Metal ion-loaded magnetic mesoporous polydopamine material, and preparation method and application thereof

CN123127972APending Publication Date: 2026-11-20NORTH HUAJIN CHEM IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611562493.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-10
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

但是,致密的PDA涂层由于比表面积较低、活性位点有限和传质速率较低,应用于样品预处理中效率有限

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123127972A_ABST
    Figure CN123127972A_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of composite materials and analysis, and relates to a metal ion loaded magnetic mesoporous polydopamine material and preparation and application. The preparation process of the metal ion loaded magnetic mesoporous polydopamine composite material is as follows: firstly, magnetic nanoparticles Fe3O4@SiO2 coated with a SiO2 shell layer are prepared; then a polydopamine shell layer is coated on the surface through in-situ polymerization; after removing the template, the magnetic mesoporous polydopamine material is obtained; finally, metal ions are further loaded to obtain the metal ion loaded magnetic mesoporous polydopamine composite material. The mesoporous polydopamine has ordered mesoporous channels, a high specific surface area and rich organic groups, can provide multiple interactions and more adsorption sites, and in combination with the metal affinity interaction provided by the loaded metal ions, shows good selective extraction capacity for target analytes. The prepared magnetic composite material can be used as an adsorbent for magnetic solid-phase extraction and determination of fluoroquinolone compounds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of composite materials and analytical technology, and relates to a metal ion-loaded magnetic mesoporous polydopamine material, its preparation method and application. Background Technology

[0002] Fluoroquinolones (FQs) are a class of chemically synthesized antibiotics. Their widespread use leads to residues in the environment and animal-derived foods, potentially increasing antibiotic resistance and allergic hypersensitivity reactions. To ensure public health and food safety, it is necessary to develop simple, rapid, and sensitive analytical methods for effective monitoring of FQs in the food environment. For accurate FQs detection, sample pretreatment before instrument analysis is particularly important due to the low concentrations and complex matrices in actual samples.

[0003] Solid-phase microextraction (SPME) offers advantages such as low sample and extractant consumption, simple operation, and integration of extraction and enrichment, making it widely applicable for the analysis of trace contaminants in samples with various matrices. Magnetic solid-phase extraction (MSME) combined with magnetic extraction materials utilizes an external magnetic field to collect adsorbed materials, offering advantages such as ease of operation and high efficiency. The morphology and shell of the magnetic extraction material are key factors affecting enrichment efficiency and selectivity. Most reported enrichment or adsorption studies targeting free radicals (FQs) are based on general interactions such as hydrogen bonding, π-π stacking, and hydrophobicity. However, selective materials with specific adsorption capabilities for FQs are scarce. Therefore, developing novel selective adsorbent materials for FQs is of great significance.

[0004] Superparamagnetic nanomaterials exhibit excellent magnetic responsiveness and have attracted significant attention in analytical chemistry, environmental monitoring, and medicinal chemistry. Magnetic nanoparticles, however, tend to aggregate easily, making it difficult to form stable dispersions. Coating with a shell material can protect and stabilize them, while also improving adsorption performance. SiO2 materials possess high biocompatibility and are easily grafted with other functional groups or modified into functionalized materials. Dopamine, rich in amino and hydroxyl groups, can polymerize in weakly alkaline solutions to form polydopamine (PDA). The resulting adhesive PDA exhibits good biocompatibility, excellent dispersibility in water, and a highly delocalized π-π conjugated system, and is easily coated onto other material surfaces. However, dense PDA coatings have limited efficiency in sample pretreatment due to their low specific surface area, limited active sites, and low mass transfer rate. Mesoporous PDAs, with their higher specific surface area and porosity, effectively address these issues.

[0005] Mesoporous PDA layers contain abundant hydroxyl and amino groups, which facilitates the design and loading of metal ions or metal oxides on their surfaces. Based on the advantages of ordered mesoporous channels, appropriate superparamagnetism, and abundant organic groups and metal ion affinity interactions, the adsorption capacity and selectivity for target analytes can be improved. FQs compounds have been shown to form complexes with metal ions, and the order of metal ion complexation ability is: Fe... 3+ / Cu 2+ >Pb 2+ >Zn 2+ >Cd 2+ .

