in an extremely slow reaction rate. The stirring and shearing forces of traditional reactors are insufficient to remove this oxide layer. Second, this reaction is a typical gas-liquid-solid three-phase reaction, and the reaction rate is limited by the mass transfer efficiency of oxygen.

[0004] In existing processes, the reaction rate is generally increased by simply increasing the oxygen flow rate or by directly adding a strong oxidant. The former has extremely low oxygen utilization, and a large amount of oxygen overflows from the reaction system before it can participate in the reaction, which greatly increases production costs. The latter introduces additional impurity ions, which affects the purity of the final manganese tetroxide product and increases the processing burden of subsequent impurity removal processes. Summary of the Invention

[0005] To address the shortcomings of existing technologies, such as low reaction efficiency, this invention provides a system and method for producing manganese tetroxide based on cyclic pre-oxidation. By constructing a segmented reaction system of pre-oxidation cyclic grinding + deep oxidation, a portion of the returned slurry is continuously circulated into the pre-oxidation reactor for grinding during the pre-oxidation stage. This continuously peels off the oxide film formed on the surface of the manganese particles, constantly exposing fresh manganese reaction surfaces and solving the problem of oxide film blocking the reaction. At the same time, the system of this invention can further promote the dispersion efficiency of oxygen in the slurry, enhance gas-liquid mass transfer, and increase the reaction rate. The prepared manganese tetroxide product has high purity and low impurity content, fully meeting the requirements for use in the field of battery materials.

[0006] To achieve the above-mentioned technical objectives, the technical solution adopted by the present invention is as follows:

[0007] According to a first embodiment of the present invention, a system for producing manganese tetroxide based on cyclic pre-oxidation is provided:

[0008] A system for producing manganese tetroxide based on cyclic pre-oxidation is disclosed. The system includes a pre-oxidation reactor and a deep oxidation reactor. An abrasive mechanism is installed inside the pre-oxidation reactor. A stirring mechanism is installed inside the deep oxidation reactor.

[0009] The pre-oxidation reactor has a pre-oxidation slurry outlet, a pre-oxidation return slurry inlet, and a pre-oxidation air inlet pipe at its lower part, and a pre-oxidation exhaust pipe at its upper part. The deep oxidation reactor has a deep oxidation slurry inlet, a deep oxidation exhaust pipe, and a deep oxidation feed pipe at its upper part, and a deep oxidation return slurry outlet, a deep oxidation air inlet pipe, and a deep oxidation discharge outlet at its lower part. The pre-oxidation slurry outlet is connected to the deep oxidation slurry inlet via a transfer pipe. The deep oxidation return slurry outlet is connected to the pre-oxidation return slurry inlet via a return slurry pipe. A circulation pump is installed on the return slurry pipe.

[0010] Preferably, the abrasive mechanism includes an abrasive drive (e.g., a motor), a rotating shaft, and a grinding wheel. The abrasive drive is disposed on the top surface of the pre-oxidation reactor. The top end of the rotating shaft passes through the top cover of the pre-oxidation reactor and is connected to the abrasive drive, while its bottom end extends downward to the lower part of the inner cavity of the pre-oxidation reactor. The grinding wheel is disposed on the rotating shaft located in the inner cavity of the pre-oxidation reactor. Preferably, the inner cavity of the pre-oxidation reactor is filled with abrasive media (e.g., spherical, cylindrical, or elliptical zirconium oxide or zirconium silicate).

[0011] Preferably, both the rotating shaft and the grinding wheel are hollow structures, and the shaft cavity is connected to the grinding wheel cavity. The grinding wheel has several vent holes, and its cavity is connected to the inner cavity of the pre-oxidation reactor through these vent holes. A pre-oxidation inlet pipe is located at the bottom of the pre-oxidation reactor, and its exhaust end extends upwards to connect with the shaft cavity. The pre-oxidation inlet pipe is connected to the bottom wall of the pre-oxidation reactor and the bottom end of the rotating shaft via rotary connectors. Preferably, the rotary connector is a sealed bearing.

[0012] Preferably, the pre-oxidation exhaust pipe is connected to the deep oxidation inlet pipe via a gas transfer pipeline. A purge feed pipe is also installed at the top of the pre-oxidation reactor.

[0013] Preferably, a heater is also provided on the outer wall of the pre-oxidation reactor, or the interior of the pre-oxidation reactor wall (side wall and / or bottom wall) is hollow to form a pre-oxidation liquid constant temperature jacket. Preferably, the heater is an electric heating plate or a microwave heater. The pre-oxidation liquid constant temperature jacket is an oil bath constant temperature jacket or a water bath constant temperature jacket.

[0014] Preferably, the stirring mechanism includes a stirring drive (e.g., a motor), a stirring shaft, and a stirring paddle. The stirring drive is disposed on the top surface of the deep oxidation reactor. The top end of the stirring shaft passes through the top cover of the deep oxidation reactor and is connected to the stirring drive, while its bottom end extends downward to the lower part of the inner cavity of the deep oxidation reactor. The stirring paddle is disposed on the stirring shaft located in the inner cavity of the deep oxidation reactor. Preferably, the stirring paddle is a stirring blade or a stirring rod.

[0015] Preferably, a heater is also provided on the outer wall of the deep oxidation reactor, or the interior of the deep oxidation reactor wall (side wall and / or bottom wall) is hollow to form a deep oxidation liquid constant temperature jacket. Preferably, the heater is an electric heating plate or a microwave heater. The deep oxidation liquid constant temperature jacket is an oil bath constant temperature jacket or a water bath constant temperature jacket.

