Iron-based adsorbent, its preparation method and application
Hollow α-Fe₂O₃ microspheres were prepared by the phenolic resin hydrogel soft template method, which solved the problem of easy sintering and agglomeration of traditional Fe₂O₃ at high temperatures. This method achieved efficient arsenic removal at high temperatures and maintained good performance in complex flue gas, making it suitable for industrial applications.
Patent Information
- Application Number
- CN202611125000.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-28
- Publication Date
- 2026-11-20
AI Technical Summary
Traditional commercial Fe₂O₃ particles are prone to sintering and agglomeration at high temperatures, leading to a decrease in specific surface area and a reduction in arsenic removal efficiency. Furthermore, existing improved methods are costly, complex, and difficult to industrialize, and the adsorbents are easily poisoned by SO₂.
Hollow-structured α-Fe₂O₃ microspheres were prepared using the phenolic resin hydrogel soft template method. EDTA was used as a chelating agent to achieve molecular-level dispersion of iron species. Arsenic was removed through a multi-step synergistic mechanism of physical adsorption-chemical oxidation-chemical fixation, and the microspheres were resistant to complex components such as SO₂.
It maintains structural integrity over a wide temperature range, efficiently removes gaseous As₂O₃, tolerates complex components such as SO₂, is easy to operate and suitable for industrialization, and the adsorbent can be regenerated and used multiple times, significantly reducing costs.
Smart Images

Figure CN123127945A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of inorganic non-metallic materials technology, specifically to an iron-based adsorbent, its preparation method, and its application. Background Technology
[0002] Arsenic-containing high-temperature flue gas generated during the smelting of non-ferrous metals (such as copper, lead, and zinc) is a major source of arsenic pollution in the atmosphere. Gaseous As2O3 is highly toxic, volatile, and insoluble in water, making it difficult to remove effectively using conventional wet desulfurization or baghouse dust collection. It is easily emitted with the flue gas, causing serious environmental pollution and health risks.
[0003] Currently, iron-based adsorbents (Fe2O3) are considered one of the most promising arsenic removal materials due to their inexpensive and readily available raw materials, stable chemical properties, and high chemical affinity for arsenic. However, in practical applications, traditional commercial Fe2O3 particles suffer from the following insurmountable drawbacks: First, the temperature of smelting flue gas is typically above 600℃, even reaching 1300℃. Commercial Fe2O3 particles are mostly solid, and at high temperatures, their surface diffusion coefficient increases, making them highly susceptible to grain boundary migration and particle agglomeration (sintering). This leads to a sharp decrease in specific surface area, a significant loss of active sites, and an exponential decline in arsenic removal efficiency. Second, although existing technologies disclose that hollow microsphere structures can improve the anti-sintering properties of materials, traditional hard template methods (such as using sulfonated polystyrene microspheres as templates) suffer from problems such as expensive templates and complex removal processes (usually requiring strong acids or organic solvents for etching), making large-scale industrial application difficult. Third, actual flue gas often contains large amounts of SO2, HCl, CO2, and water vapor. In particular, SO2 easily competes with adsorbents for adsorption, and may even react with metal oxides to form sulfates that cover the surface, leading to catalyst poisoning and deactivation. Summary of the Invention
[0004] In view of the shortcomings of the prior art, the purpose of this invention is to provide an iron-based adsorbent, its preparation method and application, in order to solve at least one of the problems in the background art.
[0005] A first aspect of the present invention is to provide a method for preparing an iron-based adsorbent, the method comprising: Resorcinol, ferric nitrate, and ethylenediaminetetraacetic acid were dissolved in deionized water at a predetermined molar ratio. The pH of the solution was adjusted to 1-2 with hydrochloric acid, and the mixture was stirred to obtain the precursor solution. The precursor solution was heated to a preset temperature, and formaldehyde solution was added dropwise to initiate the polymerization reaction. When an orange-red solid precipitate appeared, stirring was stopped, the mixture was kept at the temperature and allowed to stand, and then vacuum dried to obtain the hydrogel precursor. The hydrogel precursor was calcined in air, and after natural cooling, it was washed and dried to obtain the iron-based adsorbent.