[0006] Therefore, based on the unique properties of magnetic solid-phase microextraction and mesoporous PDA, and the good metal affinity between FQs and metal ions, it is necessary to develop a metal ion-loaded magnetic mesoporous polydopamine material for extraction and enrichment of FQs-like compounds before detection. Summary of the Invention

[0007] Based on the above, the present invention aims to develop a metal ion-loaded magnetic mesoporous polydopamine composite material for magnetic solid-phase extraction of fluoroquinolone compounds. Specifically, a magnetic nanoparticle Fe3O4@SiO2 with a SiO2 shell encapsulating Fe3O4 is prepared. Then, a polydopamine shell is grown through in-situ surface polymerization. After removing the organic template, the resulting mesoporous polydopamine magnetic material is further loaded with metal ions on its surface to obtain a metal ion-loaded magnetic mesoporous polydopamine composite material.

[0008] To achieve the above objectives, the technical solution adopted by the present invention is as follows: In a first aspect, the present invention provides a method for preparing a metal ion-supported magnetic mesoporous polydopamine composite material, specifically comprising the following steps: S1 Preparation of Fe3O4@SiO2 nanoparticles: A SiO2 shell was coated on the surface of Fe3O4 nanoparticles by sol-gel method; Preparation of in-situ polymerized mesoporous polydopamine material on Fe3O4@SiO2 surface using S2: The Fe3O4@SiO2 prepared in step S1 is dispersed in an alcohol solution until homogeneous to obtain solution A; F127 and TMB were added to an aqueous solution of alcohol and dispersed evenly to obtain solution B. Solution A was added to solution B, ammonia was added and stirred, and then dopamine hydrochloride aqueous solution was added to continue the reaction. The resulting material was washed and the template was removed to obtain Fe3O4@SiO2@mPDA. S3 Preparation of Mesoporous Polydopamine-Loaded Metal Ion Magnetic Composite Materials: The Fe3O4@SiO2@mPDA material prepared in step S2 was dispersed in an aqueous solution of metal ions, collected, washed, and dried to obtain the magnetic polydopamine material Fe3O4@SiO2@mPDA-M with surface-loaded metal ions. n+ ; The metal ion is Fe. 3+ Cu 2+ Pb 2+ Zn 2+ or Cd 2+ .

[0009] Preferably, in step S1, Fe3O4 nanoparticles are prepared by a hydrothermal method.

[0010] Preferably, the specific process for preparing Fe3O4@SiO2 nanoparticles in step S1 is as follows: 1.33 g of FeCl3·6H2O was dissolved in 40 mL of ethylene glycol, and 0.3–0.4 g of sodium citrate and 1.5–2.5 g of anhydrous sodium acetate were added. The mixture was reacted at 180–220 °C to separate Fe3O4 nanospheres.

[0011] Further, the method for coating the surface of Fe3O4 nanospheres with a SiO2 layer is as follows: the Fe3O4 material prepared above is dispersed in 100 mL of ethanol aqueous solution at a ratio of 0.2~0.4 g; after adding 7 mL of ammonia water, 0.4 mL of tetraethyl orthosilicate (TEOS) is added, and after washing, the Fe3O4@SiO2 material is collected.

[0012] Preferably, in step S2, the concentration of Fe3O4@SiO2 in solution A is 0.03~0.08 g / mL; the concentration of F127 in solution B is 10~16 mg / mL; the volume fraction of TMB in the aqueous alcohol solution is 0.01~0.02 v / v; the volume ratio of water to ethanol is 1:1; the volume ratio of solution A to solution B is 5:80~100; the amount of ammonia added is 0.4~0.8 mL; the concentration of dopamine hydrochloride aqueous solution is 80~150 mg / mL; the amount added is 5 mL; and the stirring reaction time is 2~2.5 h.

[0013] Preferably, in step S2, the obtained material is washed with water and ethanol, and the template is removed by ultrasonication using ethanol and acetone in a 2:1 (v / v) ratio.