[0016] According to a second embodiment of the present invention, a method for producing manganese tetroxide based on cyclic pre-oxidation is provided:

[0017] A method for producing manganese tetroxide based on cyclic pre-oxidation or a method for producing manganese tetroxide using a system as described in the first embodiment, the method comprising the following steps:

[0018] S1. Add metallic manganese and ammonium salt solution to the deep oxidation reactor to form slurry. Start the circulation pump and open the slurry transfer pipe and return pipe to make the slurry circulate between the pre-oxidation reactor and the deep oxidation reactor.

[0019] S2. Start the abrasive mechanism and stirring mechanism, and introduce oxidizing gas into the pre-oxidation reactor and deep oxidation reactor for pre-oxidation treatment.

[0020] S3. After the pre-oxidation treatment is completed, all the slurry is returned to the deep oxidation reactor and the abrasive mechanism, circulation pump, slurry transfer pipe and return slurry pipe are shut down. Stirring continues for deep oxidation treatment.

[0021] S4. After the deep oxidation treatment is completed, reduce the stirring rate and carry out aging treatment. After aging, perform solid-liquid separation, and wash and dry the obtained solid product in sequence to obtain the target manganese tetroxide product.

[0022] Preferably, in step S1, the metallic manganese is manganese powder or manganese flakes, and preferably, the particle size of the manganese powder or manganese flakes is 0.025~2mm.

[0023] Preferably, in step S1, the ammonium salt solution is one or more of ammonium chloride solution, ammonium sulfate solution, ammonium acetate solution, and ammonium oxalate solution, with ammonium chloride solution being the most preferred. The concentration of the ammonium salt solution is 0.1~1 mol / L, preferably 0.2~0.5 mol / L.

[0024] Preferably, in step S1, the liquid-solid mass ratio of the ammonium salt solution to metallic manganese is 2~15:1, more preferably 3~10:1.

[0025] Preferably, in step S2, the temperature of the pre-oxidation treatment (including the pre-oxidation reactor and the deep oxidation reactor) is 50~80℃, and more preferably 60~75℃.

[0026] Preferably, in step S2, the pre-oxidation treatment lasts for no less than 1 hour, and more preferably 3 to 10 hours.

[0027] Preferably, in step S2, the oxidizing gas is oxygen, and the oxygen flow rate is 0.5~2L / min, preferably 0.8~1.5L / min.

[0028] Preferably, in step S2, the rotational speed of the abrasive is not less than 500 rpm, and more preferably 800~1500 rpm. The stirring speed is not less than 200 rpm, and more preferably 300~800 rpm.

[0029] Preferably, in step S3, the endpoint of the deep oxidation treatment is that the pH of the slurry no longer changes, preferably the pH of the slurry decreases to 7.0±0.5 and remains stable for at least 1 hour.

[0030] Preferably, in step S4, the aging process by reducing the stirring rate specifically involves reducing the stirring rate to 80-180 rpm and then aging for 1-10 hours, or more preferably reducing the stirring rate to 100-150 rpm and then aging for 2-8 hours.

[0031] In this invention, the system establishes a slurry circulation path between the pre-oxidation reactor and the deep oxidation reactor. By continuously circulating a portion of the slurry into the pre-oxidation reactor for grinding, the grinding media (such as spherical, cylindrical, or elliptical zirconium oxide or zirconium silicate) and the grinding wheel continuously peel off the dense oxide film formed on the surface of the manganese particles, continuously exposing the fresh manganese reaction surface inside. This solves the problem in conventional single reaction vessels where the oxide film blocks the contact between manganese and oxidizing gases, resulting in extremely slow reaction rates or even forced termination.

[0032] In this invention, by placing the pre-oxidation slurry outlet and the pre-oxidation return slurry inlet at the bottom of the pre-oxidation reactor, the deep oxidation slurry inlet at the top of the deep oxidation reactor, and the deep oxidation return slurry outlet at the bottom of the deep oxidation reactor, the slurry can be continuously circulated along a path from the bottom of the deep oxidation reactor, into the bottom of the pre-oxidation reactor, and then out to the top of the deep oxidation reactor. This ensures that large, unreacted manganese particles are always in the circulating grinding path, while allowing some small particles that have already undergone preliminary oxidation to enter the deep oxidation stage earlier. Combined with the continuous peeling of the oxide film and exposure of fresh reaction surfaces during the pre-oxidation stage, the overall reaction efficiency is improved. It should be noted that each pipeline used for slurry and gas transportation in this invention is independently equipped with a pipeline valve.

[0033] In this invention, while existing industrial sand mills possess powerful grinding and peeling capabilities and can effectively solve surface passivation problems, their design is primarily for physical crushing. They typically employ a closed, solid shaft structure, which prevents the effective introduction of gas into the grinding chamber. Simply introducing gas through external pipes can easily lead to gas accumulation around the shaft, causing air resistance or idling, or excessively large bubbles resulting in insufficient gas-liquid contact area and low oxidation efficiency. Therefore, this invention improves upon existing industrial sand mills by designing the grinding wheel and shaft as interconnected hollow structures and creating ventilation holes on the grinding wheel surface to obtain the abrasive mechanism with its unique structure. In the pre-oxidation reactor, external oxidizing gas (preferably oxygen) is directly introduced into the internal cavity of the shaft. The oxidizing gas is directly and uniformly dispersed into the slurry of the pre-oxidation reactor through the ventilation holes on the grinding wheel surface, significantly improving the dispersion of oxygen in the slurry and enhancing the mass transfer efficiency of the gas-liquid-solid three-phase system. Furthermore, residual oxygen that has not fully reacted in the pre-oxidation reactor is transported to the deep oxidation reactor for reuse via a gas transfer pipeline (it should be noted that the deep oxidation reactor can also be independently supplied with gas through a deep oxidation gas inlet pipe, and independent gas supply is mainly carried out in the middle and late stages of crystal growth and aging), which effectively improves the overall utilization rate of oxygen and reduces production energy consumption and raw material costs.