[0006] According to one aspect of the above technical solution, the preset molar ratio of resorcinol, ferric nitrate and ethylenediaminetetraacetic acid is (15-25):(1-3):1.
[0007] According to one aspect of the above technical solution, the concentration of ferric nitrate in the precursor solution is 0.1 mol / L to 0.3 mol / L.
[0008] According to one aspect of the above technical solution, the stirring speed for mixing is 700rpm-900rpm, and the stirring time is 20min-40min.
[0009] According to one aspect of the above technical solution, the preset temperature is 80℃-90℃, the molar ratio of formaldehyde to resorcinol in the formaldehyde solution is 1:(1-3), and the concentration of the formaldehyde solution is 37%-40%.
[0010] According to one aspect of the above technical solution, the heat preservation and static setting time is 3h-5h, and the vacuum drying conditions are: drying temperature of 50℃-70℃ and drying time of 10h-14h.
[0011] According to one aspect of the above technical solution, the calcination temperature is 500℃-600℃, the heating rate is 5℃ / min-15℃ / min, and the calcination time is 3h-5h.
[0012] According to one aspect of the above technical solution, the washing process involves alternating between deionized water and anhydrous ethanol, with each wash performed 3 to 6 times. The drying temperature is 50℃-70℃, and the drying time is 10h-14h.
[0013] A second aspect of the present invention is to provide an iron-based adsorbent, wherein the iron-based adsorbent is prepared by the above-described method for preparing iron-based adsorbents, and the iron-based adsorbent is a hollow α-Fe2O3 microsphere with a diameter of 1 μm-2 μm and a shell thickness of 50 nm-100 nm. The shell is formed by stacking α-Fe2O3 nanoparticles with an average particle size of 5nm-10nm; The specific surface area of the iron-based adsorbent is 90 m². 2 / g-150m 2 / g, with a grain size of 15nm-25nm; The iron on the surface of the iron-based adsorbent exists entirely in the form of ferric iron.
[0014] A third aspect of the present invention is to provide the application of the iron-based adsorbent described above in the removal of gaseous arsenic trioxide from high-temperature flue gas, wherein the temperature range of the high-temperature flue gas is 200°C-1300°C, and the high-temperature flue gas contains at least one of water vapor, carbon dioxide, sulfur dioxide, and hydrogen chloride.
[0015] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. Overcoming the technical limitations of traditional iron-based adsorbents that are prone to sintering and agglomeration at high temperatures, this invention employs a phenolic resin hydrogel soft template method, using EDTA as a chelating agent to achieve molecular-level dispersion of iron species. After calcination, these iron species are transformed in situ into α-Fe2O3 microspheres with a hollow mesoporous structure. This hollow thin-shell structure not only endows the material with an extremely high specific surface area and abundant active sites, but more importantly, it fundamentally inhibits the long-range diffusion of iron atoms at high temperatures, effectively avoiding sintering deactivation of the material under high-temperature conditions and ensuring the structural integrity of the adsorbent over a wide temperature range.
[0016] 2. The arsenic removal process of the adsorbent of this invention follows a multi-step synergistic mechanism of physical adsorption-chemical oxidation-chemical fixation. Gaseous As2O3 is first adsorbed onto the material surface, and then oxidized to As2O5 under the synergistic effect of gaseous oxygen and lattice oxygen. Finally, it reacts with the Fe2O3 substrate to generate stable FeAsO4, achieving irreversible fixation of arsenic. Simultaneously, this adsorbent exhibits good tolerance to complex components commonly found in smelting flue gas, such as SO2, CO2, HCl, and H2O. Furthermore, the presence of an appropriate amount of SO2 promotes arsenic removal, demonstrating excellent adaptability to actual flue gas conditions.
