A system and method for preparing a waste ceramic-based porous adsorbent material for water treatment
By preparing high-performance ceramic particle adsorption filter media through a systematic process, the problems of low adsorption capacity and poor selectivity of ceramic solid waste in water treatment are solved, achieving efficient and stable pollutant adsorption, and making it suitable for different water quality conditions.
Patent Information
- Application Number
- CN202611181158.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-05
- Publication Date
- 2026-11-20
AI Technical Summary
Existing ceramic solid waste adsorption materials for water treatment suffer from problems such as low adsorption capacity, poor selectivity, and unstable molding process, making it difficult to meet the treatment needs under different water quality conditions.
A systematic process of pretreatment, activation modification, molding and granulation, and heat treatment is adopted to prepare ceramic granules adsorption filter media with high specific surface area and rich pore structure using solid waste from the ceramic industry. Impurities are removed by belt magnetic separator and manual sorting, particle size is controlled by ball milling and sieving, acid and alkali activation modification forms rich pore structure, and granulation by extruder and ball rolling machine forms uniform spherical particles. Multi-temperature zone calcination furnace ensures the stability of pore structure.
This research has enabled the high-value utilization of ceramic solid waste and produced high-performance adsorbent materials. These materials have high adsorption capacity for pollutants such as heavy metals, dyes, and phosphorus, with improved adsorption capacity, strong selectivity, stable molding, low cost, and applicability to different water quality conditions.
Smart Images

Figure CN123127947A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of water treatment technology, and more specifically, relates to a preparation system and method for waste ceramic-based porous adsorbent materials for water treatment. Background Technology
[0002] Ceramic solid waste (waste ceramic tiles, ceramic blanks, kiln slag, waste clay, etc.) is a large amount of solid waste generated by the ceramic industry. Its main components are SiO2 and Al2O3, containing trace amounts of oxides such as Ca, Mg, and Fe. It has the characteristics of stable porous framework structure, acid and alkali resistance, and high temperature resistance. After activation and modification, it can be used to prepare adsorption materials for adsorbing pollutants such as heavy metal ions, dyes, ammonia nitrogen, phosphorus, and oil. It has important application potential in the field of water treatment.
[0003] Currently, the resource utilization of ceramic solid waste is mainly concentrated in the field of building materials, such as the preparation of extensive products like ceramsite and bricks. However, research and application in the field of water treatment adsorption materials are still in their infancy. In the actual preparation process, problems such as large fluctuations in raw material composition, extensive pretreatment processes, low activation and modification efficiency, insufficient adsorption capacity, single product form, and poor regeneration performance restrict the large-scale application of ceramic-based adsorption materials. In addition, the selective adsorption capacity of ceramic-based adsorption materials prepared by existing technologies for specific pollutants (such as heavy metals, phosphorus, and fluorine) is weak, making it difficult to meet the treatment needs under different water quality conditions. In summary, in order to achieve high-value utilization of ceramic solid waste, it is urgent to solve technical problems such as low adsorption capacity, poor selectivity, and unstable molding process. Summary of the Invention
[0004] This application addresses the technical problems existing in the resource utilization technology of ceramic solid waste, such as low adsorption capacity, low activation and modification efficiency, and weak selective adsorption capacity. It provides a preparation system and method for waste ceramic-based porous adsorption materials for water treatment. The system uses ceramic industrial solid waste as raw material and prepares ceramic particle adsorption filter material with large specific surface area, rich pore structure and high adsorption capacity through systematic pretreatment, activation and modification, molding and granulation and heat treatment shaping process, thereby realizing the high-value resource utilization of ceramic solid waste.
[0005] Therefore, embodiments of this application propose a system for preparing high-efficiency adsorption materials based on ceramic solid waste, comprising a pretreatment unit, an activation and modification unit, a molding and granulation unit, and a heat treatment and shaping unit connected in sequence. The raw material enters the pretreatment unit through the raw material inlet, and after being processed by the activation and modification unit, the molding and granulation unit, and the heat treatment and shaping unit in sequence, the finished ceramic adsorption filter material is output from the finished product outlet. The four units are continuously connected through a material conveying mechanism to form a complete production line for the high-value utilization of ceramic solid waste.
[0006] The pretreatment unit includes a sorting device, a crushing device, a ball mill screening device, and a drying device. The outlet of the sorting device is connected to the inlet of the crushing device, the outlet of the crushing device is connected to the inlet of the ball mill screening device, the outlet of the ball mill screening device is connected to the inlet of the drying device, and the outlet of the drying device is connected to the activation and modification unit.
[0007] The sorting device combines a belt magnetic separator with manual sorting. The belt magnetic separator uses a permanent magnet drum to magnetically separate the ceramic waste to remove metallic impurities. The manual sorting station is located beside the belt conveyor to remove non-ceramic foreign objects. The outlet of the sorting device is connected to the inlet of the crushing device via an inclined chute to ensure smooth material transfer. The crushing device uses a jaw crusher as the primary crushing equipment. The feed opening size of the jaw crusher is matched to the maximum particle size of the sorted ceramic waste to ensure smooth feeding. The discharge outlet is equipped with an adjustment device to control the particle size range after crushing. The ball milling and screening device uses a planetary ball mill in conjunction with a standard sieve. The grinding jar and grinding balls of the planetary ball mill are made of zirconium oxide to avoid the introduction of metal impurities. The ball milling time is 1 to 3 hours to refine the ceramic solid waste particles to 60 to 200 mesh. After ball milling, the particles are screened by a vibrating screen in conjunction with a standard sieve to accurately control the particle size distribution. The drying device uses a hot air circulating drying box. The inlet air temperature of the hot air circulating drying box is set to 105℃, and the drying time is 2 to 4 hours. During the drying process, the powder is continuously turned over by a turning mechanism to ensure uniform drying. After drying, the moisture content of the ceramic powder is controlled below 1%.
[0008] The activation and modification unit includes an acid storage tank, an alkali storage tank, a metal salt solution storage tank, and an activation reactor. The outlet of the acid storage tank is connected to the acid inlet of the activation reactor via a corrosion-resistant solenoid valve. The outlet of the alkali storage tank is connected to the alkali inlet of the activation reactor via a corrosion-resistant solenoid valve. The outlet of the metal salt solution storage tank is connected to the metal salt inlet of the activation reactor via a corrosion-resistant solenoid valve. The pipelines between each storage tank and the activation reactor are made of polytetrafluoroethylene (PTFE) to withstand acid and alkali corrosion. The outlet of the activation reactor is connected to the molding and granulation unit.
[0009] Furthermore, the activation reactor is equipped with a temperature sensor, a stirring device, and a level gauge. The temperature sensor is embedded in the inner wall of the activation reactor and penetrates the reactor wall. The temperature sensor is a PT100 platinum resistance temperature sensor with a temperature measurement accuracy of ±0.1℃ to achieve precise sensing of the internal temperature of the reactor. The stirring device includes a stirring shaft and a spiral stirring blade. The top end of the stirring shaft is fixedly connected to the center hole of the reactor cover through a bearing seat. The bearing seat has a double-end mechanical seal structure to prevent leakage of the reaction liquid. The spiral stirring blade is fixedly connected to the bottom end of the stirring shaft and is located below the liquid surface inside the reactor. The stirring shaft is made of stainless steel, and the stirring speed is steplessly adjustable through a frequency converter. The preferred speed range is 100 to 300 rpm to achieve uniform stirring of the liquid inside the reactor. The level gauge is located on the side of the reactor and penetrates the reactor wall. The level gauge is a magnetic float level gauge or an ultrasonic level gauge to achieve real-time monitoring and level warning functions.