[0014] Preferably, in step S3, the concentration of Fe3O4@SiO2@mPDA in the metal ion aqueous solution is 0.15~0.30 mg / mL, the stirring time is 3.0~4.5 h, and the metal ion aqueous solution is an 80~120 mM CuCl2·2H2O aqueous solution.

[0015] Preferably, the mesoporous polydopamine shell is formed by in-situ polymerization of dopamine monomers under alkaline conditions using Pluronic F127 and 1,3,5-trimethylbenzene (TMB) as organic templates.

[0016] In a second aspect, the present invention provides a metal ion-loaded magnetic mesoporous polydopamine composite material prepared by the method described in the first aspect.

[0017] Preferably, the core of the metal ion-loaded magnetic mesoporous polydopamine composite material is magnetic nanoparticles Fe3O4@SiO2 coated with a SiO2 shell. Mesoporous polydopamine is grown in situ on the surface of the Fe3O4@SiO2, with metal ions loaded within the mesoporous channels. The Fe3O4@SiO2 nanoparticles have a size of 100–300 nm, and the magnetic composite material encapsulating the mesoporous polydopamine has a size of 200–500 nm and a BET specific surface area greater than 100 m². 2 / g.

[0018] Thirdly, the present invention provides an application of the metal ion-loaded magnetic mesoporous polydopamine composite material described in the first aspect for magnetic solid-phase extraction and enrichment of fluoroquinolone compounds.

[0019] Preferably, the magnetic solid-phase extraction of the fluoroquinolone compounds includes the following steps: Metal ion-loaded magnetic mesoporous polydopamine composite material was added to the sample solution at a concentration of 0.15–0.8 mg / mL. The pH of the sample solution was adjusted to 7–11. The target analyte in the sample solution was adsorbed by sonication for 2–8 min. The adsorbed material was collected from the sample solution with the assistance of a magnet. Next, methanol containing 2% (v / v) formic acid was used as the elution solvent and added to the metal ion-loaded magnetic mesoporous polydopamine composite material with the adsorbed target analyte collected above at a concentration of 0.12–0.50 mL / mg. The target analyte was desorbed into the elution solvent by sonication for 2–6 min. The eluent was collected with the assistance of a magnet.

[0020] Furthermore, the pH of the sample solution is adjusted using ammonia or sodium hydroxide.

[0021] Preferably, the collected eluent is filtered through a filter membrane, dried, reconstituted with 100 μL of mobile phase, and then 10 μL is injected for high performance liquid chromatography-ultraviolet detection and analysis.

[0022] Furthermore, the liquid chromatography analysis was performed using a pentafluorophenyl column (4.6 mm × 150 mm, 5 μm); the mobile phase was 0.1% (v / v) formic acid eluted isocratically with water / methanol (30 / 70, v / v), the flow rate was 1.5 mL / min; the column temperature was 35℃, and the detection wavelength was 280 nm.

[0023] Preferably, the fluoroquinolone compounds include enrofloxacin (ENR), levofloxacin (LEV), ciprofloxacin (CIP), norfloxacin (NOR), and enoxacin (ENO).

[0024] The beneficial effects of this invention are as follows: Fe3O4 nanoparticles coated with a SiO2 shell are used as magnetic cores, and a polydopamine shell is grown in situ via surface polymerization. After removing the organic template, a magnetic mesoporous polydopamine material is obtained, which is then further modified with loaded metal ions. The resulting metal ion-loaded magnetic mesoporous polydopamine composite material, based on ordered mesoporous channels, high specific surface area, appropriate superparamagnetism, and abundant organic groups and metal ion affinity interactions, can provide more active sites, exhibit high extraction efficiency and selective adsorption capacity. Combined with detection methods, it can achieve trace detection of fluoroquinolone compounds in samples. Attached Figure Description

[0025] Figure 1 The material is Fe3O4@SiO2@mPDA-Cu 2+ A schematic diagram of the preparation process.

[0026] Figure 2 Scanning electron microscope (SEM) images of materials Fe3O4 (a), Fe3O4@SiO2 (b), and Fe3O4@SiO2@mPDA (c).

