Alpha-alumina porous ceramic carrier, preparation method thereof, silver catalyst and method for producing ethylene oxide by ethylene epoxidation
By adding nanoscale high specific surface area α-Al₂O₃ to the α-alumina support, the problem of insufficient mechanical strength caused by support densification was solved, and the catalyst performance in the efficient ethylene oxidation to ethylene oxide process was improved.
Patent Information
- Application Number
- CN202510646068.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-19
- Publication Date
- 2026-11-20
Smart Images

Figure BDA0005410086250000101 
Figure BDA0005410086250000141 
Figure BDA0005410086250000151
Abstract
Description
Technical Field
[0001] This invention relates to the field of silver catalyst technology, and more specifically, to an α-alumina porous ceramic support for a silver catalyst used in the oxidation of ethylene to produce ethylene oxide, a method for preparing the same, and a method for the silver catalyst and the epoxidation of ethylene to produce ethylene oxide. Background Technology
[0002] Ethylene oxide (EO) is one of the main products of the ethylene industry, with wide applications, and its downstream product, ethylene glycol, also has high added value and various application prospects. The direct oxidation of ethylene to ethylene oxide using a silver catalyst is currently the most common synthetic route for industrial production of ethylene oxide. To date, silver catalysts remain the only effective catalysts for the industrial epoxidation of ethylene to ethylene oxide. This catalyst uses α-alumina, a ceramic material with a special pore structure, as a support.
[0003] The main performance indicators for α-alumina supports include: mechanical strength, specific surface area, pore volume, water absorption, tortuosity, and shrinkage. A suitable specific surface area provides space for the deposition of active components and catalytic additives; a suitable pore volume provides adequate space for ethylene oxidation, allowing the heat of reaction to dissipate promptly; a suitable water absorption rate controls the loading of active components and catalytic additives on the support; and suitable tortuosity and shrinkage contribute to reducing pressure drop in the production unit.
[0004] In addition, another important characteristic of the catalyst support is its mechanical strength, which includes abrasion resistance and compressive strength. In industrial applications, friction or rubbing typically occurs between catalyst particles or between the catalyst and equipment surfaces. This friction or rubbing can occur during catalyst preparation, catalyst loading, and epoxidation reactor charging, causing physical decomposition of the catalyst. This not only leads to the loss of precious metals, but the dust generated by this abrasion can also migrate out of the reaction zone with the equilibrium gas, initiating over-reactions in separators or other locations and adversely affecting the recovery system. Catalyst abrasion, especially the loss of precious metals, reduces industrial production efficiency and the economic benefits of precious metal recovery. Therefore, improving catalyst abrasion resistance is crucial.
[0005] There is a close relationship between support wear and catalyst attrition because catalysts are typically supported or immobilized in the reactor by a support. Support wear can lead to catalyst attrition, and vice versa. Support attrition can cause physical damage to the catalyst or destabilize it. For example, wear of the support material can lead to the shedding of catalyst particles, reducing the effective active surface area of the catalyst and thus affecting its performance and lifespan. On the other hand, catalyst attrition can also affect the support itself. For example, in high-temperature, high-pressure, or chemically corrosive environments, catalyst attrition can lead to the erosion or destruction of the support, thereby affecting its stability and lifespan.
[0006] Furthermore, the support needs to possess sufficient compressive strength to withstand the forces exerted on the catalyst during reactor loading and reaction. Catalyst breakage within the reactor leads to increased pressure drop and poor distribution of reactants and reaction hotspots within the catalyst bed.
[0007] US4428863A improves the compressive strength and wear resistance of the support by adding a small amount of barium aluminate or silicate as a permanent binder during the support preparation process. WO9623585A1 uses polypropylene with an average particle size of less than 400 μm and an ash content of less than 0.1 wt.% as a burnout material, improving the compressive strength and wear resistance of the catalyst. US20070185339A1 eliminates the need for catalyst pretreatment with purge gas during the start-up of the epoxidation process by contacting the catalyst or a catalyst precursor containing cationic silver with oxygen-containing processing feedstock at a temperature of at least 350°C for at least 5 minutes, effectively improving catalyst wear and enhancing catalyst mechanical strength.
[0008] Furthermore, α-alumina supports, as porous ceramic materials, require high sintering temperatures, reaching 1400-1750℃. This high sintering temperature not only poses a significant challenge to the performance of Al2O3 ceramics but also reduces the lifespan of kiln furniture, greatly increasing production costs. It has been reported that lowering the sintering temperature of Al2O3 ceramics from 1600-1650℃ to 1450-1500℃ can reduce energy consumption by 25%-35%. From the perspective of energy conservation and low cost, research on low-temperature sintering of Al2O3 ceramics is of great significance (Vacuum Electronics Technology, 2012(04):52-54).