[0010] Furthermore, the activation reactor also includes a preheating mechanism and a temperature control system. The preheating mechanism is located in the bottom jacket of the activation reactor, forming an annular heating chamber. The preheating mechanism adopts an electric heating jacket structure, and the electric heating elements are arranged in the bottom jacket to preheat the activation liquid before it enters the reactor. The temperature control system includes a PID controller and a heating resistor. The input terminal of the PID controller is connected to the output terminal of the temperature sensor to form a closed-loop control circuit. The PID controller has a self-tuning function to automatically adjust the PID parameters according to the characteristics of the reaction system, thereby achieving rapid temperature stabilization and precise temperature control. The heating resistor is a stainless steel electric heating tube, which is evenly arranged in the bottom jacket to ensure uniform heat distribution.
[0011] The molding and granulation unit includes a mixing device, a granulation device, and a pre-drying device. The inlet of the mixing device is connected to the outlet of the activation reactor and the binder storage tank, respectively. The outlet of the mixing device is connected to the inlet of the granulation device, and the outlet of the granulation device is connected to the pre-drying device. The mixing device is preferably a double-spiral conical mixer. The stirring spiral of the double-spiral conical mixer is made of stainless steel and has a wear-resistant coating on its surface. The filling coefficient of the mixer is 0.4 to 0.6 to ensure the mixing effect. The mixing time is 10 to 20 minutes to achieve uniform mixing of activated ceramic powder and binder. The pre-drying device is preferably a mesh belt pre-dryer. The mesh belt of the mesh belt pre-dryer is made of stainless steel woven mesh to have good air permeability. The running speed of the mesh belt is adjusted by a frequency converter. The pre-drying temperature is room temperature to avoid deformation of particles due to high temperature. The pre-drying time is 12 to 24 hours to control the moisture content of the pre-dried particles to 10% to 15%.
[0012] Furthermore, the granulation device includes an extruder and a ball-forming machine. The inlet of the extruder is connected to the outlet of the mixing device via a screw conveyor. The extruder contains an extrusion die with multiple forming holes of 2 to 4 mm in diameter. The extrusion die adopts a modular design to allow for replacement with dies of different hole diameters as needed. The screw speed of the extruder is adjusted via a frequency converter to control the extrusion speed of the strip-shaped granules. The inlet of the ball-forming machine is connected to the strip-shaped granule outlet of the extruder via a vibrating feeder. The machine is equipped with a rotating drum, and the inner wall of the rotating drum is provided with multiple arc-shaped baffles. The arc-shaped baffles are evenly distributed on the inner wall of the drum, and the height of the baffles is 1 / 10 to 1 / 8 of the diameter of the drum. The ball rolling machine adopts an inclined drum design with an inclination angle of 5° to 15° so that the strip-shaped particles are subjected to the combined action of gravity and centrifugal force in the rotating drum. Under the collision and friction of the arc-shaped baffles, they gradually roll into spherical particles with a diameter of 2 to 8 mm. The rotation speed of the ball rolling machine is adjusted by a frequency converter to control the sphericity.
[0013] The heat treatment shaping unit includes a roasting furnace and a cooling and screening device. The inlet of the roasting furnace is connected to the outlet of the pre-drying device, and the outlet of the roasting furnace is connected to the inlet of the cooling and screening device.
[0014] The calcining furnace adopts a roller kiln or tunnel kiln to achieve continuous production. The calcining furnace is equipped with at least three temperature zones, which correspond to the preheating zone, high temperature zone and heat preservation zone, respectively. Each temperature zone is independently equipped with a thermocouple and heating element to achieve independent temperature control. The heating rate of the calcining furnace is 5 to 15℃ / min, the calcination temperature is 700 to 850℃, and the heat preservation time is 30 to 90min. The discharge port of the calcining furnace is equipped with an automatic unloading device, which adopts a hydraulic pusher or a pneumatic pusher to automatically unload the ceramic adsorbent filter material after calcination and send it to the cooling and screening device.
[0015] Furthermore, the cooling and screening device includes a cooling mechanism and a vibrating screening mechanism. The cooling mechanism is located downstream of the discharge end of the roasting furnace. The cooling mechanism adopts either air cooling or water cooling. The air cooling method uses a high-pressure blower to force airflow to improve cooling efficiency, while the water cooling method uses a shell-and-tube heat exchanger to accelerate the cooling speed. The inlet of the vibrating screening mechanism is connected to the outlet of the cooling mechanism via a chute. The vibrating screening mechanism has at least two layers of screens. The first layer of screens has a mesh size of 8mm to remove particles larger than 8mm, and the second layer of screens has a mesh size of 2mm to remove particles smaller than 2mm. The particles between the two layers of screens constitute the finished adsorbent material with a particle size range of 2 to 8mm. The vibrating screening mechanism adopts a multi-layer stacked screen design to increase the number of screen layers as needed to obtain products with various particle size grades such as 2 to 4mm, 4 to 6mm, and 6 to 8mm. The vibrating motor is an adjustable frequency vibrating motor, and the amplitude and vibration frequency are adjusted according to the material characteristics through a frequency converter to ensure screening accuracy.
[0016] The proportions of each raw material by mass percentage are as follows: ceramic waste powder 75% to 90%, pore-forming agent 5% to 12%, binder 3% to 8%, and activating agent 2% to 5%.
[0017] The pore-forming agent is calcium carbonate or sodium bicarbonate, which decomposes and releases carbon dioxide gas during high-temperature calcination to form a rich pore structure inside the ceramic particles, thereby significantly increasing the specific surface area of the adsorbent material. The binder is bentonite or kaolin to provide good bonding performance, ensuring that the particles sinter and solidify during calcination to form stable mechanical strength. The activating agent is sodium hydroxide or potassium hydroxide, which provides a strongly alkaline environment during activation to further etch the ceramic surface, thereby generating more active adsorption sites.
[0018] The embodiments of this application also provide a method for preparing a ceramic solid waste-based high-efficiency adsorbent material using the above system, comprising the following steps: Step S1 is pretreatment: After removing impurities from the ceramic solid waste through a sorting device, it is then processed by a crushing device and a ball mill screening device for fine treatment. The sorting device uses a combination of belt magnetic separator and manual sorting to remove metallic impurities and non-ceramic foreign objects. The crushing device uses a jaw crusher for coarse crushing to break the ceramic solid waste into particles with a particle size of 10 to 50 mm. The ball mill screening device uses a planetary ball mill for fine grinding to obtain ceramic powder with a particle size of 60 to 200 mesh. Then, it is dried at 105°C for 2 to 4 hours by a drying device to obtain dried ceramic powder. After drying, the moisture content of the ceramic powder is controlled below 1%.
