A porous metal sulfide demercuration adsorbent rich in polysulfur sites, and methods of making and using the same
A porous metal sulfide adsorbent rich in polysulfide sites was prepared by co-precipitation of polysulfide solution and metal salt, which solved the problems of insufficient active sites and pore blockage in the prior art and achieved efficient mercury removal and a simple preparation process.
Patent Information
- Application Number
- CN202611410219.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-20
AI Technical Summary
Existing metal sulfide mercury removal adsorbents have few low-coordination active sulfur sites, and excessive elemental sulfur easily clogs the pores, making it difficult to improve adsorption capacity and breakthrough time. Moreover, existing modification methods have harsh process conditions and complex steps, making it difficult to simultaneously achieve active site enrichment and pore structure optimization.
A polysulfide solution is generated by reacting soluble sulfides with elemental sulfur. This solution is then co-precipitated with a metal salt solution. The polysulfide anions participate in the framework assembly and generate elemental sulfur in situ as a sacrificial template. The template is then dissolved by a washing solution to construct a porous structure, forming a porous metal sulfide adsorbent rich in low-coordination polysulfide active sites.
It achieves efficient mercury capture, improves adsorption capacity and breakthrough time, reduces gas-solid mass transfer resistance, and features a mild process and simple procedure, making it suitable for large-scale production.
Smart Images

Figure CN123127944A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of mercury removal adsorbent preparation technology, and in particular to a porous metal sulfide mercury removal adsorbent rich in polysulfide sites, its preparation method and application. Background Technology
[0002] Elemental mercury ( Mercury, characterized by high volatility, chemical inertness, and poor water solubility, is one of the most difficult forms of mercury to remove from coal-fired flue gas and industrial exhaust gases. Among existing mercury removal materials, metal sulfides, due to their sulfur sites with a strong affinity for mercury, can effectively remove it. Transform into a stable Therefore, it has attracted widespread attention. Liquid-phase precipitation is a common route for preparing metal sulfide adsorbents for mercury removal. For example, the literature "Experimental Study on Adsorption and Removal of Elemental Mercury by Nano-Zinc Sulfide" (Journal of Engineering Thermophysics, 2017) discloses the preparation of nano-zinc sulfide adsorbents by liquid-phase precipitation, utilizing its surface sulfur sites for... The chemical affinity of mercury is used to remove it. However, in metal sulfides prepared by conventional coprecipitation methods, most sulfur species are in a saturated coordination state, with few low-coordination active sulfur sites on the surface, which hinders the removal of mercury. The chemical capture capacity is limited. On the other hand, while simply increasing the sulfur content can increase the total amount of sulfur species, excessive elemental sulfur is prone to depositing on the particle surface or clogging the pores, which can obscure active sites and reduce the effective utilization rate of sulfur atoms.
[0003] Chinese patent document (application number CN201911192039.7) discloses a method for preparing mercury removal adsorbents using oxygen pressure acid leaching residue from wet zinc refining. The method involves mixing zinc oxide ore with oxygen pressure acid leaching residue rich in elemental sulfur, and then reacting it hydrothermally in a solution containing sulfur ions to generate zinc polysulfides. These polysulfides are then activated by grinding with iron salts, resulting in the formation of active sulfur and short-chain polysulfides on the adsorbent surface for mercury removal from flue gas. The prior art also points out that improper proportions can lead to residual sulfur after the reaction. This sulfur has low activity and can coat the adsorbent, reducing mercury removal performance. Therefore, while this method recognizes the adverse effects of excessive elemental sulfur and aims to introduce polysulfide active sites, these sites are introduced separately through iron salt grinding and activation. Residual elemental sulfur is only controlled as a negative factor to be avoided. Furthermore, the use of high-temperature hydrothermal and solid-phase grinding activation results in harsh process conditions and complex steps.
[0004] Furthermore, existing modification methods such as amorphization, heteroatom doping, acid etching, or external template pore creation, while improving adsorption performance to some extent, typically suffer from harsh process conditions, complex steps, high costs, and difficulty in scaling up. They also often struggle to simultaneously achieve active site enrichment and pore structure optimization, leading to insufficient utilization of internal sites, limited gas-solid mass transfer, and difficulty in further improving adsorption capacity and breakthrough time. Therefore, there is an urgent need for a method for preparing metal sulfide adsorbents that is mild, easily scalable, and capable of simultaneously constructing high-density polysulfide active sites and well-developed pore structures. Summary of the Invention
[0005] To address the problems existing in the prior art, the first objective of this invention is to provide a porous metal sulfide mercury removal adsorbent rich in polysulfide sites. This solves the problems of low-coordination active sulfur sites in metal sulfides prepared by conventional co-precipitation methods, the tendency of excess elemental sulfur to clog pores and obscure active sites, and the difficulty in improving adsorption capacity and breakthrough time. This adsorbent is rich in low-coordination polysulfide active sites due to the participation of polysulfide anions in framework assembly, and possesses a well-developed porous structure through sacrificial template dissolution. Therefore, it combines high active site density with good mass transfer performance, achieving the desired mercury removal from metal sulfides. Highly efficient capture and fixation.