[0009] In summary, how to prepare silver catalyst supports with good mechanical strength such as compressive strength and wear resistance more economically and effectively, and how to reduce the calcination temperature, remains a research hotspot in the field of silver catalysts and has important research value. Summary of the Invention
[0010] The inventors of this invention have conducted extensive and in-depth research in the field of silver catalyst and its support preparation. The results show that, typically, α-Al₂O₃ supports prepared by high-temperature calcination exhibit a high degree of densification and a specific surface area of less than 10 m². 2 / g. High specific surface area α-Al₂O₃ can maintain a uniform dispersion in nanoscale particle form, exhibiting high surface energy. Adding it as an independent aluminum source to the α-alumina support during the preparation process can provide seed crystals for crystallization during sintering, promote the densification process of the support, reduce the calcination temperature to some extent, and improve the wear resistance and compressive strength of the support to varying degrees. Based on this, the purpose of this invention is to provide an α-alumina porous ceramic support for a silver catalyst used in the ethylene oxidation to ethylene oxide production, its preparation method, and a silver catalyst and method for the ethylene epoxidation to ethylene oxide production. The α-alumina support prepared by this invention shows significantly improved wear resistance and compressive strength, and a lower calcination temperature. After loading silver and preferably various active components to prepare a silver catalyst, it exhibits good activity and selectivity in the ethylene oxidation to ethylene oxide production process.
[0011] To achieve the objectives of this invention, a first aspect of the invention provides an α-alumina porous ceramic support for a silver catalyst used in the oxidation of ethylene to produce ethylene oxide, the α-alumina porous ceramic support being prepared by a method comprising the following steps:
[0012] (1) Trihydrate Al₂O₃, pseudoboehmite, high specific surface area α-Al₂O₃, alkaline earth metal compound, pore-forming agent, zirconium-containing compound, and silicon-containing compound are mixed uniformly to obtain a solid mixture; the solid mixture, binder, and optionally water are mixed to obtain the α-alumina carrier precursor mixture; wherein the specific surface area of the high specific surface area α-Al₂O₃ is 12-220 m² / g. 2 / g;
[0013] (2) The α-alumina carrier precursor mixture is shaped, dried and calcined to obtain the α-alumina porous ceramic carrier.
[0014] A second aspect of the present invention provides a method for preparing the above-mentioned α-alumina porous ceramic carrier, the method comprising: S1. preparing an α-alumina carrier precursor mixture: uniformly mixing Al2O3 trihydrate, boehmite, high specific surface area α-Al2O3, alkaline earth metal compound, pore-forming agent, zirconium-containing compound and silicon-containing compound to obtain a solid mixture; mixing the solid mixture, a binder and optionally water to obtain the α-alumina carrier precursor mixture;
[0015] S2. The α-alumina carrier precursor mixture obtained in step S1 is shaped, dried and calcined to obtain the α-alumina porous ceramic carrier.
[0016] A third aspect of the present invention provides a silver catalyst for the oxidation of ethylene to produce ethylene oxide, the silver catalyst comprising: the above-mentioned α-alumina porous ceramic support and an active component silver supported on the α-alumina porous ceramic support;
[0017] Preferably, the silver catalyst further includes:
[0018] Alkali metals and / or alkaline earth metals, or compounds based on alkali metals and / or alkaline earth metals;
[0019] Rhenium metal and / or rhenium-based compounds; and
[0020] Optionally, the rhenium co-catalyst is preferably selected from at least one metal selected from chromium, molybdenum, tungsten and manganese, and / or selected from at least one metal compound selected from chromium metal compound, molybdenum metal compound, tungsten metal compound and manganese metal compound.
[0021] A fourth aspect of the present invention provides a method for producing ethylene oxide by epoxidation of ethylene, the method comprising: subjecting ethylene to an epoxidation reaction in the presence of the aforementioned silver catalyst to obtain ethylene oxide.
[0022] The technical solution of the present invention has the following beneficial effects:
[0023] (1) In the α-alumina carrier of the present invention, high specific surface area α-Al2O3, which exists in the form of nano-sized particles and maintains a uniform dispersion, is added to the α-alumina carrier during the preparation process as an independent aluminum source. The small particle size of the high specific surface area α-Al2O3 gives it high surface energy, thus exhibiting high activity during calcination. This effectively promotes the sintering process of the α-alumina carrier, reduces the calcination temperature of the carrier to a certain extent, and improves the wear resistance and compressive strength of the carrier to varying degrees.
[0024] (2) This invention effectively controls the compressive strength and wear rate of the support by adjusting the specific surface area and amount of high specific surface area α-Al2O3 material, while maintaining a matching specific surface area of the support, thus realizing the beneficial effect of adding high specific surface area α-Al2O3 on the support of silver catalyst. Since the high specific surface area α-Al2O3 material does not introduce other impurity elements into the silver catalyst support, it will not cause the support to generate acidic or basic active sites that are detrimental to the epoxidation reaction, and therefore will not adversely affect the performance of the silver catalyst in the process of ethylene oxidation to ethylene oxide.
[0025] (3) The silver catalyst prepared using the support of the present invention exhibits good activity and selectivity in the process of ethylene oxidation to produce ethylene oxide.