[0017] 3. The soft template method used in this invention utilizes bulk industrial chemicals such as resorcinol and formaldehyde as raw materials, eliminating the need for costly templates like sulfonated polystyrene microspheres. The preparation process involves only four steps: solution preparation, heating polymerization, drying, and calcination. It is simple to operate, highly reproducible, and suitable for large-scale industrial production. Furthermore, the saturated adsorbent can be easily regenerated using a NaOH solution boiling method, maintaining excellent adsorption performance even after multiple cycles, significantly reducing industrial application costs. Attached Figure Description
[0018] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which: Figure 1 The figures shown are the BET adsorption-desorption isotherms and pore size distribution curves of this invention. Figure 1 (a) is Comparative Example 1. Figure 1 (b) is Example 1; Figure 2 The microstructure and elemental characterization of Example 1 (H-Fe2O3) of the present invention are shown in SEM image (a), EDS elemental distribution map (b, c), TEM image (d, e) and HRTEM image (f). Figure 3These are SEM comparison images of Example 1 (H-Fe2O3) and Comparative Example 1 (commercial Fe2O3 powder) before and after treatment at 1300℃; wherein, Figure 3 (a) Figure 3 Image (b) shows SEM comparison images of Example 1 (H-Fe2O3) before and after treatment at 1300℃. Figure 3 (c) Figure 3 In the image (d), SEM images of Comparative Example 1 (commercial Fe2O3 powder) before and after treatment at 1300℃ are shown respectively. Figure 4 This is the XPS spectrum of Example 1 (H-Fe2O3) of the present invention. Detailed Implementation
[0019] To make the objectives, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings. Several embodiments of the present invention are shown in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0020] This invention provides a method for preparing an iron-based adsorbent, the method comprising: steps S1-S3, Step S1: Resorcinol, ferric nitrate and ethylenediaminetetraacetic acid are dissolved in deionized water at a preset molar ratio. The pH of the solution is adjusted to 1-2 by hydrochloric acid and stirred to obtain the precursor solution. The preset molar ratio of resorcinol, ferric nitrate, and ethylenediaminetetraacetic acid is (15-25):(1-3):1. In the precursor solution, the concentration of ferric nitrate is 0.1 mol / L-0.3 mol / L. Resorcinol and formaldehyde are comonomers of phenolic resin hydrogels and are the basic raw materials for constructing a three-dimensional organic template network. Ferric nitrate is an iron source, providing the Fe required for subsequent conversion to α-Fe2O3. 3+ EDTA, as a powerful chelating agent, has multiple carboxyl and amine groups in its molecular structure that can bind with Fe. 3+ Formation of stable six-coordinate complexes (Fe-EDTA complexes), effectively inhibiting Fe 3+ Hydrolysis precipitation in solution ensures that iron ions are uniformly dispersed at the molecular level in the precursor solution, thereby forming uniformly sized nanocrystals during subsequent polymerization and calcination.
[0021] Furthermore, hydrochloric acid was used to adjust the solution pH to a strongly acidic environment. Under these conditions, the hydroxymethylation rate of resorcinol was moderate, which was conducive to the formation of a uniformly structured phenolic resin network. At the same time, the acidic environment also promoted the stable existence of the Fe-EDTA complex. High-speed magnetic stirring (700rpm-900rpm, 20min-40min) ensured thorough mixing of the components at both the macroscopic and microscopic scales.
[0022] Step S2: Heat the precursor solution to a preset temperature, add formaldehyde solution dropwise to initiate the polymerization reaction, stop stirring when an orange-red solid precipitate appears, keep warm and let stand, and vacuum dry to obtain the hydrogel precursor. Specifically, the preset temperature is 80℃-90℃, a classic reaction temperature for phenolic resin formation, ensuring a sufficient reaction rate while avoiding excessively vigorous reactions at excessively high temperatures that could lead to structural inhomogeneity. The addition of formaldehyde triggers a condensation reaction; the active hydrogen of resorcinol undergoes electrophilic addition with the carbonyl group of formaldehyde, followed by dehydration condensation to form methylene bridges, gradually constructing a three-dimensional cross-linked phenolic resin network. During this process, the Fe-EDTA complex, uniformly dispersed in the solution, is physically embedded and chemically anchored within the growing resin network. The appearance of an orange-red solid precipitate signifies the successful formation of the phenolic resin hydrogel, while Fe... 3+ The introduction of [a specific ingredient] imparts the characteristic orange-red color to the gel. Incubation at a warm temperature for 3-5 hours ensures the polycondensation reaction is fully completed, and the resin network reaches sufficient crosslinking density and structural strength. Vacuum drying thoroughly removes moisture, yielding dried "phenolic resin-Fe [a specific ingredient]". 3+ "Composite precursor."
