Modified zeolite dehumidifying material, preparation method and application thereof
By loading a nickel-iron bimetallic catalyst into the zeolite channels, the desorption energy barrier of water molecules is reduced through catalysis, solving the problem of high regeneration temperature and high energy consumption of zeolite dehumidification rotors. This achieves low-temperature, high-efficiency regeneration and high moisture absorption capacity, making it suitable for fields such as electronics manufacturing and pharmaceuticals.
Patent Information
- Application Number
- CN202611454948.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-18
- Publication Date
- 2026-11-20
AI Technical Summary
Existing zeolite dehumidification rotors have high regeneration temperatures and high energy consumption. Traditional modification methods have limited effectiveness, and process optimization is complex, making it impossible to effectively reduce the activation energy of water molecule desorption.
In situ loading of nickel-iron bimetallic catalysts within zeolite channels reduces the interaction energy between water molecules and the pore walls through catalysis. Combining calcination and vacuum impregnation processes achieves high dispersion and stable loading of the nickel-iron bimetallic catalysts, forming metal-oxygen-silicon covalent bonds and reducing the desorption activation energy.
While maintaining high moisture absorption capacity, it significantly reduces the regeneration temperature to 70-95℃, reduces energy consumption by 45%-50%, increases moisture absorption capacity by 3.1%-7.7%, and has excellent cycle stability, making it suitable for low-energy deep dehumidification scenarios.
Smart Images

Figure CN123127950A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of air dehumidification technology, specifically to a modified zeolite dehumidification material, its preparation method, and its application. Background Technology
[0002] Rotary dehumidifier technology is one of the core methods for achieving deep dehumidification and is widely used in industrial fields with stringent humidity requirements, such as electronics manufacturing, pharmaceuticals, chemicals, and food processing. While mainstream zeolite dehumidifier rotors offer advantages such as large moisture absorption capacity and good stability, they suffer from drawbacks including high regeneration temperatures (120-180℃) and high energy consumption. Regeneration energy consumption can account for 60% or more of the total system energy consumption, severely hindering the widespread application of this technology in a low-carbon context. Traditional methods for reducing regeneration temperature mainly fall into two categories: material modification and process optimization. Regarding material modification, researchers have attempted to improve the moisture absorption performance of materials by doping with alkali metal ions and introducing hydrophilic groups, but the improvement effect on the desorption process is limited. As for process optimization, while multi-stage regeneration and waste heat recovery can reduce some energy consumption, they significantly increase system complexity and cannot effectively solve the problem of high activation energy for water molecule desorption. Summary of the Invention
[0003] The purpose of this invention is to overcome one or more shortcomings in the prior art and provide an improved method for preparing modified zeolite desiccant materials and the modified zeolite desiccant materials made therefrom, which significantly reduces the regeneration temperature while maintaining excellent moisture absorption capacity.
[0004] The present invention also provides an application of the above-mentioned modified zeolite dehumidifying material in the preparation of a dehumidifying impeller.
[0005] To achieve the above objectives, the present invention employs the following technical solution: A method for preparing a modified zeolite dehumidifying material, the method comprising: A nickel-iron bimetallic catalyst is dispersed in an organic solvent to prepare an impregnation solution; the nickel-iron bimetallic catalyst is generated by a solvothermal reaction of nickel salt and iron salt in the presence of a surfactant. The zeolite substrate is pretreated, including calcination and vacuum degassing under heating conditions, to obtain a pretreated zeolite substrate; the pretreated zeolite substrate is impregnated in the impregnation solution to obtain an intermediate, wherein the impregnation includes at least vacuum impregnation; the intermediate is calcined at a temperature greater than or equal to 300°C.
[0006] In some embodiments of the present invention, the impregnation solution comprises the nickel-iron bimetallic catalyst, the dispersant and the organic solvent; by weight percentage, the nickel-iron bimetallic catalyst accounts for 0.2wt%-0.6wt% and the dispersant accounts for 0.05wt%-0.2wt% in the impregnation solution.
[0007] Furthermore, the dispersant comprises polyvinylpyrrolidone.
[0008] Furthermore, the organic solvent is an anhydrous alcohol solvent, and even further, the anhydrous alcohol solvent includes anhydrous ethanol and / or anhydrous methanol.
[0009] According to some specific aspects of the present invention, the nickel-iron bimetallic catalyst in the impregnation solution comprises 0.2 wt%, 0.25 wt%, 0.30 wt%, 0.35 wt%, 0.40 wt%, 0.45 wt%, 0.50 wt%, 0.55 wt%, 0.60 wt%, etc., by weight percentage.
[0010] According to some specific aspects of the present invention, the dispersant in the impregnation solution comprises 0.05 wt%, 0.08 wt%, 0.10 wt%, 0.12 wt%, 0.15 wt%, 0.18 wt%, 0.20 wt%, etc., by weight percentage.
[0011] In some embodiments of the present invention, the nickel-iron bimetallic catalyst is nanoscale.