[0019] Step S2 is activation modification: Dry ceramic powder is added to an activation reactor, and acid activator is added at a mass ratio of ceramic powder: acid solution = 1:3 to 1:5 for acid activation treatment, or alkali activator is added at a mass ratio of ceramic powder: alkali = 1:0.5 to 1:1.2 for alkali activation treatment. The activation modification treatment is carried out by stirring in a water bath at 80°C for 2 to 4 hours to ensure that the activator and ceramic powder are fully in contact and react. After filtration, the powder is washed with deionized water until neutral, and then dried again at 105°C to obtain activated ceramic powder.
[0020] In the acid activation process, one or more combinations of dilute hydrochloric acid, dilute sulfuric acid, or nitric acid are used, with an acid concentration of 0.5 to 2 mol / L. Acid activation effectively removes impurities and oxides from the surface of ceramic powder to expose more active sites. In the alkali activation process, an aqueous solution of sodium hydroxide or potassium hydroxide is used, with a concentration of 1 to 5 mol / L. After alkali activation, calcination activation is required at 500 to 700°C to etch rich micropores and mesoporous structures on the ceramic surface, thereby generating a microporous and mesoporous structure. Alternatively, the activated ceramic powder is immersed in a metal salt solution, which is then dried after standing. The metal salt solution is an aqueous solution of ferric chloride, manganese chloride, lanthanum chloride, or aluminum chloride, with a metal ion concentration of 0.1 to 1.0 mol / L. The immersion time is 12 to 24 hours to allow the metal ions to fully penetrate into the ceramic matrix. Then, it is calcined at a low temperature of 300 to 500°C to obtain a metal ion-supported adsorbent material. During the calcination process, metal ions form metal oxide active sites on the ceramic surface, giving the adsorbent material a high selective adsorption capacity for specific pollutants.
[0021] Step S3 is molding and granulation: The activated ceramic powder, pore-forming agent and binder are mixed and added to the mixing device. Deionized water is added at a solid-liquid ratio of 1:0.3 to 1:0.6 and stirred evenly to obtain a mixed mud. The moisture content of the mixed mud is controlled at 25% to 35%. Then the mixed mud is molded by a granulation device. The granulation device uses an extruder and a ball rolling machine for two-step granulation. First, the mixed mud is extruded into strip-shaped particles with a diameter of 2 to 4 mm by the extruder. Then, the strip-shaped particles are ground into spherical particles with a diameter of 2 to 8 mm by the ball rolling machine. Finally, the particles are pre-dried at room temperature for 12 to 24 hours by a pre-drying device. After pre-drying, the moisture content of the particles is controlled at 10% to 15%.
[0022] Step S4 is heat treatment shaping: the pre-dried particulate adsorbent material is placed in a calcination furnace and heated to 700 to 850°C at a heating rate of 5 to 15°C / min. After holding at this temperature for 30 to 90 minutes, it is cooled to room temperature and then screened through a cooling sieving device to obtain the finished ceramic adsorbent filter material with a particle size of 2 to 8 mm.
[0023] The calcination process employs a segmented heating method: first, the temperature is raised to 300℃ at 10℃ / min and held for 20 minutes for pre-sintering treatment to remove residual moisture and volatile organic matter inside the particles; then, the temperature is raised to the set temperature at 8℃ / min for high-temperature shaping treatment to promote the stabilization of the internal structure of the particles. The cooling process adopts a stepped cooling method: first, forced air cooling is used to quickly cool to 400℃, and then natural cooling is used to slowly cool to room temperature to prevent the particles from cracking due to excessive thermal stress.
[0024] This application provides a system for monitoring and processing abnormal charging orders. It has the following beneficial effects: 1. Through a systematic process of pretreatment, activation modification, molding granulation and heat treatment, high-value utilization of ceramic solid waste is achieved. High-performance adsorbent materials are prepared using ceramic industrial solid waste as the main raw material, transforming bulk solid waste into high-value-added water treatment functional materials.
[0025] 2. Through different activation and modification processes such as acid activation, alkali activation, or metal ion loading, the pore structure and specific surface area of ceramic-based adsorbent materials are significantly improved. The resulting ceramic particle adsorbent filter media has a specific surface area of 80 to 350 m² / g, a pore volume of 0.2 to 0.6 cm³ / g, an adsorption capacity of 20 to 80 mg / g for copper ions, an adsorption capacity of 30 to 100 mg / g for lead ions, and an adsorption capacity of 15 to 50 mg / g for methyl orange.
[0026] 3. Different activation and modification processes are adopted for different types of pollutants. The acid activation process achieves efficient complexation and adsorption of heavy metal ions by forming oxygen-containing functional groups on the ceramic surface. The alkali activation process achieves electrostatic adsorption of anionic dyes and total phosphorus by enhancing the negative charge of the ceramic surface. The metal ion loading process achieves efficient and selective adsorption of fluoride ions and arsenic ions by forming metal oxide active sites on the ceramic surface.
[0027] 4. The two-step granulation process is carried out using an extruder and a ball mill. The mixed mud is extruded into strip-shaped particles through an extrusion die, and then the strip-shaped particles are ground into spherical particles with high sphericity through the collision and friction of the rotating drum and arc baffle of the ball mill. The particle size distribution is uniform, the compressive strength of the particles reaches 5 to 20 MPa, and the wear rate is less than 5%.
[0028] 5. The calcination furnace with independent temperature control in multiple temperature zones effectively avoids the problems of premature sintering and densification of particles and collapse of pore structure through the staged heating calcination process, ensuring that the adsorbent material has a stable pore structure and good adsorption performance.
[0029] 6. Two regeneration methods are provided: water washing with dilute acid immersion and thermal regeneration. The adsorbent material can be reused 5 to 10 times without significant decrease in adsorption capacity, which significantly reduces the cost of use. Attached Figure Description
[0030] Figure 1 This is a schematic diagram of the structure of the ceramic solid waste-based high-efficiency adsorption material preparation system according to an embodiment of this application; Figure 2 for Figure 1 A schematic diagram of the activation reactor in the activation modification unit; Figure 3 for Figure 1 Schematic diagram of the structure of the intermediate forming granulation unit; Figure 4 for Figure 1 Structural cross-sectional view of the heat treatment shaping unit; Figure 5 This is a flowchart of the method for preparing the ceramic solid waste-based high-efficiency adsorbent material of this application.
[0031] The components include: 101, Pretreatment Unit; 102, Activation and Modification Unit; 103, Molding and Granulation Unit; 104, Heat Treatment and Shaping Unit; 105, Raw Material Inlet; 106, Finished Product Outlet; 201, Sorting Device; 202, Crushing Device; 203, Ball Milling and Screening Device; 204, Drying Device; 301, Acid Storage Tank; 302, Alkali Storage Tank; 303, Metal Salt Solution Storage Tank; 304, Activation Reactor; 401, Mixing Device; 402, Granulation Device; 501, Calcination Furnace; 502, Cooling and Screening Device; 507, Automatic Unloading Device; 403, Pre-drying Device; 601, Temperature Sensor; 602, Stirring Device; 603, Level Gauge; 604, Preheating Mechanism; 605, Temperature Control System. 606. Stirring shaft; 607. Spiral stirring blade; 608. Bearing housing; 609. Reactor cover; 610. Bottom jacket; 611. PID controller; 612. Heating resistor; 701. Extruder; 702. Ball rolling machine; 703. Extrusion die; 704. Forming hole; 705. Rotating drum; 706. Arc-shaped baffle; 707. Strip particle outlet; 708. Spherical particle outlet; 801. Preheating zone; 802. High temperature zone; 803. Insulation zone; 805. Electric heating element; 806. Thermocouple; 901. Cooling mechanism; 902. Vibrating screening mechanism; 903. Air supply duct; 904. Exhaust duct; 905. First layer screen; 906. Second layer screen; 907. Grading outlet. Detailed Implementation
[0032] The technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.