[0023] In addition, the molar ratio of formaldehyde to resorcinol in the formaldehyde solution is 1:(1-3), the concentration of the formaldehyde solution is 37%-40%, and the vacuum drying conditions are: temperature of 50℃-70℃ and drying time of 10h-14h.
[0024] Step S3: Calcine the hydrogel precursor in air atmosphere, cool it naturally, wash and dry it to obtain the iron-based adsorbent.
[0025] Specifically, the calcination temperature is 500℃-600℃, and the calcination time is 3-5 hours. The phenolic resin organic framework first undergoes pyrolysis and carbonization, then the carbonization products react with O2 in the air to generate CO2 gas, which escapes, and the organic template is completely removed. Simultaneously, Fe, uniformly dispersed in the resin network... 3+ Under a high-temperature oxidizing atmosphere, it is transformed in situ into α-Fe₂O₃ (hematite phase) nanocrystals, Fe 3+The α-Fe₂O₃ crystals react with O₂ to form Fe₂O₃, and the crystals self-assemble and arrange themselves along the spherical outline of the template, ultimately forming α-Fe₂O₃ microspheres with a hollow structure. The calcination temperature of 500℃-600℃ was optimized to ensure complete removal of the organic template (phenolic resin is basically decomposed above 500℃) without causing excessive growth of α-Fe₂O₃ crystals due to excessive temperature. The holding time ensured sufficient removal of the template and sufficient crystallization of the crystals.
[0026] Furthermore, the heating rate of 5℃ / min-15℃ / min ensured the complete oxidation and removal of the organic template while avoiding localized overheating and structural collapse caused by excessively rapid heating. Natural cooling prevented thermal stress cracks caused by rapid cooling.
[0027] Furthermore, the washing process involves alternating between deionized water and anhydrous ethanol, with each wash performed 3-6 times. The drying temperature is 50℃-70℃, and the drying time is 10-14 hours. The alternating washing with ethanol and deionized water effectively removes residual impurity ions and unreacted raw materials.
[0028] Accordingly, the present invention also provides an iron-based adsorbent, which is prepared by the above-mentioned method for preparing iron-based adsorbents, wherein the iron-based adsorbent has a diameter of 1μm-2μm and a shell thickness of 50nm-100nm. The shell is formed by stacking α-Fe2O3 nanoparticles with an average particle size of 5nm-10nm; The specific surface area of the iron-based adsorbent is 90 m². 2 / g-150m 2 / g, with a grain size of 15nm-25nm, and a pure α-phase structure; The iron on the surface of the iron-based adsorbent exists entirely in the form of ferric iron.
[0029] In addition, the present invention also provides the application of the above-mentioned iron-based adsorbent in the removal of gaseous arsenic trioxide from high-temperature flue gas, wherein the temperature range of the high-temperature flue gas is 200℃-1300℃, and the high-temperature flue gas contains at least one of water vapor, carbon dioxide, sulfur dioxide and hydrogen chloride.
[0030] Furthermore, the iron-based adsorbent can be regenerated by alkaline boiling with NaOH solution after use, and this regeneration method can be recycled more than 6 times.
[0031] The present invention is further illustrated below with specific embodiments: Example 1 Example 1 of the present invention provides a method for preparing an iron-based adsorbent, the method comprising: steps S1-S3.
