A method for preparing aerogel material by using reverse phase microemulsion

By combining the reverse microemulsion method with atmospheric pressure drying to prepare aerogels, the problems of expensive equipment, complex processes and significant safety hazards in existing technologies have been solved, enabling low-cost and environmentally friendly preparation of aerogels and their application in thermal insulation and fireproofing materials.

CN123127922APending Publication Date: 2026-11-20FUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611601474.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-16
Publication Date
2026-11-20

Smart Images

  • Figure CN123127922A_ABST
    Figure CN123127922A_ABST
Patent Text Reader

Abstract

The application discloses a method for preparing aerogel material by using a reverse microemulsion method, and belongs to the technical field of aerogel preparation. The reverse microemulsion method is combined with normal-pressure drying, only waste liquid is produced, and the use of CO2 and ethanol is avoided, so that the cost is reduced, and the environmental protection and safety are improved. The structure of the prepared aerogel is a porous structure formed by skeleton material. The skeleton material is continuously distributed, the single diameter of the skeleton is 4-8 nm, and a large number of pores with a diameter distribution range of 5-30 nm exist in the skeleton, so that the prepared aerogel has a good application prospect in the preparation of thermal insulation materials and fireproof materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of aerogel preparation technology, specifically relating to a method for preparing aerogel materials using a reverse microemulsion method. Background Technology

[0002] Aerogels are solid materials with a three-dimensional porous network structure formed by interconnected nanoscale particles. They are characterized by their ultra-low density (0.003–0.200 g / cm³). 3 High porosity (80%–99.8%) and large specific surface area (500–1500 m²) 2 With its excellent properties such as W / (m·K) and extremely low thermal conductivity (0.005~0.1 W / (m·K)), it has shown broad application prospects in many fields such as aerospace, military equipment, industrial pipeline insulation, building energy conservation, new energy vehicles, as well as catalysis, sensing, and energy storage.

[0003] Currently, aerogels are typically prepared using the sol-gel method, which involves forming a wet gel from a precursor using the sol-gel process, followed by drying to obtain the aerogel product. Drying is a crucial step in determining whether the aerogel can maintain its nanoporous structure. Existing technologies primarily employ supercritical drying, freeze-drying, and atmospheric pressure drying as methods for drying wet gels.

[0004] Supercritical drying is currently a widely used drying method. This method utilizes CO2, ethanol, or other solvents to remove solvents from the pores of the gel under supercritical conditions, effectively avoiding pore structure collapse caused by capillary forces, thus obtaining aerogel products with excellent performance. However, supercritical drying processes have many inherent drawbacks, such as complex processes, expensive equipment, low yield, significant safety hazards, and difficulty in achieving continuous and large-scale production. These factors directly lead to high production costs and expensive products for silica aerogels, severely restricting their large-scale application.

[0005] Freeze-drying, as an alternative, removes the solvent by sublimation after freezing the wet gel. While this avoids capillary force damage to some extent, the growth of ice crystals during freezing can destroy the gel skeleton structure, usually resulting in only powder or granular products. It also faces the problems of high cost and complex process.

[0006] Atmospheric pressure drying has become a research hotspot in this field in recent years due to its advantages such as simple process, safety, low equipment requirements, and continuous production capability. However, existing atmospheric pressure drying technologies still have many shortcomings. First, during atmospheric pressure drying, as the solvent evaporates, the capillary forces generated within the gel pores cause severe shrinkage or even collapse of the gel network skeleton, resulting in significant product volume shrinkage, increased density, and damage to the pore structure. Second, to overcome these problems, existing atmospheric pressure drying processes typically require the consumption of large amounts of organic solvents (such as ethanol) for solvent replacement and the use of expensive surface modifiers to hydrophobize the gel. This not only prolongs the preparation cycle but also significantly increases production costs and environmental pollution risks. Furthermore, the long preparation cycle of existing atmospheric pressure drying processes makes it difficult to meet the needs of continuous industrial production.

[0007] In summary, among the existing aerogel preparation technologies, supercritical drying and freeze drying suffer from problems such as expensive equipment, complex processes, significant safety hazards, and difficulty in large-scale production; while atmospheric pressure drying faces problems such as severe product shrinkage, consumption of large amounts of organic solvents and expensive modifiers, long preparation cycles, and limited product form (mostly powder).