[0027] Figure 3 The N2 adsorption-desorption isotherms are for the magnetic non-mesoporous material Fe3O4@SiO2@PDA (a) and the magnetic mesoporous material Fe3O4@SiO2@mPDA (b).

[0028] Figure 4 The material is Fe3O4@SiO2@mPDA-Cu 2+ The EDS energy spectrum.

[0029] Figure 5 10 μg / mL FQs standard solution (a), Fe3O4@SiO2@mPDA-Cu 2+ Chromatograms of extraction (b) and Fe3O4@SiO2@mPDA extraction (c). Chromatogram peaks 1-5 are ENR, CIP, ENO, LEV, and NOR, respectively.

[0030] Figure 6 The material is Fe3O4@SiO2@mPDA-Cu 2+ Optimization of factors affecting extraction efficiency: (a) extraction time, (b) solution pH, (c) type of eluent, (d) elution time, and (e) elution volume. Detailed Implementation

[0031] The present invention will be further described and illustrated below with reference to the accompanying drawings and specific embodiments.

[0032] Example 1 Material Fe3O4@SiO2@mPDA-Cu 2+ Preparation: First, Fe3O4@SiO2 magnetic nanospheres were prepared. After preparing Fe3O4 magnetic nanoparticles using a one-pot hydrothermal method, a SiO2 shell was coated onto the surface of the Fe3O4 nanomagnetic core to achieve good encapsulation and morphology of the mesoporous PDA.

[0033] 1.33 g of FeCl3·6H2O was dissolved in 40 mL of ethylene glycol, and 0.37 g of sodium citrate and 2 g of anhydrous sodium acetate were added and stirred until dissolved. The mixture was stirred for 2 h and sonicated for 1 h, then transferred to a reaction vessel and reacted at 200 °C for 10 h. After cooling to room temperature, the Fe3O4 nanospheres were separated by a magnet and washed three times with deionized water and anhydrous ethanol, respectively. The obtained Fe3O4 nanospheres were dispersed in anhydrous ethanol for storage in the next step of the experiment. The Fe3O4 material prepared above was dispersed in water and ethanol in a 1:4 (v / v) mixture, sonicated until uniformly dispersed, and stirred electrically for 1 h. 7 mL of ammonia water was slowly added dropwise and stirring was continued for 1 h. Then, 0.4 mL of tetraethyl orthosilicate (TEOS) was slowly added, and the mixture was stirred at room temperature for 10 h. The Fe3O4@SiO2 material was collected and washed three times with water and anhydrous ethanol, respectively.

[0034] Next, Fe3O4@SiO2@mPDA material was prepared. 1 g of F127 and 1 mL of TMB were ultrasonically dissolved in 90 mL of water and ethanol in a 1:1 (v / v) mixture. Fe3O4@SiO2 (0.2 g of Fe3O4@SiO2 material dispersed in 5 mL of anhydrous ethanol) was slowly added under electric stirring. 0.6 mL of ammonia was added dropwise to the mixture, and after stirring for 1 h, 5 mL of dopamine hydrochloride (500 mg) aqueous solution was added, and stirring continued for 2 h. The resulting material was washed three times with water and ethanol, respectively. The template was removed by ultrasonication with ethanol and acetone in a 2:1 (v / v) mixture for 30 min (this step was repeated three times) to obtain the Fe3O4@SiO2@mPDA material.

[0035] Finally, surface loading of metal ions yields Fe3O4@SiO2@mPDA-Cu 2+ Materials. 30 mg of Fe3O4@SiO2@mPDA was dispersed in 150 mL of 100 mM CuCl2·2H2O solution and mechanically stirred for 4 h. The material was collected, washed three times successively with water and ethanol, and then vacuum dried at 60 °C to obtain surface-loaded Cu.2+ Magnetic polydopamine material with ions Fe3O4@SiO2@mPDA-Cu 2+ Its overall preparation process is as follows Figure 1 As shown.