[0032] Step S1, preparation of precursor solution: Take 2 mol resorcinol (AR, ≥99.5%), 0.2 mol ferric nitrate (AR, ≥98%), and 0.1 mol ethylenediaminetetraacetic acid (AR, ≥99.5%) and add them to 1 L of deionized water. Adjust the pH of the mixed solution to 1.5 with hydrochloric acid and stir magnetically at 800 rpm for 30 min to obtain the precursor solution. Step S2, 3D structure construction: Heat the precursor solution in an oil bath with stirring to 85°C, and quickly add 20 mL of formaldehyde (AR, 37%-40%) solution. Stop stirring when an orange-red solid precipitate appears, keep it at 85°C for 4 hours, and dry the resulting orange-red hydrogel in a vacuum drying oven until all moisture is evaporated. Step S3, calcination to remove the template: The dried hydrogel was placed in a muffle furnace and heated to 600℃ at a rate of 10℃ / min under air atmosphere, and calcined at this temperature for 4 hours to carbonize and remove the organic framework. After natural cooling, the resulting red precipitate was washed and filtered five times each with anhydrous ethanol and deionized water, and then dried in a forced-air drying oven at 60℃ for 12 hours. The iron-based adsorbent was obtained, denoted as H-Fe2O3.
[0033] Example 2 The difference between Example 2 and Example 1 of the present invention is that in step S3, the calcination temperature is changed to 550℃ and 650℃ respectively, while the other step conditions remain unchanged, and the adsorbents are respectively recorded as Example 2-1 and Example 2-2.
[0034] Example 3 The difference between Example 3 and Example 1 of the present invention is that in step S1, the pH is adjusted to 1 and 2 respectively, while the other conditions remain unchanged, and the adsorbents are respectively recorded as Example 3-1 and Example 3-2.
[0035] Example 4 The difference between Example 4 and Example 1 is that in step S1, the amount of EDTA is changed to 0 and 0.2 mol respectively, while the other conditions remain unchanged. The adsorbents are respectively recorded as Example 4-1 and Example 4-2.
[0036] Comparative Example 1 The difference between Comparative Example 1 and Example 1 of this invention is that iron-based adsorbents are not prepared, and commercial Fe2O3 powder (solid spheres) is used instead of H-Fe2O3.
[0037] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that in step S1, ethylenediaminetetraacetic acid (EDTA) is replaced with an equimolar mass of sodium citrate, while the other conditions remain unchanged.
[0038] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that in step S1, ethylenediaminetetraacetic acid (EDTA) is replaced with an equimolar mass of ethylene glycol, while the other conditions remain unchanged.
[0039] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that in step S1, ethylenediaminetetraacetic acid (EDTA) is replaced with equimolar amounts of glycerol, while the other conditions remain unchanged.
[0040] Comparative Example 5 The difference between Comparative Example 5 and Example 1 is that in step S1, ethylenediaminetetraacetic acid (EDTA) is replaced with an equimolar mass of deionized water, while the conditions of other steps remain unchanged.
[0041] Comparative Example 6 The difference between Comparative Example 6 and Example 1 is that in step S1, ferric nitrate is replaced with an equimolar mass of copper nitrate, while the conditions of other steps remain unchanged.
[0042] Comparative Example 7 The difference between Comparative Example 7 and Example 1 is that in step S1, ferric nitrate is replaced with equimolar mass of cerium nitrate, while the conditions of other steps remain unchanged.
[0043] Comparative Example 8 The difference between Comparative Example 8 and Example 1 is that in step S1, ferric nitrate is replaced with an equimolar mass of aluminum nitrate, while the conditions of other steps remain unchanged.
[0044] Arsenic removal performance tests of iron-based adsorbents prepared under different conditions: 50 mg of iron-based adsorbent (Examples 1, 2-1, 2-2, 3-1, 3-2, 4-1, and 4-2) was taken and injected together with simulated arsenic-containing flue gas into a quartz tube inside a muffle furnace. A filter cloth was installed at the end of the quartz tube to collect the adsorbent. The experimental conditions were as follows: the total arsenic trioxide content in the simulated flue gas was 0.5 mg, the flue gas flow rate was 0.1 L / min, the arsenic trioxide concentration in the flue gas was 0.0833 mg / L, the gas composition was 20% O2 + 80% N2, and the flue gas temperature was 600℃. The results are shown in Table 1.