[0026] Other features and advantages of the present invention will be described in detail in the following detailed description section. Detailed Implementation
[0027] Preferred embodiments of the invention will now be described in more detail. While preferred embodiments of the invention are described below, it should be understood that the invention can be implemented in various forms and should not be limited to the embodiments set forth herein.
[0028] A first aspect of the present invention provides an α-alumina porous ceramic support for a silver catalyst used in the oxidation of ethylene to produce ethylene oxide, the α-alumina porous ceramic support being prepared by a method comprising the following steps:
[0029] (1) Trihydrate Al₂O₃, pseudoboehmite, high specific surface area α-Al₂O₃, alkaline earth metal compound, pore-forming agent, zirconium-containing compound, and silicon-containing compound are mixed uniformly to obtain a solid mixture; the solid mixture, binder, and optionally water are mixed to obtain the α-alumina carrier precursor mixture; wherein the specific surface area of the high specific surface area α-Al₂O₃ is 12-220 m² / g. 2 / g;
[0030] (2) The α-alumina carrier precursor mixture is shaped, dried and calcined to obtain the α-alumina porous ceramic carrier.
[0031] According to the present invention, preferably, the specific surface area of the high specific surface area α-Al₂O₃ is 12-200 m². 2 / g, preferably 15-150m 2 / g.
[0032] According to the present invention, preferably, the high specific surface area α-Al2O3 is prepared by ball milling or ball milling-calcination method;
[0033] Preferably, the high specific surface area α-Al2O3 is prepared by a method comprising the following steps: drying, ball milling and optionally calcining SB powder to obtain the high specific surface area α-Al2O3.
[0034] In this invention, the above preparation method is a ball milling method when there is no calcination step and a ball milling-calcination method when there is a calcination step.
[0035] According to the present invention, preferably, the drying temperature is 80-140°C and the time is 5-24 hours;
[0036] The ball milling process uses agate grinding balls; the ball milling conditions are ball milling at 20-60Hz for 15-30 hours.
[0037] The roasting temperature is 25-1500℃, and the time is 0-8h.
[0038] According to the present invention, preferably, based on the total weight of the solid mixture, the content of the high specific surface area α-Al₂O₃ is 0.01-20 wt%, preferably 0.03-15 wt%, more preferably 0.05-12 wt%; the content of the trihydrate Al₂O₃ is 40-90 wt%, preferably 55-85 wt%; the content of the pseudoboehmite is 10-55 wt%, preferably 15-50 wt%; the content of the pore-forming agent is 5-30 wt%; the content of the alkaline earth metal compound is 0.1-5 wt%; the content of the zirconium-containing compound is 0.01-5 wt%; and the content of the silicon-containing compound is 0.01-1 wt%.
[0039] According to the present invention, preferably, the trihydrate Al2O3 is selected from at least one of gibbsite, diaspore, and diaspore;
[0040] The pore-forming agent is selected from at least one of petroleum coke, carbon powder, graphite, rosin, polyethylene, and polypropylene;
[0041] The alkaline earth metal compound is selected from at least one of the following: oxides, hydroxides, acetates, sulfates, nitrates, and oxalates of alkaline earth metals.
[0042] The zirconium-containing compound is at least one of zirconium dioxide, zirconium hydroxide, and zirconium silicate.
[0043] The silicon-containing compound is silicon dioxide and / or silicate;
[0044] Preferably, the particle size of the trihydrate Al2O3 is 20–200 μm, and the particle size of the pseudoboehmite is 1–120 μm.
[0045] In this invention, during the preparation of the α-alumina carrier, alumina trihydrate undergoes dehydration and phase transformation of different alumina phases, ultimately transforming into α-alumina.
[0046] In this invention, during the preparation of the α-alumina carrier, boehmite and binder generate an aluminum sol, which binds the components together to form an extrudable paste. During the high-temperature calcination process, boehmite is also converted into α-alumina.
[0047] According to the present invention, preferably, the α-alumina porous ceramic support has at least one of the following characteristics: α-Al₂O₃ content of 90 wt% or more; lateral crushing strength of 50–200 N / particle, preferably 55–190 N / particle; and specific surface area of 0.4–3.0 m². 2 / g, preferably 0.5~2.1m 2 / g; wear rate 2–13%.
[0048] A second aspect of the present invention provides a method for preparing the above-mentioned α-alumina porous ceramic carrier, the method comprising: S1. preparing an α-alumina carrier precursor mixture: uniformly mixing Al2O3 trihydrate, boehmite, high specific surface area α-Al2O3, alkaline earth metal compound, pore-forming agent, zirconium-containing compound and silicon-containing compound to obtain a solid mixture; mixing the solid mixture, a binder and optionally water to obtain the α-alumina carrier precursor mixture;
[0049] S2. The α-alumina carrier precursor mixture obtained in step S1 is shaped, dried and calcined to obtain the α-alumina porous ceramic carrier.