[0033] Example: Please see the appendix Figure 1 To be continued Figure 4 This application provides a system for preparing high-efficiency adsorption materials based on ceramic solid waste. The system includes a pretreatment unit 101, an activation and modification unit 102, a molding and granulation unit 103, and a heat treatment and shaping unit 104 connected in sequence. The raw material enters the pretreatment unit 101 through the raw material inlet 105. After continuous processing by the activation and modification unit 102, the molding and granulation unit 103, and the heat treatment and shaping unit 104, the finished ceramic adsorption filter material is output from the finished product outlet 106. The four units are continuously connected by material conveying mechanisms such as screw conveyors and chutes, forming a complete production line for high-value utilization of ceramic solid waste. The operation of the entire system is uniformly monitored by a central control system. The material flow rate, temperature parameters, and speed parameters between each unit are collected in real time by sensors and fed back to the control system. The control system automatically adjusts according to the preset process parameters to ensure the stability of the entire production process and the consistency of the product.
[0034] In the pretreatment unit 101, the outlet of the sorting device 201 and the inlet of the crushing device 202 are connected by an inclined chute. Under the action of gravity, the material is transferred from the sorting device 201 to the crushing device 202 for preliminary crushing. The outlet of the crushing device 202 and the inlet of the ball mill screening device 203 are connected by a vibrating feeder. The crushed material is fed evenly and stably by the frequency conversion control of the vibrating feeder. The outlet of the ball mill screening device 203 and the inlet of the drying device 204 are connected by a cyclone separator. The fine powder generated during the ball milling process is conveyed into the drying device 204 by airflow for drying. The outlet of the drying device 204 is connected to the reactor inlet of the activation and modification unit 102 by a closed screw conveyor. The dried ceramic powder is quantitatively conveyed by the screw conveyor to ensure that the material flow rate entering the activation reactor 304 is stable and controllable.
[0035] In the activation and modification unit 102, the outlet of the acid storage tank 301 is connected to the acid inlet of the activation reactor 304 through a corrosion-resistant solenoid valve and a polytetrafluoroethylene (PTFE) pipeline. The control system precisely controls the opening time and degree of the solenoid valve according to the preset activator addition amount to achieve accurate metering and delivery of the acid activator. The outlet of the alkali storage tank 302 is connected to the alkali inlet of the activation reactor 304 through the same corrosion-resistant solenoid valve and PTFE pipeline. The delivery control logic of the alkali activator is the same as that of the acid activator. The outlet of the metal salt solution storage tank 303 is connected to the metal salt inlet of the activation reactor 304 through a corrosion-resistant solenoid valve and a PTFE pipeline. The concentration and addition amount of the metal salt solution are also precisely controlled by the control system. Each storage tank is equipped with a liquid level sensor, and the liquid level signal is transmitted to the control system in real time. When the liquid level is lower than the set lower limit, the control system issues a liquid replenishment warning signal. When the liquid level is higher than the set upper limit, the control system automatically closes the inlet solenoid valve to prevent liquid overflow.
[0036] The internal structure of the activation reactor 304 is as follows Figure 2 As shown, the activation reactor 304 is equipped with a temperature sensor 601, a stirring device 602, and a level gauge 603. The reactor body is made of 316L stainless steel to withstand acid and alkali corrosion. The reactor cover 609 is connected to the reactor body by bolts and flanges for a sealed connection. A stirring shaft 606 is fixedly connected to the center hole of the reactor cover 609 via a bearing seat 608. The bearing seat 608 adopts a double-end mechanical seal structure to prevent leakage of the reaction liquid. A spiral stirring blade 607 is fixedly connected to the bottom end of the stirring shaft 606, and the spiral stirring blade 607 is submerged below the surface of the reaction liquid. The top end of the stirring shaft 606 is connected to a variable frequency motor installed above the reactor cover 609 via a coupling. The speed of the variable frequency motor is controlled by a control system according to a preset speed. The parameters are infinitely adjustable, with the preferred rotation speed range being 100 to 300 rpm to achieve uniform stirring of the liquid inside the reactor. The temperature sensor 601 is embedded in the inner wall of the activation reactor 304 and penetrates the reactor wall. The temperature sensor 601 is a PT100 type platinum resistance temperature sensor with a temperature measurement accuracy of ±0.1℃. It can accurately sense the temperature change inside the reactor and transmit the temperature signal to the temperature control system 605 in real time. The level gauge 603 is set on the side of the reactor 304 and penetrates the activation reactor wall. The level gauge 603 is a magnetic float level gauge or an ultrasonic level gauge to achieve real-time monitoring and level warning functions. The level signal is transmitted to the control system to ensure that the liquid-solid ratio is controlled within the set range.
[0037] The activation reactor 304 is also equipped with a preheating mechanism 604 and a temperature control system 605. The preheating mechanism 604 is located in the bottom jacket 610 of the activation reactor 304, forming an annular heating chamber. The preheating mechanism 604 adopts an electric heating jacket structure, with multiple stainless steel electric heating tubes evenly arranged in the bottom jacket 610 to preheat the activation liquid before it enters the reactor. The temperature control system 605 includes a PID controller 611 and a heating resistor 612. The heating resistor 612 serves as the electric heating element of the preheating mechanism 604 and is evenly arranged in the bottom jacket 610 to ensure uniform heat distribution. The input terminal of the PID controller 611 is connected to the output terminal of the temperature sensor 601 through a signal line to form a closed loop. The control loop includes a PID controller 611 with a self-tuning function to automatically adjust PID parameters according to the characteristics of the reaction system, thereby achieving rapid temperature stabilization and precise control. The heating resistor 612 is a stainless steel electric heating tube evenly arranged in the bottom jacket 610 to ensure uniform heat distribution. The control system presets the activation reaction temperature to 80℃. When the temperature sensor 601 detects that the internal temperature of the reactor is lower than the set value, the PID controller 611 automatically increases the power of the heating resistor 612 to accelerate the heating rate. When the temperature sensor 601 detects that the internal temperature of the reactor is higher than the set value, the PID controller 611 automatically decreases the power of the heating resistor 612 to prevent temperature overshoot. This cyclic adjustment stabilizes the reaction temperature near the set value.