[0012] In some embodiments of the present invention, the nickel-iron bimetallic catalyst has a sheet-like structure; further, the sheet diameter of the nickel-iron bimetallic catalyst is less than 5 μm and the thickness is less than 200 nm. According to some specific aspects of the present invention, the sheet diameter of the nickel-iron bimetallic catalyst is 1-3 μm and the thickness is 20-50 nm.
[0013] In some embodiments of the present invention, the preparation method of the nickel-iron bimetallic catalyst includes: dispersing nickel salt and iron salt in an alcohol solvent, adding a surfactant, and conducting a solvothermal reaction at 140-180°C to generate a nickel-iron bimetallic catalyst with a plate-like structure.
[0014] Furthermore, the alcohol solvent includes ethylene glycol.
[0015] According to some specific aspects of the invention, the solvothermal reaction is controlled to be carried out at temperatures of 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, or 180°C.
[0016] In some embodiments of the present invention, the nickel salt is one or a combination selected from nickel nitrate, nickel sulfate, and nickel chloride.
[0017] In some embodiments of the present invention, the iron salt is one or more combinations selected from ferric nitrate, ferric sulfate, and ferric chloride.
[0018] In some embodiments of the present invention, the molar ratio of nickel in the nickel salt to iron in the iron salt is 1:0.5-3, preferably 1:1.5-2.5. According to some specific aspects, the molar ratio of nickel in the nickel salt to iron in the iron salt is 1:0.5, 1:0.8, 1:1.0, 1:1.2, 1:1.5, 1:1.8, 1:2.0, 1:2.2, 1:2.5, 1:2.8, 1:3.0, etc.
[0019] In some embodiments of the present invention, the surfactant is sodium citrate.
[0020] In some embodiments of the present invention, the added mass of the surfactant is 0.5-1.0 times the total added mass of the nickel salt and the iron salt, for example, 0.5 times, 0.6 times, 0.7 times, 0.8 times, 0.9 times, 1.0 times, etc.
[0021] In some embodiments of the present invention, the reaction time of the solvothermal reaction is controlled to be 6-24 h, and more specifically 8-14 h.
[0022] In some embodiments of the present invention, the calcination process is controlled to be carried out at a temperature of 400-500°C, for example at temperatures of 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C or 500°C.
[0023] In some embodiments of the present invention, the roasting time of the roasting treatment is controlled to be 1-8 hours, and more specifically 2-4 hours.
[0024] In some embodiments of the present invention, the heating conditions are controlled to make the heating temperature 250-350°C, for example, 250°C, 280°C, 300°C, 320°C, 330°C, 340°C, 350°C, etc.
[0025] In some embodiments of the present invention, the gauge pressure for controlling the vacuum degree of the vacuum degassing is -0.5 to -0.01 MPa, and more specifically -0.2 to -0.05 MPa.
[0026] In some embodiments of the present invention, the method for preparing the pretreated zeolite substrate includes: calcining the zeolite substrate in air, ultrasonically cleaning it after cooling, and then degassing it under vacuum under heating conditions.
[0027] In some embodiments of the present invention, during the vacuum impregnation process, the gauge pressure of the vacuum is controlled to be -0.5 to -0.01 MPa, and the holding time is 10-60 min.
[0028] In some embodiments of the present invention, the impregnation process includes: first performing vacuum impregnation, and then standing and soaking under normal pressure; further, the standing and soaking time is 0.5-4 hours.
[0029] In some embodiments of the present invention, the volume of the impregnation liquid is more than twice the volume of the pretreated zeolite substrate, and further between 2 and 5 times, for example, it can be 2 times, 2.2 times, 2.5 times, 2.8 times, 3.0 times, 3.2 times, 3.5 times, 3.8 times, 4.0 times, 4.2 times, 4.5 times, 4.8 times, 5.0 times, etc.
[0030] In some embodiments of the present invention, the temperature of the calcination treatment is controlled to be 300-600°C, further to 400-550°C, and even further to 450-500°C.
[0031] In some embodiments of the present invention, the heating rate of the calcination treatment is controlled to be 1-10°C / min, and more specifically 1-5°C / min.
[0032] In some embodiments of the present invention, the calcination process is controlled to be carried out in an oxygen-containing atmosphere, further in an air atmosphere, and even further, the air flow rate is 0.5-2 L / min.
[0033] In some embodiments of the present invention, before the calcination treatment, drying is performed first at a temperature of 60-80°C for a time of 5-24 hours.
[0034] Another technical solution provided by the present invention is: a modified zeolite dehumidifying material prepared by the above-described method.
[0035] Another technical solution provided by the present invention is: the application of the above-mentioned modified zeolite dehumidifying material in the preparation of a dehumidifying impeller.