[0050] According to the present invention, preferably, in S2, the calcination temperature is 700-1800℃, more preferably 1100-1700℃, and even more preferably 1200-1600℃.
[0051] In this invention, as a specific embodiment, the preparation method of the α-alumina porous ceramic carrier includes: (1) preparing an α-alumina carrier precursor mixture: mixing Al2O3 trihydrate, boehmite, high specific surface area α-Al2O3, alkaline earth metal compound, pore-forming agent, zirconium-containing compound and silicon-containing compound evenly to obtain a solid mixture; mixing the solid mixture, binder and optional water to obtain the α-alumina carrier precursor mixture;
[0052] (2) The precursor mixture obtained in step (1) is shaped to obtain a shaped body;
[0053] (3) The molded body obtained in step (2) is dried and calcined to obtain the α-alumina porous ceramic carrier.
[0054] In this invention, the method for obtaining the molded body in step (2) can be performed according to conventional techniques in the art. The shape of the molded body can be annular, spherical, cylindrical, or porous cylindrical. The mixture obtained by mixing the solid powder with the binder and optionally water needs to be kneaded in a kneading machine for 10–60 minutes to form an extrudable paste. This paste is then molded in a molding machine into annular, spherical, cylindrical, single-hole or multi-hole cylindrical, or foliage-shaped objects.
[0055] In this invention, the drying and calcining methods in step (3) can be performed using conventional methods in the art. Preferably, the molded body can be dried to a free water content of less than 10 wt%, the drying temperature can be 20–100°C, and the drying time can be controlled between 20 and 48 hours depending on the moisture content. The calcination process of the α-alumina carrier is a one-step calcination, with a calcination temperature of 700–1800°C, preferably 1100–1700°C, and more preferably 1200–1600°C.
[0056] A third aspect of the present invention provides a silver catalyst for the oxidation of ethylene to produce ethylene oxide, the silver catalyst comprising: the above-mentioned α-alumina porous ceramic support and an active component silver supported on the α-alumina porous ceramic support;
[0057] Preferably, the silver catalyst further includes:
[0058] Alkali metals and / or alkaline earth metals, or compounds based on alkali metals and / or alkaline earth metals;
[0059] Rhenium metal and / or rhenium-based compounds; and
[0060] Optionally, the rhenium co-catalyst is preferably selected from at least one metal selected from chromium, molybdenum, tungsten and manganese, and / or selected from at least one metal compound selected from chromium metal compound, molybdenum metal compound, tungsten metal compound and manganese metal compound.
[0061] In this invention, the silver catalyst can be prepared by known methods or any conventional method. For example, the above-mentioned α-alumina support is typically impregnated with a solution containing sufficient amounts of an organic amine, a silver compound, an alkali metal promoter, an alkaline earth metal promoter, an optional rhenium promoter, and an optional co-promoter of the rhenium promoter.
[0062] According to the present invention, the silver catalyst further includes depositing other elements on an α-alumina support, said other elements including one or more of phosphorus, boron, chromium and titanium.
[0063] According to a preferred embodiment of the present invention, the silver catalyst is prepared by a method comprising the following steps: I) impregnating an α-alumina support prepared according to the method of the present invention with a solution containing sufficient amounts of an organic amine, a silver compound, an alkali metal auxiliary agent, an alkaline earth metal auxiliary agent, an optional rhenium auxiliary agent, and an optional rhenium auxiliary co-auxiliary agent; II) leaching the impregnation solution; III) activating the support obtained in step II) in an oxygen-containing gas to prepare the silver catalyst.
[0064] According to the present invention, in the preparation of the silver catalyst, the organic amine may be selected from one or more of 1,2-propanediamine, 1,3-propanediamine, ethylenediamine, 1,2-butanediamine, 1,3-butanediamine, pyridine, ethylamine, n-propylamine, n-butylamine, isobutylamine, tert-butylamine, sec-butylamine, ethanolamine, propanolamine, and butanolamine; the silver compound may be selected from one or more of silver oxide, silver nitrate, and silver oxalate; the alkali metal promoter may be selected from one or more of lithium, sodium, potassium, rubidium, and cesium; the alkaline earth metal promoter may be selected from one or more of magnesium, calcium, strontium, and barium; the rhenium promoter may be selected from one or more of rhenium oxide, ammonium perrhenate, perrhenic acid, and cesium perrhenate; and the co-promoter of the rhenium promoter may be selected from one or more of oxoanions in the form of salts or acids of cerium, sulfur, molybdenum, and chromium.
[0065] According to the present invention, the mass of silver element accounts for 10-40% of the mass of the silver catalyst; the mass of alkali metal promoter accounts for 5-2000 ppm of the mass of the silver catalyst; the mass of alkaline earth metal promoter accounts for 5-20000 ppm of the mass of the silver catalyst; the mass of rhenium promoter accounts for 50-10000 ppm of the mass of the silver catalyst; and the mass of rhenium co-promoter accounts for 0-5000 ppm, preferably 5-5000 ppm, of the mass of the silver catalyst.
