A kind of biochar load bismuth trioxide composite material, preparation method and application thereof
The preparation method of bismuth trioxide composite material supported on biochar solves the problems of small specific surface area, easy agglomeration and poor removal of organic pollutants in the treatment of high-concentration chloride ion wastewater and landfill leachate in the existing technology, and achieves a highly efficient synergistic removal effect of chloride ions and organic pollutants.
Patent Information
- Application Number
- CN202611442929.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-20
AI Technical Summary
Existing bismuth trioxide materials suffer from problems such as small specific surface area, limited number of active sites, easy aggregation, poor removal effect on organic pollutants, and insufficient stability when treating wastewater with high concentration of chloride ions and landfill leachate.
The preparation of biochar-supported bismuth trioxide composite material involves specific steps including preparing biochar from coffee grounds, polydopamine coating, hydrothermal reaction, and multiple calcinations, which result in the uniform deposition of bismuth oxide on the surface of the biochar, thereby improving the dispersibility and activity of the material.
It significantly reduces chloride ion concentration, color, and TOC content in landfill leachate, enhances the synergistic removal effect of organic pollutants, and improves the stability and active site utilization of the material.
Smart Images

Figure CN123127953A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of water treatment technology, specifically to a biochar-supported bismuth trioxide composite material, its preparation method, and its application. Background Technology
[0002] Currently, high concentrations of chloride ions are a significant problem in the advanced treatment of landfill leachate. Studies have shown that Bi(III) oxide materials can achieve efficient dechlorination by reacting with chloride ions to generate BiOCl. Li et al. reported a Bi(III) oxide dechlorination material in their paper, "Removal and recovery of chloride ions in concentrated leachate by Bi(III) containing oxides quantum dots / two-dimensional flake," which can achieve highly efficient removal of chloride ions from concentrated leachate.
[0003] Furthermore, Chinese patent CN201110064626.5, "Method for Removing Chlorine from Zinc Sulfate Solution Containing Chloride Using Bismuth Trioxide," discloses a method for removing high concentrations of chloride ions using bismuth-based materials. This method involves the reaction of a bismuth-based compound with chloride ions in the solution to generate bismuth oxychloride (BiOCl), thereby achieving highly efficient chloride ion removal. This technology provides a new approach for removing chloride ions from high-salinity wastewater and landfill leachate, and has certain advantages in dechlorination efficiency.
[0004] However, this patent primarily focuses on the removal efficiency of chloride ions, with limited research on the synergistic removal of organic pollutants such as color and humic substances in landfill leachate. Furthermore, bismuth-based materials are prone to aggregation, limiting the utilization rate of active sites. Therefore, developing a novel bismuth-based composite material that combines highly efficient dechlorination capabilities with synergistic removal of organic pollutants remains of significant research value.
[0005] ② Briefly describe the current state of the background technology, such as its main structure or working principle, etc. Currently, the main methods for treating high-concentration chloride ion wastewater and landfill leachate include membrane separation, ion exchange, chemical precipitation, electrochemical methods, and bismuth-based dechlorination. Among these, bismuth-based dechlorination has attracted widespread attention due to its high chloride ion selectivity.
[0006] Chinese patent CN201110064626.5 discloses a dechlorination technology based on Bi(III) oxides. It uses Bi(III) oxides, such as bismuth trioxide, as dechlorination materials. Under acidic conditions, Bi(III) reacts with chloride ions to generate bismuth oxychloride (BiOCl), thereby achieving efficient removal and recovery of chloride ions from wastewater. Its main working principle is as follows:
[0007] This technology utilizes the affinity of Bi(III) for chloride ions to achieve selective fixation of chloride ions, and has good application prospects in the field of dechlorination of high-salt wastewater and landfill leachate.
[0008] ③ Objectively evaluate the background technology and point out its main advantages and disadvantages; The aforementioned bismuth-based dechlorination technology has advantages such as high chloride ion removal efficiency, good selectivity, and the ability to recover chloride ions as resources, and has certain application value in the field of high chloride ion wastewater treatment.
