Magnetic molecular MOF composite material, preparation method and application thereof

By forming a polydopamine interlayer on Fe₃O₄ nanoparticles and growing a UiO-66-NH₂ shell in a eutectic solvent, combined with molecular imprinting technology, the prepared magnetic molecularly imprinted MOF material achieved efficient and safe selective adsorption of enrofloxacin under normal pressure, solving the problems of high pressure and toxic solvents in traditional methods, and is suitable for the removal of antibiotic residues in milk.

CN123127964APending Publication Date: 2026-11-20ZHEJIANG WANLI UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611321488.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing technologies for removing enrofloxacin residues from milk suffer from problems such as complex operation, high cost, poor selectivity, and environmental pollution. In particular, the synthesis of traditional MOF materials relies on high pressure and toxic solvents, making it difficult to achieve efficient and safe adsorption and recovery.

Method used

Using Fe₃O₄ nanoparticles as the magnetic core, a polydopamine intermediate layer is formed through dopamine self-polymerization. A UiO-66-NH₂ shell layer is grown in situ in a choline chloride-acetamide eutectic solvent. Combined with molecular imprinting technology, a core-shell structured magnetic molecularly imprinted MOF composite material is prepared, achieving atmospheric pressure synthesis and highly selective adsorption.

Benefits of technology

A magnetic molecularly imprinted MOF material was prepared under normal pressure and non-toxic solvent conditions. It has high selectivity and high efficiency in removing enrofloxacin, and is suitable for removing antibiotic residues in complex food matrices. It also has rapid magnetic separation and environmental protection characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123127964A_ABST
    Figure CN123127964A_ABST
Patent Text Reader

Abstract

The application provides a magnetic molecular MOF composite material and a preparation method and application thereof, the composite material takes Fe3O4 nanoparticles as a magnetic core, forms a polydopamine (PDA) intermediate layer through self-polymerization of dopamine, takes a choline chloride-acetamide deep eutectic solvent (DES) as a green reaction medium, and grows a UiO-66-NH2 shell layer in situ under normal pressure conditions to prepare a core-shell structure Fe3O4@PDA@UiO-66-NH2 carrier, and takes enrofloxacin as a template molecule, itaconic acid as a functional monomer, and pentaerythritol triacrylate as a crosslinking agent to prepare a molecularly imprinted polymer under irradiation, the material has superparamagnetism, can be quickly separated under an external magnetic field, and has specific recognition ability to enrofloxacin due to imprinted cavities, an imprint factor is 1.30, and a selectivity coefficient is 1.29. The removal rate of the material to enrofloxacin in milk can reach 80.6% to 98.2%, the whole preparation process does not need high pressure and toxic organic solvents, the operation is simple, and the material has a good application prospect in the field of selective adsorption and removal of antibiotic residues in food.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of antibiotic residue removal technology, and in particular to a magnetic molecular MOF composite material, its preparation method and application. Background Technology

[0002] Fluoroquinolones are widely used in livestock and poultry farming due to their broad antibacterial spectrum, strong bactericidal activity, and wide distribution in the body. Enrofloxacin, as a representative of the third-generation fluoroquinolones, exhibits good antibacterial activity against Gram-negative bacteria and some Gram-positive bacteria, and is widely used for the prevention and treatment of mastitis, respiratory infections, and digestive diseases in dairy cows. However, enrofloxacin has a long metabolic cycle in animals, and after entering the human body through the food chain, it may disrupt the balance of intestinal flora, induce the spread and expression of bacterial resistance genes, and cause allergic reactions such as rashes and phototoxicity in some individuals. Therefore, developing efficient and economical technologies for removing enrofloxacin residues from milk is of great significance for ensuring the safety of dairy products and reducing the antibiotic load on the environment.

[0003] Currently, the main methods for treating antibiotic residues in milk include heat inactivation, membrane separation, and enzymatic degradation. Heating is simple to operate, but may affect the natural conformation of milk proteins and the flavor of dairy products. Membrane separation has high retention efficiency, but it requires high selectivity and flux of the membrane material and has high operating costs. Enzymatic degradation has mild reaction conditions, but the stability of the enzyme is greatly affected by factors such as pH and temperature, and the cost of enzyme preparations is relatively high. Adsorption is considered a more promising method for residue removal due to its advantages such as mild operating conditions, no introduction of byproducts, and recyclable adsorbents. The key to adsorption lies in the design of the adsorbent material; an ideal adsorbent should possess high adsorption capacity, rapid adsorption kinetics, good selectivity, and convenient recovery performance.

[0004] Metal-organic frameworks (MOFs) are crystalline porous materials assembled from metal ions or metal clusters and organic ligands through coordination bonds. They possess structural characteristics such as high specific surface area, tunable pore size, and diverse framework composition. In antibiotic adsorption, the open metal sites of MOFs can interact with functional groups such as carboxyl, carbonyl, and amino groups in antibiotic molecules through coordination, hydrogen bonding, and π-π stacking, thereby achieving effective enrichment of target molecules. The UiO-66 series of MOFs uses zirconium oxide clusters as secondary structural units, constructed with terephthalic acid or substituted terephthalic acid ligands. Their significant characteristics include good water resistance and high thermal stability, and they are not prone to framework collapse in aqueous environments. Introducing amino-functionalized 2-aminoterephthalic acid as a ligand, UiO-66-NH2 retains high stability while additionally providing a -NH2 group with hydrogen bond donor-acceptor capabilities, which enhances the adsorption affinity for antibiotic molecules containing polar groups.

[0005] However, MOF particles, ranging in size from nanometers to micrometers, are difficult to recover quickly from liquid systems using conventional filtration or centrifugation, limiting the recycling efficiency of the adsorbent. Introducing magnetic nanoparticles into MOF composite systems can endow the materials with magnetic response properties. Fe3O4 nanoparticles possess advantages such as superparamagnetism, good biocompatibility, and mature preparation processes. They can achieve rapid solid-liquid separation under an applied magnetic field and are easily redispersed after the magnetic field is removed.

[0006] Deep eutectic solvents (DES), as a new type of green solvent, are formed by mixing hydrogen bond donors and hydrogen bond acceptors in a certain molar ratio and then bonding them through hydrogen bonding. They have characteristics such as low melting point, good thermal stability, low vapor pressure, non-flammability, and biodegradability.

[0007] Molecular imprinting is an effective method for constructing specific recognition sites. Using the target molecule as a template, functional monomers and template molecules are pre-assembled via non-covalent or covalent bonds before polymerization. After cross-linking polymerization, the template molecule is immobilized in the polymer network. After template elution, vacancies complementary to the template molecule in spatial structure and chemical functional groups are left in the polymer matrix. These vacancies can selectively recognize and recombine template molecules and their structural analogs from complex samples. Introducing a molecularly imprinted layer onto the surface of MOF composite materials can leverage the high specific surface area of ​​MOFs, providing multiple adsorption sites, while also improving the specificity of target molecule recognition through imprinted vacancies and reducing interference from coexisting matrix components.

[0008] CN115368498A discloses the introduction of DES as a functional monomer into a magnetic MOF molecular imprinting system. However, the DES is only used as a functional monomer, and the MOF support is still synthesized under high pressure using the traditional DMF (N,N-dimethylformamide) solvothermal method, which does not fundamentally solve the safety issues of using toxic organic solvents and high-pressure operation. Furthermore, the use of thermally initiated polymerization has limitations such as high energy consumption, long cycle time, and poor controllability. In addition, the template molecule of this method is benzylamine hydrochloride, and the application target is drug residues in the aquatic environment; the selective adsorption of fluoroquinolone antibiotics in complex food matrices such as milk is still lacking research.

[0009] CN118122279A discloses the application of magnetic MOF composite materials in the adsorption and removal of pollutants in water. However, this patent application mainly protects the use of magnetic MOF materials in drug adsorption. The structural design and preparation methods of the materials themselves are disclosed in a relatively brief manner, without mentioning the selective recognition ability of specific target molecules. Its application in complex matrices (such as dairy products) lacks research. Moreover, the patent does not mention the use of green synthesis methods such as eutectic solvents (DES), and the preparation of its magnetic MOF materials still relies on traditional DMF solvents, which is inconsistent with the development direction of green chemistry.