[0008] Therefore, developing a simple, low-cost, and short-cycle atmospheric pressure drying method for aerogels is of great practical significance for promoting the large-scale production and widespread application of aerogels. Summary of the Invention

[0009] The purpose of this invention is to provide a method for preparing aerogel materials using a reverse microemulsion method. By combining the reverse microemulsion method with atmospheric pressure drying, the preparation process is simplified and environmental and safety issues are reduced, thereby solving the environmental and safety problems caused by the complexity of existing aerogel preparation technologies and the large amount of organic solvents used.

[0010] To achieve the above objectives, the present invention adopts the following technical solution: A method for preparing aerogel materials using a reverse microemulsion method specifically includes the following steps: (1) Mix the framework material precursor and solvent and sonicate until dissolved to obtain a framework material precursor solution; (2) Stir the oil phase solvent, surfactant and solvent evenly, and then add them to the solution obtained in step (1), and stir for 10~100 min; (3) Prepare an acid solution containing a crosslinking agent and add it to the solution obtained in step (2), and stir for 12-24 hours; (4) The solution obtained in step (3) is centrifuged, washed and dried to obtain aerogel material; The aerogel material comprises a porous network structure with a nanoskeleton diameter of 4–8 nm, a pore size of 2–20 nm, a porous network structure size of 1–100 μm, and a density of 10–150 kg / m³. 3 Surface area is 600-1500 m² 2 / g.

[0011] Furthermore, the precursor material of the skeleton material mentioned in step (1) includes: tetraethyl orthosilicate, methyl orthosilicate, polysiloxane, methyltrimethoxysilane, methyltriethoxysilane, sodium silicate, silica sol, rice husk, fly ash, cerium nitrate, yttrium nitrate, lanthanum nitrate, praseodymium nitrate, neodymium nitrate, promethium nitrate, samarium nitrate, europium nitrate, gadolinium nitrate, holmium nitrate, dysprosium nitrate, lutetium nitrate, erbium nitrate, terbium nitrate, thulium nitrate, ytterbium nitrate, tetrabutyl titanate, titanium tetrachloride, titanium sulfate, zirconium oxychloride, zirconium propoxide, ferric nitrate, ferric sulfate, ferric chloride, zinc nitrate, sulfur The solvent is one or any combination of several of the following: zinc nitrate, zinc chloride, copper nitrate, copper sulfate, copper chloride, magnesium nitrate, magnesium sulfate, magnesium chloride, nickel nitrate, nickel sulfate, nickel chloride, cobalt nitrate, cobalt sulfate, cobalt chloride, indium nitrate, indium sulfate, indium chloride, sodium tungstate, tungsten ethoxide, sodium vanadate, vanadium oxysulfate, barium oxalate, titanium oxalate, strontium oxalate, lead oxalate, bismuth oxalate, etc.; the solvent is one or any combination of several of the following: water, methanol, anhydrous ethanol, n-propanol, isopropanol, n-butanol, isobutanol, n-pentanol, isopentanol, n-hexanol, 2-hexanol, n-heptanol, n-octanol, 2-octanol, n-nonanol, n-decanol, n-dodecylol.

[0012] Furthermore, the solid-liquid ratio of the skeleton material precursor and the solvent in step (1) is 1:5~1000.

[0013] Furthermore, the oil phase solvent mentioned in step (2) is one or any combination of several of the following: n-hexane, n-heptane, n-octane, n-hexanol, isooctane, cyclohexane, petroleum ether, kerosene, soybean oil, olive oil, peanut oil, rapeseed oil, castor oil, corn oil, sunflower seed oil, coconut oil, cottonseed oil, isopropyl myristate, ethyl oleate, isopropyl palmitate, medium-chain triglycerides, glycerol caprylate, long-chain triglycerides, oleic acid, and caprylic acid.

[0014] Further, the surfactant mentioned in step (2) is hexadecyltrimethylammonium bromide, dioctadecyldimethylammonium chloride, sodium dodecyl sulfate, sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, sodium succinate sulfonate, sodium di(2-ethylhexyl)sulfonated succinate, sorbitan fatty acid ester, polyoxyethylene sorbitan fatty acid ester, polyethylene glycol octylphenyl ether, polyoxyethylene fatty alcohol ether, polyoxyethylene octylphenyl ether, octylphenol polyoxyethylene ether, KH-550, KH-560, KH-570, methoxy polyethylene glycol silane, egg white albumin, N,N-dimethylformamide, sodium hydroxide, potassium hydroxide, ammonia, sodium borohydride, potassium borohydride, etc., or any combination thereof; the solvent mentioned in step (2) is water, methanol, anhydrous ethanol, n-propanol, isopropanol, n-butanol, isobutanol, n-pentanol, isopentanol, n-hexanol, 2-hexanol, n-heptanol, n-octanol, 2-octanol, n-nonanol, n-decanol, n-dodecylol, or any combination thereof.