[0045] Table 1:
[0046] As shown in Table 1, the optimal synthesis conditions for the iron-based adsorbent are pH=1.5, EDTA addition of 0.1 mol in step S1, and calcination temperature of 600℃ in step 3.
[0047] Adsorbent characterization: The obtained adsorbent was subjected to BET test and SEM and EDS spectral tests.
[0048] like Figures 1-4 As shown, BET test results indicate that the specific surface area of the obtained adsorbent is superior to that of the commercial Fe2O3 powder in Comparative Example 1. The shell is formed by the stacking of nanoparticles with an average particle size of approximately 1 μm-2 μm, and the shell thickness is approximately 50 nm-100 nm. The shell is composed of α-Fe2O3 nanoparticles with an average particle size of 5 nm-10 nm, and no other iron oxide impurities are present. XPS analysis shows that the iron on the adsorbent surface is entirely in the form of ferric iron (Fe2O3). 3+ It exists in the form of ).
[0049] Arsenic removal performance test: 50 mg of iron-based adsorbent (Example 1) was taken and injected together with simulated arsenic-containing flue gas into a quartz tube inside a muffle furnace. Filter cloth was installed at the end of the quartz tube to collect the adsorbent. The experimental conditions were as follows: the total arsenic trioxide content in the simulated flue gas was 0.5 mg, the flue gas flow rate was 0.1 L / min, the arsenic trioxide concentration in the flue gas was 0.0833 mg / L, the gas composition was 20% O2 + 80% N2, and the flue gas temperature was 200℃-1300℃. The results are shown in Table 2.
[0050] Table 2:
[0051] Table 3:
[0052] As shown in Tables 2 and 3, the iron-based adsorbent maintains high efficiency across an ultra-wide temperature range of 200℃ to 1300℃. Particularly in the 1000℃-1300℃ range, the adsorbent... Figure 4 XRD analysis of the adsorbent after the reaction showed that the arsenic trioxide captured by the adsorbent existed in the form of FeAsO4, with an adsorption capacity maintained above 7.16 mg / g, far superior to commercial Fe2O3 (Comparative Example 1 shows that commercial Fe2O3 almost failed at 1300℃). As shown in Table 3, H-Fe2O3 could still maintain 67.22 mg / g under ultra-high temperature conditions of 1300℃. 2 The specific surface area of / g fully demonstrates the significant role of the hollow structure in resisting sintering.
[0053] To investigate the effect of different flue gas atmospheres on the arsenic removal performance of the adsorbent, 20 mg of adsorbent H-Fe2O3 was taken and injected together with simulated arsenic-containing flue gas into a quartz tube inside a muffle furnace. A filter cloth was installed at the end of the quartz tube to collect the adsorbent. The experimental conditions were: arsenic content in the simulated flue gas was 0.2 mg, flue gas flow rate was 0.1 L / min, and reaction temperature was controlled at 600℃. Adsorption tests were conducted under different flue gas atmospheres, and the results are shown in Table 4.
[0054] Table 4:
[0055] Table 4 shows that the presence of O2 is crucial for arsenic removal (efficiency is halved under anaerobic conditions). More importantly, in an atmosphere containing SO2, when the SO2 concentration is ≤10% (approximately 0.8 g / kg), the arsenic removal efficiency not only does not decrease but actually increases slightly (reaching a maximum of 95.1%). The presence of SO2 generates sulfate ions on the adsorbent surface, which is beneficial for arsenic capture, confirming the promoting effect of SO2. Even at a high SO2 concentration of 20%, the efficiency remains at 86.3%, demonstrating extremely strong sulfur resistance. Even under simulated industrial conditions, when SO2 and H2O are present simultaneously in the smelting flue gas, good adsorption performance is still achieved. It also exhibits good tolerance to CO2, HCl, and H2O.