[0010] Against this backdrop, there is an urgent need to find a selective adsorption material that can remove enrofloxacin from milk more efficiently, safely, and reusably without the use of DMF solvent, thus providing a greener and more feasible technical approach for the removal of enrofloxacin from dairy products. Summary of the Invention

[0011] To address the aforementioned problems, this invention provides a magnetic molecular MOF composite material, its preparation method, and its applications. This composite material uses Fe3O4 nanoparticles as the magnetic core, forms a polydopamine (PDA) interlayer through dopamine self-polymerization, and uses choline chloride-acetamide eutectic solvent (DES) as a green reaction medium to grow a UiO-66-NH2 shell layer in situ under ambient pressure, thus preparing a core-shell structure Fe3O4@PDA@UiO-66-NH2 support. Using enrofloxacin as a template molecule, itaconic acid as a functional monomer, and pentaerythritol triacrylate as a crosslinking agent, a molecularly imprinted polymer (MIP@Fe3O4@PDA@UiO-66-NH2) is prepared through photo-initiated polymerization. This material exhibits superparamagnetism and can be rapidly separated under an applied magnetic field. Imprinted holes endow it with specific recognition ability for enrofloxacin, with an imprinting factor of 1.30 and a selectivity coefficient of 1.29. This material can achieve a removal rate of 80.6%~98.2% for enrofloxacin in milk. The preparation process of this invention requires no high pressure or toxic organic solvents, is simple to operate, and has good application prospects in the field of selective adsorption and removal of antibiotic residues in food.

[0012] On one hand, the present invention provides a magnetic molecularly imprinted MOF composite material for selectively adsorbing enrofloxacin, having a core-shell structure, including a magnetic nanoparticle core and a metal-organic framework shell layer encapsulating the surface of the magnetic nanoparticle core; the surface of the metal-organic framework shell layer is further provided with a molecularly imprinted polymer layer; the molecularly imprinted polymer layer contains three-dimensional imprinted cavities of enrofloxacin; the metal-organic framework shell layer is prepared based on a eutectic solvent.

[0013] The classic synthetic route for metal-organic framework shells (such as UiO-66-NH2) uses DMF as a solvent and carries out a solvothermal reaction in a high-pressure reactor at 120 °C. DMF has a certain degree of toxicity, and its large-scale use is inconsistent with the development direction of green chemistry. Furthermore, high-pressure operation also places additional requirements on equipment safety.

[0014] Eutectic solvents (DES), as a novel green solvent, are formed by hydrogen bonding through the mixing of hydrogen bond donors and acceptors in a certain molar ratio. They possess properties such as low melting point, good thermal stability, low vapor pressure, non-flammability, and biodegradability. Introducing DES into the preparation process of magnetic MOF composites holds promise for achieving a simpler and more environmentally friendly synthetic route.

[0015] This invention replaces the traditional toxic solvent DMF with a eutectic solvent (DES) and successfully synthesizes MOF shells under normal pressure conditions. This not only avoids the safety hazards of high-pressure operation and the environmental pollution of organic solvents, but also allows DES to be recycled due to its low vapor pressure, which is in line with the concept of green chemistry.

[0016] Meanwhile, the composite material provided by this invention possesses a multi-layered composite structure of magnetic nanoparticle core-MOF shell-molecular imprinted layer, bringing synergistic advantages: First, the magnetic core endows the material with excellent superparamagnetism, enabling rapid solid-liquid separation under an applied magnetic field, solving the engineering problem of the difficulty in recovering traditional MOF powder; second, the high specific surface area and other characteristics of MOF enable effective enrichment of target molecules; finally, the surface molecular imprinted layer constructs three-dimensional imprinted cavities that are complementary to the target molecules in terms of spatial structure and chemical functional groups through photo-initiated polymerization, endowing the material with the specific recognition ability of target molecules and effectively reducing the competitive interference of coexisting components in complex milk matrices. The multi-layered structure performs its respective functions and works synergistically to achieve the functional integration of "convenience of magnetic separation - high specific surface area of ​​MOF - high selectivity of imprinting".

[0017] Furthermore, the eutectic solvent is composed of a hydrogen bond donor and a hydrogen bond acceptor; the hydrogen bond acceptor is choline chloride, and the hydrogen bond donor is acetamide.

[0018] The eutectic solvent (DES) composed of choline chloride as the hydrogen bond acceptor and acetamide as the hydrogen bond donor has multiple synergistic advantages: First, the choline chloride-acetamide system can form a homogeneous and transparent liquid at 80°C, with a melting point much lower than the individual melting points of each component, and a moderate viscosity, which is conducive to the full dissolution of ZrCl4 and 2-aminoterephthalic acid and the uniform nucleation and growth of UiO-66-NH2 crystals; Second, the DES has extremely low vapor pressure, is non-flammable, and biodegradable, fundamentally eliminating the high toxicity and high-pressure safety hazards of the traditional DMF solvothermal method, and realizing the green synthesis of MOF shells under normal pressure and 120°C conditions; Third, the rich hydrogen bond network in the DES system can gently control the growth direction and size of MOF crystals, avoiding agglomeration or structural defects caused by excessively rapid crystal growth, and ensuring the continuity and crystallinity of the shell; Finally, the DES can be recycled and reused after simple treatment, further reducing the preparation cost and environmental impact, meeting the needs of large-scale applications.

[0019] Furthermore, the molar ratio of choline chloride to acetamide is 1:2.

[0020] This invention strictly controls the molar ratio of choline chloride to acetamide at 1:2, which is a key parameter for achieving optimal performance of the DES system. This ratio is the optimal proportion for the choline chloride-acetamide system to form a minimum eutectic point, maximally reducing the melting point of the system. A transparent and homogeneous liquid phase can be formed at 80°C, exhibiting good thermal stability and suitable viscosity. This ensures sufficient dissolution of ZrCl4 and the 2-aminoterephthalic acid precursor, while providing a mild and uniform chemical microenvironment for the heterogeneous nucleation and growth of UiO-66-NH2 crystals. Simultaneously, the optimal hydrogen bond network formed between the hydrogen bond donor (acetamide) and hydrogen bond acceptor (choline chloride) in the DES at this ratio can effectively address the Zr... 4+ The coordination process was appropriately controlled to effectively avoid incomplete coating or crystal agglomeration caused by excessively rapid crystal growth, ensuring continuous, dense, and uniform growth of the MOF shell on the PDA-modified Fe3O4 surface. Furthermore, the 1:2 ratio imparts suitable polarity to DES, facilitating complete solvent removal via water or alcohol washing after the reaction, thus preventing residual solvent from interfering with subsequent molecularly imprinted polymerization and adsorption performance. Deviations from this ratio will lead to increased melting point, increased viscosity, or hydrogen bond network imbalance in DES, thereby affecting the crystallinity and coating effect of the MOF shell.

[0021] Furthermore, the magnetic nanoparticles are Fe3O4 nanoparticles, and the metal-organic framework shell is UiO-66-NH2.

[0022] Furthermore, a polymer interlayer is also included between the Fe3O4 nanoparticles and the metal-organic framework shell, preferably a polydopamine layer.

[0023] The surface of Fe3O4 alone lacks active sites that match the nucleation of MOF. When producing MOF directly in the DES system, there are often problems such as uneven growth of MOF crystals, incomplete coating or low loading. Therefore, it is necessary to introduce an interface modification layer between Fe3O4 and MOF.

[0024] Polydopamine (PDA), a biomimetic adhesive polymer, can be obtained by the self-polymerization of dopamine hydrochloride under weakly alkaline and aerobic conditions. The PDA molecular chain contains abundant phenolic hydroxyl, amino, and imine groups, which can form strong bonds with various inorganic and organic surfaces through hydrogen bonding, coordination interactions, or covalent bonds. Experiments have shown that, compared with unmodified Fe3O4, the Fe3O4@PDA@MOF composite material exhibits significantly improved MOF shell continuity and coverage.