[0015] Furthermore, in step (2), the ratio of oil phase solvent, surfactant and solvent is 500-1000mL: 5mg-100g: 500-1000mL.

[0016] Furthermore, the crosslinking agent mentioned in step (3) is one or any combination of N,N'-methylenebisacrylamide, epichlorohydrin, glutaraldehyde, divinylbenzene, pentaerythritol triacrylate, polyethylene glycol diacrylate, calcium chloride, sodium trimetaphosphate, genipin, potassium oleate, polyethylene glycol, polyacrylic acid, polyvinylpyrrolidone, lithium hydroxide, sodium hydroxide, and potassium hydroxide; the acid solution is one or any combination of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, hydrofluoric acid, acetic acid, oxalic acid, formic acid, oleic acid, and citric acid.

[0017] Furthermore, in step (3), the acid solution of the crosslinking agent has an acid concentration of 0.1~18 mol / L, the crosslinking agent accounts for 1-10% of the solution mass, and the total volume of the acid solution containing the crosslinking agent is 0.01~5L.

[0018] Furthermore, the drying temperature in step (4) is 50~200℃, and the time is 3~24h.

[0019] The present invention also provides the application of the aerogel material prepared by the above method in the preparation of thermal insulation materials and fireproof materials.

[0020] The beneficial effects of this invention are as follows: (1) This invention uses a reverse microemulsion method to prepare aerogels, which have a porous structure formed by a framework material. The framework material is continuously distributed, with the diameter of a single fiber ranging from 4 to 8 nm, and contains a large number of pores with diameters ranging from 5 to 30 nm. Compared with traditional aerogels, the advantages of this porous structure composed of a continuous nanofiber framework are: ① When subjected to force, the stress can be effectively transmitted and dispersed along the long axis of a single fiber, rather than being concentrated at the particle contact point as in traditional aerogels, thus improving strength; ② According to the Knudsen effect, when the pore diameter is smaller than the mean free path of air molecules (approximately 70 nm at room temperature), air molecules cannot freely collide and transfer heat, causing a sharp decrease in the thermal conductivity of the gas. Pores of 5–30 nm are much smaller than 70 nm and can effectively suppress gas heat conduction.

[0021] (2) The present invention adopts centrifugation, washing and atmospheric pressure drying process, which only produces waste liquid and avoids the large-scale use of CO2 and ethanol. While reducing costs, it improves environmental protection and safety. The production equipment is simple and more suitable for large-scale production. Attached Figure Description

[0022] Figure 1 This is a SEM image of the aerogel material prepared in Example 1.

[0023] Figure 2 This is a TEM image of the aerogel material prepared in Example 1.

[0024] Figure 3 The image shows a SEM image of the silica nanoparticles prepared in Comparative Example 1. Detailed Implementation

[0025] The present invention will be further described in detail below with reference to specific embodiments. The present invention includes, but is not limited to, the following embodiments, and all equivalent substitutions and improvements made based on the technical solutions of the present invention are within the protection scope of the present invention.

[0026] Example 1 (1) Place 5g of tetraethyl orthosilicate and 1000mL of water in a beaker and sonicate until completely dissolved to obtain a silicon precursor solution.

[0027] (2) Mix 1000 mL of n-hexane, 5 g of cetyltrimethylammonium bromide and 1000 mL of methanol until homogeneous and transparent, then add to the precursor solution obtained in step (1) and stir for 10 min.

[0028] (3) Prepare 5000 mL of hydrochloric acid solution containing crosslinking agent N,N'-methylenebisacrylamide, with a hydrochloric acid concentration of 1 mol / L and N,N'-methylenebisacrylamide accounting for 5% of the solution mass, and add the solution to the solution obtained in step (2) and stir for 12 h.

[0029] (4) Centrifuge the solution obtained in step (3), collect the solid precipitate, wash it, and dry it at 50℃ for 24 hours to obtain the aerogel material. The density of the obtained aerogel material is 20 kg / m³. 3 The surface area is 1000 m² 2 / g.

