Anti-carbon deposition catalyst for methyl methacrylate synthesis and preparation method thereof

By using an Al₂O₃-MgO-ZrO₂ composite support and a Cs₂O catalyst, the problem of catalyst deactivation due to carbon buildup was solved, achieving efficient, stable, and low-cost operation of MMA production.

CN123127977APending Publication Date: 2026-11-20QINGDAO HUICHENG PETROCHEM TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611389911.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-09
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In existing MMA production processes, solid alkali catalysts are prone to carbon buildup and deactivation, resulting in short single-pass lifespans, which affect the stable operation of the equipment and production costs.

Method used

A catalyst using Al₂O₃-MgO-ZrO₂ as the ternary composite support and Cs₂O as the active component was developed. The support structure and distribution of the active component were optimized through hydrothermal treatment and stepwise rinsing techniques to form a stable catalyst.

Benefits of technology

It achieves high efficiency, stability and long lifespan of the catalyst, improves MMA yield and selectivity, reduces production and maintenance costs, and is suitable for industrial continuous production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123127977A_ABST
    Figure CN123127977A_ABST
Patent Text Reader

Abstract

The application discloses a kind of methyl methacrylate synthesis with anti-carbon deposition catalyst and preparation method thereof, belong to catalytic material technical field.The catalyst with Al2O3-MgO-ZrO2 as ternary composite carrier, Cs2O is active component;When preparing, pseudo-boehmite, light magnesium oxide, monoclinic zirconium oxide are mixed with starch granulation, and the carrier precursor is hydrothermally treated to water vapor atmosphere, then it is washed by ammonia water, cesium nitrate, zirconium nitrate step by step, and the finished product catalyst is prepared after drying high-temperature calcination.The catalyst of the application is used for methyl propionate and formaldehyde condensation to prepare MMA reaction, with the advantages of high yield, good selectivity, strong anti-carbon deposition capacity, long single-pass service life, simple and controllable preparation process, suitable for fixed bed continuous industrial production, and wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of organic chemical catalysts, and in particular to an anti-coking catalyst for the synthesis of methyl methacrylate and its preparation method. Background Technology

[0002] Methyl methacrylate (MMA) is a key monomer in the production of products such as plexiglass, acrylic resins, coatings, and adhesives. It is widely used in chemical, building materials, electronics, and automotive industries, and market demand continues to grow steadily. Current mainstream MMA production processes include the acetone cyanohydrin method and the isobutylene oxidation method. These processes generally suffer from problems such as reliance on petroleum resources for raw materials, lengthy processes, significant environmental pressures, and high production costs, making it difficult to meet the requirements of modern chemical industry for green, low-carbon, efficient, and economical development.

[0003] The Alpha process, starting with basic coal chemical and petrochemical feedstocks such as ethylene, CO, methanol, and formaldehyde, features high atom economy, low carbon emissions, and significant raw material cost advantages. Production costs are reduced by approximately 40% compared to traditional routes, making it a core development direction for the upgrading and large-scale production of MMA. The process mainly consists of two steps: the first step involves the carbonylation reaction of ethylene, methanol, and CO to synthesize methyl propionate; the second step involves the condensation of methyl propionate and formaldehyde under the action of a solid alkali catalyst to produce MMA. The second condensation reaction is the key step determining the overall process efficiency and product economics.

[0004] Currently, most solid base catalysts used in industrial applications are based on Cs / Zr and Cs-Zr-Sb systems, which generally suffer from defects such as unreasonable support pore structure and mismatch between surface acid-base distribution and reaction requirements. During continuous reactions, carbon deposits easily form on the catalyst surface and rapidly accumulate, clogging pores and covering active sites, leading to rapid catalytic activity decay. Single-pass lifespan is generally less than 700 hours, requiring frequent regeneration or catalyst replacement, severely impacting the continuous and stable operation of the unit, significantly increasing production energy consumption and operating costs, and becoming a core bottleneck restricting the large-scale promotion of the Alpha MMA process.

[0005] To address the problems of traditional catalysts such as easy carbon deposition and deactivation, and short single-pass life, there is an urgent need to develop a special catalyst with excellent anti-carbon deposition performance, high activity and selectivity, and long-term stable operation. By optimizing the support composition, pore structure and active component loading method, the catalytic performance and service life can be improved simultaneously to meet the actual needs of continuous industrial production of Alpha MMA. Summary of the Invention

[0006] The purpose of this invention is to provide an anti-coking catalyst for the synthesis of methyl methacrylate and its preparation method, so as to solve the problems existing in the prior art.