[0025] The present invention introduces polydopamine (PDA) as a polymer intermediate layer between the Fe3O4 magnetic core and the UiO-66-NH2 shell. This is the key to the synthesis of the UiO-66-NH2 shell in the eutectic solvent (DES) reaction system, and it is also the key to the high-quality core-shell structure of the composite material and its ability to efficiently adsorb enrofloxacin.

[0026] Firstly, the exposed Fe3O4 nanoparticles lack active nucleation sites that match the UiO-66-NH2 crystals, often leading to uneven MOF crystal growth, low loading, or even isolated nucleation during direct composite formation. PDA molecular chains are rich in catechol groups and amino groups, which can effectively anchor Zr through chelation. 4+ Ions form high-density nucleation sites on the surface of the PDA layer, thereby inducing UiO-66-NH2 to grow in situ, uniformly and continuously on the surface of the magnetic core in the presence of DES, ensuring the complete coverage of the shell and structural stability.

[0027] Secondly, the PDA coating significantly improves the dispersion stability of Fe3O4 nanoparticles in the DES system, effectively avoiding the agglomeration and precipitation of magnetic cores, and ensuring that the surface of each magnetic core can be uniformly contacted with the precursor solution during MOF synthesis, thereby achieving uniform and controllable shell thickness.

[0028] Third, PDA has biomimetic adhesion properties, which can firmly bind to the Fe3O4 surface through various non-covalent forces such as hydrogen bonding, coordination, and π-π stacking. At the same time, the active functional groups on its surface can form stable connections with the MOF framework, acting as a "molecular glue" bridge to ensure the structural integrity of the composite structure in subsequent molecular imprinting polymerization and adsorption applications, and prevent shell detachment.

[0029] Fourth, the PDA layer itself is rich in π-electron systems and polar functional groups, which can produce a pre-enrichment effect on enrofloxacin molecules through π-π stacking and hydrogen bonding, forming a synergistic recognition mechanism with surface imprinted holes, which is beneficial to improving adsorption capacity and selectivity.

[0030] In summary, the polydopamine (PDA) interlayer, acting as a "molecular glue," not only improves the dispersion stability of Fe3O4 but also chelates Zr through its catechol groups. 4+ The ions provide heterogeneous nucleation sites for UiO-66-NH2, ensuring the continuous and uniform growth of the MOF shell on the magnetic core surface in the DES system; they can also form a synergistic recognition mechanism with surface imprinted holes, improving the adsorption capacity and selectivity of enrofloxacin.

[0031] Furthermore, the functional monomer used in the molecular imprinting polymerization is itaconic acid, and the crosslinking agent used is pentaerythritol triacrylate.

[0032] The use of itaconic acid as a functional monomer and pentaerythritol triacrylate as a crosslinking agent to prepare the molecularly imprinted polymer layer is a key synergistic design for the efficient recognition of enrofloxacin in this molecularly imprinted system. Studies have shown that magnetic molecularly imprinted MOF composite materials prepared using eutectic solvents, combined with itaconic acid as a functional monomer and pentaerythritol triacrylate as a crosslinking agent to prepare the molecularly imprinted polymer layer, can more effectively improve the selective adsorption of enrofloxacin in milk.

[0033] Furthermore, the composite material exhibits superparamagnetism with a saturation magnetization of 40-55 emu / g; and / or, the BET specific surface area of ​​the composite material is 20-50 m². 2 / g.

[0034] Furthermore, the composite material has an imprinting factor ≥1.2 and a selectivity coefficient ≥1.2 for enrofloxacin.

[0035] On the other hand, the present invention provides a method for preparing the magnetic molecularly imprinted composite material as described above, wherein the preparation method uses a screened and determined eutectic solvent as the sole reaction medium, and includes the following steps: (1) Provide magnetic nanoparticles; (2) A polymer intermediate layer is coated on the surface of magnetic nanoparticles to obtain a magnetic nanoparticle core; (3) Using a eutectic solvent as the reaction medium, a metal-organic framework shell is grown in situ on the surface of the magnetic nanoparticle core to obtain a magnetic core-shell metal-organic framework composite material. (4) Using enrofloxacin as a template, molecular imprinting polymerization was carried out on the surface of the magnetic core-shell metal-organic framework composite material to form a molecular imprinted polymer layer. After the template molecules were washed off, the magnetic molecular imprinted composite material was obtained.

[0036] Further, in step (2), the polymer intermediate layer is a polydopamine layer, which is formed by the self-polymerization of dopamine on the surface of the magnetic nanoparticles under weakly alkaline conditions.

[0037] In some embodiments, this invention uses Fe3O4 nanoparticles as the magnetic core, PDA as the interfacial adhesion layer, and choline chloride-acetamide DES as the green reaction medium to prepare Fe3O4@PDA@UiO-66-NH2 magnetic core-shell composite material under normal pressure. Using this composite material as a carrier and enrofloxacin as a template molecule, a molecularly imprinted polymer is prepared by photoinitiated surface imprinting polymerization.

[0038] Further, in step (3), the metal-organic framework shell is grown in situ under normal pressure and 100-140°C; preferably, the reaction temperature is 120°C.

[0039] Further, in step (4), the functional monomer used in the molecular imprinting polymerization is itaconic acid, and the crosslinking agent used is pentaerythritol triacrylate; the molecular imprinting polymerization adopts photoinitiated polymerization; preferably, the light source for the photoinitiated polymerization is an LED light source; more preferably, the wavelength of the LED light source is 450nm.

[0040] In some embodiments, this invention uses Fe3O4 nanoparticles prepared by a solvothermal method as the magnetic core, forms a polydopamine (PDA) interlayer through room-temperature self-polymerization of dopamine, and uses choline chloride-acetamide eutectic solvent (DES) as a green reaction medium to grow a UiO-66-NH2 shell in situ at 120°C under ambient pressure, thus preparing a core-shell structured Fe3O4@PDA@UiO-66-NH2 magnetic composite material. Based on this, using enrofloxacin as a template molecule, itaconic acid as a functional monomer, and pentaerythritol triacrylate as a crosslinking agent, polymerization is initiated under 450nm LED illumination to prepare a magnetic molecularly imprinted composite material (MIP@Fe3O4@PDA@UiO-66-NH2).

[0041] In several methods, X-ray diffraction (XRD), X-ray photoelectron spectroscopy (XPS), scanning electron microscopy (SEM), specific surface area analysis (BET), and vibrating sample magnetometer (VSM) were used to characterize the structure, composition, specific surface area, and magnetic properties of the magnetic molecularly imprinted composite material. The structure and physicochemical properties of the magnetic molecularly imprinted composite material were analyzed using various characterization techniques, and the adsorption kinetics, isotherms, and selectivity of enrofloxacin were investigated. The results showed that the molecularly imprinted material retained the Fe3O4 crystal phase and the characteristic diffraction peaks of UiO-66-NH2, and the BET specific surface area was 32.73 m². 2The saturation magnetization was 46.9 emu / g. XPS analysis confirmed the introduction of the PDA layer and the UiO-66-NH2 shell. Selective adsorption experiments showed that the molecularly imprinted material adsorbed more enrofloxacin than the non-imprinted material, with an imprinting factor (IF) of 1.30 and a selectivity coefficient (SC) of 1.29. Adsorption kinetics and isotherm studies indicated that the adsorption process conformed to the pseudo-second-order kinetic model and the Freundlich isotherm model. This material shows promising application potential in the selective adsorption and removal of fluoroquinolone antibiotic residues in milk.

[0042] In another aspect, the present invention provides the application of choline chloride-acetamide eutectic solvent in the preparation of the magnetic molecularly imprinted composite material as described above, wherein the choline chloride-acetamide eutectic solvent serves as a reaction medium for in-situ growth of a metal-organic framework shell on the surface of a magnetic polymer core under normal pressure; the magnetic molecularly imprinted composite material is used for selective adsorption and removal of enrofloxacin from dairy products.