[0034] In this invention, a dense oxide film formed on the surface of metallic manganese is continuously peeled off through a cyclic pre-oxidation grinding process, solving the problem of the oxide film blocking the continuous reaction and effectively improving the overall reaction rate. By outputting oxidizing gas from the hollow rotating shaft and grinding wheel, it can both assist stirring and promote the uniform dispersion of oxygen in the slurry, thus enhancing the gas-liquid mass transfer effect. The oxygen that is not fully reacted in the pre-oxidation stage can be passed into the deep oxidation reactor for secondary use, improving oxygen utilization, reducing production costs, and avoiding the introduction of impurity ions. The prepared manganese tetroxide has high purity, meeting the requirements for use in battery-grade materials.

[0035] In this invention, both the pre-oxidation reactor and the deep oxidation reactor use electric heating (e.g., electric heating plate or microwave heater) or water bath or oil bath heating to achieve temperature control of the reaction system. Preferably, the oil bath method is used, that is, a jacketed chamber (i.e., a pre-oxidation liquid constant temperature jacket and a deep oxidation liquid constant temperature jacket) is opened in the wall (side wall and / or bottom wall) of the pre-oxidation reactor and the deep oxidation reactor. By continuously introducing oil of a certain temperature into the jacketed chamber, the internal temperature of the reactor is kept constant.

[0036] In this invention, when preparing manganese tetroxide using the system of this invention, the entire reaction process is divided into three stages: the initial crushing and pre-oxidation stage: pure metallic manganese is mixed with the reaction base liquid (ammonium salt solution) to form a mixed slurry, and the slurry is circulated between the pre-oxidation reactor and the deep oxidation reactor by the circulation pump (the pumping flow rate is generally 100~1000L / h); oxidizing gas is axially dispersed into the pre-oxidation reactor through the abrasive mechanism, and the physical shear force of the grinding media is used to break the oxide passivation layer on the surface of the manganese sheet, so that the fresh manganese interface comes into contact with oxygen for oxidation, and the generated grinding pre-oxidation slurry is then returned to the deep oxidation reactor (generally, the pre-oxidation reactor and the deep oxidation reactor are designed with staggered heights, so that the slurry in the pre-oxidation reactor can be input into the deep oxidation reactor through the transfer pipe under the action of gravity). Intermediate crystal growth stage: After the pre-oxidation of metallic manganese is completed, the grinding operation of the abrasive mechanism in the pre-oxidation reactor is stopped; all the pre-oxidized slurry in the pre-oxidation reactor is discharged into the deep oxidation reactor to continue the reaction (using a circulating pump for reverse suction, while simultaneously purging the chamber with inert gas through the top purge feed pipe, and using gas pressure purging and bottom back suction to discharge the residual slurry in the chamber back into the deep oxidation reactor), promoting the growth of manganese tetroxide crystals in a homogeneous suspension. Late aging stage: When the pH of the system in the deep oxidation reactor no longer changes (generally, the pH decreases to approximately 7.0 and remains stable for more than 1 hour), the stirring speed is reduced in the deep oxidation reactor to carry out the aging reaction. Aging promotes the dissolution of small crystals and the growth of large crystals, resulting in a more uniform crystal size distribution and a more stable crystal structure in the final product. The obtained product is easier to wash and filter subsequently, improving product yield and purity. In other words, the present invention adopts a segmented reaction process. First, the oxide film is stripped and initially oxidized in the pre-oxidation stage, and then fully oxidized in the deep oxidation reactor. Finally, the target product is obtained by aging and crystallization. The entire production process does not require the introduction of additional strong oxidants and will not introduce impurity ions. The prepared manganese tetroxide product has high purity and low impurity content, which can directly meet the requirements for the use of battery-grade manganese tetroxide. The process is green and environmentally friendly and suitable for large-scale industrial production.

[0037] Compared with the prior art, the beneficial technical effects of the present invention are as follows:

[0038] 1. Significantly improve reaction conversion rate and reaction rate: This invention constructs an external circulation system between the reactor and the sand mill, and utilizes the mechanical shearing force of the grinding media in the sand mill to continuously peel off the oxide passivation layer on the surface of the manganese metal sheet, so that the fresh metal surface can undergo an in-situ oxidation reaction with oxygen, effectively avoiding reaction stagnation caused by surface passivation, improving the conversion rate of manganese metal and shortening the reaction cycle.

[0039] 2. Effectively improve oxygen utilization: A hollow ventilated grinding wheel is used for axial gas supply. The rotation of the grinding wheel shears and disperses the gas into the slurry for primary pre-oxidation. At the same time, the unreacted residual gas discharged from the top of the sand mill is introduced into the bottom of the reactor for secondary bubbling reaction, realizing the cascade series utilization of gaseous oxidant and improving the gas-liquid-solid three-phase mass transfer efficiency and total oxygen utilization rate.

[0040] 3. Protection of Crystal Morphology and Structure: This invention employs a three-stage decoupled process to physically isolate the early high-shear pre-oxidation from the later low-shear crystal growth and aging processes. The crystal growth and aging stages are carried out in a deep oxidation reactor without abrasive media, and the fluid shear force is reduced simultaneously, avoiding continuous mechanical stress that could damage the surface of the manganese tetroxide crystals, thus ensuring the sphericity and structural integrity of the final product. Attached Figure Description

[0041] Figure 1 This is a schematic diagram of the overall structure of the system described in this invention.

[0042] Figure 2 This is a schematic diagram of the pre-oxidation reactor described in this invention.