[0056] Adsorption-regeneration cycle test: Adsorption process: 20 mg of adsorbent H-Fe2O3 was injected together with simulated arsenic-containing flue gas into a quartz tube inside a muffle furnace. A filter cloth was installed at the end of the quartz tube to collect the adsorbent. The experimental conditions were: arsenic content in the simulated flue gas was 1 mg, flue gas flow rate was 0.1 L / min, flue gas composition was 20% O2 + 80% N2, and adsorption temperature was 600℃.
[0057] Regeneration process: After adsorption saturation, desorption and thermal activation regeneration are performed using NaOH solution alkaline boiling: the saturated adsorbent is placed in NaOH solution (concentration 2 mol / L) and boiled at 100℃ for 2 hours, so that the arsenate ions in FeAsO4 react with OH-. - The adsorbent is released through ion exchange, while simultaneously regenerating the Fe2O3 active sites. The regenerated adsorbent is washed three times with deionized water, dried at 50°C for 2 hours, and then used for the next adsorption cycle. Five cycles were performed, and the results are shown in Table 5.
[0058] Table 5:
[0059] As shown in Table 5, after six alkaline boiling regenerations, the adsorption efficiency of the adsorbent remained above 76.8% of the initial value, indicating that the adsorbent has a stable structure, a simple and effective regeneration process, and has the potential for industrial application.
[0060] Chelating agent screening and comparison experiment: Experimental method: The adsorbents prepared in Example 1 and Comparative Examples 2-5 were subjected to adsorption performance tests. The adsorption process was the same as that in the adsorption-regeneration cycle test. The results are shown in Table 6.
[0061] Table 6:
[0062] As shown in Table 6, EDTA, due to its unique spatial structure and strong chelation constant, can more effectively control Fe. 3+ The dispersion and release of EDTA resulted in the preparation of an adsorbent with smaller crystallites and a superior structure, exhibiting significantly better arsenic removal performance than other comparative examples. This demonstrates the crucial role of EDTA in this invention.
[0063] Arsenic removal performance test comparison: Test method: The adsorbents of Example 1 and Comparative Example 1 were subjected to performance tests, which were the same as those for arsenic removal performance tests. The results are shown in Table 7.
[0064] Table 7:
[0065] As shown in Table 7, within the temperature range of 200℃-900℃, the saturated adsorption capacity of Example 1 (H-Fe2O3) of the present invention remained stable at 6.76 mg / g-9.15 mg / g, reaching a peak of 9.15 mg / g at 600℃. In contrast, the adsorption capacity of Comparative Example 1 (commercial Fe2O3 powder) in this temperature range was only 0.92 mg / g-2.18 mg / g, significantly lower, and its performance degradation was more pronounced with increasing temperature. The difference between the two was 3-8 times. Within the temperature range of 1000℃-1300℃, the adsorption capacity of Comparative Example 1 (commercial Fe2O3 powder) dropped sharply to below 0.68 mg / g, almost losing its arsenic removal ability. In contrast, Example 1 (H-Fe2O3) maintained a saturated adsorption capacity retention rate of over 71.6% (7.16 mg / g at 1300℃), and as... Figure 3 As shown, Comparative Example 1 (commercial Fe2O3 powder) underwent severe sintering and agglomeration at 1300℃, with particles tightly clustered into dense lumps, resulting in a sharp drop in specific surface area and a significant loss of active sites. In contrast, Example 1 (H-Fe2O3), after undergoing the same ultra-high temperature treatment, maintained a clear and intact hollow mesoporous microsphere morphology, without exhibiting obvious sintering and agglomeration.
[0066] Comparison with other metal oxide hollow microspheres: Take 50 mg of the above-mentioned adsorbent (Example 1, Comparative Examples 6-8), and inject the adsorbent and simulated arsenic-containing flue gas together into a quartz tube inside a muffle furnace. A filter cloth is installed at the end of the quartz tube to collect the adsorbent. The experimental conditions were as follows: the total arsenic trioxide content in the simulated flue gas was 0.5 mg, the flue gas flow rate was 0.1 L / min, the arsenic trioxide concentration in the flue gas was 0.0833 mg / L, the gas composition was 20% O2 + 80% N2, and the flue gas temperature was 600℃. The results are shown in Table 8.