[0036] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art: During the experiment, the inventors of this invention unexpectedly discovered that loading a nickel-iron bimetallic catalyst onto a zeolite substrate and achieving high dispersion and stable loading through a specific process can reduce the desorption energy barrier of water molecules at the molecular level, achieving low-temperature regeneration while maintaining high moisture absorption capacity. At the same time, the modified zeolite dehumidifying material of this invention can still maintain a performance retention rate of over 85% after multiple adsorption-desorption cycles. Attached Figure Description
[0037] Figure 1 This is a schematic flowchart of the preparation method of the modified zeolite dehumidifying material of the present invention; Figure 2 This is a SEM image of the nickel-iron bimetallic catalyst prepared in Example 1 of the present invention; Figure 3 This is a schematic diagram illustrating the dehumidification performance test of the materials involved in the embodiments and comparative examples of the present invention. Detailed Implementation
[0038] The present invention aims to improve the shortcomings of conventional zeolite dehumidification materials, such as high regeneration temperature and high energy consumption.
[0039] The main inventive concept of this invention is to achieve low-temperature and high-efficiency regeneration by loading a nickel-iron bimetallic catalyst in situ within the zeolite channels and using catalysis to reduce the interaction energy between water molecules and the zeolite pore walls.
[0040] Meanwhile, this invention further achieves highly dispersed and stable loading of nickel-iron bimetallic catalysts on zeolite substrates. Typically, small-sized, especially nano-sized, catalysts are prone to agglomeration, and simple impregnation loading makes it difficult to fully realize catalytic performance and achieve long-term stable operation. Extensive experimental research by the inventors revealed that by pre-treating the zeolite substrate, including calcination and vacuum degassing under heating conditions, followed by vacuum impregnation and then high-temperature calcination, not only can nickel-iron bimetallic catalysts be loaded in situ within the zeolite channels, but the loading can also be stabilized. Analysis suggests that the pre-treatment process removes impurities from the zeolite substrate, releases pores, and activates the substrate, thus facilitating efficient loading of the nickel-iron bimetallic catalyst during vacuum impregnation. Furthermore, the surface of nickel-iron bimetallic catalysts typically readily forms metal-hydroxyl structures, and the zeolite substrate, due to its material properties, also contains silanol groups. This invention, through high-temperature calcination, effectively promotes the covalent bonding of hydroxyl groups on the catalyst with the silanol groups on the zeolite surface, forming metal-oxygen-silicon covalent bonds, achieving chemical anchoring and stable loading of the catalyst.
[0041] Furthermore, the catalyst of the present invention preferably has a sheet-like structure, which is more conducive to electron transport and enhances the catalytic performance of the catalyst. After being combined with the zeolite substrate, on the one hand, the presence of the sheet structure makes it less prone to pore blockage and facilitates the formation of new and stable channels with the zeolite substrate, ensuring the number of active sites while providing effective catalytic activity. On the other hand, after the sheet structure is combined with the zeolite substrate, it is easier to maintain a stable nanoscale dispersion state during the regeneration process. The special spatial morphology of the pore structure of the zeolite substrate makes it less prone to transfer and agglomeration, thereby maintaining stable and sufficient exposure of Ni / Fe bimetallic active sites.
[0042] Furthermore, based on the inventors' further analysis and mechanism research, it is believed that the main mechanism of action of the nickel-iron bimetallic catalyst of the present invention includes: Ni acting as an electron donor to cations (such as Na) on the zeolite pore walls. + Ca 2+ The catalyst provides electrons, moderately weakening the electrostatic attraction of cations to oxygen atoms in water molecules. Fe acts as an active center, with its 3d orbital electrons overlapping with the antibonding orbitals of the OH bonds in water molecules, reducing the polarity of the OH bonds and moderately weakening the excessively strong hydrogen bonding between water molecules and the pore walls. Through the synergistic effect of these two mechanisms, without disrupting the zeolite pore structure and the number of adsorption sites, the desorption activation energy of water molecules within the zeolite pores is reduced, allowing the regeneration temperature to drop from 120-180℃ to 70-95℃, resulting in a 45%-50% reduction in energy consumption. Simultaneously, since the catalyst only alters the desorption kinetics and does not affect the number of adsorption sites, and the Ni / Fe active center provides additional adsorption affinity, the moisture absorption capacity of the modified material remains unchanged and even increases (see Table 2 data, moisture absorption capacity increased by 3.1%~7.7%).
[0043] According to some specific aspects of the present invention, the material obtained by the present invention also has a high specific surface area (e.g., up to 438~455 m²). 2 With its unobstructed microporous mass transfer channels, this technology maintains high moisture absorption capacity while significantly reducing the regeneration temperature from the traditional 120-180°C to 70-95°C, while still achieving a desorption rate exceeding 90%. Furthermore, due to the structural stability provided by covalent bond anchoring, the material retains over 88% of its performance after 20 adsorption-desorption cycles. This technology is suitable for rotary dehumidification systems, providing a highly stable and long-cycle-life material solution for low-energy-consumption deep dehumidification scenarios in electronics manufacturing, pharmaceuticals, and chemicals, effectively promoting energy conservation and carbon reduction in the industrial dehumidification field.