[0030] (5) The aerogel material is then thoroughly mixed with the dried PET chips in an airflow mixer. The aerogel material accounts for 5% of the total mass. It is heated to 300°C to melt and the melt is pressed into the spinning assembly. It is extruded from the micropores of the spinneret to form a liquid stream. The liquid stream is cooled in a side-blowing device (wind temperature about 20°C) and solidified into a nascent fiber. This fiber is the super heat-insulating polyester fiber with a thermal conductivity of 0.03 W / (m·K).

[0031] Example 2 (1) Place 50 g of methyl orthosilicate and 1500 mL of water in a beaker and sonicate until completely dissolved to obtain a silicon precursor solution.

[0032] (2) Stir 500 mL of n-heptane, 5 mg of bis(octadecyl)dimethylammonium chloride and 1000 mL of anhydrous ethanol until homogeneous and transparent, and then add them to the precursor solution obtained in step (1) and stir for 100 min.

[0033] (3) Prepare 10 mL of sulfuric acid solution containing crosslinking agent epichlorohydrin, with a sulfuric acid concentration of 18 mol / L and epichlorohydrin accounting for 3% of the solution mass; and add the solution to the solution in step (2) and stir for 24 h.

[0034] (4) Centrifuge the solution obtained in step (3), collect the solid precipitate, wash it, and dry it at 200℃ for 3 hours to obtain the aerogel material. The density of the obtained aerogel material is 30 kg / m³. 3 The surface area is 1050 m² 2 / g.

[0035] (5) Disperse the aerogel material in water at a solid-liquid ratio of 1:10 to obtain a sol suspension. Then, add glass fiber mat and soak for 3 hours to ensure it is fully immersed in the glass fiber mat. Then, dry in an oven at 100℃ until the water is completely evaporated and the glass fiber mat is completely dry to obtain the aerogel mat. Cut it into 30 cm × 30 cm × 0.5 cm dimensions for use as thermal insulation for lithium battery cells. The resistance test process is as follows: Aerogel felt was placed between two battery modules, and one module was heated using a heating element at a power of 1000W for 500 seconds. The temperature change of the other module was collected and calculated. The thermal resistance of the aerogel felt was found to be 0.012 W / (m·K), which is significantly lower than the thermal conductivity of mica board (0.23 W / (m·K). This effectively prevents heat diffusion and acts as a "fireproof partition".

[0036] Example 3 (1) Place 10 g of methyltrimethoxysilane and 2000 mL of water in a beaker and sonicate until completely dissolved to obtain a silicon precursor solution.

[0037] (2) Mix 1000mL kerosene, 10g sodium dodecyl sulfate and 1000mL n-propanol and stir until homogeneous and transparent. Then add it to the precursor solution obtained in step (1) and stir for 80 min.

[0038] (3) Prepare 500 mL of nitric acid solution containing the crosslinking agent glutaraldehyde, wherein the concentration of nitric acid is 10 mol / L and glutaraldehyde accounts for 3% of the solution mass, and add the solution to the solution in step (2) and stir for 18 h; (4) Centrifuge the solution obtained in step (3), collect the solid precipitate, wash it, and dry it at 150 °C for 5 h to obtain the aerogel material. The density of the obtained aerogel material is 18 kg / m³. 3 The surface area is 1100 m² 2 / g.

[0039] (5) Add the treated quicklime emulsion, quartz mortar, aerogel material, reinforcing fiber, water glass (as binder and additive) and water to the mixer in a mass ratio of 1:1:0.05:0.05:0.3:1 and mix at high speed to form a uniform suspension slurry.

[0040] (6) The mixed slurry is sent into a gel tank and heated at 100 °C for 5 hours. Then it is poured directly into a mold and pressed into shape by a high-pressure hydraulic press. The molded wet blank is sent into an autoclave and undergoes a hydrothermal synthesis reaction in saturated steam at high temperature and high pressure (200 °C, 2 MPa) for 10 hours. The autoclaved board is sent into a drying kiln and dried with hot air at 180 °C to obtain gel insulation material.

[0041] (7) Apply a 1 cm thick gel insulation material to the outer surface of the petroleum distillation column for insulation. Without insulation, the bottom temperature of the column is 340~350 ℃. After covering with a 1 cm thick gel insulation material, the bottom temperature of the column is maintained at room temperature, which greatly reduces heat loss and improves distillation efficiency.

[0042] Example 4 (1) Place 50 g of cerium nitrate and 1500 mL of water in a beaker and sonicate until completely dissolved to obtain a silicon precursor solution.

[0043] (2) Mix 1000mL of oleic acid, 100g of sodium hydroxide and 500mL of isopropanol until homogeneous and transparent, then add to the precursor solution obtained in step (1) and stir for 100 min.