[0043] Figure 3 This is a schematic diagram of the deep oxidation reactor described in this invention.

[0044] Figure reference numerals: 1: Pre-oxidation reactor; 101: Pre-oxidation slurry outlet; 102: Pre-oxidation return slurry inlet; 103: Pre-oxidation air inlet pipe; 104: Pre-oxidation exhaust pipe; 105: Rotary connector; 106: Purge feed pipe; 107: Pre-oxidation liquid constant temperature jacket; 2: Deep oxidation reactor; 201: Deep oxidation slurry inlet; 202: Deep oxidation return slurry outlet; 203: Deep oxidation air inlet pipe; 204: Deep oxidation discharge outlet; 205: Deep oxidation exhaust pipe; 206: Deep oxidation feed pipe; 207: Deep oxidation liquid constant temperature jacket; 3: Abrasive mechanism; 301: Abrasive drive; 302: Rotating shaft; 303: Grinding wheel; 4: Stirring mechanism; 401: Stirring drive; 402: Stirring shaft; 403: Stirring paddle; 5: Slurry transfer pipe; 6: Return slurry pipe; 7: Circulation pump; 8: Gas transfer pipe. Detailed Implementation

[0045] The technical solution of the present invention will be illustrated below with examples. The scope of protection sought by the present invention includes, but is not limited to, the following embodiments.

[0046] A system for producing manganese tetroxide based on cyclic pre-oxidation is disclosed. The system includes a pre-oxidation reactor 1 and a deep oxidation reactor 2. An abrasive mechanism 3 is installed inside the cavity of the pre-oxidation reactor 1. A stirring mechanism 4 is installed inside the cavity of the deep oxidation reactor 2.

[0047] The pre-oxidation reactor 1 has a pre-oxidation slurry outlet 101, a pre-oxidation return slurry inlet 102, and a pre-oxidation air inlet pipe 103 at its lower part, and a pre-oxidation exhaust pipe 104 at its upper part. The deep oxidation reactor 2 has a deep oxidation slurry inlet 201, a deep oxidation exhaust pipe 205, and a deep oxidation feed pipe 206 at its upper part, and a deep oxidation return slurry outlet 202, a deep oxidation air inlet pipe 203, and a deep oxidation discharge outlet 204 at its lower part. The pre-oxidation slurry outlet 101 is connected to the deep oxidation slurry inlet 201 via a transfer pipe 5. The deep oxidation return slurry outlet 202 is connected to the pre-oxidation return slurry inlet 102 via a return slurry pipe 6. A circulation pump 7 is installed on the return slurry pipe 6.

[0048] Preferably, the abrasive mechanism 3 includes an abrasive drive 301, a rotating shaft 302, and a grinding wheel 303. The abrasive drive 301 is disposed on the top cover surface of the pre-oxidation reactor 1. The top end of the rotating shaft 302 passes through the top cover of the pre-oxidation reactor 1 and is connected to the abrasive drive 301, while its bottom end extends downward to the lower part of the inner cavity of the pre-oxidation reactor 1. The grinding wheel 303 is disposed on the rotating shaft 302 located in the inner cavity of the pre-oxidation reactor 1. Preferably, the inner cavity of the pre-oxidation reactor 1 is filled with abrasive media (e.g., spherical, cylindrical, or elliptical zirconium oxide or zirconium silicate).

[0049] Preferably, both the rotating shaft 302 and the grinding wheel 303 are hollow structures, and the shaft cavity of the rotating shaft 302 is connected to the wheel cavity of the grinding wheel 303. The grinding wheel 303 has several vent holes, and its cavity is connected to the inner cavity of the pre-oxidation reactor 1 through these vent holes. The pre-oxidation inlet pipe 103 is located at the bottom of the pre-oxidation reactor 1, and its exhaust end extends upwards to connect with the shaft cavity of the rotating shaft 302. The pre-oxidation inlet pipe 103 is connected to the bottom wall of the pre-oxidation reactor 1 and the bottom end of the rotating shaft 302 via a rotary connector 105. Preferably, the rotary connector 105 is a sealed bearing.

[0050] Preferably, the pre-oxidation exhaust pipe 104 is connected to the deep oxidation inlet pipe 203 via a gas transfer pipe 8. A purge feed pipe 106 is also provided at the top of the pre-oxidation reactor 1.

[0051] Preferably, a heater is also provided on the outer wall of the pre-oxidation reactor 1, or the interior of the wall (side wall and / or bottom wall) of the pre-oxidation reactor 1 is hollow to form a pre-oxidation liquid constant temperature jacket 107. Preferably, the heater is an electric heating plate or a microwave heater. The pre-oxidation liquid constant temperature jacket 107 is an oil bath constant temperature jacket or a water bath constant temperature jacket.

[0052] Preferably, the stirring mechanism 4 includes a stirring drive 401, a stirring shaft 402, and a stirring paddle 403. The stirring drive 401 is disposed on the top cover surface of the deep oxidation reactor 2. The top end of the stirring shaft 402 passes through the top cover of the deep oxidation reactor 2 and is connected to the stirring drive 401, while its bottom end extends downward to the lower part of the inner cavity of the deep oxidation reactor 2. The stirring paddle 403 is disposed on the stirring shaft 402 located in the inner cavity of the deep oxidation reactor 2. Preferably, the stirring paddle 403 is a stirring blade or a stirring rod.

[0053] Preferably, a heater is also provided on the outer wall of the deep oxidation reactor 2, or the interior of the wall (side wall and / or bottom wall) of the deep oxidation reactor 2 is hollow to form a deep oxidation liquid constant temperature jacket 207. Preferably, the heater is an electric heating plate or a microwave heater. The deep oxidation liquid constant temperature jacket 207 is an oil bath constant temperature jacket or a water bath constant temperature jacket.