[0006] The second objective of this invention is to provide a method for preparing the aforementioned porous metal sulfide mercury removal adsorbent rich in polysulfide sites, solving the problems of existing modification methods, such as harsh process conditions, complex steps, and difficulty in simultaneously achieving active site enrichment and pore structure optimization. This method uses a polysulfide solution obtained by reacting soluble sulfides with elemental sulfur as a sulfur source, co-precipitating it with a metal salt solution. This allows polysulfide anions to directly participate in the assembly of the metal sulfide framework and generate elemental sulfur in situ during precipitation as a sacrificial template. The template elemental sulfur is then dissolved out with a washing solution. This process simultaneously constructs polysulfide active sites and a porous structure without introducing an external hard template or strong acid etching. The process is mild, simple, and easily scalable.
[0007] The third objective of this invention is to provide the application of the above-mentioned porous metal sulfide mercury removal adsorbent rich in polysulfide sites in the removal of mercury from mercury-containing gases, thereby solving the problems of existing mercury removal adsorbents. The limitations of chemical trapping capacity and short breakthrough time are addressed. In this application, the abundant polysulfide sites on the adsorbent surface and... Strong interactions occur and stable substances are generated. The well-developed pore structure promotes It diffuses into the interior of the particles, thereby improving mercury removal efficiency and extending the penetration time.
[0008] This invention provides a method for preparing a porous metal sulfide mercury removal adsorbent rich in polysulfide sites, comprising the following steps: dissolving a soluble sulfide in water and reacting it with elemental sulfur at a molar ratio of 1:1 to 1:5 to obtain a polysulfide solution; adding a transition metal salt solution to the polysulfide solution for a co-precipitation reaction to obtain a metal sulfide precursor containing polysulfide species and in-situ generated elemental sulfur; performing solid-liquid separation on the metal sulfide precursor to obtain a solid precipitate, which is then washed, desulfurized, and dried to obtain the mercury removal adsorbent.
[0009] Furthermore, the in-situ generated elemental sulfur serves as a sacrificial template; the washing liquid in the washing process is a liquid medium capable of converting elemental sulfur into soluble sulfur-containing species or dissolving elemental sulfur.
[0010] The mechanism of the technical solution provided by this invention lies in the reaction of soluble sulfides with elemental sulfur to generate polysulfide anions ( In a polysulfide solution, the sulfur source is in an excess state. When polysulfide anions co-precipitate with metal ions, they directly participate in the assembly of the metal sulfide framework, introducing non-stoichiometric polysulfide species into the framework and forming low-coordination polysulfide active sites on the surface. Simultaneously, the excess sulfur precipitates in situ as elemental sulfur during precipitation, dispersing within the precipitate as a sacrificial template. Subsequently, the template elemental sulfur is converted into soluble sulfur-containing species or dissolved and removed using a washing solution. After in-situ dissolution, the template leaves interconnected pores in the metal sulfide, forming a porous structure and reducing gas-solid mass transfer resistance. The polysulfide species within the framework remain undissolved, retaining as active sites. Without this washing treatment, the in-situ generated elemental sulfur will remain on the particle surface or within the pores, obscuring active sites and clogging the pores. If the polysulfide solution is not used as the sulfur source, the product sulfur species are in a saturated coordination state, lacking polysulfide active sites, and no template can be dissolved during washing. The soluble sulfides referred to in this invention are sulfides that are soluble in water and can react with elemental sulfur to form polysulfide solutions, such as sodium sulfide, potassium sulfide, lithium sulfide, and ammonium sulfide.
[0011] As a preferred embodiment, in the step of obtaining the polysulfide solution, the soluble sulfide is sodium sulfide. Sodium sulfide has high solubility, is inexpensive and readily available, and the process of reacting with elemental sulfur to generate sodium polysulfide solution is mature, facilitating the large-scale preparation of sulfur sources.
[0012] As a preferred embodiment, the reaction is carried out with stirring under an inert atmosphere, namely nitrogen or argon. Polysulfide anions have strong reducing properties; reacting under an inert atmosphere prevents them from being oxidized by oxygen in the air, thus avoiding the loss of active sulfur species. Stirring ensures uniform dispersion of elemental sulfur in the solution, accelerating the formation of polysulfides.
[0013] As a preferred embodiment, the reaction temperature is 60–90°C, the time is 1–6 h, and the stirring speed is 500–700 rpm; the preferred temperature is 75–90°C, more preferably 80°C; the preferred time is 2–4 h, more preferably 3–4 h; and the preferred stirring speed is 550–650 rpm, more preferably 600 rpm. If the temperature is too low, the reaction between elemental sulfur and sulfide ions will be insufficient, resulting in inadequate polysulfide formation; if the temperature is too high, energy consumption will increase and solution evaporation will accelerate. Within the above-mentioned temperature, time, and stirring speed range, elemental sulfur can be fully converted into polysulfide anions.