[0066] In the silver catalyst preparation method of the present invention, activation is carried out in an oxygen-containing mixed gas, which includes an air stream or a nitrogen-oxygen mixed gas with an oxygen content of not more than 21%; the activation temperature is 180-700℃ and the activation time is 1-120 min.
[0067] In this invention, to prepare the silver catalyst, an aqueous solution of silver nitrate is first reacted with an aqueous solution of ammonium oxalate or oxalic acid to precipitate silver oxalate. The precipitate is then filtered, washed with deionized water until no nitrate ions are present, and then silver oxalate is dissolved in an aqueous solution of an organic amine. An alkali metal auxiliary agent, an alkaline earth metal auxiliary agent, an optional rhenium auxiliary agent, and a co-auxiliary agent of the rhenium auxiliary agent are added to prepare an impregnation solution. The α-alumina support prepared by the method described in this invention is impregnated with the obtained impregnation solution, the impregnation solution is filtered, activated, and finally the silver catalyst is prepared.
[0068] To obtain silver catalysts with high silver content and / or additive content, the present invention can prepare silver-containing catalysts by one or more impregnation methods.
[0069] The alkali metals, alkaline earth metals, rhenium additives, and optional rhenium co-additives added during the preparation of the silver catalyst of the present invention can be deposited on the support before, during, or after impregnation of silver, or they can be deposited on the support after the silver compound is activated and reduced.
[0070] A fourth aspect of the present invention provides a method for producing ethylene oxide by epoxidation of ethylene, the method comprising: subjecting ethylene to an epoxidation reaction in the presence of the aforementioned silver catalyst to obtain ethylene oxide.
[0071] In this invention, the olefin may include one or more of styrene, propylene, ethylene, and 1,3-butadiene. The olefin epoxidation reactor may be any apparatus capable of performing an epoxidation reaction.
[0072] The present invention is further illustrated by the following examples:
[0073] The present invention will be further described below with reference to the embodiments, but the scope of the present invention is not limited to these embodiments.
[0074] Determination of the catalytic performance of silver catalysts:
[0075] The selectivity of the silver catalyst prepared in this invention was tested using a laboratory microreactor evaluation apparatus. The reactor used in the microreactor evaluation apparatus was a stainless steel reaction tube with an inner diameter of 4 mm, placed within a heating mantle. The catalyst was packed in 1 ml volume, with inert packing material at the bottom, ensuring the catalyst bed was located in the isothermal zone of the heating mantle.
[0076] In the following embodiments and comparative examples: the determination conditions for activity and selectivity used in this invention are shown in Table 1:
[0077] Table 1
[0078]
[0079] Once the above reaction conditions are stabilized, the composition of the gas at the reactor inlet and outlet is continuously measured. After volume shrinkage correction, the selectivity is calculated using the following formula:
[0080] Selective
[0081] Where ΔEO is the difference in ethylene oxide concentration between the reactor outlet gas and the inlet gas, and ΔCO2 is the difference in carbon dioxide concentration between the reactor outlet gas and the inlet gas, the average of more than 10 sets of test data is taken as the test result for that day.
[0082] In the following embodiments and comparative examples: the lateral crushing strength of the alumina carrier was measured using a DLⅡ type intelligent particle strength tester. The carrier sample was selected, and the radial crushing strength was measured and the average value was taken. The wear rate of the carrier was measured using ASTM D4058-96. The specific surface area was determined using the nitrogen physical adsorption BET method.
[0083] In the following examples and comparative examples: the particle size of the gibbsite used is 20-200 μm, and the particle size of the pseudoboehmite used is 1-120 μm.
[0084] Comparative Example 1
[0085] 430.9 g of gibbsite, 130.0 g of pseudoboehmite, 4.1 g of barium oxalate, 56.0 g of petroleum coke, 2.0 g of silica, and 4.3 g of zirconium hydroxide were weighed and mixed evenly. The mixture was then transferred to a kneader, and dilute nitric acid (nitric acid:water = 2:9, volume ratio) was added until a paste that could be extruded was formed. The paste was then placed in an extruder and extruded into seven-hole columnar materials. These materials were dried at 100°C for 30 hours to reduce the free water content to below 10%. The dried seven-hole columnar materials were then calcined in a natural gas kiln at 1525°C for 5 hours. Finally, they were cooled to room temperature to obtain the α-alumina support. The α-alumina support prepared in Comparative Example 1 was designated Ccar-1, and its relevant physical properties are shown in Table 2.
[0086] Examples 1-5 illustrate the preparation of the alumina support provided by the present invention.
[0087] Example 1
[0088] Preparation of high specific surface area α-Al2O3: SB powder was dried at 80℃ for 19 h, then placed in a 500 mL corundum grinding jar with a 2 cm diameter agate grinding ball and ball-milled at a set power of 40 Hz for 15 h to obtain high specific surface area α-Al2O3, designated Al2O3-HBET. RT The specific surface area of the material, determined by the nitrogen physical adsorption BET method, was 97.3 m². 2 / g.