[0067] Table 8:
[0068] As shown in Table 8, at 600℃, the adsorption capacities of Comparative Examples 6, 7, and 8 were 3.84 mg / g, 3.61 mg / g, and 6.77 mg / g, respectively, all significantly lower than that of Example 1 (9.15 mg / g). This indicates that H-Fe2O3 not only has a higher chemical affinity for arsenic, but also exhibits a stronger thermodynamic tendency to react with arsenic to form FeAsO4, demonstrating the superiority of iron-based materials in the field of arsenic removal.
[0069] In the description of this specification, references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0070] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this patent should be determined by the appended claims.
Claims
1. A method for preparing an iron-based adsorbent, characterized in that, The method includes: Resorcinol, ferric nitrate, and ethylenediaminetetraacetic acid were dissolved in deionized water at a predetermined molar ratio. The pH of the solution was adjusted to 1-2 with hydrochloric acid, and the mixture was stirred to obtain the precursor solution. The precursor solution was heated to a preset temperature, and formaldehyde solution was added dropwise to initiate the polymerization reaction. When an orange-red solid precipitate appeared, stirring was stopped, the mixture was kept at the temperature and allowed to stand, and then vacuum dried to obtain the hydrogel precursor. The hydrogel precursor was calcined in air, and after natural cooling, it was washed and dried to obtain the iron-based adsorbent.
2. The method for preparing the iron-based adsorbent according to claim 1, characterized in that, The preset molar ratio of resorcinol, ferric nitrate and ethylenediaminetetraacetic acid is (15-25):(1-3):
1.
3. The method for preparing the iron-based adsorbent according to claim 2, characterized in that, In the precursor solution, the concentration of ferric nitrate is 0.1 mol / L to 0.3 mol / L.
4. The method for preparing the iron-based adsorbent according to claim 1, characterized in that, The stirring speed is 700rpm-900rpm and the stirring time is 20min-40min.
5. The method for preparing the iron-based adsorbent according to claim 1, characterized in that, The preset temperature is 80℃-90℃, the molar ratio of formaldehyde to resorcinol in the formaldehyde solution is 1:(1-3), and the concentration of the formaldehyde solution is 37%-40%.
6. The method for preparing the iron-based adsorbent according to claim 5, characterized in that, The heat preservation and static setting time is 3-5 hours, and the vacuum drying conditions are: drying temperature of 50℃-70℃ and drying time of 10-14 hours.
7. The method for preparing the iron-based adsorbent according to claim 1, characterized in that, The calcination temperature is 500℃-600℃, the heating rate is 5℃ / min-15℃ / min, and the calcination time is 3h-5h.
8. The method for preparing the iron-based adsorbent according to claim 1, characterized in that, The washing process involves alternating between deionized water and anhydrous ethanol, with each wash performed 3 to 6 times. The drying temperature is 50℃-70℃, and the drying time is 10h-14h.
9. An iron-based adsorbent, said iron-based adsorbent being prepared by the method for preparing the iron-based adsorbent according to any one of claims 1-8, characterized in that, The iron-based adsorbent is a hollow α-Fe2O3 microsphere with a diameter of 1μm-2μm and a shell thickness of 50nm-100nm. The shell is formed by stacking α-Fe2O3 nanoparticles with an average particle size of 5nm-10nm; The specific surface area of the iron-based adsorbent is 90 m². 2 / g-150m 2 / g, with a grain size of 15nm-25nm; The iron on the surface of the iron-based adsorbent exists entirely in the form of ferric iron.
10. The application of the iron-based adsorbent as described in claim 9 in the removal of gaseous arsenic trioxide from high-temperature flue gas, characterized in that, The temperature range of the high-temperature flue gas is 200℃-1300℃, and the high-temperature flue gas contains at least one of water vapor, carbon dioxide, sulfur dioxide and hydrogen chloride.