[0054] Example 1

[0055] like Figure 1-3 As shown, a system for producing manganese tetroxide based on cyclic pre-oxidation is disclosed. The system includes a pre-oxidation reactor 1 and a deep oxidation reactor 2. An abrasive mechanism 3 is installed inside the cavity of the pre-oxidation reactor 1. A stirring mechanism 4 is installed inside the cavity of the deep oxidation reactor 2.

[0056] The pre-oxidation reactor 1 has a pre-oxidation slurry outlet 101, a pre-oxidation return slurry inlet 102, and a pre-oxidation air inlet pipe 103 at its lower part, and a pre-oxidation exhaust pipe 104 at its upper part. The deep oxidation reactor 2 has a deep oxidation slurry inlet 201, a deep oxidation exhaust pipe 205, and a deep oxidation feed pipe 206 at its upper part, and a deep oxidation return slurry outlet 202, a deep oxidation air inlet pipe 203, and a deep oxidation discharge outlet 204 at its lower part. The pre-oxidation slurry outlet 101 is connected to the deep oxidation slurry inlet 201 via a transfer pipe 5. The deep oxidation return slurry outlet 202 is connected to the pre-oxidation return slurry inlet 102 via a return slurry pipe 6. A circulation pump 7 is installed on the return slurry pipe 6.

[0057] Example 2

[0058] The embodiment 1 is repeated, except that the abrasive mechanism 3 includes an abrasive drive 301, a rotating shaft 302, and a grinding wheel 303. The abrasive drive 301 is disposed on the top cover surface of the pre-oxidation reactor 1. The top end of the rotating shaft 302 passes through the top cover of the pre-oxidation reactor 1 and is connected to the abrasive drive 301, while its bottom end extends downward to the lower part of the inner cavity of the pre-oxidation reactor 1. The grinding wheel 303 is disposed on the rotating shaft 302 located in the inner cavity of the pre-oxidation reactor 1.

[0059] Example 3

[0060] Example 2 was repeated, except that the inner cavity of the pre-oxidation reactor 1 was filled with grinding media.

[0061] Example 4

[0062] The embodiment 3 is repeated, except that both the rotating shaft 302 and the grinding wheel 303 are hollow structures, and the shaft cavity of the rotating shaft 302 is connected to the wheel cavity of the grinding wheel 303. The grinding wheel 303 has several vent holes, and its cavity is connected to the inner cavity of the pre-oxidation reactor 1 through these vent holes. The pre-oxidation inlet pipe 103 is located at the bottom of the pre-oxidation reactor 1, and its exhaust end extends upwards to connect with the shaft cavity of the rotating shaft 302. The pre-oxidation inlet pipe 103 is connected to the bottom wall of the pre-oxidation reactor 1 and the bottom end of the rotating shaft 302 via a rotating connector 105.

[0063] Example 5

[0064] Example 4 is repeated, except that the rotating connector 105 is a sealed bearing.

[0065] Example 6

[0066] Example 5 is repeated, except that the pre-oxidation exhaust pipe 104 is connected to the deep oxidation inlet pipe 203 via the gas transfer pipe 8. A purge feed pipe 106 is also provided at the top of the pre-oxidation reactor 1.

[0067] Example 7

[0068] Example 6 was repeated, except that a microwave heater was also provided on the outer wall of the pre-oxidation reactor 1.

[0069] Example 8

[0070] Example 6 is repeated, except that the interior of the pre-oxidation reactor 1 (including the side walls and bottom walls) is hollow to form a pre-oxidation liquid constant temperature jacket 107. The pre-oxidation liquid constant temperature jacket 107 is a water bath constant temperature jacket.

[0071] Example 9

[0072] The process is repeated in Embodiment 8, except that the stirring mechanism 4 includes a stirring drive 401, a stirring shaft 402, and a stirring paddle 403. The stirring drive 401 is disposed on the top cover surface of the deep oxidation reactor 2. The top end of the stirring shaft 402 passes through the top cover of the deep oxidation reactor 2 and is connected to the stirring drive 401, while its bottom end extends downward to the lower part of the inner cavity of the deep oxidation reactor 2. The stirring paddle 403 is disposed on the stirring shaft 402 located in the inner cavity of the deep oxidation reactor 2.

[0073] Example 10

[0074] Example 9 is repeated, except that the stirring paddle 403 is a stirring blade.

[0075] Example 11

[0076] Example 10 is repeated, except that an electric heating plate is also provided on the outer wall of the deep oxidation reactor 2.

[0077] Example 12

[0078] Example 10 is repeated, except that the interior of the deep oxidation reactor 2 (including the side walls and bottom walls) is hollow to form a deep oxidation liquid isothermal jacket 207. The deep oxidation liquid isothermal jacket 207 is an oil bath isothermal jacket.

[0079] The system described in this invention is used as follows: First, metallic manganese and a reaction base liquid (e.g., ammonium chloride solution) are optionally added to a pre-oxidation reactor 1 (pre-filled with 60-85% grinding media with a particle size of 0.3-1 mm) and / or a deep oxidation reactor 2. Then, the circulation pump 7 is started and the transfer pipe 5 and return pipe 6 are opened, so that the slurry circulates between the pre-oxidation reactor 1 and the deep oxidation reactor 2. Then, oxygen is introduced into the pre-oxidation reactor 1 and the deep oxidation reactor 2 through the pre-oxidation air inlet pipe 103, the rotating shaft 302 and the cavity channel in the grinding wheel 303, the pre-oxidation exhaust pipe 104, and the deep oxidation air inlet pipe 203. At the same time, the abrasive mechanism 3 and the stirring mechanism 4 are started to perform pre-oxidation treatment. After the pre-oxidation treatment is completed, the abrasive mechanism 3 is shut down. The circulating pump 7 is used for reverse suction, and nitrogen gas is blown into the pre-oxidation reactor 1 through the purge feed pipe 106, ensuring that the slurry in the pre-oxidation reactor 1 is returned to the deep oxidation reactor 2. Then, the circulating pump 7 is shut down, and the transfer pipe 5 and return pipe 6 are opened, maintaining the stirring, temperature, and oxygen supply in the deep oxidation reactor 2 for deep oxidation treatment. After the deep oxidation treatment is completed, the stirring rate in the deep oxidation reactor 2 is reduced to allow for aging. After aging, a solid product is obtained through solid-liquid separation. The solid product is washed with deionized water (1-10 times) and then dried (80-150℃) to obtain the target manganese tetroxide product.