[0014] As a preferred embodiment, the molar ratio of the soluble sulfide to the elemental sulfur is 1:3 to 1:5. At this preferred ratio, the excess sulfur content is higher, resulting in a more complete in-situ generation of elemental sulfur templates during co-precipitation. This leads to a richer variety of polysulfide sites and more developed pores in the resulting adsorbent, further improving mercury removal efficiency.
[0015] As a preferred embodiment, the transition metal salt is at least one of zinc salt, copper salt, iron salt, cobalt salt, and nickel salt.
[0016] As a preferred embodiment, the zinc salt is one or more of zinc nitrate, zinc sulfate, and zinc chloride; the cobalt salt is one or more of cobalt nitrate, cobalt sulfate, and cobalt chloride; and the nickel salt is one or more of nickel nitrate, nickel sulfate, and nickel chloride.
[0017] As a preferred embodiment, the copper salt is one or more of copper nitrate, copper sulfate, and copper chloride; the iron salt is one or more of ferric nitrate, ferric sulfate, and ferric chloride.
[0018] As a preferred embodiment, in the coprecipitation reaction, the ratio of the total molar amount of metal ions in the metal salt to the molar amount of the soluble sulfide is 1:0.8 to 1:1.2. At this ratio, the metal ions react fully with the sulfur source, and the polysulfide anions participate excessively in framework assembly, ensuring the formation of polysulfide species and in-situ elemental sulfur templates in the precursor.
[0019] As a preferred embodiment, the metal salt solution is added completely within 20–40 minutes. Slow addition prevents the local concentration of metal ions from becoming excessively high, ensuring a uniform co-precipitation reaction and resulting in a uniform distribution of polysulfide species and elemental sulfur templates in the obtained precursor particles.
[0020] As a preferred embodiment, the coprecipitation reaction is carried out with stirring at a temperature of 60–90°C for 1–6 hours and a stirring speed of 500–700 rpm; the preferred temperature is 75–90°C, more preferably 80°C; the preferred time is 2–4 hours, more preferably 2–3 hours; and the preferred stirring speed is 550–650 rpm, more preferably 600 rpm. These conditions ensure a complete coprecipitation reaction and effective embedding of polysulfide anions into the metal sulfide framework.
[0021] As a preferred embodiment, the drying temperature is 50–80°C, and the drying time is 10–18 h; the temperature is preferably 55–75°C, more preferably 60°C; the drying time is preferably 12–16 h, more preferably 12 h. If the temperature is too low or the time is too short, the drying will be insufficient; if the temperature is too high, it may lead to the decomposition of polysulfide species or the collapse of the pore structure. Within the above ranges, moisture can be sufficiently removed while maintaining the stability of polysulfide sites and the pore structure.
[0022] As a preferred option, the drying is vacuum drying.
[0023] As a preferred embodiment, the solid precipitate is first ground and passed through a 100-200 mesh sieve before the washing process; after washing, the solid is subjected to solid-liquid separation, cleaning, and drying, and then ground and passed through a 100-200 mesh sieve again. Grinding and sieving before washing disperses the solid precipitate, increases its specific surface area, and fully exposes the internal elemental sulfur template, facilitating the penetration of the washing liquid and dissolution of the template; grinding and sieving of the finished product ensures that the adsorbent particle size matches the fixed bed packing requirements, reducing bed pressure drop and improving gas-solid contact.
[0024] As a preferred embodiment, the grinding and sieving process is performed through a 200-mesh sieve.
[0025] As a preferred option, the cleaning is performed using deionized water and ethanol.
[0026] As a preferred embodiment, the washing solution is at least one selected from sodium sulfide solution, potassium sulfide solution, lithium sulfide solution, ammonium sulfide solution, sodium hydrosulfide solution, potassium hydrosulfide solution, ammonium hydrosulfide solution, sodium sulfite solution, potassium sulfite solution, and ammonium sulfite solution. The sulfide and hydrosulfide solutions contain sulfide anions that react with elemental sulfur to form soluble polysulfide anions, and the sulfite solution reacts with elemental sulfur to form soluble thiosulfates, thereby converting the template elemental sulfur into soluble sulfur-containing species for removal.
[0027] As a preferred embodiment, the washing liquid is one or more of sodium sulfide solution, potassium sulfide solution and lithium sulfide solution, and more preferably sodium sulfide solution.