[0044] See Figure 1 As shown, the preparation method of the modified zeolite dehumidifying material of the present invention includes: A nickel-iron bimetallic catalyst is dispersed in an organic solvent to prepare an impregnation solution; the nickel-iron bimetallic catalyst is generated by a solvothermal reaction of nickel salt and iron salt in the presence of a surfactant. The zeolite substrate is pretreated, including calcination and vacuum degassing under heating conditions, to obtain a pretreated zeolite substrate. The pretreated zeolite substrate is impregnated in the impregnation solution to obtain an intermediate, wherein the impregnation process includes at least vacuum impregnation. The intermediate is subjected to calcination treatment at a temperature greater than or equal to 300°C.
[0045] The above-mentioned solution will be further described below with reference to specific embodiments; it should be understood that these embodiments are used to illustrate the basic principles, main features and advantages of the present invention, and the present invention is not limited to the scope of the following embodiments; the implementation conditions used in the embodiments can be further adjusted according to specific requirements, and the implementation conditions not specified are usually the conditions in conventional experiments.
[0046] Unless otherwise specified in the following examples, all raw materials are commercially available or prepared by conventional methods in the art.
[0047] In the following description, nickel nitrate hexahydrate was purchased from Sinopharm Chemical Reagent Co., Ltd., grade C223150025; ferric nitrate nonahydrate was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., grade F100211; sodium citrate was purchased from Sinopharm Chemical Reagent Co., Ltd., grade CATOCCFD201067100MG; and polyvinylpyrrolidone (PVP, K29-32) was purchased from Sinopharm Chemical Reagent Co., Ltd., grade XW01900339802.
[0048] Example 1 This example provides a method for preparing a modified zeolite dehumidifying material, the method comprising: Weigh 2.91 g of nickel nitrate hexahydrate and 8.08 g of ferric nitrate nonahydrate, dissolve them in 100 mL of ethylene glycol, and stir until completely dissolved; add 4.41 g of sodium citrate, and continue stirring for 30 min. Transfer the mixture to a hydrothermal reactor, seal it, and react at 140 °C for 12 h. After the reaction, centrifuge to separate the product, wash it three times alternately with deionized water and anhydrous ethanol, and dry it under vacuum at 60 °C for 12 h to obtain the nickel-iron bimetallic catalyst. See [Image of SEM image]. Figure 2 As shown, it can be seen that it has a basically nanoscale sheet-like structure.
[0049] Weigh 0.3 g of the nickel-iron bimetallic catalyst prepared according to the above method, disperse it in 100 mL of anhydrous ethanol, add 0.04 g of polyvinylpyrrolidone (PVP), and sonicate for 30 min to obtain a uniform and stable impregnation solution.
[0050] Take 13X type honeycomb zeolite and cut it into pieces approximately 10 cm × 10 cm × 10 cm in size, with a volume of approximately 1.0 dm³. 3 The sample was placed in a muffle furnace and calcined at 400℃ for 4 h to remove organic impurities. After cooling, it was ultrasonically cleaned with deionized water for 15 min, and then vacuum degassed at 250℃ (gauge pressure of vacuum is -0.09 MPa) for 6 h. After activation, it was cooled to room temperature.
[0051] The activated zeolite was placed in the impregnation solution prepared according to the above method, and the volume of the impregnation solution was controlled to be twice the volume of the zeolite. The vacuum was drawn to -0.09 MPa (gauge pressure) and maintained for 30 min. After restoring to normal pressure, it was allowed to stand and soak for 2 h.
[0052] The impregnated zeolite was removed and dried at 70℃ for 10 h; then it was transferred to a tube furnace and heated to 450℃ at a rate of 2℃ / min under air atmosphere, and calcined at a constant temperature for 4 h with an air flow rate of 0.5 L / min; it was then naturally cooled to room temperature to obtain the modified zeolite dehumidifying material.
[0053] Example 2 This example provides a method for preparing a modified zeolite dehumidifying material, the method comprising: Weigh 3.57 g of nickel chloride hexahydrate and 6.06 g of ferric nitrate nonahydrate, dissolve them in 100 mL of ethylene glycol, and stir until completely dissolved; add 6.62 g of sodium citrate, and continue stirring for 30 min. Transfer the mixture to a hydrothermal reactor, seal it, and react at 160 °C for 10 h. After the reaction is complete, centrifuge to separate the product, wash it three times alternately with deionized water and anhydrous ethanol, and dry it under vacuum at 70 °C for 10 h to obtain the nickel-iron bimetallic catalyst.
[0054] Weigh 0.4 g of the nickel-iron bimetallic catalyst prepared according to the above method, disperse it in 125 mL of anhydrous ethanol, add 0.1 g of polyvinylpyrrolidone (PVP), and sonicate for 30 min to obtain a uniform and stable impregnation solution.