[0038] In the molding and granulation unit 103, the inlet of the mixing device 401 is connected to the reactor outlet of the activation reactor 304 via a screw conveyor and to the binder storage tank via another screw conveyor. The activated ceramic powder discharged from the activation reactor 304 and the binder discharged from the binder storage tank are precisely proportioned and uniformly fed through the frequency conversion control of the screw conveyor. The mixing device 401 preferably adopts a double-spiral conical mixer. The stirring screw of the double-spiral conical mixer is made of stainless steel and has a wear-resistant coating on the surface to extend its service life. The filling coefficient of the mixer is controlled between 0.4 and 0.6 to ensure the mixing effect. The mixing time is set to 10 to 20 minutes to achieve uniform mixing of activated ceramic powder and binder. The outlet of the mixing device 401 is connected to the granulation inlet of the granulation device 402 via a mixed mud conveying pipe. The moisture content of the mixed mud is controlled between 25% and 35% to ensure good molding performance and mechanical strength.
[0039] The specific structure of the granulation device 402 is as follows: Figure 3As shown, the granulation device 402 includes two parts: an extruder 701 and a pelletizing machine 702. The inlet of the extruder 701 is connected to the outlet of the mixing device 401 via a screw conveyor. The extruder 701 contains an extrusion die 703 with multiple forming holes 704 of 2 to 4 mm in diameter. The extrusion die 703 adopts a modular design, allowing for the replacement of dies with different hole diameters to obtain strip-shaped granules of different diameters. The screw speed of the extruder 701 is adjusted by a frequency converter to control the extrusion speed of the strip-shaped granules; the preferred screw speed range is 30 to 60 rpm. The strip-shaped granule outlet 707 of the extruder 701 is connected to the inlet of the pelletizing machine 702 via a vibrating feeder. The vibration frequency and amplitude of the vibrating feeder are adjusted by a frequency converter to control the flow rate into the pelletizing machine 702. For the flow rate of strip-shaped particles 02, the ball rolling machine 702 is equipped with a rotating drum 705 inside. The inner wall of the rotating drum 705 is provided with multiple arc-shaped baffles 706, which are evenly distributed on the inner wall of the drum. The height of the baffles is 1 / 10 to 1 / 8 of the drum diameter. The ball rolling machine 702 adopts an inclined drum design with an inclination angle of 5 to 15°. The rotating drum 705 rotates at an adjustable speed under the drive of a variable frequency motor, preferably in the range of 20 to 40 rpm. The strip-shaped particles are subjected to the combined action of gravity and centrifugal force in the rotating drum 705. Under the collision and friction of the arc-shaped baffles 706, they gradually roll into spherical particles. The diameter of the spherical particles is controlled within the range of 2 to 8 mm. The spherical particle outlet 708 of the ball rolling machine 702 is connected to the pre-drying inlet of the pre-drying device 403 through a chute.
[0040] The pre-drying device 403 preferably adopts a mesh belt pre-dryer. The mesh belt of the mesh belt pre-dryer is made of stainless steel woven mesh to have good air permeability. The running speed of the mesh belt is adjusted by a frequency converter to adapt to different pre-drying time requirements. The pre-drying temperature is room temperature to avoid deformation and cracking of the particles due to high temperature. The pre-drying time is controlled between 12 and 24 hours to keep the moisture content of the pre-dried particles between 10% and 15%. During the pre-drying process, the pre-drying device 403 is equipped with a turning mechanism to turn the particles regularly to prevent sticking and deformation. The moisture content of the pre-dried particles is monitored in real time by an online moisture sensor and the signal is fed back to the control system to accurately control the pre-drying time.
[0041] The heat treatment and shaping unit 104 includes a calcining furnace 501 and a cooling and screening device 502. The inlet of the calcining furnace 501 is connected to the outlet of the pre-drying device 403 via an automatic feeding device. The automatic feeding device uses a hydraulic or pneumatic pusher to achieve automated feeding. The calcining furnace 501 preferably adopts a roller kiln or a tunnel kiln to achieve continuous large-scale production. The calcining furnace 501 is equipped with at least three temperature zones, corresponding to the preheating zone 801, the high-temperature zone 802, and the heat preservation zone 803, respectively. Each temperature zone is independently equipped with a temperature measuring thermocouple 806 and an electric heating element 805 to achieve independent temperature control. The calcination process adopts a segmented heating method, first heating from the room at a heating rate of 10℃ / min. The temperature is raised to 300℃ and held for 20 minutes for pre-sintering treatment to remove residual moisture and volatile organic matter inside the particles. Then, the temperature is raised from 300℃ to the set temperature at a rate of 8℃ / min for high-temperature shaping treatment to promote the stabilization of the internal structure of the particles. The calcination temperature is set to 700 to 850℃, the holding time is set to 30 to 90 minutes, and the heating rate is set to 5 to 15℃ / min. The discharge port of the calcination furnace 501 is equipped with an automatic unloading device 507. The automatic unloading device 507 uses a hydraulic pusher or a pneumatic pusher to automatically unload the ceramic adsorption filter material after calcination and send it to the cooling and screening device 502 to realize automated discharge.
[0042] The cooling and screening device 502 includes a cooling mechanism 901 and a vibrating screening mechanism 902. The cooling mechanism 901 is located downstream of the discharge end of the calcining furnace 501. The cooling mechanism 901 adopts either air cooling or water cooling. The air cooling method uses a high-pressure blower to force air in, and cold air is sent into the cooling chamber through the air supply pipe 903 to exchange heat with the high-temperature ceramsite. The waste heat gas is discharged through the exhaust pipe 904. The cooling efficiency is high and there is no water consumption, making it suitable for production in water-scarce areas. The water cooling method uses a shell-and-tube heat exchanger. The refrigerant exchanges heat with the high-temperature ceramsite through the tube side of the heat exchanger. The cooling speed is fast and it is suitable for large-scale industrial production. After the ceramsite temperature drops to room temperature, it enters the vibrating screening mechanism 902 for screening.
[0043] The inlet of the vibrating screening mechanism 902 is connected to the outlet of the cooling mechanism 901 via a chute. The vibrating screening mechanism 902 has at least two layers of screens. The first layer, screen 905, has an 8mm mesh size to remove particles larger than 8mm. These particles are collected through the grading outlet 907 and can be returned to the crushing device 202 for reprocessing. The second layer, screen 906, has a 2mm mesh size to remove particles smaller than 2mm. These particles are considered defective and are collected in a hopper for recycling. The two layers of screens... The particles between the particles are finished adsorbent materials with a particle size range of 2 to 8 mm. They are output as finished ceramic adsorbent filter media from the middle grading outlet 907 of the vibrating screening mechanism 902. The vibrating screening mechanism 902 adopts a multi-layer stacked screen design to increase the number of screen layers as needed to obtain products with various particle size grades such as 2 to 4 mm, 4 to 6 mm, and 6 to 8 mm to meet different application requirements. The vibrating motor adopts an adjustable frequency vibrating motor. The amplitude and vibration frequency are adjusted according to the material characteristics through a frequency converter to ensure screening accuracy and screening efficiency.