[0007] To achieve the above objectives, the present invention provides the following solution:

[0008] This invention provides an anti-coking catalyst for MMA synthesis, wherein the catalyst uses Al2O3-MgO-ZrO2 as a ternary composite support and Cs2O as the active component; the ratio of the ternary composite support is Al2O3:MgO:ZrO2=(69.5~92.7):(10~20):(3~10), and the Cs2O loading is 0.5-2.0% of the molar amount of ZrO2.

[0009] The present invention also provides a method for preparing the above-mentioned anti-coking catalyst for MMA synthesis, comprising the following steps:

[0010] (1) Mix boehmite, light magnesium oxide, monoclinic zirconium oxide and starch in a mass ratio of (60-80):(10-20):(3-10):(1-5) to obtain a dry mixture.

[0011] (2) Add NaOH solution to the dry mixture, stir and granulate to obtain the precursor;

[0012] (3) The precursor is placed in a water vapor atmosphere and hydrothermally treated at 90-110°C for 40-55 min to obtain the carrier precursor;

[0013] (4) The carrier precursor is immersed in water at 60-80℃, dried, and then sequentially rinsed with a first ammonia solution, a cesium nitrate solution, a second ammonia solution, and a zirconium nitrate solution, and dried after each rinse; by adjusting the amount of cesium nitrate and zirconium nitrate, the molar amount of Cs2O in the final anti-coking catalyst for MMA synthesis is 0.5% to 2.0% of the molar amount of ZrO2;

[0014] (5) The product washed in step (4) is dried and then calcined at 320-400°C to obtain the anti-coking catalyst for MMA synthesis.

[0015] Furthermore, the mass concentration of the NaOH solution is 10-20%; the amount of NaOH solution added is 15% to 25% of the total mass of the dry mixture.

[0016] Furthermore, the calcination time in step (5) is 2-3.5h, and the drying temperature in step (5) is 100-120℃.

[0017] Further, in step (4), the mass fraction of the first ammonia solution and the second ammonia solution is 5% to 10%, the concentration of the cesium nitrate solution is 0.05 to 0.2 mol / L, and the concentration of the zirconium nitrate solution is 0.1 to 0.3 mol / L.

[0018] Furthermore, the rinsing time for the first ammonia solution is 10-20 min, the rinsing time for the cesium nitrate solution is 20-30 min, the rinsing time for the second ammonia solution is 10-20 min, and the rinsing time for the zirconium nitrate solution is 20-30 min; after each rinsing, the solution is dried until no free droplets remain.

[0019] Further, in step (4), the amount of cesium nitrate solution used is 1.5-3.0 times the mass of the carrier precursor, and the amount of zirconium nitrate solution used is 1.5-3.0 times the mass of the carrier precursor.

[0020] This invention selects boehmite, light magnesium oxide, and monoclinic zirconium oxide as precursors and basic components of a ternary composite support. Boehmite, as a precursor of Al2O3, is converted to Al2O3 after subsequent calcination and dehydration, providing a stable framework structure and suitable specific surface area for the catalyst. Light magnesium oxide serves directly as a source of MgO, used to regulate the alkalinity of the catalyst surface, optimize the adsorption and activation performance of reactants during the reaction, and inhibit coking. Monoclinic zirconium oxide, as the initial source of ZrO2, not only forms a stable ternary composite support with Al2O3 and MgO, improving the structural stability of the support, but also synergistically enhances the catalytic activity of the catalyst with the active components. Starch serves as a pore-forming agent, used to regulate the pore structure of the catalyst, providing smooth diffusion channels for reactants and products, further improving the anti-coking ability. NaOH solution, as a liquid phase, can form liquid bridges between solid powder particles (boehmite, magnesium oxide, zirconium oxide, and starch). Compared with pure water, NaOH solution typically has a higher viscosity, which is beneficial for forming more stable liquid bridges. Therefore, in a rotating granulator, it is easier to agglomerate powder into spheres, resulting in particles with more uniform particle size. Additionally, NaOH solution is a strong alkali, which can cause a certain degree of extension or gelatinization of starch molecular chains, enhancing the effect of starch as a temporary framework and binder, making the particles more stable before subsequent processing. Cesium nitrate and zirconium nitrate, as active components and zirconium source supplementary precursors, provide the material basis for the formation of Cs₂O active components and additional ZrO₂ in the final catalyst. Ammonia solution is used to rinse and adjust the surface properties of the support precursor, promoting uniform loading of the active component precursor.