[0055] Take 13X type honeycomb zeolite and cut it into pieces approximately 10 cm × 10 cm × 10 cm in size, with a volume of approximately 1.0 dm³. 3 The sample was placed in a muffle furnace and calcined at 400℃ for 4 h to remove organic impurities. After cooling, it was ultrasonically cleaned with deionized water for 15 min, and then vacuum degassed at 300℃ (gauge pressure of vacuum is -0.09 MPa) for 6 h. After activation, it was cooled to room temperature.
[0056] The activated zeolite was placed in the impregnation solution prepared according to the above method, and the volume of the impregnation solution was controlled to be twice the volume of the zeolite. The vacuum was drawn to -0.09 MPa (gauge pressure) and maintained for 30 min. After restoring to normal pressure, it was allowed to stand and soak for 2 h.
[0057] The impregnated zeolite was removed and dried at 60℃ for 8 h; then it was transferred to a tube furnace and heated to 450℃ at a rate of 2℃ / min under air atmosphere, and calcined at a constant temperature for 3 h with an air flow rate of 1.5 L / min; it was then naturally cooled to room temperature to obtain the modified zeolite dehumidifying material.
[0058] Example 3 This example provides a method for preparing a modified zeolite dehumidifying material, the method comprising: Weigh 2.91 g of nickel nitrate hexahydrate and 8.08 g of ferric nitrate nonahydrate, dissolve them in 100 mL of ethylene glycol, and stir until completely dissolved; add 4.41 g of sodium citrate, and continue stirring for 30 min. Transfer the mixture to a 150 mL hydrothermal reactor, seal it, and react at 140 °C for 12 h. After the reaction is complete, centrifuge to separate the product, wash it three times alternately with deionized water and anhydrous ethanol, and dry it under vacuum at 60 °C for 12 h to obtain the nickel-iron bimetallic catalyst.
[0059] Weigh 0.5 g of the nickel-iron bimetallic catalyst prepared according to the above method, disperse it in 150 mL of anhydrous ethanol, add 0.24 g of polyvinylpyrrolidone (PVP), and sonicate for 30 min to obtain a uniform and stable impregnation solution.
[0060] Take 13X type honeycomb zeolite and cut it into pieces approximately 10 cm × 10 cm × 10 cm in size, with a volume of approximately 1.0 dm³. 3 The sample was placed in a muffle furnace and calcined at 500℃ for 2 h to remove organic impurities. After cooling, it was ultrasonically cleaned with deionized water for 15 min, and then degassed under vacuum at 300℃ (gauge pressure of vacuum is -0.09 MPa) for 6 h. After activation, it was cooled to room temperature.
[0061] The activated zeolite was placed in the impregnation solution prepared according to the above method, and the volume of the impregnation solution was controlled to be twice the volume of the zeolite. The vacuum was drawn to -0.09 MPa (gauge pressure) and maintained for 30 min. After restoring to normal pressure, it was allowed to stand and soak for 2 h.
[0062] The impregnated zeolite was removed and dried at 60℃ for 8 h; then it was transferred to a tube furnace and heated to 450℃ at a rate of 2℃ / min under air atmosphere, and calcined at a constant temperature for 3 h with an air flow rate of 1.5 L / min; it was then naturally cooled to room temperature to obtain the modified zeolite dehumidifying material.
[0063] Comparative Example 1 The unsupported catalyst-free 13X honeycomb zeolite underwent the same pretreatment steps as in Example 1: 13X honeycomb zeolite was taken and cut into pieces approximately 10 cm × 10 cm × 10 cm in size, with a volume of approximately 1.0 dm³. 3 The sample was placed in a muffle furnace and calcined at 400℃ for 4 h to remove organic impurities. After cooling, it was ultrasonically cleaned with deionized water for 15 min, and then vacuum degassed at 250℃ (gauge pressure of vacuum is -0.09 MPa) for 6 h. After activation, it was cooled to room temperature.
[0064] Comparative Example 2 This example provides a method for preparing a modified zeolite dehumidifying material, which is basically the same as in Example 1, except that: the impregnation process is not vacuumed, and after loading, it is not calcined at high temperature, but only dried at low temperature.
[0065] Specifically, the preparation process is as follows: Weigh 2.91 g of nickel nitrate hexahydrate and 8.08 g of ferric nitrate nonahydrate, dissolve them in 100 mL of ethylene glycol, and stir until completely dissolved; add 4.41 g of sodium citrate, and continue stirring for 30 min. Transfer the mixed solution to a hydrothermal reactor, seal it, and react at 140 °C for 12 h. After the reaction is complete, centrifuge to separate the product, wash it three times alternately with deionized water and anhydrous ethanol, and dry it under vacuum at 60 °C for 12 h to obtain the nickel-iron bimetallic catalyst.
[0066] Weigh 0.3 g of the nickel-iron bimetallic catalyst prepared according to the above method, disperse it in 100 mL of anhydrous ethanol, add 0.04 g of polyvinylpyrrolidone (PVP), and sonicate for 30 min to obtain a uniform and stable impregnation solution.