[0043] In another aspect, the present invention provides the application of the magnetic molecularly imprinted MOF composite material or the magnetic molecularly imprinted composite material prepared by the method described above in the selective adsorption and removal of antibiotics.

[0044] Furthermore, the antibiotic is a fluoroquinolone antibiotic; preferably, the fluoroquinolone antibiotic is enrofloxacin.

[0045] Furthermore, the application is to selectively adsorb and remove fluoroquinolone antibiotic residues in dairy products; preferably, the dairy product is milk.

[0046] The beneficial effects of this invention include: 1. By using a eutectic solvent as the sole reaction medium, UiO-66-NH2 shells are grown in situ on the Fe3O4 surface under normal pressure, completely replacing the traditional DMF solvothermal method. This fundamentally eliminates the safety hazards of using highly toxic organic solvents and high-pressure operation, aligning with the development direction of green chemistry.

[0047] 2. Choline chloride-acetamide was selected as the eutectic solvent to ensure the synthesis effect of the UiO-66-NH2 shell and to guarantee the composite material's ability to remove enrofloxacin from milk.

[0048] 3. Using polydopamine (PDA) as the core-shell intermediate layer not only improves the dispersion stability of Fe3O4, but also chelates Zr through its catechol groups. 4+ The ions provide heterogeneous nucleation sites for UiO-66-NH2, ensuring the continuous and uniform growth of the MOF shell on the magnetic core surface in the DES system; they can also form a synergistic recognition mechanism with surface imprinted holes, improving the adsorption capacity and selectivity of enrofloxacin.

[0049] 4. Itaconic acid was selected as the functional monomer and pentaerythritol triacrylate as the crosslinking agent to prepare the molecularly imprinted polymer layer. The imprinting factor (IF) for enrofloxacin was 1.30 and the selectivity coefficient (SC) was 1.29, which effectively improved the selective adsorption effect of enrofloxacin in milk.

[0050] 5. Polymerization is initiated by 450nm LED illumination, and the polymerization time is only 40 minutes (20 minutes of illumination + 5 minutes of rest + 20 minutes of illumination). It has low energy consumption, short cycle, and simple operation, making it more suitable for large-scale production.

[0051] 6. A four-layer core-shell structure consisting of "Fe3O4 magnetic core - PDA intermediate layer - UiO-66-NH2 shell layer - molecular imprinted layer" was constructed. Each of the four layers performs its own function and works synergistically to achieve the functional integration of convenient magnetic separation, high specific surface area of ​​MOF, and high selectivity of imprinting.

[0052] 7. The prepared composite material exhibits superparamagnetism, with a saturation magnetization of 46.9 emu / g and a BET specific surface area of ​​32.73 m². 2 / g, the adsorption kinetics conform to the pseudo-second-order model (Rg). 2 =0.990), the isotherm conforms to the Freundlich model (R² = 0.990). 2 =0.972), the removal rate of enrofloxacin in milk can reach 80.6%~98.2%.

[0053] In summary, this invention provides a green preparation method that does not require DMF or high-pressure operation throughout the entire process. The resulting magnetic molecularly imprinted MOF composite material has high selective recognition ability, rapid magnetic separation performance and good applicability to practical samples, and has broad application prospects in the selective adsorption and removal of fluoroquinolone antibiotic residues in dairy products. Attached Figure Description

[0054] Figure 1 Figure 1 shows the XRD patterns of the MIP in Example 1. Figure 1a shows the XRD pattern of the MIP when the diffraction angle is 0-10°; Figure 1b shows the XRD pattern of the MIP when the diffraction angle is 10-80°. Figure 2 XPS spectra before and after the MIP imprint in Example 1; Figure 3 The SEM and EDS spectra are from Example 1; Figure 4 The MIP hysteresis loop in Example 1; Figure 5 The BET specific surface area of ​​the composite material in Example 1; where a is before imprinting; b is after imprinting; Figure 6 The results are the adsorption kinetics experimental results from Example 1; where a is the adsorption amount-time curve; b is the pseudo-first-order kinetic fit; and c is the pseudo-second-order kinetic fit. Figure 7 The adsorption isotherms are shown in Example 1; where a is the Langmuir model and b is the Freundlich model. Figure 8 The infrared spectrum of the Fe3O4@PDA@UiO-66-NH2 composite material in Example 2 is shown; where (a) is the menthol-pyruvic acid DES system (1:1) and (b) is the choline chloride-ethylene glycol DES system (1:2). Figure 9 Infrared spectrum of Fe3O4@PDA@UiO-66-NH2 composite material in Example 2: choline chloride: acetamide (1:2). Detailed Implementation

[0055] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments. These embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Unless otherwise specified, the materials and reagents used in the following embodiments are commercially available.

[0056] Example 1: Preparation of Magnetic Molecular MOF Composite Materials I. Reagents and Instruments The reagents were: iron(II,III) oxide (Fe3O4), tris(II,III) aminomethane (Tris), dopamine hydrochloride, zirconium tetrachloride (ZrCl4), 2-aminoterephthalic acid, choline chloride, acetamide, enrofloxacin (purity ≥98%), norfloxacin (purity ≥98%), itaconic acid, pentaerythritol triacrylate (PETA), and diphenylphosphine oxide (DPPO); methanol, acetonitrile, and ethanol were all of chromatographic grade. All reagents were purchased from Sinopharm Chemical Reagent Co., Ltd.

[0057] An X-ray diffractometer (XRD, Haoyuan Company) was used for phase analysis; an X-ray photoelectron spectroscopy (XPS, ThermoFisher Scientific Nexsa, USA) was used for surface elemental composition and chemical state analysis; a scanning electron microscope (SEM, Zeiss) equipped with an energy-dispersive X-ray spectrometer (EDS, Oxford Xplore 30) was used for morphological observation and micro-area elemental analysis. A surface area and pore size analyzer (NovaWin, Quantachrome) was used for N2 adsorption-desorption testing; a vibrating sample magnetometer (VSM, Lake Shore 8604, USA) was used for magnetic property testing; and a high-performance liquid chromatograph (HPLC, Agilent Technologies) equipped with an ultraviolet detector was used for quantitative analysis of enrofloxacin concentration in the adsorption experimental solution.

[0058] II. Preparation of Magnetic Molecular MOF Composite Materials 1. Preparation of eutectic solvents Choline chloride and acetamide were mixed at a molar ratio of 1:2 and magnetically stirred in an 80°C water bath for 2 hours to obtain a transparent and homogeneous liquid, DES, which was then placed in a desiccator for later use.

[0059] 2. Synthesis of Fe3O4@PDA core-shell particles 150 mg Fe3O4 was dispersed in 180 mL Tris-HCl buffer (pH 8.5, 10 mmol / L) and sonicated for 15 min. Then, 150 mg dopamine hydrochloride was added, and the mixture was mechanically stirred at room temperature for 6 h. Dopamine hydrochloride self-polymerized on the Fe3O4 surface to form a polydopamine layer (PDA). After magnetic separation, the product was washed three times with water and freeze-dried for 24 h to obtain Fe3O4@PDA.

[0060] 3. Synthesis of Fe3O4@PDA@UiO-66-NH2 composite material 0.63 g ZrCl4 and 0.62 g 2-aminoterephthalic acid were dissolved in 25 mL DES, and 0.1 g Fe3O4@PDA was added. The mixture was ultrasonically dispersed for 10 min. The mixture was transferred to a glass sample vial and reacted in a 120°C oven at ambient pressure for 12 h. The product was washed successively with ethanol and water, magnetically separated, and then freeze-dried to obtain Fe3O4@PDA@UiO-66-NH2.