[0021] In this invention, the precursor is subjected to hydrothermal treatment at 95–110°C for 40–55 min in a steam atmosphere. This step is crucial for optimizing the microstructure of the carrier. During the hydrothermal treatment, the steam promotes the initial dehydration and crystal transformation of boehmite, while simultaneously enabling a closer interaction between the MgO, monoclinic ZrO2, and Al2O3 precursors. This optimizes the microstructure of the ternary composite carrier and enhances its thermal stability and structural integrity. Furthermore, the hydrothermal environment can initially clear the initial pores formed by starch pore formation, creating conditions for the uniform loading of subsequent active components, ultimately resulting in a structurally stable and uniformly dispersed carrier precursor.

[0022] In this invention, the precursor carrier is wetted with water, dried, and then sequentially rinsed with a first ammonia solution, a cesium nitrate solution, a second ammonia solution, and a zirconium nitrate solution, with each rinse being dried. This step is crucial for controlling the distribution of active components and the final composition of the catalyst. First, rinsing with the ammonia solution adjusts the charge properties of the precursor carrier surface, creating suitable adsorption sites that facilitate the uniform adsorption of the two precursor salts, cesium nitrate and zirconium nitrate. Subsequently, rinsing with the cesium nitrate solution removes Cs... + Loaded on the surface and pores of the support, the zirconium nitrate solution is used to rinse and replenish the Zr source. The loading of the two precursor salts is controlled by precisely adjusting the solution concentration and dosage to ensure that the molar amount of Cs2O in the catalyst after final calcination is 0.5% to 2.0% of the total ZrO2 molar amount. The total ZrO2 includes two parts: the monoclinic zirconium oxide fed in step (1) and the ZrO2 generated by the subsequent calcination and decomposition of zirconium nitrate in step (4). The stepwise rinsing method can avoid mutual interference between the two precursor salts and ensure that the active component Cs2O and the supplemented ZrO2 are uniformly dispersed on the surface of the support, forming a synergistic effect with the ternary support, thereby improving the catalytic activity and anti-coking ability.

[0023] Step (5) of this invention, which involves drying the washed product and calcining it at 320–400°C, is a crucial step in the final formation and component transformation of the catalyst. The drying process removes free moisture from the material, preventing rapid evaporation of moisture during calcination and thus preventing catalyst particle cracking. During the high-temperature calcination, on the one hand, boehmite is completely dehydrated and converted into Al2O3, forming a stable Al2O3-MgO-ZrO2 ternary composite support with MgO, the initial monoclinic ZrO2, and ZrO2 generated by the decomposition of zirconium nitrate. On the other hand, cesium nitrate is thermally decomposed into Cs2O active component, ultimately forming the target catalyst with Al2O3-MgO-ZrO2 as the ternary composite support and Cs2O as the active component. Simultaneously, starch is completely decomposed and volatilized during calcination, forming a uniform pore structure inside the catalyst, further optimizing the specific surface area, pore volume, and pore size distribution of the catalyst, providing sufficient active sites and diffusion channels for the condensation reaction of methyl propionate and formaldehyde, ultimately achieving the technical effects of high product yield, high selectivity, anti-coking, and long lifespan.

[0024] The present invention further provides a method for synthesizing MMA, using the above-mentioned anti-coking catalyst for MMA synthesis as the catalytic medium; further, methyl propionate and formaldehyde are continuously condensed to prepare MMA under the conditions of reaction temperature 280-380℃, reaction pressure 0.8-1.2MPa, and methyl propionate:formaldehyde = 1:1.2-1.5 (molar ratio).

[0025] The present invention discloses the following technical effects:

[0026] The anti-coking catalyst for MMA synthesis provided by this invention effectively solves the problems of low activity, easy coking, and short lifespan of traditional catalysts.

[0027] This invention's catalyst, through a scientifically designed stepwise loading process and optimized steps such as hydrothermal treatment and calcination, achieves uniform dispersion of active components, significantly improving catalytic efficiency and stability. MMA yield remains consistently above 88%, selectivity exceeds 95%, and it exhibits outstanding resistance to coking, enabling long-term stable operation. Compared to traditional catalysts, it boasts stronger structural stability, a longer service life, and eliminates the need for frequent replacements, effectively reducing production and maintenance costs.

[0028] The preparation process of this invention is simple and controllable, requires no complex equipment, can be directly adapted to existing fixed-bed production processes without modifying existing equipment, meets the needs of industrial continuous production, has excellent catalytic performance and industrial applicability, has high value for promotion and application, and can significantly improve MMA production efficiency and reduce production costs. Attached Figure Description

[0029] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0030] Figure 1 The pore size distribution curves are for the catalysts prepared in Examples 1-5. Detailed Implementation

[0031] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0032] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Any stated value or intermediate value within a stated range, as well as each smaller range between any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.