[0089] Weigh out 380.0g of gibbsite (Al₂O₃ trihydrate), 130.0g of pseudoboehmite, and 57.0g of Al₂O₃-HBET. RT 4.1g barium oxalate, 56.0g petroleum coke, 2.0g silica, and 4.3g zirconium hydroxide were mixed evenly and then transferred to a kneader. Dilute nitric acid (nitric acid:water = 2:9, volume ratio) was added until a paste that could be extruded was formed. The paste was then placed in an extruder and extruded into seven-hole columnar materials. The materials were dried at 100°C for 30 hours to reduce the free water content to below 10%. The dried seven-hole columnar materials were then calcined in a natural gas kiln at 1480°C for 5 hours. Finally, the materials were cooled to room temperature to obtain the α-alumina support. The α-alumina support prepared in Example 1 was designated Scar-1, and its relevant physical properties are shown in Table 2.
[0090] Example 2
[0091] Preparation of high specific surface area α-Al2O3: SB powder was dried at 100℃ for 16 h, then placed in a 500 mL corundum grinding jar with a 2 cm diameter agate grinding ball and ball-milled at a set power of 30 Hz for 24 h. Afterward, it was calcined at 400℃ for 4 h to obtain high specific surface area α-Al2O3, designated Al2O3-HBET. 400 The specific surface area of the material, determined by the nitrogen physical adsorption BET method, was 80.1 m². 2 / g.
[0092] Weigh out 380.0g of gibbsite, 130.0g of pseudoboehmite, and 66.3g of Al₂O₃-HBET. 400 4.1g barium oxalate, 56.0g petroleum coke, 2.0g silicon dioxide, and 4.3g zirconium hydroxide were mixed evenly and then transferred to a kneader. Dilute nitric acid (nitric acid:water = 2:9, volume ratio) was added until a paste that could be extruded was formed. The paste was then placed in an extruder and extruded into seven-hole columnar materials. The materials were dried at 100°C for 30 hours to reduce the free water content to below 10%. The dried seven-hole columnar materials were then calcined in a natural gas kiln at 1480°C for 5 hours. Finally, the materials were cooled to room temperature to obtain the α-alumina support. The α-alumina support prepared in Example 2 was designated Scar-2, and its relevant physical properties are shown in Table 2.
[0093] Example 3
[0094] Preparation of high specific surface area α-Al2O3: SB powder was dried at 100℃ for 16 h, then placed in a 500 mL corundum grinding jar with a 2 cm diameter agate grinding ball and ball-milled at a set power of 30 Hz for 24 h. Afterward, it was calcined at 800℃ for 2 h to obtain high specific surface area α-Al2O3, designated Al2O3-HBET. 800 The specific surface area of the material, determined by the nitrogen physical adsorption BET method, was 67.7 m². 2 / g.
[0095] Weigh out 380.0g of gibbsite, 130.0g of pseudoboehmite, and 68.1g of Al₂O₃-HBET. 8004.1g barium oxalate, 56.0g petroleum coke, 2.0g silica, and 4.3g zirconium hydroxide were mixed evenly and then transferred to a kneader. Dilute nitric acid (nitric acid:water = 2:9, volume ratio) was added until a paste that could be extruded was formed. The paste was then placed in an extruder and extruded into seven-hole columnar materials. The materials were dried at 100°C for 30 hours to reduce the free water content to below 10%. The dried seven-hole columnar materials were then calcined in a natural gas kiln at 1470°C for 4.5 hours. Finally, the materials were cooled to room temperature to obtain the α-alumina support. The α-alumina support prepared in Example 3 was designated Scar-3, and its relevant physical properties are shown in Table 2.
[0096] Example 4
[0097] Preparation of high specific surface area α-Al₂O₃: SB powder was dried at 90℃ for 14 h, then placed in a 500 mL corundum grinding jar with a 2 cm diameter agate grinding ball and ball-milled at a set power of 35 Hz for 22 h. Afterward, it was calcined at 1000℃ for 2 h to obtain high specific surface area α-Al₂O₃, designated Al₂O₃-HBET. 1000 The specific surface area of the material, determined by the nitrogen physical adsorption BET method, was 49.4 m². 2 / g.
[0098] Weigh out 380.0g of gibbsite, 130.0g of pseudoboehmite, and 50.9g of Al₂O₃-HBET. 1000 4.1g barium oxalate, 56.0g petroleum coke, 2.0g silica, and 4.3g zirconium hydroxide were mixed evenly and transferred to a kneader. Dilute nitric acid (nitric acid:water = 2:9, volume ratio) was added until a paste that could be extruded was formed. The paste was then placed in an extruder and extruded into seven-hole columnar materials. These materials were dried at 100°C for 30 hours to reduce the free water content to below 10%. The dried seven-hole columnar materials were then calcined in a natural gas kiln at 1470°C for 4.5 hours. Finally, they were cooled to room temperature to obtain the α-alumina support. The α-alumina support prepared in Example 4 was designated Scar-4, and its relevant physical properties are shown in Table 2.