[0061] 4. Preparation of molecularly imprinted polymers Using enrofloxacin as a template molecule and itaconic acid as a functional monomer, surface molecularly imprinted polymers (MIPs) were prepared by photoinitiated polymerization: 0.05 g of enrofloxacin and 0.2 g of itaconic acid were dissolved in 10 mL of acetonitrile and mechanically stirred at room temperature for 5 h for pre-assembly. Fe3O4@PDA@UiO-66-NH2 was added and ultrasonically dispersed for 15 min. 0.05 g of pentaerythritol triacrylate (a crosslinking agent) and 0.1 g of diphenylphosphine oxide (a photoinitiator) were added, and after nitrogen purging for 10 min to remove oxygen, polymerization was carried out under 450 nm LED illumination (20 min irradiation, 5 min pause, 20 min irradiation). The product was collected by magnetic separation, and the template molecule was eluted with methanol:acetonitrile (9:1, v / v) until enrofloxacin was undetectable in the supernatant, thus obtaining the MIP.

[0062] The steps for non-imprinted polymers (NIPs) are the same except that no template molecules are added.

[0063] II. Characterization of Magnetic Molecular MOF Composites 1. XRD Analysis Figure 1The XRD (X-ray diffraction) pattern of the MIP shows that the sample exhibits characteristic diffraction peaks of Fe3O4 at 2θ = 30.1°, 35.5°, 43.1°, 53.4°, 57.0° and 62.6°, corresponding to the (220), (311), (400), (422), (511) and (440) crystal planes, indicating that the Fe3O4 magnetic core maintained the spinel structure during PDA coating, UiO-66-NH2 growth and molecular imprinting.

[0064] The Fe3O4@PDA@UiO-66-NH2 exhibits new diffraction peaks at 2θ = 7.4° and 8.5°, corresponding to the (111) and (200) crystal planes of UiO-66-NH2, respectively, confirming the successful loading of the UiO-66-NH2 shell. The characteristic peaks of UiO-66-NH2 in the MIP sample still exist, although their intensity is slightly reduced, and their positions have not shifted, indicating that the molecular imprinting process has not altered the crystal structure of UiO-66-NH2.

[0065] 2. XPS Analysis XPS (X-ray photoelectron spectroscopy) full spectrum analysis ( Figure 2 The results showed that the surface of the unimprinted sample contained characteristic peaks of C 1s, N 1s, O 1s, Fe 2p, and Zr 3d. The imprinted sample showed a new F 1s peak (approximately 685 eV), originating from fluorine atoms in the enrofloxacin molecule, indicating that the template molecule had been successfully embedded into the polymer matrix.

[0066] Semi-quantitative analysis results (Table 1) showed that after imprinting, the C content decreased from 65.25 at% to 54.51 at%, the O content increased from 23.84 at% to 32.30 at%, the Fe content increased from 2.02 at% to 5.39 at%, and the F content was 0.79 at. Zr was not detected after imprinting, which may be related to the coverage of the surface imprint layer.

[0067] Table 1. XPS elemental content (at%) before and after MIP imprinting

[0068] 3. SEM and EDS analysis EDS energy dispersive spectroscopy ( Figure 3 The results confirmed that the material contains elements such as C, O, Fe, and Si. The Zr signal is weak, which is consistent with the XPS results. It is speculated that this is due to the thin UiO-66-NH2 shell.

[0069] 4. VSM Analysis hysteresis loop ( Figure 4The results show that the coercivity of the MIP material is close to zero, exhibiting superparamagnetic characteristics, with a saturation magnetization of 46.9 emu / g. This is lower than that of pure Fe3O4, attributed to the introduction of the non-magnetic PDA layer, the UiO-66-NH2 shell, and the imprinted polymer layer. This magnetization is sufficient to meet the requirements for rapid separation under an applied magnetic field.

[0070] 5. BET Analysis N2 adsorption-desorption isotherm ( Figure 5 The sample exhibits type IV hysteresis loops, with H3-type hysteresis rings appearing in the P / P0 = 0.4~1.0 range, a typical characteristic of mesoporous materials. The BET specific surface area of ​​the unimprinted sample is 12.98 m². 2 / g, increased to 32.73 m after imprinting. 2 / g (Table 2), the increase in specific surface area is attributed to the introduction of imprinted holes. Compared with other MOFs of this type in other literature, its lower specific surface area may be related to the limited growth of MOF crystals in the DES system and the coverage of the pores by the PDA layer.

[0071] Table 2. BET specific surface area and pore structure parameters of materials

[0072] 6. HPLC Quantitative Method for Enrofloxacin The Symmetry C8 column (4.6×150 mm, 5 μm) was used. The mobile phase was 0.025 mmol / L phosphoric acid aqueous solution (adjusted to pH=3 with triethylamine)-acetonitrile-methanol (volume ratio 80:15:5). The column flow rate was 1.0 mL / min, the detection wavelength was 285 nm, the column temperature was 30 ℃, and the injection volume was 20 μL.

[0073] The standard curve regression equation is: y = 27736x + 7097.5 (R²) 2 = 0.999), the limit of detection (LOD) was 0.104 μg / mL, and the limit of quantitation (LOQ) was 0.316 μg / mL.

[0074] 7. Adsorption Experiment Adsorption kinetics experiment: 20 mg of MIP or NIP was placed in a centrifuge tube, and 4 mL of enrofloxacin aqueous solution (10 μg / mL) was added. The mixture was shaken at room temperature. After magnetic separation at preset time points (1, 5, 7, 10, 12, 30, 60 min), the supernatant was collected, and the residual concentration was determined by HPLC. The adsorption amount was calculated according to formula (1): q t =(C0-C t Equation (1) is: ) × V / m Where q t The adsorption amount at time t (mg / g), C0 and Ct The initial and time t values ​​are (μg / mL), respectively; V is the solution volume (mL); and m is the material mass (mg).

[0075] Adsorption isotherm experiment: Take 20 mg of MIP or NIP and add 4 mL of enrofloxacin solution with different initial concentrations (5, 10, 25, 50, 100 μg / mL). Shake at room temperature for 12 min, and measure the concentration of the supernatant after magnetic separation. The equilibrium adsorption capacity is calculated according to formula (2): q e =(C0-C e Equation (2) is: ) × V / m Where, q e To achieve equilibrium adsorption capacity (mg / g), C e C0 is the equilibrium concentration (μg / mL), V is the initial concentration (μg / mL), m is the solution volume (mL), and m is the material mass (mg).

[0076] Selectivity experiment: Take 20 mg of MIP and NIP respectively, add 4 mL of enrofloxacin or norfloxacin solution (concentration of 10 μg / mL), shake at room temperature for 12 min, and measure the concentration of the supernatant. The imprinting factor (IF) and selectivity coefficient (SC) are calculated according to equations (3) and (4) respectively: IF = Q MIP / Q NIP (3) SC =IF 恩诺沙星 / IF 诺氟沙星 (4) in, and The adsorption amounts of the target analyte by MIP and NIP are respectively. and These are the imprinting factors for enrofloxacin and norfloxacin, respectively.

[0077] 8. Adsorption kinetics The effect of contact time on adsorption capacity was investigated under the conditions of 10 μg / mL enrofloxacin aqueous solution, 20 mg MIP or NIP, 4 mL solution volume, and room temperature. The results are as follows: Figure 6As shown in Figure a, the adsorption capacity of MIP increased with time: 0.15 mg / g at 1 min, 0.32 mg / g at 5 min, 1.60 mg / g at 7 min, 1.65 mg / g at 10 min, and 1.98 mg / g at 12 min, after which it remained essentially constant (1.99 mg / g at 60 min). The adsorption equilibrium time was approximately 12 min. The adsorption capacity of NIP was lower than that of MIP at all time points, with 1.69 mg / g at 12 min and 1.61 mg / g at 60 min.