[0028] As a preferred embodiment, the concentration of the washing solution is 0.025–0.15 mol / L, the washing process is carried out with stirring, the temperature is 60–90℃, the time is 0.5–2 h, and the stirring speed is 500–700 rpm. The washing temperature is preferably 75–90℃, more preferably 80℃; the time is preferably 0.5–1.5 h, more preferably 1–1.5 h; and the stirring speed is preferably 550–650 rpm, more preferably 600 rpm.
[0029] If the concentration of the washing solution is too low, the elemental sulfur template will not dissolve sufficiently and the pores will not form completely; if the concentration is too high, it will waste reagents. Within the above-mentioned concentration, temperature and time range, the elemental sulfur template can be selectively dissolved while the polysulfide species in the framework can be preserved.
[0030] As a preferred embodiment, the concentration of the washing solution is 0.025–0.1 mol / L, more preferably 0.075–0.1 mol / L.
[0031] This invention also provides a porous metal sulfide mercury removal adsorbent rich in polysulfide sites, prepared by any of the methods described above. The adsorbent's metal sulfide framework is rich in low-coordinated polysulfide active sites and possesses a porous structure formed by template dissolution; taking the zinc sulfide system as an example, its Raman spectrum is at approximately 260 cm⁻¹. -1 Approximately 345 cm -1 While exhibiting the characteristic peaks of the zinc sulfide skeleton at approximately 420 cm⁻¹, -1 and approximately 460–470 cm -1 An additional peak appears at 400 cm⁻¹, which can be attributed to the characteristic peaks of polysulfide species, while zinc sulfide prepared by conventional coprecipitation methods shows a peak at 400 cm⁻¹. -1 The absence of obvious spectral peaks indicates that the adsorbent obtained in this invention is rich in polysulfide sites. Under scanning electron microscopy, pores formed after template dissolution can be seen distributed on the surface and inside of the particles, while the samples of comparative examples 1 to 4 have a dense sheet-like or blocky morphology and no well-developed pores.
[0032] This invention provides the application of the aforementioned porous metal sulfide mercury removal adsorbent rich in polysulfide sites in the removal of mercury from mercury-containing gases. The mercury-containing gas can be coal-fired flue gas or industrial tail gas. In application, the adsorbent is packed into a reactor such as a fixed bed. The mercury-containing gas passes through the adsorbent bed, and the polysulfide sites on the adsorbent surface and within the pores interact with the adsorbent. Strong interactions occur, oxidizing and fixing it into a stable form. The well-developed porous structure reduces gas-solid mass transfer resistance, enabling... It diffuses into the interior of the particles, making full use of the internal sites, thereby increasing the adsorption capacity and extending the breakthrough time.
[0033] Compared with the prior art, the beneficial technical effects of the technical solution provided by the present invention are as follows:
[0034] 1) The porous metal sulfide mercury removal adsorbent rich in polysulfide sites provided by this invention has a framework rich in low-coordination polysulfide active sites and a porous structure formed by sacrificial template dissolution. The polysulfide sites are related to... Strong interactions generate stability pore structure promotes It diffuses inward, possessing both high active site density, high porosity, and good mass transfer performance.
[0035] 2) The preparation method provided by this invention uses a polysulfide solution as a sulfur source, co-precipitates to generate elemental sulfur sacrificial templates in situ, and uses washing liquid to dissolve the templates to create pores. Under the condition of not introducing external hard templates and strong acid etching, polysulfide active sites and porous structures are constructed simultaneously. The process conditions are mild, the raw materials are cheap and readily available, and the process is simple, making it suitable for large-scale preparation. Moreover, this strategy is applicable to various metal sulfide systems such as zinc, cobalt, and nickel, and has good universality.
[0036] 3) In the technical solution provided by this invention, the three steps of polysulfide anion coprecipitation to introduce polysulfide sites, in-situ elemental sulfur as a sacrificial template, and washing solution dissolving the template to create pores work together to simultaneously achieve enrichment of active sites and optimization of pore structure: if ordinary zinc sulfide is not treated with polysulfide precursor and is only washed with sodium sulfide, the mercury removal efficiency drops to 7.63%, which is lower than the 10.36% of the unwashed one, indicating that the washing step is not independently beneficial; if polysulfide precursor is used but not washed, residual elemental sulfur blocks the pores, and the penetration adsorption capacity is only 22.08 mg / g; only by combining the three can a balance between high efficiency and high penetration capacity be achieved. Attached Figure Description
[0037] Figure 1 The Raman spectrum of the adsorbent prepared in Example 1;
[0038] Figure 2 The Raman spectrum of the adsorbent prepared in Example 2;
[0039] Figure 3 The Raman spectrum of the adsorbent prepared in Example 3;
[0040] Figure 4 The Raman spectrum of the adsorbent prepared in Example 4;
[0041] Figure 5 The Raman spectrum of the adsorbent prepared in Example 5;
[0042] Figure 6 Raman spectrum of the adsorbent prepared in Comparative Example 1;
[0043] Figure 7 SEM image of the adsorbent prepared in Example 3;
[0044] Figure 8 SEM image of the adsorbent prepared in Example 6;
[0045] Figure 9 SEM image of the adsorbent prepared in Example 7;
[0046] Figure 10 SEM image of the adsorbent prepared in Example 8;
[0047] Figure 11 SEM image of the adsorbent prepared in Example 9;
[0048] Figure 12 SEM image of the adsorbent prepared in Example 10;
[0049] Figure 13 SEM image of the adsorbent prepared in Comparative Example 1;
[0050] Figure 14 SEM image of the adsorbent prepared in Comparative Example 2;
[0051] Figure 15 SEM image of the adsorbent prepared in Comparative Example 3;
[0052] Figure 16 SEM image of the adsorbent prepared in Comparative Example 4;
[0053] Figure 17 SEM image of the adsorbent prepared in Comparative Example 5;
[0054] Figure 18 The breakthrough curve of the adsorbent prepared in Example 8;
[0055] Figure 19 The breakthrough curve is for the adsorbent prepared in Comparative Example 1.