[0044] In actual industrial production applications, the proportions of the solid materials in the molding and granulation stage, by mass percentage, are as follows: ceramic waste powder 75% to 90%, pore-forming agent 5% to 12%, binder 3% to 8%, and activation agent 2% to 5%. Among them, the pore-forming agent is selected from calcium carbonate or sodium bicarbonate, which decomposes and releases carbon dioxide gas during high-temperature calcination to form a rich pore structure inside the ceramsite, thereby significantly increasing the specific surface area of the adsorbent material. The binder is selected from bentonite or kaolin to provide good bonding performance, ensuring that the particles sinter and solidify during calcination to form stable mechanical strength. The activation agent is selected from sodium hydroxide or potassium hydroxide, which provides a strongly alkaline environment during the activation process to further etch the ceramic surface and generate more active adsorption sites.
[0045] Reference Figure 5 The preparation method provided in this application includes the following specific steps.
[0046] Step S1 is pretreatment. Ceramic solid waste is fed into the sorting device 201 through the raw material inlet 105. As the ceramic solid waste passes through the belt magnetic separator, the permanent magnet roller below the belt magnetically attracts and separates metallic impurities. Simultaneously, a manual sorting station is set up next to the belt conveyor line, where operators remove non-ceramic foreign objects such as plastic, wood blocks, and glass. The sorted ceramic solid waste enters the crushing device 202 through an inclined chute for coarse crushing. The crushing device 202 is a jaw crusher. Under the squeezing action of the jaw plates, the ceramic solid waste is crushed into particles with a diameter of 10 to 50 mm. The discharge port of the jaw crusher is equipped with an adjustment device to control the particle size range after crushing. The coarsely crushed material is then fed by a vibrating feeder. The powder is fed evenly into the ball mill screening device 203, which uses a planetary ball mill in conjunction with a standard sieve. The grinding jar and grinding balls of the planetary ball mill are made of zirconium oxide to avoid the introduction of metal impurities. The ball milling time is set to 1 to 3 hours to refine the ceramic solid waste particles to 60 to 200 mesh. The powder after ball milling is screened by a vibrating screen in conjunction with a standard sieve. The powder with qualified particle size enters the drying device 204 for drying. The drying device 204 uses a hot air circulating drying box with the inlet air temperature set at 105℃ and the drying time set to 2 to 4 hours. During the drying process, the powder is continuously turned over by a turning mechanism to ensure uniform drying. After drying, the moisture content of the ceramic powder is controlled below 1%.
[0047] Step S2 is activation modification. Dry ceramic powder is quantitatively conveyed to activation reactor 304 via a screw conveyor. Depending on the target product type, different activation modification processes such as acid activation, alkali activation, or metal ion loading are selected. For acid activation, one or more combinations of dilute hydrochloric acid, dilute sulfuric acid, or nitric acid are used as the acid solution, with the acid concentration controlled between 0.5 and 2 mol / L. The ceramic powder to acid solution is precisely metered via a solenoid valve at a mass ratio of 1:3 to 1:5 and then pumped into activation reactor 304. A variable frequency motor is started to drive the stirring shaft 606 to rotate, causing the spiral stirring blades 607 to uniformly stir the liquid inside the reactor. The stirring speed is controlled at 100 to 300 rpm to ensure that the acid solution and ceramic powder are in full contact and react. At the same time, the temperature control system 605 raises the reaction temperature to 80°C and keeps it stable through the preheating mechanism 604. The PID controller 611 automatically adjusts the power of the heating resistor 612 according to the temperature signal fed back by the temperature sensor 601 to maintain a constant reaction temperature. The acid activation reaction time is controlled at 2 to 4 hours to allow the acid solution to fully etch the surface of the ceramic powder and remove impurities and oxides. After filtration, the powder is repeatedly washed with deionized water until neutral, and then dried again by the drying device 204 at 105°C to obtain acid-activated ceramic powder.
[0048] The alkali activation process uses sodium hydroxide or potassium hydroxide aqueous solution as the alkali solution, with the concentration controlled at 1 to 5 mol / L. The ceramic powder to alkali is precisely metered by a solenoid valve and pumped into the activation reactor 304 at a mass ratio of 1:0.5 to 1:1.2. The activation and modification treatment is carried out by stirring in a water bath at 80°C for 2 to 4 hours. After alkali activation, it is further activated by calcination in a muffle furnace at 500 to 700°C to etch rich micropores and mesopores on the ceramic surface. The calcination time is 1 to 2 hours and the heating rate is 5 to 10°C / min. During the calcination process, the ceramic matrix undergoes a phase transformation to form a more stable pore structure. After filtration, washing with water and drying, alkali-activated ceramic powder is obtained.
[0049] The metal ion loading process is carried out after acid activation or alkali activation treatment. The activated ceramic powder is immersed in a metal salt solution and allowed to stand for impregnation. The metal salt solution can be an aqueous solution of ferric chloride, manganese chloride, lanthanum chloride, or aluminum chloride. The metal ion concentration is controlled at 0.1 to 1.0 mol / L, and the immersion time is controlled at 12 to 24 hours to allow the metal ions to fully penetrate into the ceramic matrix. After immersion, excess solution is removed by vacuum filtration. The powder is then dried in a drying oven at 105 to 120°C for 2 to 4 hours, and then calcined in a muffle furnace at 300 to 500°C for 1 to 2 hours. During the calcination process, metal ions generate metal oxide active sites in situ on the ceramic surface, giving the adsorbent material a high selective adsorption capacity for specific pollutants, thereby obtaining a metal ion loaded adsorbent material.
[0050] Step S3 involves molding and granulation. Activated ceramic powder, pore-forming agent, and binder are mixed in a specific ratio and added to the mixing device 401. Simultaneously, deionized water is added at a solid-liquid ratio of 1:0.3 to 1:0.6. After the double-spiral conical mixer is started, the two stirring spirals rotate in opposite directions to thoroughly mix the activated ceramic powder, binder, and deionized water to obtain a mixed slurry. The mixing time is set to 10 to 20 minutes, and the moisture content of the mixed slurry is controlled between 25% and 35% to ensure good molding performance and mechanical strength. After mixing, the mixed slurry is conveyed to the inlet of the extruder 701 via a screw conveyor. The screw of the extruder 701 rotates under the drive of a variable frequency motor, extruding the mixed slurry through the forming holes 704 of the extrusion die 703. The extrusion die 703 has multiple diameters... The forming holes 704, with a diameter of 2 to 4 mm, can extrude the mixed mud into strip-shaped particles of the corresponding diameter. The strip-shaped particles are conveyed from the strip-shaped particle outlet 707 of the extruder 701 to the inlet of the ball rolling machine 702 via a vibrating feeder. The rotating drum 705 of the ball rolling machine 702 rotates at an adjustable speed under the drive of a variable frequency motor. The arc-shaped baffles 706 on the inner wall of the rotating drum 705 generate collision and friction on the strip-shaped particles during the rotation of the drum, causing them to gradually roll into spherical particles. The diameter of the spherical particles is controlled within the range of 2 to 8 mm. After forming, the spherical particles are pre-dried at room temperature for 12 to 24 hours by the pre-drying device 403. During the pre-drying process, the turning mechanism of the pre-drying device 403 turns the particles regularly to prevent sticking and deformation. After pre-drying, the moisture content of the particles is controlled within 10% to 15%.