[0078] The MIP adsorption data were fitted using pseudo-first-order and pseudo-second-order kinetic models. The pseudo-first-order model expression is ln(q e - q t ) = ln q e - k1t, the quasi-second-order model expression is t / q t = 1 / (k2q e 2 ) + t / q e Fitting results ( Figure 6 b、 Figure 6 c and Table 3 show the correlation coefficient (R²) of the quasi-secondary model to the MIP data. 2 = 0.990) is higher than the first-tier (R 2 =0.938), and the equilibrium adsorption capacity calculated by the pseudo-second-order model (2.03 mg / g) is close to the experimental value (1.99 mg / g). These results indicate that the adsorption of enrofloxacin by MIP is primarily chemisorption, and the adsorption rate is controlled by the chemical bonding between the adsorbent and adsorbate (such as hydrogen bonding and π-π stacking). This result is consistent with the specific recognition mechanism of molecularly imprinted materials—multi-site synergistic chemical interactions exist between the functional groups in the imprinted cavity and the target molecule.

[0079] Table 3. Pseudo-first-order and pseudo-second-order dynamic fitting parameters

[0080] Where, q e exp is the experimental value, q e ,cal is the calculated value.

[0081] 9. Adsorption isotherm The equilibrium adsorption capacities of MIP and NIP were investigated within an initial concentration range of 5–100 μg / mL, and the results are as follows: Figure 7 As shown in Figure a, the adsorption capacity of both materials increases with increasing equilibrium concentration. The data were fitted using Langmuir and Freundlich models. The linear form of the Langmuir model is C0. e / q e = 1 / (K_L Q m ) + C e / Q m The Freundlich model has the linear form ln q e = ln K_F + (1 / n) ln C e .

[0082] The fitting results (Table 4) show that the Freundlich model is suitable for MIP(R) 2 = 0.972) and NIP(R 2 The goodness of fit of the model (= 0.998) is better than that of the Langmuir model (MIP R). 2 = 0.501, NIP R 2 = 0.286), indicating that the adsorption process conforms to the characteristics of multilayer non-uniform adsorption. The K_F value of MIP (6.90) is higher than that of NIP (4.75), indicating that MIP has a stronger adsorption affinity. The 1 / n value of MIP is 0.917, which is between 0.1 and 1.0, indicating that the adsorption process is favorable. The extremely low fit of NIP to the Langmuir model indicates that its surface adsorption site distribution is highly non-uniform and lacks the characteristics of monolayer saturated adsorption, which is consistent with its non-specific adsorption nature.

[0083] Table 4. Fitting parameters for Langmuir and Freundlich isotherms

[0084] 10. Selective adsorption Using norfloxacin as a structural analog, the selective adsorption capacity of MIP and NIP for enrofloxacin and norfloxacin was investigated, and the results are shown in Table 5. The adsorption capacity of MIP for enrofloxacin was 24.00 μg, and that of NIP was 18.50 μg, with an imprinting factor (IF) of 1.30. The adsorption capacity of MIP for norfloxacin was 29.81 μg, and that of NIP was 29.53 μg, with an IF of 1.01. The selectivity coefficient (SC) was 1.29, indicating that MIP has a superior recognition ability for the template molecule enrofloxacin compared to its structural analog norfloxacin.

[0085] It is worth noting that the absolute adsorption amounts of norfloxacin on both MIP and NIP were higher than those of enrofloxacin (MIP: 29.81 μg vs. 24.00 μg; NIP: 29.53 μg vs. 18.50 μg). This is related to the smaller molecular size and higher diffusion rate of norfloxacin, reflecting the difference in non-specific physical adsorption between the two. However, the imprinting factor (IF) better reflects the nature of specific recognition: the IF of MIP for enrofloxacin (1.30) was significantly higher than that of norfloxacin (1.01), indicating that the imprinted holes provided a more significant affinity enhancement for the template molecule enrofloxacin. The SC value greater than 1.0 further confirms the good selectivity of the material for enrofloxacin. This result is consistent with the basic principle of molecular imprinting—the imprinted holes have an optimal match with the template molecule enrofloxacin in terms of shape and functional group arrangement, while the structural analog norfloxacin cannot obtain the same recognition enhancement due to the difference in substituents.

[0086] Table 5. Adsorption capacity of MIP and NIP for enrofloxacin and norfloxacin

[0087] 11. Material stability and reusability All adsorption experiments in this study used the same batch of synthesized MIP material. During the kinetic (7 time points) and isotherm (5 concentration points) tests, the material underwent 12 independent adsorption-magnetic separation-washing operations. In the kinetic data, the adsorption capacity of MIP was 1.98 mg / g at 12 min and 1.99 mg / g at 60 min, which were essentially consistent (relative deviation less than 1%), indicating that the material maintained stable adsorption performance even after 1 hour of oscillation and multiple operations. These results preliminarily suggest that the material possesses good operational stability and reusability potential.

[0088] 12. Analysis of actual milk samples Take 4 mL of milk sample (Yili, skim milk), add four concentrations of enrofloxacin standard solution (0.5, 2.0, 5.0, and 10 μg / mL, respectively), and then determine the removal rate according to the adsorption experiment method described in section 7.

[0089] After adsorption, the milk sample underwent pretreatment before subsequent analysis. Pretreatment included: accurately measuring 4 mL of milk sample and mixing it with 4 mL of 1 mol / L trichloroacetic acid solution. The mixture was thoroughly shaken and centrifuged at 20°C and 10,000 rpm for 5 min. The supernatant was collected and filtered through a 0.22 μm × 25 mm syringe filter. The resulting filtrate was collected for subsequent analysis.

[0090] The experimental results are shown in Table 6. No chromatographic peak was observed at the enrofloxacin retention time in the blank milk sample, indicating that the selected milk matrix did not contain enrofloxacin residue. When the spiked concentrations were 5.0 μg / mL and 10.0 μg / mL, the average removal rates of MIP reached 95.9% (RSD=3.0%) and 98.2% (RSD=5.5%), respectively, indicating that the material exhibited good adsorption performance at high spiked concentrations.

[0091] The removal rates were low at spiked concentrations of 1.0 μg / mL and 0.5 μg / mL, possibly due to the lower mass transfer driving force at low concentrations. Furthermore, the 0.5 μg / mL concentration was close to the method's limit of quantitation (LOQ = 0.316 μg / mL), suggesting that in practical applications, the amount of material used or the sample processing volume should be appropriately increased to improve adsorption efficiency at low concentration levels. These results indicate that MIP has a certain removal capacity for enrofloxacin in milk, especially at concentrations above 5.0 μg / mL, where the adsorption efficiency is very high.

[0092] Table 6. Results of the spiked removal experiment of enrofloxacin in milk by MIP

[0093] Note: ND indicates not detected; the removal rate here is the removal rate of the spiked sample substance by the MIP; the value is expressed as mean ± standard deviation (n=3).

[0094] As can be seen, this embodiment successfully synthesized Fe3O4@PDA@UiO-66-NH2 magnetic MOF composite material under normal pressure using choline chloride-acetamide DES as a green reaction medium. Using this composite material as a carrier, MIP@Fe3O4@PDA@UiO-66-NH2 with selective recognition ability for enrofloxacin was prepared by surface molecular imprinting technology.

[0095] XRD and XPS characterization results confirmed the successful loading of the PDA layer and UiO-66-NH2 shell on the Fe3O4 surface, and the molecular imprinting process did not destroy the crystal structure of the material. BET analysis showed that the specific surface area after imprinting (32.73 m²) was [missing information]. 2 / g) compared to the original imprint (12.98 m) 2 The saturation magnetization ( / g) is significantly increased. VSM tests show that the material exhibits superparamagnetism, with a saturation magnetization of 46.9 emu / g.

[0096] The adsorption kinetic data conform to the pseudo-second-order model (R0). 2 = 0.990), chemisorption is the rate-determining step. The isotherm data conform to the Freundlich model (R² = 0.990). 2= 0.972), and the K_F value of MIP (6.90) was higher than that of NIP (4.75). Selectivity experiments showed that the imprinting factor of MIP for enrofloxacin was 1.30 and the selectivity coefficient was 1.29. The adsorption performance of the same batch of material remained stable after multiple operations.