[0099] Example 5
[0100] Preparation of high specific surface area α-Al2O3: SB powder was dried at 90℃ for 14 h, then placed in a 500 mL corundum grinding jar with a 2 cm diameter agate grinding ball and ball-milled at a set power of 35 Hz for 22 h. Afterward, it was calcined at 1200℃ for 2 h to obtain high specific surface area α-Al2O3, designated Al2O3-HBET. 1200 The specific surface area of the material, determined by the nitrogen physical adsorption BET method, was 37.0 m². 2 / g.
[0101] Weigh out 380.0g of gibbsite, 130.0g of pseudoboehmite, and 50.9g of Al₂O₃-HBET. 1200 4.1g barium oxalate, 56.0g petroleum coke, 2.0g silicon dioxide, and 4.3g zirconium hydroxide were mixed evenly and transferred to a kneader. Dilute nitric acid (nitric acid:water = 2:9, volume ratio) was added until a paste that could be extruded was formed. The paste was then placed in an extruder and extruded into seven-hole columnar materials. The materials were dried at 100°C for 30 hours to reduce the free water content to below 10%. The dried seven-hole columnar materials were then calcined in a natural gas kiln at 1460°C for 4.5 hours. Finally, the materials were cooled to room temperature to obtain the α-alumina support. The α-alumina support prepared in Example 5 was designated Scar-5, and its relevant physical properties are shown in Table 2.
[0102] Table 2
[0103]
[0104] Catalyst preparation example:
[0105] Weigh 140g of silver nitrate and dissolve it in 150ml of deionized water. Weigh 64g of ammonium oxalate and dissolve it in 520ml of deionized water to obtain silver nitrate solution and ammonium oxalate solution. Mix the two solutions under vigorous stirring to form a white silver oxalate precipitate. Aging for more than 30 minutes, filtering, and washing the precipitate with deionized water until no nitrate ions are present. The filter cake contains approximately 60% silver and 15% water. Add 82g of n-propylamine and 75g of deionized water to a stirred glass flask to prepare a mixture. Slowly add the prepared silver oxalate paste (the filter cake obtained above) to the mixture, stirring continuously until completely dissolved. The amount of silver oxalate paste added should make the impregnation solution contain 22% silver (by mass). Then, add 0.8g of cesium acetate, 0.5g of barium acetate, and 0.5g of ammonium perrhenate in sequence, and then add deionized water to make the total mass of the solution reach 400g. Mix well to prepare the impregnation solution for later use. Take 20g of each of the Ccar-1, Scar-1, Scar-2, Scar-3, Scar-4, and Scar-5 supports and place them into a vacuum-capable container. Pour in the prepared impregnation solution to immerse the supports, and evacuate to below 10mmHg. Maintain this for approximately 30 minutes, then filter to remove excess solution. Finally, place the impregnated supports in air at 320℃ and heat for 3 minutes. After cooling, the silver catalyst is prepared. The Ccar-1, Scar-1, Scar-2, Scar-3, Scar-4, and Scar-5 supports correspond to the catalyst numbers Ccat-1, Scat-1, Scat-2, Scat-3, Scat-4, and Scat-5.
[0106] Catalyst performance evaluation:
[0107] The activity and selectivity of the prepared catalyst samples at different times were determined using the microreactor evaluation device described above under the aforementioned process conditions. The test results are listed in Table 3.
[0108] Table 3
[0109]
[0110] Comparing the data in Tables 2 and 3, it can be seen that adding high specific surface area α-Al₂O₃, existing in the form of nano-sized particles and maintaining a uniform dispersion, as an independent aluminum source to the α-alumina support not only effectively promotes the sintering process of the α-alumina support and reduces the calcination temperature to some extent, but also improves the wear resistance and compressive strength of the support to varying degrees. By adjusting the specific surface area and the amount of high specific surface area α-Al₂O₃ material added, the compressive strength and wear rate of the support can be effectively controlled, while maintaining a matching specific surface area, thus realizing the beneficial effect of high specific surface area α-Al₂O₃ on the support for silver catalysts. Furthermore, since the high specific surface area α-Al₂O₃ material does not introduce other impurity elements into the silver catalyst support, the silver catalyst prepared on this support exhibits good activity and selectivity in the ethylene epoxidation to ethylene oxide reaction, without adversely affecting the catalyst performance.
[0111] The various embodiments of the present invention have been described above. These descriptions are exemplary and not exhaustive, nor are they limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. An α-alumina porous ceramic support for a silver catalyst used in the oxidation of ethylene to produce ethylene oxide, characterized in that, The α-alumina porous ceramic support is prepared by a method comprising the following steps: (1) Trihydrate Al₂O₃, pseudoboehmite, high specific surface area α-Al₂O₃, alkaline earth metal compound, pore-forming agent, zirconium-containing compound, and silicon-containing compound are mixed uniformly to obtain a solid mixture; the solid mixture, binder, and optionally water are mixed to obtain the α-alumina carrier precursor mixture; wherein the specific surface area of the high specific surface area α-Al₂O₃ is 12-220 m² / g. 2 / g; (2) The α-alumina carrier precursor mixture is shaped, dried and calcined to obtain the α-alumina porous ceramic carrier.