[0009] However, this type of technology still has the following shortcomings: (1) The specific surface area of a single bismuth trioxide material is relatively small and the number of active sites is limited, which is not conducive to the full contact and mass transfer of chloride ions; (2) Bismuth trioxide particles are prone to agglomeration, which leads to a decrease in actual utilization rate; (3) Existing studies mainly focus on the removal effect of chloride ions, while less attention is paid to the synergistic removal of pollutants such as color, humic substances and dissolved organic matter in landfill leachate; (4) The material recycling performance and engineering application stability still need to be further improved.
[0010] Therefore, developing a novel composite material that combines efficient dechlorination capabilities with synergistic removal of organic pollutants is of great significance for the deep treatment of landfill leachate. Summary of the Invention
[0011] The purpose of this invention is to provide a biochar-supported bismuth trioxide composite material, its preparation method, and its application, in order to solve the problems mentioned in the background art.
[0012] To achieve the above objectives, the present invention provides the following technical solution: A method for preparing a biochar-supported bismuth trioxide composite material, the method comprising the following steps: S1. Preparation of biochar from coffee grounds; S2. Place the biochar prepared in step S1 in a Tris-HCl buffer solution containing dopamine, stir continuously for 12-16 h, then oxidize, and dry at 30-40℃ to constant weight to obtain polydopamine-coated biochar. S3. The polydopamine-coated biochar obtained in step S2 is impregnated in bismuth nitrate solution for 5-10 minutes, and then the filtered product is washed with methanol. S4. The product washed with methanol in step S3 is immersed in a methanol solution containing trimesic acid for hydrothermal reaction, then filtered, and the filtered product is washed with methanol to obtain the reactant. S5. Calcining the reactants obtained in step S4 at 700-800℃ in a nitrogen atmosphere for 1-2 hours; S6. After the reactants calcined in step S5 are cooled, they are calcined again in air at 170-200℃ for 2-4 hours to obtain biochar-supported bismuth trioxide composite material.
[0013] Furthermore, the specific method for preparing biochar from coffee grounds in step S1 includes the following steps: S101. After washing the coffee grounds with deionized water, dry them at 80-90 ℃ for 10-12 hours and pass them through an 80-mesh sieve. S102. The coffee grounds treated in step S101 are calcined at 450-600℃ for 2-3 hours under a nitrogen atmosphere.
[0014] Furthermore, in step S2, the concentration of dopamine is 5-10 mg / ml, and the mass ratio between biochar and Tris-HCl buffer solution containing dopamine is 1:(8-10).
[0015] Furthermore, in step S3, the concentration of the bismuth nitrate solution is 0.04-0.06 mol / L, and the mass ratio between the polydopamine-coated biochar and the bismuth nitrate solution is 1:20.
[0016] Furthermore, in step S4, the concentration of trimellitic acid in the methanol solution of trimellitic acid is 0.1-0.2 mol / L, and the mass ratio between the methanol solution containing trimellitic acid in step S4 and the polydopamine-coated biochar in step S3 is 20:1.
[0017] Furthermore, in step S4, the temperature of the hydrothermal reaction is 100-120℃, and the time of the hydrothermal reaction is 15-25h.
[0018] A biochar-supported bismuth trioxide composite material is prepared by the above-described method for preparing biochar-supported bismuth trioxide composite materials.
[0019] The above-mentioned biochar-supported bismuth trioxide composite material is used to reduce chloride ion concentration, color, and TOC content in landfill leachate.