[0044] (3) Prepare 500 mL of nitric acid solution containing the crosslinking agent glutaraldehyde, with a nitric acid concentration of 10 mol / L and glutaraldehyde accounting for 3% of the solution mass. Add this solution to the solution in step (2) and stir for 16 h. (4) Centrifuge the solution obtained in step (3), collect the solid precipitate, wash it, and dry it at 150 °C for 5 h to obtain the aerogel material. The density of the obtained aerogel material is 32 kg / m³. 3 The surface area is 1200 m² 2 / g.

[0045] Example 5 (1) Place 20 g of titanium tetrachloride and 1500 mL of n-hexanol in a beaker and sonicate until completely dissolved to obtain a titanium precursor solution.

[0046] (2) Mix 1000mL of oleic acid, 100g of sodium hydroxide and 500mL of water and stir until homogeneous and transparent. Then add the precursor solution obtained in step (1) and stir for 60 min.

[0047] (3) Prepare 500 mL of acetic acid solution containing potassium oleate as a crosslinking agent. The concentration of acetic acid is 3 mol / L and the potassium oleate accounts for 5% of the solution mass. Add the solution to the solution in step (2) and stir for 12 h. (4) Centrifuge the solution obtained in step (3), collect the solid, wash it, and dry it at 150 °C for 5 h to obtain the aerogel material. The density of the obtained aerogel material is 50 kg / m³. 3 The surface area is 1350 m² 2 / g.

[0048] Comparative Example 1 (1) Place 500g of tetraethyl orthosilicate and 1000mL of water in a beaker and sonicate until completely dissolved to obtain a silicon precursor solution.

[0049] (2) Mix 1000 mL of n-hexane, 1000 mg of cetyltrimethylammonium bromide and 1000 mL of methanol until homogeneous and transparent, and then add to the precursor solution obtained in step (1) and stir for 30 min.

[0050] (3) Prepare 500 mL of hydrochloric acid solution containing crosslinking agent N,N'-methylenebisacrylamide, with a hydrochloric acid concentration of 1 mol / L and N,N'-methylenebisacrylamide accounting for 5% of the solution mass, and add the solution to the solution in step (2) and stir for 12 h; (4) Centrifuge the solution obtained in step (3), collect the solid precipitate, wash it and dry it at 50°C for 24 hours to obtain spherical silica material.

[0051] Figure 1 This is a SEM image of the aerogel material prepared in Example 1. It can be seen that the aerogel exhibits flocculent aggregation with extremely small particles.

[0052] Figure 2 This is a TEM image of the aerogel material prepared in Example 1. It can be seen that the aerogel material has a porous structure formed by a framework material. The framework material is continuously distributed, with individual framework strands having a diameter of 4–8 nm, and the framework contains a large number of pores with diameters ranging from 5–30 nm.

[0053] Figure 3 The image shows a SEM image of the silica nanoparticles prepared in Comparative Example 1. It can be seen that the silica nanoparticles have a particle size distribution ranging from 100 to 1000 nanometers and exhibit adhesion.

[0054] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made within the scope of the claims of the present invention should be included in the scope of the present invention.

Claims

1. A method for preparing aerogel materials using a reverse microemulsion method, characterized in that: Specifically, the steps include the following: (1) Mix the framework material precursor and solvent and sonicate until dissolved to obtain a framework material precursor solution; (2) Stir the oil phase solvent, surfactant and solvent evenly, and then add them to the precursor solution obtained in step (1) and stir for 10~100 min; (3) Prepare an acid solution containing a crosslinking agent and add it to the solution obtained in step (2), and stir for 12-24 hours; (4) The solution obtained in step (3) is centrifuged, washed and dried to obtain aerogel material; The aerogel material comprises a porous network structure with a nanoskeleton diameter of 4–8 nm, a pore size of 2–20 nm, a porous network structure size of 1–100 μm, and a density of 10–150 kg / m³. 3 Surface area is 600-1500 m² 2 / g.