[0080] Method Example 1

[0081] S1. An ammonium chloride solution (approximately 0.2 mol / L) and manganese metal powder (99.9% purity, approximately 200 mesh particle size) are added to the deep oxidation reactor 2 at a liquid-to-solid mass ratio of 8:1 and stirred to form a suspension slurry. Then, the circulation pump 7 is started (flow rate controlled at 500 L / h), and the transfer pipe 5 and return pipe 6 are opened, allowing the slurry to circulate between the pre-oxidation reactor 1 and the deep oxidation reactor 2. Zirconia beads with a particle size of approximately 0.8 mm are filled into the pre-oxidation reactor 1, with a filling rate of approximately 75%.

[0082] S2. Start the abrasive mechanism 3 (controlling the rotation speed of the rotating shaft 302 to 1000 rpm) and the stirring mechanism 4 (controlling the rotation speed of the stirring shaft 402 to 300 rpm), and introduce pure oxygen (99.999%, flow rate of 1 L / min) into the pre-oxidation reactor 1 through the pre-oxidation inlet pipe 103, the rotating shaft 302, and the grinding wheel 303. Excess oxygen enters the deep oxidation reactor 2 through the pre-oxidation exhaust pipe 104, the gas transfer pipe 8, and the deep oxidation inlet pipe 203. At the same time, constant temperature oil is introduced into the pre-oxidation liquid constant temperature jacket 107 and the deep oxidation liquid constant temperature jacket 207 to maintain the slurry temperature in the pre-oxidation reactor 1 and the deep oxidation reactor 2 at 75°C, and the pre-oxidation reaction is carried out continuously for 6 hours.

[0083] S3. After the pre-oxidation treatment is completed, all the slurry is returned to the deep oxidation reactor 2 and the abrasive mechanism 3, circulation pump 7, slurry transfer pipe 5 and return slurry pipe 6 are turned off. The oxygen introduction rate, temperature and stirring in the deep oxidation reactor 2 are kept constant and the reaction continues until the pH value of the slurry drops to between 7.0 and 7.5 and can remain stable for 1 hour (total time is about 4 hours).

[0084] S4. After the deep oxidation treatment is completed, reduce the stirring speed in the deep oxidation reactor 2 to 100 rpm and age for 2 hours. After aging, filter and wash the obtained solid product 5 times with deionized water. Finally, dry it in an oven at 110℃ to obtain manganese tetroxide product (purity is about 98.80%, average D50 is about 8.0 μm).

[0085] Method Example 2

[0086] S1. Ammonium chloride solution (approximately 0.3 mol / L) and manganese metal powder (99.8% purity, approximately 200 mesh particle size) are added to the deep oxidation reactor 2 at a liquid-to-solid mass ratio of 10:1 and stirred to form a suspension slurry. Then, the circulation pump 7 is started (flow rate controlled at 500 L / h), and the transfer pipe 5 and return pipe 6 are opened, allowing the slurry to circulate between the pre-oxidation reactor 1 and the deep oxidation reactor 2. Zirconia beads with a particle size of approximately 0.5 mm are filled into the pre-oxidation reactor 1, with a filling rate of approximately 80%.

[0087] S2. Start the abrasive mechanism 3 (controlling the rotation speed of the rotating shaft 302 to 1200 rpm) and the stirring mechanism 4 (controlling the rotation speed of the stirring shaft 402 to 400 rpm), and introduce pure oxygen (99.999%, flow rate 1.2 L / min) into the pre-oxidation reactor 1 through the pre-oxidation inlet pipe 103, the rotating shaft 302, and the grinding wheel 303. Excess oxygen enters the deep oxidation reactor 2 through the pre-oxidation exhaust pipe 104, the gas transfer pipe 8, and the deep oxidation inlet pipe 203. At the same time, constant temperature oil is introduced into the pre-oxidation liquid constant temperature jacket 107 and the deep oxidation liquid constant temperature jacket 207 to maintain the slurry temperature in the pre-oxidation reactor 1 and the deep oxidation reactor 2 at 75°C, and the pre-oxidation reaction is carried out continuously for 5 hours.

[0088] S3. After the pre-oxidation treatment is completed, all the slurry is returned to the deep oxidation reactor 2 and the abrasive mechanism 3, circulation pump 7, slurry transfer pipe 5 and return slurry pipe 6 are turned off. The oxygen introduction rate, temperature and stirring in the deep oxidation reactor 2 are kept constant and the reaction continues until the pH value of the slurry drops to between 7.0 and 7.5 and can remain stable for 1 hour (total time is about 3 hours).

[0089] S4. After the deep oxidation treatment is completed, reduce the stirring rate in the deep oxidation reactor 2 to 150 rpm and age for 4 hours. After aging, filter and wash the obtained solid product 5 times with deionized water. Finally, dry it in an oven at 110℃ to obtain manganese tetroxide product (purity is about 99.2%, average D50 is about 5.0 μm).