[0020] Compared with the prior art, the beneficial effects of the present invention are: 1. The composite material prepared in this invention can effectively reduce the chloride ion concentration, color, and TOC content in landfill leachate; 2. In this invention, polydopamine is coated onto biochar, and then a MOF material is formed on the polydopamine. After two heat treatments, bismuth oxide is formed on the surface of the biochar. The bismuth oxide has good dispersibility, and compared with the composite material formed directly by acid-base adjustment, it has a better treatment effect on pollutants in landfill leachate. Attached Figure Description
[0021] Figure 1 This is a process flow diagram of the present invention; Figure 2 This is a process flow diagram for preparing biochar in this invention; Figure 3 This is a three-dimensional fluorescence image of the landfill filtrate that has not undergone composite material treatment in this invention. Figure 4 This is a three-dimensional fluorescence image of the composite material prepared in Example 1 of this invention after treating landfill filtrate for 4 hours; Figure 5 This is a three-dimensional fluorescence image of the composite material prepared in Example 1 of this invention after treating landfill filtrate for 12 hours; Figure 6 This is a three-dimensional fluorescence image of the composite material prepared in Example 1 of this invention after treating landfill filtrate for 24 hours. Figure 7 This is a physical image of the composite material prepared in Example 1 of this invention. Detailed Implementation
[0022] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0023] Please see Figures 1 to 7 The present invention provides: Example 1
[0024] A method for preparing a biochar-supported bismuth trioxide composite material, the method comprising the following steps: S1. Preparation of biochar from coffee grounds; S2. Place 10g of biochar prepared in step S1 into 90g of Tris-HCl buffer solution containing dopamine. The concentration of dopamine is 8mg / ml and the pH of the Tris-HCl buffer solution is 8.5. Stir continuously for 15h, then oxidize and dry at 35℃ to constant weight to obtain polydopamine-coated biochar. S3. Impregnate 10g of polydopamine-coated biochar obtained in step S2 in 200g of 0.05mol / L bismuth nitrate solution for 8min, and then filter the product and wash it with methanol. S4. The product washed with methanol in step S3 is immersed in 200g of methanol solution containing trimellitic acid, the concentration of trimellitic acid in the methanol solution is 0.15mol / L, and a hydrothermal reaction is carried out at a temperature of 110℃ for 15h. After filtration, the filtered product is washed with methanol to obtain the reactant. S5. Calcine the reactants obtained in step S4 at 750°C in a nitrogen atmosphere for 1.5 h. S6. After cooling the calcined reactants in step S5, they are calcined again at 180°C in air for 3 hours to obtain biochar-supported bismuth trioxide composite material. The specific method for preparing biochar from coffee grounds in step S1 above includes the following steps: S101. Wash 20g of coffee grounds with deionized water, dry them at 85℃ for 11 hours, and then pass them through an 80-mesh sieve. S102. The coffee grounds treated in step S101 are calcined at 500°C for 2.5 hours under a nitrogen atmosphere.
[0025] Example 2
[0026] A method for preparing a biochar-supported bismuth trioxide composite material, the method comprising the following steps: S1. Preparation of biochar from coffee grounds; S2. Place 10g of biochar prepared in step S1 into 80g of Tris-HCl buffer solution containing dopamine. The concentration of dopamine is 5mg / ml and the pH of the Tris-HCl buffer solution is 8.5. Stir continuously for 12h to react, then oxidize and dry at 30℃ to constant weight to obtain polydopamine-coated biochar. S3. Impregnate 10g of polydopamine-coated biochar obtained in step S2 in 200g of 0.04mol / L bismuth nitrate solution for 5min, and then filter the product and wash it with methanol. S4. The product washed with methanol in step S3 is immersed in 200g of methanol solution containing trimellitic acid, the concentration of trimellitic acid in the methanol solution is 0.1mol / L, and a hydrothermal reaction is carried out at a temperature of 100℃ for 20h. After filtration, the filtered product is washed with methanol to obtain the reactant. S5. Calcine the reactants obtained in step S4 at 700°C in a nitrogen atmosphere for 1 hour. S6. After cooling the calcined reactants in step S5, they were calcined again at 170°C in air for 2 hours to obtain a biochar-supported bismuth trioxide composite material. The specific method for preparing biochar from coffee grounds in step S1 above includes the following steps: S101. Wash 20g of coffee grounds with deionized water, dry them at 80℃ for 10 hours, and then pass them through an 80-mesh sieve. S102. The coffee grounds treated in step S101 are calcined at 450°C for 2 hours under a nitrogen atmosphere.