[0056] Figure 20 The breakthrough curve is shown for the adsorbent prepared in Comparative Example 3. Detailed Implementation
[0057] The technical solution of the present invention will be further described below with reference to embodiments. It should be understood that the following embodiments are only for illustrating the present invention and are not intended to limit the scope of protection of the present invention. Conventional adjustments made by those skilled in the art to the reaction raw materials, concentration, temperature, time, and post-treatment conditions without departing from the concept of the present invention should be included within the scope of protection of the present invention.
[0058] In the following examples and comparative examples, the concentration of the metal salt solution used was 0.1 mol / L; sodium sulfide was used as the soluble sulfide; and the preparation of the polysulfide solution, co-precipitation reaction, and washing were all carried out with stirring. Any equivalent raw materials and conditions that can achieve the same effect can be used as substitutes.
[0059] Example 1
[0060] A 0.1 mol / L zinc sulfate aqueous solution was prepared as the metal source solution. Sodium sulfide was dissolved in deionized water, and elemental sulfur was added under a nitrogen atmosphere, wherein the molar ratio of sodium sulfide to elemental sulfur was 1:1. The reaction was stirred at 80 °C to obtain a sodium polysulfide solution.
[0061] The zinc sulfate solution was slowly added to the sodium polysulfide solution over 30 min, and the reaction was continued with stirring at 80 °C for 3 h. After the reaction was completed, the precipitate was collected by centrifugation, washed with deionized water and ethanol, and vacuum dried at 60 °C for 12 h. The precipitate was then ground and sieved to obtain the zinc sulfide precursor.
[0062] The obtained precursor was dispersed in a 0.1 mol / L sodium sulfide solution and washed with stirring at 80 °C for 1 h to convert the template elemental sulfur in the precursor into soluble polysulfide anions and remove it. The solid was then collected by centrifugation, washed with deionized water and ethanol, dried under vacuum at 60 °C for 12 h, ground and sieved to obtain a porous zinc sulfide adsorbent rich in polysulfide sites.
[0063] Example 2
[0064] This embodiment is basically the same as Example 1, except that the molar ratio of sodium sulfide to elemental sulfur is 1:2 during the preparation of the sodium polysulfide solution. The subsequent coprecipitation reaction and post-washing conditions are the same as in Example 1, resulting in a porous zinc sulfide adsorbent rich in polysulfide sites.
[0065] Example 3
[0066] This embodiment is basically the same as Example 1, except that the molar ratio of sodium sulfide to elemental sulfur is 1:3 during the preparation of the sodium polysulfide solution. The subsequent co-precipitation reaction and post-washing conditions are the same as in Example 1, yielding a porous zinc sulfide adsorbent rich in polysulfide sites. Figures 1-5 As shown, the Raman spectra of Examples 1-5 are at approximately 260 cm⁻¹. -1 Approximately 345cm -1 While exhibiting characteristic peaks of the zinc sulfide skeleton at approximately 420 cm⁻¹, -1 and approximately 460–470 cm -1 The appearance of an additional peak, a characteristic peak of polysulfide species, indicates that the obtained adsorbent is rich in polysulfide sites. For example... Figure 7As shown in the scanning electron microscope image of Example 3, pores formed by the dissolution of template elemental sulfur are distributed on the surface and inside of the particles, indicating that a porous structure has been formed.
[0067] Example 4
[0068] This embodiment is basically the same as Example 1, except that the molar ratio of sodium sulfide to elemental sulfur is 1:4 during the preparation of the sodium polysulfide solution. The subsequent co-precipitation reaction and post-washing conditions are the same as in Example 1, resulting in a porous zinc sulfide adsorbent rich in polysulfide sites.