2. The method according to claim 1, characterized in that: The precursor materials for the framework material mentioned in step (1) include: tetraethyl orthosilicate, methyl orthosilicate, polysiloxane, methyltrimethoxysilane, methyltriethoxysilane, sodium silicate, silica sol, cerium nitrate, yttrium nitrate, lanthanum nitrate, praseodymium nitrate, neodymium nitrate, promethium nitrate, samarium nitrate, europium nitrate, gadolinium nitrate, holmium nitrate, dysprosium nitrate, lutetium nitrate, erbium nitrate, terbium nitrate, thulium nitrate, ytterbium nitrate, tetrabutyl titanate, titanium tetrachloride, titanium sulfate, zirconium oxychloride, zirconium propoxide, ferric nitrate, ferric sulfate, ferric chloride, zinc nitrate, zinc sulfate, and zinc chloride. The solvent is one or any combination of several of the following: copper nitrate, copper sulfate, copper chloride, magnesium nitrate, magnesium sulfate, magnesium chloride, nickel nitrate, nickel sulfate, nickel chloride, cobalt nitrate, cobalt sulfate, cobalt chloride, indium nitrate, indium sulfate, indium chloride, sodium tungstate, tungsten ethoxide, sodium vanadate, vanadium oxysulfate, barium oxalate, titanium oxalate, strontium oxalate, lead oxalate, bismuth oxalate, etc.; the solvent is one or any combination of several of the following: water, methanol, anhydrous ethanol, n-propanol, isopropanol, n-butanol, isobutanol, n-pentanol, isopentanol, n-hexanol, 2-hexanol, n-heptanol, n-octanol, 2-octanol, n-nonanol, n-decanol, n-dodecylol.

3. The method according to claim 1, characterized in that, The solid-liquid ratio of the skeleton material precursor and the solvent in step (1) is 1:5~1000.

4. The method according to claim 1, characterized in that, The oil phase solvent mentioned in step (2) is one or any combination of several of the following: n-hexane, n-heptane, n-octane, n-hexanol, isooctane, cyclohexane, petroleum ether, kerosene, soybean oil, olive oil, peanut oil, rapeseed oil, castor oil, corn oil, sunflower seed oil, coconut oil, cottonseed oil, isopropyl myristate, ethyl oleate, isopropyl palmitate, medium-chain triglycerides, glycerol caprylate, long-chain triglycerides, oleic acid, and caprylic acid.

5. The method according to claim 1, characterized in that, The surfactant mentioned in step (2) is hexadecyltrimethylammonium bromide, dioctadecyldimethylammonium chloride, sodium dodecyl sulfate, sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, sodium succinate sulfonate, sodium di(2-ethylhexyl)sulfonated succinate, sorbitan fatty acid ester, polyoxyethylene sorbitan fatty acid ester, polyethylene glycol octylphenyl ether, polyoxyethylene fatty alcohol ether, polyoxyethylene octylphenyl ether, octylphenol polyoxyethylene ether, KH-550, KH-560, KH-570, methoxy polyethylene glycol silane, egg white albumin, N,N-dimethylformamide, sodium hydroxide, potassium hydroxide, ammonia, sodium borohydride, potassium borohydride, etc., or any combination thereof; the solvent mentioned in step (2) is water, methanol, anhydrous ethanol, n-propanol, isopropanol, n-butanol, isobutanol, n-pentanol, isopentanol, n-hexanol, 2-hexanol, n-heptanol, n-octanol, 2-octanol, n-nonanol, n-decanol, n-dodecylol, or any combination thereof.

6. The method according to claim 1, characterized in that, The ratio of oil phase solvent, surfactant and solvent used in step (2) is 500-1000mL: 5mg-100g: 500-1000mL.

7. The method according to claim 1, characterized in that, The crosslinking agent mentioned in step (3) is one or any combination of N,N'-methylenebisacrylamide, epichlorohydrin, glutaraldehyde, divinylbenzene, pentaerythritol triacrylate, polyethylene glycol diacrylate, calcium chloride, sodium trimetaphosphate, genipin, potassium oleate, polyethylene glycol, polyacrylic acid, polyvinylpyrrolidone, lithium hydroxide, sodium hydroxide, and potassium hydroxide; the acid solution is one or any combination of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, hydrofluoric acid, acetic acid, oxalic acid, formic acid, oleic acid, and citric acid.

8. The method according to claim 1, characterized in that, The acid solution of the crosslinking agent mentioned in step (3) has an acid concentration of 0.1~18 mol / L, the crosslinking agent accounts for 1-10% of the solution mass, and the total volume of the acid solution containing the crosslinking agent is 0.01~5L.

9. The method according to claim 1, characterized in that, The drying temperature in step (4) is 50~200℃, and the time is 3~24h.

10. The application of the aerogel material prepared by the method according to any one of claims 1-9 in the preparation of thermal insulation materials and fireproof materials.