[0067] Take 13X type honeycomb zeolite and cut it into pieces approximately 10 cm × 10 cm × 10 cm in size, with a volume of approximately 1.0 dm³. 3 The sample was placed in a muffle furnace and calcined at 400℃ for 4 h to remove organic impurities. After cooling, it was ultrasonically cleaned with deionized water for 15 min, and then vacuum degassed at 250℃ (gauge pressure of vacuum is -0.09 MPa) for 6 h. After activation, it was cooled to room temperature.
[0068] The activated zeolite is placed in the impregnation solution prepared according to the above method, and the volume of the impregnation solution is controlled to be twice the volume of the zeolite. It is then allowed to stand and soak for 2 hours under normal pressure without vacuuming. During this period, it can be gently shaken to ensure that the liquid and solid are in full contact.
[0069] The impregnated zeolite was removed and dried at 70°C for 10 hours. It was then removed from the high-temperature calcination in a tube furnace and allowed to cool naturally to room temperature to obtain the modified zeolite dehumidifying material.
[0070] Performance testing During the preparation of all the above materials, the zeolite substrate is cut into 1.0 dm pieces. 3 After the cube was formed, the selected sample was weighed and the mass of the pretreated zeolite substrate under no-load conditions was recorded as m0.
[0071] Take the materials obtained in Examples 1-3 and Comparative Examples 1-2, dry them to constant weight and record their mass m1. Record the loading of the dehumidifying effective component as Δm0. Then: △m0=m1-m0; The dried material was placed in a testing machine to test its dehumidification performance (e.g., ...). Figure 3As shown in the figure, the cavity cross-section of this testing machine is 1.0 dm. 2 A square sample was placed inside, with no air leakage (the honeycomb surface facing the wind). An airflow of 15℃, 85% relative humidity, and 2.0 m / s was introduced. The sample adsorbed for 7.5 minutes, then was removed and its mass m2 was recorded. The adsorption amount was denoted as Δm1. The level of adsorption is used to characterize the dehumidification performance of the material. Then: △m1=m2-m1; Subsequently, desorption performance was tested. The sample was placed in a dedicated desorption device (without any air leakage after the sample was placed in the desorption chamber). Desorption was performed for 2.5 minutes with flowing hot air at a face velocity of 2.0 m / s at two different temperatures: 80℃ and 120℃. The mass m³ (80℃) and m³ (120℃) were then recorded. The desorption amount was denoted as Δm². The desorption rate characterizes the desorption performance of the material. Therefore: △m2=|m3-m2|; Desorption rate = (△m2 / △m1) × 100%; The specific surface area data of different adsorbent materials are shown in Table 1.
[0072] Table 1 According to the technical solution of the present invention, the specific surface area of the dehumidifying materials obtained in each embodiment and the comparative example shows significant differences. Comparative example 1 is the original 13X type honeycomb zeolite without catalyst loading, which has a complete and unobstructed pore structure and the highest specific surface area, reaching 520 m². 2 / g, close to the theoretical intrinsic value of 13X zeolite. The specific surface areas of Examples 1-3 are 455 m², respectively. 2 / g、438m 2 / g and 442 m 2 Although the specific surface area (S / g) was slightly lower than that of Comparative Example 1 (a decrease of approximately 12% to 16%), it remained at a relatively high level. This indicates that the process employed in this invention can effectively introduce the nickel-iron bimetallic catalyst into the zeolite channels. Subsequent calcination causes the catalyst to condense with the silanol groups on the pore wall to form Ni-O-Si and Fe-O-Si covalent bonds, firmly anchoring the nanoparticles to the pore wall surface and effectively inhibiting particle agglomeration and pore blockage. Therefore, the specific surface area did not decrease significantly. Analysis suggests that the slight differences in specific surface area among the three examples are mainly related to the matching of impregnation liquid volume and PVP dosage: when the impregnation liquid volume increased from 2 to 3 times the zeolite volume and the PVP dosage increased from 0.05 wt% to 0.20 wt%, the nanocrystals were more fully dispersed in the liquid phase, which is beneficial for forming a more uniform loading layer in the channels, thereby maintaining the specific surface area at a better level. In contrast, the specific surface area of Comparative Example 2 was only 368 m². 2The specific surface area was the lowest among the five samples, with a concentration of / g. This is because the impregnation process did not involve a vacuum. Under normal pressure, the impregnation solution could not overcome diffusion resistance to effectively transport the nanoparticles to the depths of the pores. The nickel-iron bimetallic catalyst mainly accumulated on the outer surface and pore openings of the zeolite. Furthermore, the lack of a high-temperature calcination and curing step prevented the formation of covalent bonds for anchoring. Consequently, the nanocatalyst material underwent severe agglomeration during drying due to capillary forces, forming a large number of micron-sized agglomerates that blocked the micropore inlets. Nitrogen molecules could not enter the pores, resulting in a significant loss of specific surface area. The above results fully demonstrate that the synergistic effect of the process in this invention is the key to achieving high dispersion loading of the catalyst within the zeolite pores while maintaining pore unobstructed flow.