[0069] Example 5
[0070] This embodiment is basically the same as Example 1, except that the molar ratio of sodium sulfide to elemental sulfur is 1:5 during the preparation of the sodium polysulfide solution. The subsequent coprecipitation reaction and post-washing conditions are the same as in Example 1, resulting in a porous zinc sulfide adsorbent rich in polysulfide sites.
[0071] Example 6
[0072] This embodiment is basically the same as Example 3, except that the concentration of the sodium sulfide solution used in the post-washing treatment is 0.025 mol / L. The remaining steps are the same as in Example 3, resulting in a porous zinc sulfide adsorbent rich in polysulfide sites after washing with a low concentration of sodium sulfide. Figure 8 As shown in the scanning electron microscope image of Example 6, pores formed on the particle surface after template dissolution can be seen.
[0073] Example 7
[0074] This embodiment is basically the same as Example 3, except that the concentration of the sodium sulfide solution used in the post-washing treatment is 0.05 mol / L. The remaining steps are the same as in Example 3, yielding a porous zinc sulfide adsorbent rich in polysulfide sites. Figure 9 As shown in the scanning electron microscope image of Example 7, bowl-shaped pores and secondary pits are visible, and the pore structure is well-developed.
[0075] Example 8
[0076] This embodiment is basically the same as Example 3, except that the concentration of the sodium sulfide solution used in the post-washing treatment is 0.075 mol / L. The remaining steps are the same as in Example 3, yielding a porous zinc sulfide adsorbent rich in polysulfide sites. Figure 10 As shown, the scanning electron microscope image of Example 8 reveals multiple open pores of varying sizes with clear edges and no elemental sulfur filling the pores, indicating that the elemental sulfur in the template has been dissolved. Figure 18 As shown, the breakthrough curve of Example 8 continued to rise within about 1320 min, and the 60% breakthrough mercury adsorption capacity reached 46.21 mg / g, indicating that it has high adsorption capacity and long breakthrough time.
[0077] Example 9
[0078] This embodiment illustrates the applicability of the method of the present invention in nickel sulfide systems. A 0.1 mol / L nickel salt solution is prepared as the metal source solution; the nickel salt can be nickel nitrate, nickel sulfate, or nickel chloride. A sodium polysulfide solution is prepared according to a molar ratio of sodium sulfide to elemental sulfur of 1:3. The nickel salt solution is slowly added to the sodium polysulfide solution, and a co-precipitation reaction is carried out at 80°C. After the reaction, the solution is centrifuged, washed, dried, and ground to obtain a nickel sulfide precursor. Subsequently, the nickel sulfide precursor is dispersed in a 0.075 mol / L sodium sulfide solution, washed at 80°C for 1 h, centrifuged, washed, dried, ground, and sieved to obtain a porous nickel sulfide adsorbent rich in polysulfide sites. Figure 11 As shown in the scanning electron microscope image of Example 9, multiple pores and cavities are distributed on the surface of the loosely packed particles.
[0079] Example 10
[0080] This embodiment illustrates the applicability of the method of the present invention in cobalt sulfide systems. A 0.1 mol / L cobalt salt solution is prepared as the metal source solution; the cobalt salt can be cobalt nitrate, cobalt sulfate, or cobalt chloride. A sodium polysulfide solution is prepared according to a molar ratio of sodium sulfide to elemental sulfur of 1:3. The cobalt salt solution is slowly added to the sodium polysulfide solution, and a coprecipitation reaction is carried out at 80°C. After the reaction, the mixture is centrifuged, washed, dried, and ground to obtain a cobalt sulfide precursor. Subsequently, the cobalt sulfide precursor is dispersed in a 0.075 mol / L sodium sulfide solution, washed at 80°C for 1 h, centrifuged, washed, dried, ground, and sieved to obtain a porous cobalt sulfide adsorbent rich in polysulfide sites. Figure 12 As shown in the scanning electron microscope image of Example 10, erosion pits and depressions are formed along the fracture zone on the substrate surface, indicating that template dissolution pore-forming is also applicable to cobalt systems.
[0081] Comparative Example 1
[0082] A 0.1 mol / L zinc sulfate solution was prepared as the metal source solution. Sodium sulfide was dissolved in deionized water without adding elemental sulfur, i.e., the molar ratio of sodium sulfide to elemental sulfur was 1:0. The zinc sulfate solution was slowly added to the sodium sulfide solution, and the reaction was carried out at 80°C for 2 h. After the reaction, the sample was obtained by centrifugation, washing, and drying. This comparative example did not undergo post-washing with sodium sulfide; the concentration of the post-wash solution was 0 mol / L. Figure 6 As shown, the Raman spectrum of Comparative Example 1 is only at approximately 260 cm⁻¹. -1 Approximately 345 cm -1 The peaks at 400 cm⁻¹ exhibit the characteristic structure of zinc sulfide skeleton. -1The absence of obvious spectral peaks indicates that ordinary zinc sulfide lacks polysulfide sites. For example... Figure 13 As shown, the scanning electron microscope image of Comparative Example 1 shows dense, sheet-like particles with a smooth, flat surface and no well-developed pores. Figure 19 As shown, the 93% penetration mercury adsorption capacity of Comparative Example 1 was only 0.73 mg / g, which was significantly lower than that of Example 8, indicating that the mercury removal effect of ordinary zinc sulfide was poor.