[0090] Method Example 3

[0091] S1. Ammonium chloride solution (approximately 0.4 mol / L) and manganese metal powder (99.5% purity, approximately 200 mesh particle size) are added to the deep oxidation reactor 2 at a liquid-to-solid mass ratio of 6:1 and stirred to form a suspension slurry. Then, the circulation pump 7 is started (flow rate controlled at 500 L / h), and the transfer pipe 5 and return pipe 6 are opened, allowing the slurry to circulate between the pre-oxidation reactor 1 and the deep oxidation reactor 2. Zirconium silicate beads with a particle size of approximately 1.0 mm are filled into the pre-oxidation reactor 1, with a filling rate of approximately 70%.

[0092] S2. Start the abrasive mechanism 3 (controlling the rotation speed of the rotating shaft 302 to 800 rpm) and the stirring mechanism 4 (controlling the rotation speed of the stirring shaft 402 to 250 rpm), and introduce pure oxygen (99.999%, flow rate 0.8 L / min) into the pre-oxidation reactor 1 through the pre-oxidation inlet pipe 103, the rotating shaft 302, and the grinding wheel 303. Excess oxygen enters the deep oxidation reactor 2 through the pre-oxidation exhaust pipe 104, the gas transfer pipe 8, and the deep oxidation inlet pipe 203. At the same time, constant temperature oil is introduced into the pre-oxidation liquid constant temperature jacket 107 and the deep oxidation liquid constant temperature jacket 207 to maintain the slurry temperature in the pre-oxidation reactor 1 and the deep oxidation reactor 2 at 75°C, and the pre-oxidation reaction is carried out continuously for 8 hours.

[0093] S3. After the pre-oxidation treatment is completed, all the slurry is returned to the deep oxidation reactor 2 and the abrasive mechanism 3, circulation pump 7, slurry transfer pipe 5 and return slurry pipe 6 are turned off. The oxygen introduction rate, temperature and stirring in the deep oxidation reactor 2 are kept constant and the reaction continues until the pH value of the slurry drops to between 7.0 and 7.5 and can remain stable for 1 hour (total time is about 5 hours).

[0094] S4. After the deep oxidation treatment is completed, reduce the stirring rate in the deep oxidation reactor 2 to 80 rpm and age for 6 hours. After aging, filter and wash the obtained solid product 5 times with deionized water. Finally, dry it in an oven at 110℃ to obtain manganese tetroxide product (purity is about 98.50%, average D50 is about 18.0 μm).

[0095] Comparative Example 1

[0096] Ammonium chloride solution (approximately 0.2 mol / L) and manganese metal powder (purity 99.9%, particle size approximately 200 mesh) were added to a reaction vessel at a liquid-to-solid mass ratio of 8:1. The product was obtained under the following reaction conditions: reaction temperature 75℃, stirring speed 300 rpm, feeding interval 10 min, feeding number 6 times, oxygen flow rate 1 L / min, and reaction time 20 h. The obtained solid product was washed 5 times with deionized water and finally dried in an oven at 110℃ to obtain manganese tetroxide product (purity approximately 97.68%, average D50 approximately 8.82 μm).

[0097] Comparative Example 2

[0098] Ammonium chloride solution (approximately 0.3 mol / L) and manganese metal powder (purity 99.8%, particle size approximately 200 mesh) were added to a reaction vessel at a liquid-to-solid mass ratio of 10:1. The product was obtained under the following reaction conditions: reaction temperature 75℃, stirring speed 400 rpm, feeding interval 10 min, feeding number 6 times, oxygen flow rate 1 L / min, and reaction time 20 h. The obtained solid product was washed 5 times with deionized water and finally dried in an oven at 110℃ to obtain manganese tetroxide product (purity approximately 97.93%, average D50 approximately 7.28 μm).

[0099] In this invention, the above embodiments are merely preferred embodiments and are not intended to limit the scope of the invention. Those skilled in the art should understand that any equivalent modifications or substitutions made without departing from the scope of the technical solutions disclosed in this invention should be covered within the protection scope of this invention.

Claims

1. A system for producing manganese tetroxide based on cyclic pre-oxidation, characterized in that: The system includes a pre-oxidation reactor (1) and a deep oxidation reactor (2); an abrasive mechanism (3) is provided in the inner cavity of the pre-oxidation reactor (1); and a stirring mechanism (4) is provided in the inner cavity of the deep oxidation reactor (2). The pre-oxidation reactor (1) is provided with a pre-oxidation slurry outlet (101), a pre-oxidation return slurry inlet (102) and a pre-oxidation air inlet pipe (103) at the bottom and a pre-oxidation exhaust pipe (104) at the top. The deep oxidation reactor (2) is provided with a deep oxidation slurry inlet (201), a deep oxidation exhaust pipe (205) and a deep oxidation feed pipe (206) at the top and a deep oxidation return slurry outlet (202), a deep oxidation air inlet pipe (203) and a deep oxidation discharge outlet (204) at the bottom. The pre-oxidation slurry outlet (101) is connected to the deep oxidation slurry inlet (201) through a transfer pipe (5). The deep oxidation return slurry outlet (202) is connected to the pre-oxidation return slurry inlet (102) through a return slurry pipe (6). A circulation pump (7) is provided on the return slurry pipe (6).

2. The system according to claim 1, characterized in that: The abrasive mechanism (3) includes an abrasive drive (301), a rotating shaft (302), and a grinding wheel (303); the abrasive drive (301) is disposed on the top cover surface of the pre-oxidation reactor (1); the top end of the rotating shaft (302) passes through the top cover of the pre-oxidation reactor (1) and is connected to the abrasive drive (301), and its bottom end extends downward to the lower part of the inner cavity of the pre-oxidation reactor (1); the grinding wheel (303) is disposed on the rotating shaft (302) located in the inner cavity of the pre-oxidation reactor (1); preferably, the inner cavity of the pre-oxidation reactor (1) is filled with abrasive media.