[0073] Table 2 shows the numerical records of different adsorbent loading, desorption amount, desorption rate, and cycle loss mass.
[0074] Table 2 As shown in Table 2, the embodiments of the present invention and the comparative examples exhibit significant differences in moisture absorption, low-temperature desorption performance, and cycle stability. The specific analysis is as follows: (1) Comparison of moisture absorption performance. The moisture absorption of the original zeolite in Comparative Example 1 was 28.6 g. The moisture absorption of Comparative Example 2 was only 24.3 g, which was a decrease of 15.0% compared with the original zeolite, because the catalyst agglomerated and blocked the pores due to the lack of vacuuming and calcination. Moreover, since irreversible pore blockage had already occurred in the early preparation stage, the pore damage would not be repaired by the subsequent catalyst shedding. Therefore, the moisture absorption did not recover after 20 cycles. The moisture absorption of Examples 1 to 3 were 30.1 g, 29.5 g and 30.8 g, respectively, which were 5.2%, 3.1% and 7.7% higher than the original zeolite in Comparative Example 1. This shows that the introduction of the nickel-iron bimetallic catalyst not only did not occupy too many adsorption sites, but also enhanced the adsorption affinity of water molecules on the inner wall of the zeolite pores through the Ni / Fe bimetallic active center, thus achieving a synergistic gain in moisture absorption capacity.
[0075] (2) Comparison of low-temperature desorption performance. The original zeolite in Comparative Example 1 achieved a desorption rate of 91.6% at 120℃, which was good. However, when the desorption temperature dropped to 80℃, its desorption rate dropped sharply to only 32.5%, indicating that the adsorption force of the original zeolite on water molecules was too strong. Under low-temperature conditions, water molecules could not obtain enough energy to overcome the desorption activation energy and escape from the pores. It is believed that this is the fundamental reason why traditional zeolite rotors must rely on high-temperature regeneration. The desorption rates of Comparative Example 2 at 80℃ and 120℃ were 41.7% and 74.8%, respectively, which were still significantly lower than those of the original zeolite at 120℃. The desorption rate at 80℃ was also not ideal, indicating that the uncalcined and solidified physical supported catalyst failed to form an effective synergy with the zeolite and could not significantly reduce the desorption activation energy.
[0076] In comparison, the desorption rates of Examples 1-3 at 80°C reached 92.4%, 90.8%, and 93.7%, respectively, which were basically the same as their desorption rates at 120°C (95.2%, 94.1%, and 96.0%), and all reached or even exceeded the desorption rate level of the original zeolite in Comparative Example 1 at 120°C (91.6%). This indicates that the vacuum impregnation and covalent bond anchoring process of the present invention highly disperses the Ni / Fe bimetallic active sites on the inner wall of the zeolite channels. Ni, as an electron donor, weakens the electrostatic attraction of cations on the pore walls to water molecules, and the coupling of Fe's 3d orbitals with the antibonding orbitals of OH bonds reduces the hydrogen bonding force. The dual mechanism synergistically reduces the desorption activation energy of water molecules, making the thermal energy at 80°C sufficient to drive efficient desorption of water molecules. This is the first time that efficient regeneration of zeolite dehumidifying materials at a low temperature of 80°C has been achieved.
[0077] (3) Comparison of Cyclic Stability. After 20 adsorption-desorption cycles, the moisture retention rates of Examples 1-3 were 95.3%, 94.9%, and 94.8%, respectively, all exceeding 94%, indicating that the catalyst treated by the process of this invention is firmly bonded to the zeolite substrate, and there is no significant shedding or agglomeration during repeated thermal cycling and airflow scouring. The moisture retention rate of the original zeolite in Comparative Example 1 was 97.2%, slightly higher than that of the Examples, but this was only possible because it had to be regenerated at a high temperature of 120°C. If it was at 80°C, its effective desorption amount was extremely low, and it was practically impossible to complete a complete cycle. The moisture retention rate of Comparative Example 2 was only 56.0%, and a large amount of catalyst was lost after cycling, indicating that the catalyst, which only relied on physical adhesion, lacked chemical bonding with the substrate and had weak bonding force, making it difficult to meet the requirements for long-term stable operation in practical applications.
[0078] The above results demonstrate that the process for preparing the modified zeolite dehumidifying material of this invention successfully achieves high dispersion and robust loading of the nickel-iron bimetallic catalyst within the zeolite channels. This allows the dehumidifying material to maintain increased moisture absorption while significantly reducing the regeneration temperature from over 120℃ to 80℃, achieving a desorption rate exceeding 90%, and exhibiting excellent cycle stability. This material provides a practical solution for low-energy rotary dehumidification technology.
[0079] The above embodiments are only for illustrating the technical concept and features of the present invention, and are intended to enable those skilled in the art to understand the content of the present invention and implement it accordingly. They should not be construed as limiting the scope of protection of the present invention. All equivalent changes or modifications made in accordance with the spirit and essence of the present invention should be covered within the scope of protection of the present invention.