[0083] Comparative Example 2
[0084] This comparative example is essentially the same as Comparative Example 1, except that the obtained ordinary zinc sulfide sample was further washed with a 0.075 mol / L sodium sulfide solution. This comparative example is used to illustrate the effect of sodium sulfide washing alone on the adsorbent structure and active sites in the absence of a polysulfide precursor. Figure 14 As shown, the scanning electron microscope image of Comparative Example 2 still shows dense, sheet-like particles, with no pores formed by template dissolution.
[0085] Comparative Example 3
[0086] This comparative example is essentially the same as Example 3, using a 0.1 mol / L zinc sulfate solution as the metal source solution, with a sodium sulfide to elemental sulfur molar ratio of 1:3 to prepare the zinc sulfide precursor. The difference lies in that the obtained zinc sulfide precursor is not subjected to post-washing with sodium sulfide solution; that is, the post-washing solution concentration is 0 mol / L. This comparative example is used to illustrate the role of sodium sulfide washing in removing the elemental sulfur template, forming a porous structure, and exposing polysulfide sites. Figure 15 As shown, the scanning electron microscope image of Comparative Example 3 shows blocky particles composed of multiple stacked plates, with a relatively rough surface but no interconnected pores, indicating that residual elemental sulfur has not been removed. Figure 20 As shown, the 60% penetration mercury adsorption capacity of Comparative Example 3 was only 22.08 mg / g, which was significantly lower than that of Example 8, indicating that the pores were blocked and the internal sites were not fully utilized when the template elemental sulfur was not removed by washing.
[0087] Comparative Example 4
[0088] This comparative example is essentially the same as Example 9, except that the obtained nickel sulfide precursor is not post-washed with sodium sulfide solution; that is, the concentration of the post-wash solution is 0 mol / L. This comparative example is used to illustrate the effect of sodium sulfide washing on the formation of the adsorbent pore structure and the exposure of polysulfide sites. Figure 16 As shown, the scanning electron microscope image of Comparative Example 4 shows plate-shaped particles with relatively flat surfaces, on which fine particle aggregates are attached, without pores formed by template dissolution.
[0089] Comparative Example 5
[0090] This comparative example is essentially the same as Example 10, except that the obtained cobalt sulfide precursor is not post-washed with sodium sulfide solution; that is, the concentration of the post-wash solution is 0 mol / L. This comparative example is used to illustrate the effect of sodium sulfide washing on the formation of the adsorbent pore structure and the exposure of polysulfide sites. Figure 17 As shown, the scanning electron microscope image of Comparative Example 5 shows regular particles with fine particle agglomerates attached to the surface, without pores formed by template dissolution.
[0091] The adsorbents obtained in each embodiment and comparative example were ground and sieved, and 100-200 mesh particles were packed into a fixed-bed reactor to evaluate the mercury removal performance of the adsorbents on simulated mercury-containing gas. During the test, a mercury-containing gas stream was used as the reaction gas, the total gas velocity was controlled at 1 L / min, and the fixed-bed adsorption experiment was conducted at a suitable temperature. The mercury removal efficiency was calculated according to Equation 1:
[0092] Formula 1: ;
[0093] In Equation 1, Total gas flow rate (unit: L / min); Inlet mercury concentration (unit: μg / m³); Mercury concentration at the outlet (unit: μg / m³); Adsorption time (unit: min); , These are the start and end times of adsorption, respectively (unit: min). Mercury removal efficiency (unit: %). The effects of each adsorbent are shown in Table 1.
[0094] Table 1 Mercury removal efficiency of the adsorbent
[0095]
[0096] The comparison results between the embodiments of the present invention and the comparative examples confirm the technical effects described in the invention. For example... Figures 1-6 As shown, the Raman spectra of Examples 1-5 are at approximately 260 cm⁻¹. -1 Approximately 345 cm -1 While exhibiting characteristic peaks of the zinc sulfide skeleton at approximately 420 cm⁻¹, -1 and approximately 460–470 cm -1 An additional peak at 400 cm⁻¹ appears, which can be attributed to polysulfide species, while in Comparative Example 1 it appears at 400 cm⁻¹. -1 The absence of obvious spectral peaks confirms that the adsorbent obtained in this invention is rich in polysulfide active sites; for example Figures 7-17As shown, the particles in Examples 3, 6-10 have pores formed after the template elemental sulfur is dissolved, distributed on the surface and inside. In contrast, Comparative Examples 1-5 exhibit a dense, sheet-like or blocky morphology without well-developed pores, confirming that washing and dissolving the template is key to constructing a porous structure. Figures 18-20 As shown in Table 1, Example 8 achieved a 60% penetration mercury adsorption capacity of 46.21 mg / g and a mercury removal efficiency of 99.92%, while Comparative Example 1 had a mercury removal efficiency of only 10.36% and an adsorption capacity of only 0.73 mg / g at 93% penetration. Comparative Example 3 had a 60% penetration mercury adsorption capacity of only 22.08 mg / g and a mercury removal efficiency of 87.73%. The mercury removal efficiency of Comparative Example 2 even decreased to 7.63%, which was lower than that of the unwashed Comparative Example 1. This confirms that the three steps of polysulfide anion coprecipitation to introduce polysulfide sites, in-situ elemental sulfur as a sacrificial template, and washing solution dissolving the template to create pores can work together to simultaneously achieve active site enrichment and pore structure optimization, significantly improving mercury removal efficiency and penetration capacity.