2. The α-alumina porous ceramic carrier according to claim 1, wherein, The specific surface area of the high specific surface area α-Al₂O₃ is 12-200 m². 2 / g, preferably 15-150m 2 / g.
3. The α-alumina porous ceramic support according to claim 1 or 2, wherein, The high specific surface area α-Al2O3 was prepared by ball milling or ball milling-calcination method; Preferably, the high specific surface area α-Al2O3 is prepared by a method comprising the following steps: drying, ball milling and optionally calcining SB powder to obtain the high specific surface area α-Al2O3.
4. The α-alumina porous ceramic support according to claim 3, wherein, The drying temperature is 80-140℃, and the time is 5-24 hours; The ball milling process uses agate grinding balls; the ball milling conditions are ball milling at 20-60Hz for 15-30 hours. The roasting temperature is 25-1500℃, and the time is 0-8h.
5. The α-alumina porous ceramic support according to claim 1, wherein, Based on the total weight of the solid mixture, the content of the high specific surface area α-Al₂O₃ is 0.01-20 wt%, preferably 0.03-15 wt%, more preferably 0.05-12 wt%; the content of the trihydrate Al₂O₃ is 40-90 wt%, preferably 55-85 wt%; the content of the pseudoboehmite is 10-55 wt%, preferably 15-50 wt%; the content of the pore-forming agent is 5-30 wt%; the content of the alkaline earth metal compound is 0.1-5 wt%; the content of the zirconium-containing compound is 0.01-5 wt%; and the content of the silicon-containing compound is 0.01-1 wt%.
6. The α-alumina porous ceramic support according to claim 1, wherein, The trihydrate Al2O3 is selected from at least one of trihydrate gibbsite, argillaceous gibbsite, and balsamic gibbsite. The pore-forming agent is selected from at least one of petroleum coke, carbon powder, graphite, rosin, polyethylene, and polypropylene; The alkaline earth metal compound is selected from at least one of the following: oxides, hydroxides, acetates, sulfates, nitrates, and oxalates of alkaline earth metals. The zirconium-containing compound is at least one of zirconium dioxide, zirconium hydroxide, and zirconium silicate. The silicon-containing compound is silicon dioxide and / or silicate; Preferably, the particle size of the trihydrate Al2O3 is 20–200 μm, and the particle size of the pseudoboehmite is 1–120 μm.
7. The α-alumina porous ceramic support according to claim 1, wherein, The α-alumina porous ceramic carrier has at least one of the following characteristics: α-Al₂O₃ content of 90 wt% or more; lateral crushing strength of 50–200 N / particle, preferably 55–190 N / particle; and specific surface area of 0.4–3.0 m². 2 / g, preferably 0.5~2.1m 2 / g; wear rate 2–13%.
8. The method for preparing the α-alumina porous ceramic support according to any one of claims 1-7, characterized in that, The preparation method includes: S1. Preparing an α-alumina carrier precursor mixture: mixing Al2O3 trihydrate, boehmite, high specific surface area α-Al2O3, alkaline earth metal compound, pore-forming agent, zirconium-containing compound and silicon-containing compound uniformly to obtain a solid mixture; mixing the solid mixture, binder and optional water to obtain the α-alumina carrier precursor mixture; S2. The α-alumina carrier precursor mixture obtained in step S1 is shaped, dried and calcined to obtain the α-alumina porous ceramic carrier.
9. The preparation method according to claim 8, wherein, In S2, the calcination temperature is 700-1800℃, preferably 1100-1700℃, and more preferably 1200-1600℃.
10. A silver catalyst for the oxidation of ethylene to produce ethylene oxide, characterized in that, The silver catalyst comprises: the α-alumina porous ceramic support as described in any one of claims 1-7 and the active component silver supported on the α-alumina porous ceramic support; Preferably, the silver catalyst further includes: Alkali metals and / or alkaline earth metals, or compounds based on alkali metals and / or alkaline earth metals; Rhenium metal and / or rhenium-based compounds; and Optionally, the rhenium co-catalyst is preferably selected from at least one metal selected from chromium, molybdenum, tungsten and manganese, and / or selected from at least one metal compound selected from chromium metal compound, molybdenum metal compound, tungsten metal compound and manganese metal compound.
11. A method for producing ethylene oxide by epoxidation of ethylene, characterized in that, The method includes: subjecting ethylene to an ethylene epoxidation reaction in the presence of the silver catalyst described in claim 10 to obtain ethylene oxide.
Citation Information
Patent Citations
Process for treating a catalyst, the catalyst, and use of the catalyst
US20070185339A1
Alumina compositions of improved strength useful as catalyst supports.
US4428863A
Alkylene oxide catalyst and process
WO1996023585A1