[0027] Example 3
[0028] A method for preparing a biochar-supported bismuth trioxide composite material, the method comprising the following steps: S1. Preparation of biochar from coffee grounds; S2. Place 10g of biochar prepared in step S1 into 100g of Tris-HCl buffer solution containing dopamine. The pH of the Tris-HCl buffer solution is 8.5 and the concentration of dopamine is 10mg / ml. Stir continuously for 16h to react, then oxidize and dry at 40℃ to constant weight to obtain polydopamine-coated biochar. S3. Impregnate 10g of polydopamine-coated biochar obtained in step S2 in 200g of 0.06mol / L bismuth nitrate solution for 10min, and then filter the product and wash it with methanol. S4. The product washed with methanol in step S3 is immersed in 200g of methanol solution containing trimellitic acid, the concentration of trimellitic acid in the methanol solution is 0.2mol / L, and a hydrothermal reaction is carried out at a temperature of 120℃ for 25h. After filtration, the filtered product is washed with methanol to obtain the reactant. S5. Calcine the reactants obtained in step S4 at 800°C in a nitrogen atmosphere for 2 hours. S6. After cooling the calcined reactants in step S5, they were calcined again at 200°C in air for 4 hours to obtain a biochar-supported bismuth trioxide composite material. The specific method for preparing biochar from coffee grounds in step S1 above includes the following steps: S101. Wash 20g of coffee grounds with deionized water, dry them at 90℃ for 12 hours, and then pass them through an 80-mesh sieve. S102. The coffee grounds processed in step S101 are calcined at 600°C for 3 hours under a nitrogen atmosphere.
[0029] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that step S2 is omitted, while the remaining steps are exactly the same as in Example 1.
[0030] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that step S4 was omitted. The product washed with methanol in step S3 was immersed in a methanol solution, and then sodium hydroxide solution was added dropwise to adjust the pH to 10. The reaction was carried out for 1.5 hours, and then steps S5 and S6 were continued.
[0031] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that the preparation process of the composite material is as follows: 10g of biochar is dispersed in 500mL of deionized water and stirred for 30 min. 200g of 0.05mol / L bismuth nitrate solution is prepared, Bi(NO3)3•5H2O is added to 200mL of deionized water, and an appropriate amount of 1mol / L nitric acid solution is added to aid dissolution. The bismuth nitrate solution is added to the biochar solution and stirred for 2 h to ensure thorough stirring. 1mol / L NaOH solution is slowly added dropwise to adjust the pH of the system to 10. The mixture is centrifuged and washed multiple times with deionized water and ethanol to remove free nitrate ions. It is dried in a vacuum at 80℃ for 12 h and heated to 500℃ in a tube furnace at a nitrogen atmosphere at a rate of 5℃ and held for 2 h. The method of Comparative Example 3 is to directly adjust the acid-base balance to achieve the precipitation of bismuth oxide on the biochar, thus completing the preparation of the composite material.
[0032] In the specific embodiments of this invention, bismuth nitrate is Bi(NO3)3•5H2O.
[0033] Take 100 mL of landfill leachate and adjust the pH to 1 with 1 mol / L sulfuric acid. At this time, the chloride ion content in the leachate is 1220 mg / L, the color is 1037 degrees, and the TOC is 264 mg / L. The results of treating landfill leachate with the composite materials from Examples 1-3 and Comparative Examples 1-3, under pH=1 conditions, are shown in Table 1 below: Table 1: Results of treating landfill filtrate with composite materials prepared in Examples 1-3 and Comparative Examples 1-3
[0034] Landfill leachate chloride concentration detection To determine the chloride ion content in the leachate, a sodium chloride standard curve was prepared. First, sodium chloride solutions with different chloride ion concentrations (5 mg / L, 10 mg / L, 15 mg / L, 20 mg / L) were prepared to construct a chloride ion concentration standard curve. The preparation method for the standard curve is as follows: Weigh 1.648 g of NaCl, dissolve it in an appropriate amount of deionized water, transfer it to a 1 L volumetric flask, dilute to volume, and mix well to prepare a 1000 mg / L chloride solution. - The standard stock solution is the mother solution V1. Take 0.5 mL, 1 mL, 1.5 mL, and 2 mL of solution V1 and dilute to 100 mL volumetric flasks, namely V2, V3, V4, and V5, respectively. Take 6-7 mL of each and load it into an ion chromatography tube for injection. Dilute to 2 L with 0.955 g sodium carbonate and 0.235 g sodium bicarbonate as eluent and filter.