[0097] Example 2: Screening of Eutectic Solvents 1. Preliminary Experiment To screen suitable eutectic solvent (DES) systems for the green synthesis of magnetic MOF composites, preliminary experiments were conducted before the formal experiments. The synthesis of Fe3O4@PDA core-shell particles, the growth conditions of the UiO-66-NH2 shell, and other operating parameters were kept consistent with Example 1, with only the composition of the DES changed, including the following three groups: 1. Menthol-pyruvic acid (molar ratio 1:1); 2. Choline chloride-ethylene glycol (molar ratio 1:2); 3. Choline chloride-acetamide (molar ratio 1:2) (Example 1).

[0098] ZrCl4 and 2-aminoterephthalic acid were dissolved in two different DES solutions, and an equal amount of Fe3O4@PDA was added. After ultrasonic dispersion, the mixture was reacted at 120 °C under normal pressure for 12 h. The products were washed with ethanol and water, magnetically separated, and freeze-dried. The functional group characteristics of the composite materials obtained under the two conditions were preliminarily characterized by Fourier transform infrared spectroscopy (FTIR) to evaluate the effect of the DES system on the loading effect of the MOF shell.

[0099] To preliminarily evaluate the effect of different DES systems on the loading effect of the UiO-66-NH2 shell on the Fe3O4@PDA surface, the products obtained under the two DES systems were characterized by FTIR, and the results are as follows: Figure 8 As shown.

[0100] Comparison of the infrared spectra of the products from the DES-a and DES-b systems revealed that the DES-a system (menthol: pyruvic acid) sample showed a higher infrared spectrum at 1710 cm⁻¹. -1 A distinct shoulder peak appears nearby, attributed to the stretching vibration (–COOH) of the uncoordinated carboxylic acid C=O. The presence of this signal suggests that some of the 2-aminoterephthalic acid ligands in the menthol:pyruvate DES system may not have been completely deprotonated and reacted with Zr. 4+ Coordination issues lead to low crystallinity or ligand deficiency in the MOF framework. Simultaneously, this sample exhibits low crystallinity at 1250 cm⁻¹. -1 and 1090cm -1 The presence of additional absorption peaks at this point may be related to the C–O–C stretching vibrations of menthol residues or pyruvic acid, suggesting that the DES component was not completely washed away and may remain in the product.

[0101] DES-b system (choline chloride-ethylene glycol) sample at 3300 cm -1 The nearby O–H absorption peaks are relatively broader and stronger, possibly related to the hydrogen bonding and residues of numerous hydroxyl groups in choline chloride and ethylene glycol. This sample shows an absorption peak at 1380 cm⁻¹. -1 The intensity of the carboxylate symmetric stretching vibration peak at 1580 cm⁻¹ is significantly lower than that of the DES-a system, while at 1580 cm⁻¹... -1 The presence of a weak C=C skeletal vibration peak at this location may indicate limited growth of the UiO-66-NH2 skeleton in this DES system. Furthermore, the DES-b sample exhibits a relatively weak C=C skeletal vibration peak at 1040–1080 cm⁻¹. -1 A set of strong absorption peaks appeared within the range, which can be attributed to the bending vibration of C–O–H and the stretching vibration of C–O, indicating that the ethylene glycol component remains in the product in large quantities and is difficult to completely remove by conventional washing.

[0102] The product obtained from the DES-c system (choline chloride-acetamide, molar ratio 1:2) Figure 9 ) at 1380cm -1 A clear and moderately strong symmetric stretching vibration peak of the carboxylate group is observed at 1710 cm⁻¹. -1 No obvious C=O absorption peak of uncoordinated carboxylic acid was observed nearby, indicating that the 2-aminoterephthalic acid ligand was completely deprotonated, and that it was compatible with Zr. 4+ The coordination was adequate, and the UiO-66-NH2 framework was well formed. This sample was sized at 1040–1090 cm⁻¹. -1 The presence of only a weak absorption peak within the range indicates that the DES component (choline chloride / acetamide) was thoroughly removed after ethanol-water washing, resulting in a low residual amount. Furthermore, the sample showed a low absorption peak at 1580 cm⁻¹. -1 The absorption peak (the C=C skeletal vibration of the benzene ring) is clearly identifiable, further confirming that the aromatic ligand was successfully introduced into the skeletal structure.

[0103] In summary, although all three DES systems can induce partial growth of UiO-66-NH2 on the Fe3O4@PDA surface, there are significant differences: the DES-a (menthol:pyruvic acid) system exhibits incomplete ligand coordination (1710 cm⁻¹). -1The DES-b (choline chloride: ethylene glycol) system exhibited the weakest MOF characteristic peak intensity and severe ethylene glycol residue. The DES-c (choline chloride: acetamide) system demonstrated the best ligand coordination efficiency (no uncoordinated carboxylic acid peaks, moderate carboxylate peak intensity) and optimal washability (weakest DES residue peaks), thus it was selected as the primary DES system for the main experiment. This screening result highlights the significant influence of DES composition (especially the type of hydrogen bond donor) on MOF crystal formation and product purity, providing experimental evidence for the controllable synthesis of magnetic MOF composites in green solvent systems.

[0104] Example 3: Screening of polymer intermediate layers This example investigated the effects of different polymer interlayers on the structural integrity and adsorption properties of magnetic molecular MOF composites. The eutectic solvent (DES) system, UiO-66-NH2 shell growth conditions, molecularly imprinted polymerization conditions, and other operating parameters were kept consistent with Example 1, with only the type of interlayer modification on the Fe3O4 nanoparticle surface changed. The following three sets of experiments were conducted: Group 1, No intermediate layer group: Fe3O4 nanoparticles are directly used for in-situ growth of UiO-66-NH2 in the DES system; Group 2, PDA intermediate layer group: Fe3O4 surface coated with polydopamine (PDA) layer (same as Example 1); Group 3, SiO2 Intermediate Layer Group: Fe3O4 surface coated with a silica (SiO2) layer. The SiO2 layer was coated onto the Fe3O4 surface using a sol-gel method: 150 mg Fe3O4 was ultrasonically dispersed in a mixed solution of 80 mL ethanol and 20 mL deionized water, then 1.0 mL ammonia (25 wt%) and 0.5 mL tetraethyl orthosilicate (TEOS) were added, and the mixture was mechanically stirred at room temperature for 6 h. After magnetic separation, the product was washed three times with ethanol and deionized water, and then freeze-dried for 24 h to obtain Fe3O4@SiO2.

[0105] Using Fe3O4@intermediate layer@UiO-66-NH2 with three different intermediate layers as carriers, three sets of magnetic molecular MOF composite materials were prepared according to the same method as in Example 1: MIP@Fe3O4@UiO-66-NH2 (no intermediate layer), MIP@Fe3O4@PDA@UiO-66-NH2 (PDA intermediate layer) and MIP@Fe3O4@SiO2@UiO-66-NH2 (SiO2 intermediate layer).

[0106] The three materials were observed by scanning electron microscopy (SEM), analyzed by X-ray diffraction (XRD), and tested by magnetic properties (VSM). The adsorption experimental conditions were the same as in Example 1: 20 mg of MIP material was added to 4 mL of enrofloxacin solution (10 μg / mL), shaken at room temperature for 12 min, and after magnetic separation, the supernatant was collected. The residual concentration was determined by HPLC, and the equilibrium adsorption capacity q was calculated. e Each experiment was repeated three times, and the results are expressed as mean ± standard deviation.

[0107] SEM observations showed that in the group without an intermediate layer (Fe3O4@UiO-66-NH2), the distribution of UiO-66-NH2 crystals on the Fe3O4 surface was extremely uneven. A large number of MOF crystals nucleated and grew individually in the DES system, rather than being coated on the magnetic core surface, indicating that the exposed Fe3O4 surface lacks active nucleation sites that match the UiO-66-NH2 crystals.

[0108] In the PDA intermediate layer group (Fe3O4@PDA@UiO-66-NH2), the UiO-66-NH2 shell is continuously and uniformly coated on the Fe3O4@PDA surface, with no obvious individual nucleation particles observed. This confirms that the PDA layer chelates Zr through its catechol groups. 4+ The ions provide ample heterogeneous nucleation sites for UiO-66-NH2.