[0080] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
Claims
1. A method for preparing a modified zeolite dehumidifying material, characterized in that, The preparation method includes: A nickel-iron bimetallic catalyst is dispersed in an organic solvent to prepare an impregnation solution; the nickel-iron bimetallic catalyst is generated by a solvothermal reaction of nickel salt and iron salt in the presence of a surfactant. The zeolite substrate is pretreated, including calcination and vacuum degassing under heating conditions, to obtain a pretreated zeolite substrate; the pretreated zeolite substrate is impregnated in the impregnation solution to obtain an intermediate, wherein the impregnation includes at least vacuum impregnation; the intermediate is calcined at a temperature greater than or equal to 300°C.
2. The preparation method of the modified zeolite dehumidifying material according to claim 1, characterized in that, The impregnation solution comprises the nickel-iron bimetallic catalyst, the dispersant, and the organic solvent; by weight percentage, the nickel-iron bimetallic catalyst accounts for 0.2wt%-0.6wt% and the dispersant accounts for 0.05wt%-0.2wt% in the impregnation solution. Furthermore, the dispersant comprises polyvinylpyrrolidone; Furthermore, the organic solvent is an anhydrous alcohol solvent, and even further, the anhydrous alcohol solvent includes anhydrous ethanol and / or anhydrous methanol; Furthermore, the nickel-iron bimetallic catalyst is nanoscale.
3. The method for preparing the modified zeolite dehumidifying material according to claim 1 or 2, characterized in that, The nickel-iron bimetallic catalyst has a sheet-like structure; further, the sheet diameter of the nickel-iron bimetallic catalyst is less than 5 μm and the thickness is less than 200 nm; even further, the sheet diameter of the nickel-iron bimetallic catalyst is 1-3 μm and the thickness is 20-50 nm.
4. The preparation method of the modified zeolite dehumidifying material according to claim 1, characterized in that, The preparation method of the nickel-iron bimetallic catalyst includes: dispersing nickel salt and iron salt in an alcohol solvent, adding a surfactant, and conducting a solvothermal reaction at 140-180℃ to generate a nickel-iron bimetallic catalyst with a plate-like structure; further, the alcohol solvent includes ethylene glycol.
5. The method for preparing the modified zeolite dehumidifying material according to claim 1 or 4, characterized in that, The nickel salt is selected from one or more combinations of nickel nitrate, nickel sulfate, and nickel chloride; and / or, The iron salt is selected from one or more combinations of ferric nitrate, ferric sulfate, and ferric chloride; and / or, The molar ratio of nickel in the nickel salt to iron in the iron salt is 1:0.5-3, preferably 1:1.5-2.5; and / or, The surfactant is sodium citrate; and / or, The surfactant is added at a mass of 0.5-1.0 times the total mass of the nickel salt and the iron salt; and / or, The reaction time of the solvothermal reaction is controlled to be 6-24 h, and more specifically 8-14 h.
6. The method for preparing the modified zeolite dehumidifying material according to claim 1, characterized in that, The calcination treatment is controlled to be carried out at a temperature of 400-500℃; and / or, the calcination time of the calcination treatment is controlled to be 1-8h; and / or, the heating conditions are controlled to make the heating temperature 250-350℃; and / or, the gauge pressure of the vacuum degree of the vacuum degassing is controlled to be -0.5~-0.01MPa, further -0.2~-0.05MPa; and / or, the preparation method of the pretreated zeolite substrate includes: calcining the zeolite substrate in air, ultrasonically cleaning it after cooling, and then vacuum degassing it under heating conditions.
7. The preparation method of the modified zeolite dehumidifying material according to claim 1, characterized in that, During the vacuum impregnation process, the gauge pressure of the vacuum is controlled at -0.5 to -0.01 MPa, and the holding time is 10-60 min; and / or, The impregnation process includes: first, vacuum impregnation, then static soaking under normal pressure; further, the static soaking time is 0.5-4 hours; and / or, The volume of the impregnation solution is more than twice the volume of the pretreated zeolite substrate, and further between two and five times.
8. The method for preparing the modified zeolite dehumidifying material according to claim 1, characterized in that, The calcination temperature is controlled at 300-600℃, further at 400-550℃, and even further at 450-500℃; and / or, the heating rate of the calcination is controlled at 1-10℃ / min, further at 1-5℃ / min; and / or, the calcination is carried out in an oxygen-containing atmosphere, further in an air atmosphere, and even further, the air flow rate is 0.5-2L / min; and / or, before the calcination, drying is performed at a temperature of 60-80℃ for a time of 5-24h.
9. A modified zeolite dehumidifying material prepared by the method of preparing the modified zeolite dehumidifying material according to any one of claims 1-8.
10. The application of the modified zeolite dehumidifying material according to claim 9 in the preparation of a dehumidifying impeller.