[0035] Detection of chloride ion content in landfill leachate: Take 1 mL of filtered leachate and dilute it to 100 mL in a volumetric flask with deionized water. Pass the diluted leachate through a cation exchange column (Na type) to remove metal ions and filter impurities through a 0.22 μm aqueous filter head. Then take 6-7 mL and inject it into an ion chromatography tube for analysis.
[0036] Landfill leachate color detection The platinum-cobalt colorimetric method follows GB / T 11903-1989, "Determination of Color in Water". This method is suitable for clean water, lightly polluted water with a slightly yellow tint, relatively clean surface water, groundwater, and drinking water.
[0037] First, take 2 mL, 4 mL, 6 mL, and 8 mL of the purchased 500-color platinum-cobalt colorimetric solution and dilute to 10 mL in volumetric flasks to prepare standard solutions with colorimetric values of 100, 200, 300, and 400. Immediately measure the absorbance at a wavelength of 455 nm using an ultraviolet spectrophotometer and zero the instrument with ultrapure water.
[0038] Determination of color of landfill leachate: Take an appropriate amount of leachate, filter it through a 0.45μm filter membrane, measure the absorbance at a wavelength of 455 nm, and convert the color value through a standard curve.
[0039] Landfill leachate TOC testing After filtering the landfill leachate through a 0.45 μm filter membrane, 1 mL of the sample was diluted to a 100 mL volumetric flask to reduce matrix interference. The treated sample was then transferred to a sample vial and immediately analyzed using a total organic carbon analyzer.
[0040] Three-dimensional fluorescence detection of landfill leachate After filtering the landfill leachate through a 0.45 μm filter membrane, 1 mL was diluted to a 50 mL volumetric flask and immediately sent to a fluorescence spectrophotometer for detection. The excitation wavelength was set to 200 nm-450 nm, the emission wavelength to 200 nm-600 nm, the excitation and emission wavelength step to 5 nm, the slit width to 5 nm, and the scan rate to 2400 nm / min to analyze the fluorescence peak distribution characteristics.
[0041] Before treatment, the landfill filtrate had a chloride ion content of 1220 mg / L, a color of 1037 degrees, and a TOC of 264 mg / L. As shown in Table 1, the composite material in Example 1 of this invention showed better treatment effects on chloride ions, color, and TOC than Comparative Examples 1-3, especially in chloride ion treatment. Comparative Example 1 omitted step S2, i.e., the addition of a polydopamine layer on biochar. The functional groups of the polydopamine layer readily adsorb bismuth ions from the solution. Comparative Example 2 omitted the hydrothermal reaction step. In step S4, an organic ligand was added, which, under hydrothermal reaction, could react with bismuth ions to form a mof material on the surface of the polydopamine layer. The bismuth oxide formed by the mof material had a better specific surface area and was less prone to aggregation. Comparative Example 3, using a general approach, directly precipitated bismuth oxide on biochar through acid-base adjustment, but its effect was weaker than that of Example 1.
[0042] Furthermore, three-dimensional fluorescence analysis showed that, as Figure 3-6 As shown, Figure 3-6 The figures show the three-dimensional fluorescence images of the composite material prepared in Example 1 at 0h, 4h, 12h and 24h after treating landfill filtrate (EX represents excitation wavelength, EM represents emission wavelength, and intensity represents fluorescence intensity). It can be seen from the figures that the fluorescence peaks of humic substances and fulvic acids are significantly weakened, indicating that the composite material can simultaneously reduce some organic pollutants in the leachate.
[0043] This invention comprises six steps. Step 1 involves forming biochar. Step 2 involves forming a polydopamine layer on the surface of the biochar. Step 3 involves uniformly attaching bismuth ions to the surface of the polydopamine layer by utilizing its abundant functional groups and a short-time impregnation process. Step 4 involves forming a mof material on the surface of the polydopamine layer through a hydrothermal reaction in a solution containing organic ligands. Step 5 involves calcination in an inert gas, which carbonizes the mof material and the polydopamine layer, further enhancing their absorption of TOC and color in landfill filtrate. Additionally, bismuth ions are gradually converted into bismuth in the inert gas. Step 6 involves a second heating treatment in air. During this heating process, bismuth is gradually converted into bismuth oxide under the action of oxygen, completing the adsorption treatment of chloride ions in the solution.