[0109] In the SiO2 intermediate layer group (Fe3O4@SiO2@UiO-66-NH2), UiO-66-NH2 crystals are also coated on the surface of Fe3O4@SiO2 to a certain extent, but the shell uniformity is not as good as that of the PDA group, and MOF crystal agglomeration occurs in some areas.

[0110] Following the method provided in Example 1, the equilibrium adsorption capacity and removal rate of three groups of MIP materials for enrofloxacin in milk (10 μg / mL, 4 mL, 20 mg material, shaken at room temperature for 12 min) are compared as shown in Table 7.

[0111] Table 7. Comparison of the adsorption performance of different intermediate layer MIP materials for enrofloxacin in skim milk.

[0112] Note: Initial concentration 10 μg / mL, solution volume 4 mL, material dosage 20 mg, adsorption time 12 min, n=3.

[0113] The results showed that the PDA interlayer group had significantly better equilibrium adsorption capacity (1.98 mg / g) and removal rate (99.0%) for enrofloxacin than the group without interlayer (0.82 mg / g, 41.0%) and the SiO2 interlayer group (1.21 mg / g, 60.5%). The adsorption capacity of the PDA interlayer group was 2.4 times that of the group without interlayer and 1.6 times that of the SiO2 interlayer group.

[0114] It is evident that PDA is the most effective polymer interlayer between the Fe3O4 magnetic core and the UiO-66-NH2 shell, significantly improving the loading and uniformity of the MOF shell, thereby enhancing the adsorption performance of the composite material for enrofloxacin. Therefore, PDA was selected as the interlayer material in subsequent experiments.

[0115] Example 4: Screening of Molecularly Imprinted Polymer Layers To screen the optimal molecularly imprinted polymer layer composition suitable for the surface of a magnetic core-shell MOF support, while keeping the support (Fe3O4@PDA@UiO-66-NH2), template molecule (enrofloxacin), photoinitiation polymerization conditions, and other operating parameters consistent with Example 1, only the types and combinations of functional monomers and crosslinking agents were changed, and the following three sets of experiments were set up: Group 1 uses methacrylic acid (MAA) as a functional monomer and ethylene glycol dimethacrylate (EGDMA) as a crosslinking agent; Group 2 uses acrylamide (AM) as a functional monomer and N,N'-methylenebisacrylamide (MBAA) as a crosslinking agent; Group 3 uses itaconic acid (IA) as a functional monomer and pentaerythritol triacrylate (PETA) as a crosslinking agent (the same as in Example 1).

[0116] Enrofloxacin (template molecule) and the corresponding functional monomer were dissolved in 10 mL of acetonitrile and pre-assembled by stirring at room temperature for 5 h. 20 mg of Fe3O4@PDA@UiO-66-NH2 support was added, and the mixture was ultrasonically dispersed for 15 min. The corresponding crosslinking agent and photoinitiator diphenylphosphine oxide (DPPO) were added, and after nitrogen purging for 10 min to remove oxygen, polymerization was carried out under 450 nm LED illumination (20 min irradiation, 5 min pause, 20 min irradiation). The product was collected by magnetic separation, and the template molecule was eluted with methanol:acetonitrile (9:1, v / v) until enrofloxacin was undetectable in the supernatant, thus preparing three imprinted polymers.

[0117] The feed ratio (molar ratio) of each group was kept consistent. Following the method provided in Example 1, the equilibrium adsorption capacity and removal rate of the three groups of MIP materials for enrofloxacin in milk (10 μg / mL, 4 mL, 20 mg material, shaken at room temperature for 12 min) were compared, as shown in Table 8.

[0118] Table 8. Comparison of the adsorption performance of MIPs prepared with different molecularly imprinted polymer layers for enrofloxacin in skim milk.

[0119] Table 9 shows that the adsorption capacity and removal rate of enrofloxacin in milk differed significantly among the three groups of MIP materials: the itaconic acid-pentaerythritol triacrylate combination selected in this invention was significantly superior to the other two groups in both adsorption capacity and removal rate. This combination endows the MIP@Fe3O4@PDA@UiO-66-NH2 composite material with excellent specific recognition ability for enrofloxacin. Therefore, itaconic acid is preferably used as the functional monomer and pentaerythritol triacrylate as the crosslinking agent for the preparation of the molecularly imprinted polymer layer.

[0120] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent modifications or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.

Claims

1. A magnetic molecularly imprinted MOF composite material, characterized in that, It has a core-shell structure, including a magnetic nanoparticle core and a metal-organic framework shell layer wrapped around the surface of the magnetic nanoparticle core; the surface of the metal-organic framework shell layer is also provided with a molecularly imprinted polymer layer; the molecularly imprinted polymer layer contains three-dimensional imprinted cavities of enrofloxacin. The metal-organic framework shell was prepared using a eutectic solvent.

2. The magnetic molecularly imprinted MOF composite material as described in claim 1, characterized in that, The eutectic solvent consists of a hydrogen bond donor and a hydrogen bond acceptor; the hydrogen bond acceptor is choline chloride and the hydrogen bond donor is acetamide.

3. The magnetic molecularly imprinted MOF composite material as described in claim 2, characterized in that, The molar ratio of choline chloride to acetamide is 1:2; the magnetic nanoparticles are Fe3O4 nanoparticles; and the metal-organic framework shell is UiO-66-NH2.

4. The magnetic molecularly imprinted MOF composite material as described in claim 3, characterized in that, A polymer interlayer is also included between the Fe3O4 nanoparticles and the metal-organic framework shell, preferably a polydopamine layer.

5. The magnetic molecularly imprinted MOF composite material as described in claim 1, characterized in that, The molecularly imprinted polymer layer uses itaconic acid as the functional monomer and pentaerythritol triacrylate as the crosslinking agent.

6. The method for preparing the magnetic molecularly imprinted composite material according to any one of claims 1-5, characterized in that, Includes the following steps: (1) Provide magnetic nanoparticles; (2) A polymer intermediate layer is coated on the surface of magnetic nanoparticles to obtain a magnetic nanoparticle core; (3) Using a eutectic solvent as the reaction medium, a metal-organic framework shell is grown in situ on the surface of the magnetic nanoparticle core to obtain a magnetic core-shell metal-organic framework composite material. (4) Using enrofloxacin as a template, molecular imprinting polymerization was carried out on the surface of the magnetic core-shell metal-organic framework composite material to form a molecular imprinted polymer layer. After the template molecules were washed off, the magnetic molecular imprinted composite material was obtained.

7. The preparation method according to claim 6, characterized in that, In step (2), the polymer intermediate layer is a polydopamine layer, which is formed by the self-polymerization of dopamine on the surface of the magnetic nanoparticles under weakly alkaline conditions.

8. The preparation method according to claim 7, characterized in that, In step (3), the metal-organic framework shell is grown in situ under normal pressure and 100-140°C; preferably, the reaction temperature is 120°C.

9. The preparation method according to claim 8, characterized in that, In step (4), the functional monomer used in the molecular imprinting polymerization is itaconic acid, and the crosslinking agent used is pentaerythritol triacrylate; the molecular imprinting polymerization is photoinitiated polymerization; preferably, the light source for the photoinitiated polymerization is an LED light source; more preferably, the wavelength of the LED light source is 450nm.

10. The use of choline chloride-acetamide eutectic solvent in the preparation of the magnetic molecularly imprinted composite material as described in any one of claims 1 to 5, characterized in that, The choline chloride-acetamide eutectic solvent is used as the reaction medium to grow a metal-organic framework shell in situ on the surface of a magnetic polymer core under normal pressure; the magnetic molecularly imprinted composite material is used for the selective adsorption and removal of enrofloxacin from dairy products.

Citation Information

Patent Citations

  • Preparation method and application of eutectic solvent type molecularly imprinted polymer based on magnetic metal organic framework material carrier

    CN115368498A

  • Application of magnetic MOFs composite material in medicine adsorption

    CN118122279A