[0097] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. All equivalent variations made in accordance with the concept of the present invention should be covered within the scope of protection of the present invention.
Claims
1. A method for preparing a porous metal sulfide mercury removal adsorbent rich in polysulfide sites, characterized in that, The process includes the following steps: dissolving a soluble sulfide in water and reacting it with elemental sulfur at a molar ratio of 1:1 to 1:5 to obtain a polysulfide solution; A transition metal salt solution was added to the polysulfide solution for coprecipitation reaction to obtain a metal sulfide precursor containing polysulfide species and in-situ generated elemental sulfur. The metal sulfide precursor is subjected to solid-liquid separation to obtain a solid precipitate, which is then washed, desulfurized, and dried to obtain a mercury removal adsorbent.
2. The method for preparing a porous metal sulfide mercury removal adsorbent rich in polysulfide sites according to claim 1, characterized in that: The soluble sulfide is sodium sulfide; the reaction is carried out under an inert atmosphere with stirring, the inert atmosphere being nitrogen or argon; the reaction temperature is 60–90°C, the time is 1–6 h, and the stirring speed is 500–700 rpm; the molar ratio of the soluble sulfide to the elemental sulfur is 1:3–1:
5.
3. The method for preparing a porous metal sulfide mercury removal adsorbent rich in polysulfide sites according to claim 1, characterized in that: The transition metal salt is at least one of zinc, copper, iron, cobalt, and nickel; the zinc salt is at least one of zinc nitrate, zinc sulfate, and zinc chloride; the cobalt salt is at least one of cobalt nitrate, cobalt sulfate, and cobalt chloride; and the nickel salt is at least one of nickel nitrate, nickel sulfate, and nickel chloride.
4. The method for preparing a porous metal sulfide mercury removal adsorbent rich in polysulfide sites according to claim 1, characterized in that: In the coprecipitation reaction, the ratio of the total molar amount of metal ions in the metal salt to the molar amount of soluble sulfide is 1:0.8 to 1.2; the metal salt solution is added completely within 20 to 40 minutes; the coprecipitation reaction is carried out with stirring at a temperature of 60 to 90°C for 1 to 6 hours and a stirring speed of 500 to 700 rpm.
5. The method for preparing a porous metal sulfide mercury removal adsorbent rich in polysulfide sites according to claim 1, characterized in that: The drying temperature is 50–80°C, and the time is 10–18 h.
6. The method for preparing a porous metal sulfide mercury removal adsorbent rich in polysulfide sites according to claim 1, characterized in that: The solid precipitate is first ground and passed through a 100-200 mesh sieve before washing and desulfurization treatment; after washing and desulfurization treatment, the solid is dried and then ground and passed through a 100-200 mesh sieve.
7. The method for preparing a porous metal sulfide mercury removal adsorbent rich in polysulfide sites according to claim 1, characterized in that: The washing solution for desulfurization is at least one of sodium sulfide solution, potassium sulfide solution, lithium sulfide solution, ammonium sulfide solution, sodium hydrosulfide solution, potassium hydrosulfide solution, ammonium hydrosulfide solution, sodium sulfite solution, potassium sulfite solution, and ammonium sulfite solution.
8. The method for preparing a porous metal sulfide mercury removal adsorbent rich in polysulfide sites according to claim 7, characterized in that: The concentration of the washing solution is 0.025–0.15 mol / L; the washing process is carried out with stirring at a temperature of 60–90°C for 0.5–2 h and a stirring speed of 500–700 rpm.
9. A porous metal sulfide adsorbent rich in polysulfide sites for mercury removal, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 8.
10. Application of the porous metal sulfide mercury removal adsorbent rich in polysulfide sites as described in claim 9: Removal of mercury from mercury-containing gases.
Citation Information
Patent Citations
A method for preparing mercury removal adsorbent using oxygen pressure acid leaching residue from wet zinc refining
CN110801803B