[0051] Step S4 is heat treatment and shaping. The pre-dried particulate adsorbent material is conveyed to the calcination furnace 501 via an automatic feeding device. In the preheating zone 801 of the calcination furnace 501, the particles are first heated from room temperature to 300°C at a heating rate of 10°C / min and held at this temperature for 20 minutes for pre-sintering. During this stage, residual moisture inside the particles evaporates and escapes, and volatile organic compounds decompose and are discharged, preparing for subsequent high-temperature shaping. The pre-sintering temperature should not be too high and the time should not be too long, otherwise the particles will sinter and densify prematurely, affecting the final adsorption performance. After pre-sintering, the particles enter the high-temperature zone 802 and continue to be heated to the set temperature at a heating rate of 8°C / min for high-temperature shaping. The high-temperature setting process involves controlling the temperature between 700 and 850°C. At this temperature, the pore-forming agent inside the particles decomposes and releases carbon dioxide gas to form a rich pore structure. The binder sintersects and solidifies under high temperature to form a stable particle skeleton. After high-temperature setting, the particles are placed in the heat preservation zone 803 for heat preservation treatment. The heat preservation time is set to 30 to 90 minutes to fully stabilize the internal structure of the particles. The high-temperature setting temperature should not exceed 900°C, otherwise it will cause the pore structure to collapse and the specific surface area to decrease. After calcination, the automatic unloading device 507 is activated to automatically unload the ceramic adsorption filter material and send it to the cooling and screening device 502 for cooling treatment.
[0052] The cooling process employs a stepped cooling method to prevent cracks in the particles due to excessive thermal stress. The high-temperature ceramsite first enters the cooling mechanism 901 and is rapidly cooled to 400°C using forced air cooling. A high-pressure blower sends cold air into the cooling chamber through the air supply pipe 903 to exchange heat efficiently with the high-temperature ceramsite. Waste heat gas is discharged through the exhaust pipe 904. After cooling to 400°C, the process switches to natural cooling and slowly cools to room temperature. During natural cooling, thermal stress is gradually released to prevent cracks from forming. The cooled ceramsite then enters the vibrating screening mechanism 902 for screening. Particles larger than 8mm are removed through an 8mm screen, and particles smaller than 2mm are removed through a 2mm screen. The particles between the two screens are the finished adsorption material with a particle size range of 2 to 8mm, which is output from the grading outlet 907 as the finished ceramsite adsorption filter material.
[0053] The performance indicators of the ceramic solid waste-based high-efficiency adsorbent material prepared in this application are as follows: specific surface area of 80 to 350 m² / g, pore volume of 0.2 to 0.6 cm³ / g, average pore size of 2 to 10 nanometers, adsorption capacity for copper ions of 20 to 80 mg / g, adsorption capacity for lead ions of 30 to 100 mg / g, adsorption capacity for methyl orange of 15 to 50 mg / g, particle compressive strength of 5 to 20 MPa, and wear rate of less than 5%. The above performance indicators were measured and verified by specific surface area and pore size analyzer, scanning electron microscope, atomic absorption spectrometer and other testing equipment.
[0054] The three activation and modification processes provided in this application are applicable to different pollutant treatment scenarios. The acid activation process is suitable for treating wastewater containing heavy metal ions such as copper, lead, cadmium, and zinc ions. After acid activation, the ceramic surface forms abundant oxygen-containing functional groups such as hydroxyl and carboxyl groups, which achieve efficient adsorption of heavy metal ions through complexation. The alkali activation process is suitable for treating wastewater containing anionic dyes such as methyl orange, methylene blue, and Congo red, as well as total phosphorus. After alkali activation, the negative charge on the ceramic surface is enhanced, achieving efficient adsorption of cationic pollutants through electrostatic attraction. At the same time, the microporous to mesoporous structure formed by alkali activation has excellent adsorption performance for phosphorus. The metal ion loading process is suitable for treating wastewater containing anionic pollutants such as fluoride and arsenic ions. By loading metal ions such as iron, manganese, lanthanum, and aluminum, active sites of metal oxides are formed, achieving efficient and selective adsorption of fluoride and arsenic through ion exchange and surface complexation.
[0055] This application also provides a method for regenerating high-efficiency adsorbent materials based on ceramic solid waste to extend service life and reduce usage costs. The water washing and dilute acid soaking regeneration method involves rinsing the used adsorbent material with deionized water 3 to 5 times to remove suspended matter attached to the surface, then soaking it in 0.1 to 0.5 mol / L dilute hydrochloric acid or dilute sulfuric acid for 2 to 4 hours to desorb the adsorbed pollutants into the solution. After filtration, it is washed with deionized water until neutral and dried at 105°C for reuse. The thermal regeneration method involves placing the used adsorbent material in a calcining furnace 501 and holding it at 300 to 500°C for 1 to 2 hours to thermally decompose and volatilize the adsorbed pollutants. After cooling to room temperature, it can be reused. Using the above regeneration methods, the adsorbent material can be reused 5 to 10 times without significant decrease in adsorption capacity.
[0056] In practical applications, ceramic solid waste-based high-efficiency adsorbent materials can be used in various water treatment scenarios. In electroplating wastewater treatment, adsorbent materials prepared by acid activation process have high adsorption capacity for heavy metal ions such as copper, nickel, and zinc ions, and the concentration of heavy metals in the effluent can be reduced to below the national emission standards. In dyeing and printing wastewater treatment, adsorbent materials prepared by alkali activation process have high adsorption capacity for dye molecules such as methyl orange and methylene blue, and have a significant effect on color removal. In phosphorus-containing wastewater treatment, the microporous to mesoporous structure formed by alkali activation has selective adsorption of phosphate ions and can be used for the treatment of eutrophication of lakes. In fluoride-containing wastewater treatment, adsorbent materials prepared by metal ion loading process achieve high-efficiency removal of fluoride ions through active sites of metal oxides such as lanthanum and iron, and can be used for the treatment of fluoride-containing wastewater in the semiconductor industry. In the deep treatment of drinking water, adsorbent materials can be used to remove trace heavy metals and organic pollutants to ensure drinking water safety.
[0057] Although embodiments of this application have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of this application, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A system for preparing waste ceramic-based porous adsorbent materials for water treatment, characterized in that, It includes a pretreatment unit (101), an activation and modification unit (102), a molding and granulation unit (103), and a heat treatment and shaping unit (104) that are connected in sequence. The pretreatment unit (101) includes a sorting device (201), a crushing device (202), a ball mill screening device (203), and a drying device (204) connected in sequence; The activation and modification unit (102) includes an activation reactor (304), the outlet of the drying device (204) is connected to the inlet of the activation reactor (304), and the activation reactor (304) is also connected to an acid storage tank (301), an alkali storage tank (302) and a metal salt solution storage tank (303). The molding and granulation unit (103) includes a mixing device (401), a granulation device (402), and a pre-drying device (403). The outlet of the activation reactor (304) is connected to the inlet of the mixing device (401), the outlet of the mixing device (401) is connected to the inlet of the granulation device (402), and the outlet of the granulation device (402) is connected to the inlet of the pre-drying device (403). The heat treatment shaping unit (104) includes a calcining furnace (501) and a cooling screening device (502). The outlet of the pre-drying device (403) is connected to the inlet of the calcining furnace (501), and the outlet of the calcining furnace (501) is connected to the cooling screening device (502). The entire preparation system is monitored by a central control system.