[0036] Example 2 Material Fe3O4@SiO2@mPDA-Cu 2+ The characterization results are as follows: The morphology of the material was characterized using scanning electron microscopy, and the results are as follows: Figure 2 As shown, both Fe3O4 and Fe3O4@SiO2 are nanospheres with uniform distribution. After coating with a SiO2 shell, the particle size of the Fe3O4@SiO2 microspheres increases. The Fe3O4@SiO2@mPDA material obtained after coating with PDA has relatively uniform size, good dispersion, and uniform coating.

[0037] The magnetic non-mesoporous material Fe3O4@SiO2@PDA and the magnetic mesoporous material Fe3O4@SiO2@mPDA were characterized using the N2 isothermal adsorption method. The N2 adsorption-desorption isotherms are shown below. Figure 3 As shown. The BET specific surface area of ​​the Fe3O4@SiO2@mPDA material is 104.710 m². 2 The g / g ratio is significantly greater than that of Fe3O4@SiO2@PDA material (25.848 m). 2 / g), which is beneficial for loading metal ions and improving extraction performance.

[0038] The Fe3O4@SiO2@mPDA-Cu model was further verified by energy dispersive spectroscopy (EDS). 2+ The successful preparation of materials, such as Figure 4 As shown in the figure. The elemental distribution, as revealed by EDS energy dispersive spectroscopy, shows that copper accounts for 11.18% by weight, confirming that Cu... 2+ The successful introduction of [the technology / mechanism].

[0039] Example 3 Characterization of FQs extraction performance: Five FQs compounds were used as target analytes, and the Fe3O4@SiO2@mPDA-Cu material was analyzed and characterized by HPLC-UV. 2+ The magnetic solid-phase extraction performance of the five FQs. The five FQs were enrofloxacin (ENR), levofloxacin (LEV), ciprofloxacin (CIP), norfloxacin (NOR), and enoxacin (ENO). Figure 5 As shown, under the same extraction conditions, Cu-loaded... 2+ Fe3O4@SiO2@mPDA-Cu 2+ The enrichment effect of the material is significantly higher than that of Fe3O4@SiO2@mPDA material, indicating that Cu2+ Metal complexation interactions with FQs play an important role in extraction.

[0040] Example 4 Investigation of experimental factors affecting extraction efficiency: To achieve higher extraction and enrichment efficiency, the effects of Fe3O4@SiO2@mPDA-Cu on... 2+ The main parameters of magnetic solid-phase extraction (FQs) for materials were investigated and optimized, including extractant dosage, sample solution pH, extraction time, eluent type and volume, and elution time. The results are as follows: Figure 6 As shown. Optimized Fe3O4@SiO2@mPDA-Cu 2+ The magnetic solid-phase extraction conditions for the material were as follows: 25 mL sample solution, sample pH of 9, 4 mg extractant, extraction time of 6 min by sonication, 0.5 mL methanol (containing 2% (v / v) formic acid) as the elution solvent, and 4 min by sonication for desorption. The collected eluent was dried, reconstituted with 100 μL of mobile phase, and then 10 μL was injected for HPLC-UV analysis.

[0041] This invention prepares a metal ion-supported magnetic mesoporous polydopamine composite material for magnetic solid-phase extraction and enrichment of fluoroquinolone compounds. The prepared material exhibits good extraction performance, and the magnetic solid-phase extraction method developed based on the material is simple and rapid.

[0042] The above-described embodiments are merely illustrative of the implementation methods of the present invention, but should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these modifications and improvements all fall within the protection scope of the present invention.

Claims

1. A method for preparing a metal ion-supported magnetic mesoporous polydopamine composite material, characterized in that, Includes the following steps: S1 Preparation of Fe3O4@SiO2 nanoparticles: A SiO2 shell was coated on the surface of Fe3O4 nanoparticles by sol-gel method; Preparation of in-situ polymerized mesoporous polydopamine material on Fe3O4@SiO2 surface using S2: The Fe3O4@SiO2 prepared in step S1 is dispersed in an alcohol solution until homogeneous to obtain solution A; F127 and TMB were added to an aqueous solution of alcohol and dispersed evenly to obtain solution B. Solution A was added to solution B, ammonia was added and stirred, and then dopamine hydrochloride aqueous solution was added to continue the reaction. The resulting material was washed and the template was removed to obtain Fe3O4@SiO2@mPDA. S3 Preparation of Mesoporous Polydopamine-Loaded Metal Ion Magnetic Composite Materials: The Fe3O4@SiO2@mPDA material prepared in step S2 was dispersed in an aqueous solution of metal ions, collected, washed, and dried to obtain the magnetic polydopamine material Fe3O4@SiO2@mPDA-M with surface-loaded metal ions. n+ ; The metal ion is Fe. 3+ Cu 2+ Pb 2+ Zn 2+ or Cd 2+ .