3. The system according to claim 2, characterized in that: Both the rotating shaft (302) and the grinding wheel (303) are hollow structures, and the shaft cavity of the rotating shaft (302) is connected to the wheel cavity of the grinding wheel (303). The grinding wheel (303) has several ventilation holes, and the wheel cavity of the grinding wheel (303) is connected to the inner cavity of the pre-oxidation reactor (1) through the ventilation holes. The pre-oxidation inlet pipe (103) is located at the bottom of the pre-oxidation reactor (1), and the exhaust end of the pre-oxidation inlet pipe (103) extends upward and is connected to the shaft cavity of the rotating shaft (302). The pre-oxidation inlet pipe (103) is connected to the bottom wall of the pre-oxidation reactor (1) and the bottom end of the rotating shaft (302) through a rotating connector (105). Preferably, the rotating connector (105) is a sealed bearing.

4. The system according to any one of claims 1-3, characterized in that: The pre-oxidation exhaust pipe (104) is connected to the deep oxidation inlet pipe (203) through the gas transfer pipe (8); a purge feed pipe (106) is also provided at the top of the pre-oxidation reactor (1).

5. The system according to any one of claims 1-4, characterized in that: A heater is also provided on the outer wall of the pre-oxidation reactor (1), or the interior of the wall (side wall and / or bottom wall) of the pre-oxidation reactor (1) is hollow to form a pre-oxidation liquid constant temperature jacket (107); preferably, the heater is an electric heating plate or a microwave heater; the pre-oxidation liquid constant temperature jacket (107) is an oil bath constant temperature jacket or a water bath constant temperature jacket.

6. The system according to any one of claims 1-5, characterized in that: The stirring mechanism (4) includes a stirring drive (401), a stirring shaft (402), and a stirring paddle (403); the stirring drive (401) is disposed on the top cover surface of the deep oxidation reactor (2); the top end of the stirring shaft (402) passes through the top cover of the deep oxidation reactor (2) and is connected to the stirring drive (401), and its bottom end extends downward to the lower part of the inner cavity of the deep oxidation reactor (2); the stirring paddle (403) is disposed on the stirring shaft (402) located in the inner cavity of the deep oxidation reactor (2); preferably, the stirring paddle (403) is a stirring blade or a stirring rod.

7. The system according to any one of claims 1-6, characterized in that: A heater is also provided on the outer wall of the deep oxidation reactor (2), or the interior of the wall (side wall and / or bottom wall) of the deep oxidation reactor (2) is hollow to form a deep oxidation liquid constant temperature jacket (207); preferably, the heater is an electric heating plate or a microwave heater; the deep oxidation liquid constant temperature jacket (207) is an oil bath constant temperature jacket or a water bath constant temperature jacket.

8. A method for producing manganese tetroxide based on cyclic pre-oxidation or a method for producing manganese tetroxide using the system described in any one of claims 1-7, characterized in that: The method includes the following steps: S1. Add the manganese metal and ammonium salt solution to the deep oxidation reactor (2) to form a slurry, start the circulation pump (7) and open the transfer pipe (5) and return pipe (6) so that the slurry circulates between the pre-oxidation reactor (1) and the deep oxidation reactor (2); S2. Start the abrasive mechanism (3) and the stirring mechanism (4), and introduce oxidizing gas into the pre-oxidation reactor (1) and the deep oxidation reactor (2) for pre-oxidation treatment; S3. After the pre-oxidation treatment is completed, all the slurry is returned to the deep oxidation reactor (2) and the abrasive mechanism (3), circulation pump (7), slurry transfer pipe (5) and return slurry pipe (6) are turned off. Stirring is continued for deep oxidation treatment. S4. After the deep oxidation treatment is completed, reduce the stirring rate and carry out aging treatment. After aging, perform solid-liquid separation, and wash and dry the obtained solid product in sequence to obtain the target manganese tetroxide product.

9. The method according to claim 8, characterized in that: In step S1, the metallic manganese is manganese powder or manganese flakes, preferably with a particle size of 0.025~2mm; and / or In step S1, the ammonium salt solution is one or more of ammonium chloride solution, ammonium sulfate solution, ammonium acetate solution, and ammonium oxalate solution, preferably an ammonium chloride solution; The concentration of the ammonium salt solution is 0.1~1 mol / L, preferably 0.2~0.5 mol / L; and / or In step S1, the liquid-solid mass ratio of the ammonium salt solution to metallic manganese is 2~15:1, preferably 3~10:

1.

10. The method according to claim 8 or 9, characterized in that: In step S2, the pre-oxidation treatment temperature is 50~80℃, preferably 60~75℃; the pre-oxidation treatment duration is not less than 1 hour, preferably 3~10 hours; the oxidizing gas is oxygen, and the oxygen flow rate is 0.5~2L / min, preferably 0.8~1.5L / min; the abrasive rotation speed is not less than 500 rpm, preferably 800~1500 rpm; the stirring speed is not less than 200 rpm, preferably 300~800 rpm; and / or In step S3, the endpoint of the deep oxidation treatment is that the pH of the slurry no longer changes, preferably the pH of the slurry decreases to 7.0 ± 0.5 and remains stable for at least 1 hour; and / or In step S4, the aging process by reducing the stirring rate specifically involves reducing the stirring rate to 80-180 rpm and aging for 1-10 hours, preferably reducing the stirring rate to 100-150 rpm and aging for 2-8 hours.