2. The preparation system for waste ceramic-based porous adsorbent material for water treatment according to claim 1, characterized in that, The outlet of the sorting device (201) is connected to the inlet of the crushing device (202) via an inclined chute; the crushing device (202) is a jaw crusher, and the outlet of the crushing device (202) is connected to the inlet of the ball mill screening device (203) via a vibrating feeder; the outlet of the ball mill screening device (203) is connected to the inlet of the drying device (204) via a cyclone separator; the outlet of the drying device (204) is connected to the inlet of the activation reactor (304) via a closed screw conveyor.
3. The preparation system for waste ceramic-based porous adsorbent material for water treatment according to claim 1, characterized in that, The outlets of the acid storage tank (301), the alkali storage tank (302), and the metal salt solution storage tank (303) are all connected to the corresponding inlet of the activation reactor (304) via corrosion-resistant solenoid valves and polytetrafluoroethylene pipelines, respectively; each of the storage tanks is equipped with a liquid level sensor that is communicatively connected to the central control system.
4. The preparation system for waste ceramic-based porous adsorbent material for water treatment according to claim 1, characterized in that, The activation reactor (304) includes a reactor body and a reactor cover (609) sealed to the reactor body; the stirring shaft (606) of the stirring device (602) is connected to the central hole of the reactor cover (609) through a bearing seat (608) with a double-end mechanical seal structure; a spiral stirring blade (607) is fixedly connected to the bottom end of the stirring shaft (606), and the top end of the stirring shaft (606) is connected to a variable frequency motor through a coupling; the activation reactor (304) is also equipped with a temperature sensor (601) embedded in the inner wall and a liquid level gauge (603) penetrating the wall.
5. The preparation system for waste ceramic-based porous adsorbent material for water treatment according to claim 4, characterized in that, The activation reactor (304) is also provided with a preheating mechanism (604) and a temperature control system (605); the bottom jacket (610) of the activation reactor (304) forms an annular heating chamber, and the preheating mechanism (604) is disposed in the bottom jacket (610); the temperature control system (605) includes a PID controller (611) and a heating resistor (612), the heating resistor (612) is uniformly arranged in the bottom jacket (610) as an electric heating element of the preheating mechanism (604), and the input end of the PID controller (611) is connected to the output end of the temperature sensor (601) to form a closed-loop control circuit.
6. The preparation system for waste ceramic-based porous adsorbent material for water treatment according to claim 1, characterized in that, The mixing device (401) is a double-helix conical mixer. The stirring helix of the double-helix conical mixer is made of stainless steel with a wear-resistant coating on the surface. The inlet of the mixing device (401) is connected to the outlet of the activation reactor (304) and the binder storage tank through a screw conveyor.
7. The preparation system for waste ceramic-based porous adsorbent material for water treatment according to claim 1, characterized in that, The granulation device (402) includes an extruder (701) and a ball mill (702); the inlet of the extruder (701) is connected to the outlet of the mixing device (401), and the extruder (701) is provided with an extrusion die (703) with multiple forming holes (704) inside; the strip-shaped particle outlet (707) of the extruder (701) is connected to the inlet of the ball mill (702) through a vibrating feeder; the ball mill (702) is provided with an inclined rotating drum (705) inside, and multiple arc-shaped baffles (706) are evenly arranged on the inner wall of the rotating drum (705); the spherical particle outlet (708) of the ball mill (702) is connected to the pre-drying inlet of the pre-drying device (403) through a chute; the pre-drying device (403) is a mesh belt pre-dryer, and the mesh belt pre-dryer is provided with a turning mechanism inside.
8. The preparation system for waste ceramic-based porous adsorbent material for water treatment according to claim 1, characterized in that, The inlet of the roasting furnace (501) is connected to the outlet of the pre-drying device (403) via an automatic feeding device using hydraulic or pneumatic push rods; the roasting furnace (501) is provided with at least three temperature zones, corresponding to the preheating zone (801), the high temperature zone (802), and the heat preservation zone (803), respectively, and each temperature zone is independently equipped with a temperature measuring thermocouple (806) and an electric heating element (805); the outlet of the roasting furnace (501) is provided with an automatic unloading device (507) using hydraulic or pneumatic push rods.
9. The preparation system for waste ceramic-based porous adsorbent material for water treatment according to claim 1, characterized in that, The cooling and screening device (502) includes a cooling mechanism (901) and a vibrating screening mechanism (902) located downstream of the discharge end of the roasting furnace (501); the cooling mechanism (901) is connected to an air supply pipe (903) and an air duct (904); the inlet of the vibrating screening mechanism (902) and the outlet of the cooling mechanism (901) are connected by a chute; the vibrating screening mechanism (902) is provided with at least two layers of screens, including a first layer of screen (905) for removing large-diameter particles and a second layer of screen (906) for removing small-diameter particles, and a grading outlet (907) is provided between the two layers of screens to output the finished ceramic adsorption filter material.
10. A method for preparing a waste ceramic-based porous adsorbent material for water treatment, based on the preparation system for a waste ceramic-based porous adsorbent material for water treatment according to any one of claims 1 to 9, characterized in that, Specifically, the following steps are included: Step S1 is pretreatment. The ceramic solid waste is fed into the sorting device (201) from the raw material inlet (105) to remove impurities. After being coarsely crushed by the crushing device (202), it is fed into the ball mill screening device (203) for fine processing. The qualified powder is then fed into the drying device (204) for drying to obtain dry ceramic powder. Step S2 is activation modification. The dried ceramic powder is transported to the activation reactor (304). Depending on the target product type, an acid activation process, an alkali activation process, or a metal ion loading process is selected for activation modification to obtain activated ceramic powder. Specifically, the acid activation process involves adding acid solution and stirring, filtering, washing with water until neutral, and drying in a drying oven. The alkali activation process involves adding alkali solution and stirring in a water bath, followed by calcination activation in a muffle furnace, then filtering, washing, and drying. The metal ion loading process involves immersing the powder in a metal salt solution after acid or alkali activation, then removing excess solution through vacuum filtration, drying, and calcining at low temperature in a muffle furnace. Step S3 is molding and granulation. The activated ceramic powder, pore-forming agent and binder are added to the mixing device (401), and deionized water is added to mix evenly to obtain a mixed mud. The mixed mud is extruded into strip-shaped particles by the extruder (701) of the granulation device (402), and then gradually rolled into spherical particles by the ball rolling machine (702) under the combined action of gravity and centrifugal force. Then it is pre-dried by the pre-drying device (403). Step S4 is heat treatment shaping. The pre-dried particles are conveyed to the calcination furnace (501) and successively pass through the preheating zone (801), the high temperature zone (802) and the heat preservation zone (803) for segmented heating and calcination. After calcination, they enter the cooling and screening device (502), are cooled in stages by the cooling mechanism (901), and are screened in multiple layers by the vibrating screening mechanism (902) and output as finished ceramic adsorption filter material through the grading outlet (907) and the finished product outlet (106).