2. The method for preparing the metal ion-supported magnetic mesoporous polydopamine composite material according to claim 1, characterized in that, In step S1, Fe3O4 nanoparticles are prepared by a hydrothermal method.

3. The method for preparing the metal ion-supported magnetic mesoporous polydopamine composite material according to claim 1, characterized in that, In step S1, the specific process for preparing Fe3O4@SiO2 nanoparticles is as follows: 1.33 g of FeCl3·6H2O was dissolved in 40 mL of ethylene glycol, and 0.3–0.4 g of sodium citrate and 1.5–2.5 g of anhydrous sodium acetate were added. The mixture was reacted at 180–220 °C to obtain Fe3O4 nanomagnetic spheres.

4. The method for preparing the metal ion-supported magnetic mesoporous polydopamine composite material according to claim 1, characterized in that, The method for coating the surface of Fe3O4 nanospheres with SiO2 is as follows: The Fe3O4 material prepared above is dispersed in 100 mL of ethanol aqueous solution at a ratio of 0.2~0.4 g; after adding 7 mL of ammonia water, 0.4 mL of tetraethyl orthosilicate (TEOS) is added, and after washing, Fe3O4@SiO2 material is collected.

5. The method for preparing the metal ion-supported magnetic mesoporous polydopamine composite material according to claim 1, characterized in that, In step S2, the concentration of Fe3O4@SiO2 in solution A is 0.03~0.08 g / mL; the concentration of F127 in solution B is 10~16 mg / mL; the volume fraction of TMB in the aqueous alcohol solution is 0.01~0.02 v / v; the volume ratio of water to ethanol is 1:1; the volume ratio of solution A to solution B is 5:80~100; the amount of ammonia added is 0.4~0.8 mL of ammonia added per 80~100 mL of solution B; the concentration of dopamine hydrochloride aqueous solution is 80~150 mg / mL; and the amount added is 5 mL of the dopamine hydrochloride aqueous solution added per 80~100 mL of solution B.

6. The method for preparing the metal ion-supported magnetic mesoporous polydopamine composite material according to claim 1, characterized in that, In step S2, the obtained material is washed with water and ethanol, and the template is removed by ultrasonication using ethanol and acetone in a 2:1 (v / v) ratio.

7. The method for preparing the metal ion-supported magnetic mesoporous polydopamine composite material according to claim 1, characterized in that, In step S3, the concentration of Fe3O4@SiO2@mPDA in the metal ion aqueous solution is 0.15~0.30 mg / mL; the metal ion aqueous solution is an 80~120 mM CuCl2·2H2O aqueous solution.

8. A metal ion-loaded magnetic mesoporous polydopamine composite material prepared by the method of any one of claims 1 to 7.

9. The application of the metal ion-supported magnetic mesoporous polydopamine composite material according to claim 8, characterized in that, Used for magnetic solid-phase extraction and enrichment of fluoroquinolone compounds.

10. The application of the metal ion-supported magnetic mesoporous polydopamine composite material according to claim 9, characterized in that, The fluoroquinolone compounds include enrofloxacin, levofloxacin, ciprofloxacin, norfloxacin, and enoxacin; The magnetic solid phase extraction and enrichment specifically includes the following steps: the composite material is added to the sample solution to adsorb the target analyte, and after magnetic separation, it is eluted with a methanol solution containing formic acid. The eluent is collected for analysis. The amount of composite material used is 0.15~0.8 mg / mL, the pH of the sample solution is adjusted to 7~11, and ultrasonic extraction is performed for 2~8 min.