[0044] Compared with traditional methods, this invention facilitates the uniform sedimentation of bismuth oxide on biochar, thereby improving the absorption capacity of waste in landfill filtrate.
[0045] In addition, the changes in chloride ion, color and TOC content after treating landfill filtrate with biochar and bismuth oxide alone were tested in this invention. After treatment, the chloride ion concentrations were 1015 mg / L and 516 mg / L, the color was 251 and 196, and the TOC content was 198 mg / L and 184 mg / L, respectively. The treatment effect of biochar and bismuth oxide alone was significantly weaker than that of the composite material prepared in this invention.
[0046] Figure 7 The image shown is a physical picture of the composite material prepared in Example 1 of this invention. The composite material prepared in this invention is in the form of a black powder.
[0047] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a biochar-supported bismuth trioxide composite material, characterized in that, The preparation method includes the following steps: S1. Preparation of biochar from coffee grounds; S2. Place the biochar prepared in step S1 in a Tris-HCl buffer solution containing dopamine, stir continuously for 12-16 h, then oxidize, and dry at 30-40℃ to constant weight to obtain polydopamine-coated biochar. S3. The polydopamine-coated biochar obtained in step S2 is impregnated in bismuth nitrate solution for 5-10 minutes, and then the filtered product is washed with methanol. S4. The product washed with methanol in step S3 is immersed in a methanol solution containing trimesic acid for hydrothermal reaction, then filtered, and the filtered product is washed with methanol to obtain the reactant. S5. Calcining the reactants obtained in step S4 at 700-800℃ in a nitrogen atmosphere for 1-2 hours; S6. After the reactants calcined in step S5 are cooled, they are calcined again in air at 170-200℃ for 2-4 hours to obtain biochar-supported bismuth trioxide composite material.
2. The method for preparing the biochar-supported bismuth trioxide composite material according to claim 1, characterized in that, The specific method for preparing biochar from coffee grounds in step S1 includes the following steps: S101. After washing the coffee grounds with deionized water, dry them at 80-90 ℃ for 10-12 hours and pass them through an 80-mesh sieve. S102. The coffee grounds treated in step S101 are calcined at 450-600℃ for 2-3 hours under a nitrogen atmosphere.
3. The method for preparing the biochar-supported bismuth trioxide composite material according to claim 1, characterized in that, In step S2, the concentration of dopamine is 5-10 mg / ml, and the mass ratio between biochar and Tris-HCl buffer solution containing dopamine is 1:(8-10).
4. The method for preparing the biochar-supported bismuth trioxide composite material according to claim 1, characterized in that, In step S3, the concentration of the bismuth nitrate solution is 0.04-0.06 mol / L, and the mass ratio between the polydopamine-coated biochar and the bismuth nitrate solution is 1:
20.
5. The method for preparing the biochar-supported bismuth trioxide composite material according to claim 1, characterized in that, In step S4, the concentration of pyromellitic acid in the methanol solution of pyromellitic acid is 0.1-0.2 mol / L, and the mass ratio between the methanol solution containing pyromellitic acid in step S4 and the polydopamine-coated biochar in step S3 is 20:
1.
6. The method for preparing the biochar-supported bismuth trioxide composite material according to claim 1, characterized in that, In step S4, the hydrothermal reaction temperature is 100-120℃ and the hydrothermal reaction time is 15-25h.
7. A biochar-supported bismuth trioxide composite material, characterized in that, The bismuth trioxide composite material supported on biochar as described in any one of claims 1-6 was prepared.
8. The application of the biochar-supported bismuth trioxide composite material as described in claim 7 in reducing chloride ion concentration, color, and TOC content in landfill leachate.
Citation Information
Patent Citations
Method for removing chlorine from chlorine-containing zinc sulfate solution by using bismuth trioxide
CN102154552A