[0033] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.

[0034] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be readily apparent to those skilled in the art. This specification and embodiments are merely exemplary.

[0035] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.

[0036] It should be noted that any aspects not described in detail in this invention are conventional practices in the field and are not the focus of this invention.

[0037] The catalyst of this invention uses Al2O3-MgO-ZrO2 as a ternary composite support and Cs2O as the active component; wherein, the Cs2O loading is 0.5-2.0% of the molar amount of ZrO2, the catalyst has a specific surface area of ​​140-210 m² / g, a pore volume of 0.3-0.5 cm³ / g, and an average pore size of 10-16 nm.

[0038] Example 1

[0039] This embodiment provides a method for preparing an anti-coking catalyst for MMA synthesis, the steps of which are as follows:

[0040] (1) According to the raw material feeding mass ratio of 68:18:8:2, add pseudoboehmite (Al2O3 precursor), light magnesium oxide, monoclinic zirconium oxide and starch to a tiltable rotary granulator and stir at room temperature for 40 min until the mixture is uniform to obtain dry mixed material.

[0041] (2) Add 15% by mass of dilute NaOH solution (20% of the total mass of dry mixed material) to the above dry mixed material, stir at 4000 r / min for 10 min, then adjust to 1500 r / min for granulation for 20 min to obtain a particle precursor with a particle size of 3-4 mm.

[0042] (3) The particle precursor was placed in a normal pressure water vapor atmosphere and hydrothermally treated at 100°C for 45 min to obtain the carrier precursor;

[0043] (4) Cool the carrier precursor to room temperature, immerse it in 70°C deionized water, and dry it through a plate and frame filter until there is no free water. Then rinse it sequentially with 8% ammonia water for 15 min, 0.1 mol / L cesium nitrate solution (the amount of cesium nitrate solution is 2.6 times the mass of the carrier precursor) for 25 min, 8% ammonia water for 15 min, and 0.2 mol / L zirconium nitrate solution (the amount of zirconium nitrate solution is 2.5 times the mass of the carrier precursor) for 25 min. After each rinse, dry it until there are no free droplets. (Among them, cesium nitrate and zirconium nitrate are used as active component precursors and are loaded at 1.0% of the final Cs2O loading amount of ZrO2 molar amount).

[0044] (5) The washed material was dried in hot air circulation at 110℃ for 3 h, and then heated to 350℃ at a rate of 5℃ / min and calcined for 2.5 h to obtain catalyst A.

[0045] Example 2

[0046] This embodiment provides a method for preparing an anti-coking catalyst for MMA synthesis, the steps of which are as follows:

[0047] (1) According to the raw material feeding mass ratio of 65:20:8:2, add pseudoboehmite (Al2O3 precursor), light magnesium oxide, monoclinic zirconium oxide and starch into a tiltable rotary granulator and stir at room temperature for 45 min until the mixture is uniform to obtain dry mixed material.

[0048] (2) Add 20% by mass of dilute NaOH solution to the above dry mixed material (the amount added is 22% of the total mass of the dry mixed material), stir at 4000 r / min for 10 min, then adjust to 1500 r / min for granulation for 20 min to obtain a particle precursor with a particle size of 2-3 mm.

[0049] (3) The particle precursor was placed in a normal pressure water vapor atmosphere and hydrothermally treated at 105℃ for 50 min to obtain the carrier precursor;

[0050] (4) Cool the carrier precursor to room temperature, immerse it in 75°C deionized water, and dry it through a plate and frame filter until there is no free water. Then rinse it sequentially with 10% ammonia water for 12 min, 0.15 mol / L cesium nitrate solution (the amount of cesium nitrate solution is 1.5 times the mass of the carrier precursor) for 20 min, 10% ammonia water for 12 min, and 0.25 mol / L zirconium nitrate solution (the amount of zirconium nitrate solution is 1.5 times the mass of the carrier precursor) for 20 min. After each rinse, dry it until there are no free droplets. (Among them, cesium nitrate and zirconium nitrate are used as active component precursors and are loaded at 1.0% of the final Cs2O loading amount of ZrO2 molar amount).

[0051] (5) The washed material was dried in hot air circulation at 110℃ for 3 h, and then heated to 360℃ at a rate of 5℃ / min and calcined for 2.5 h to obtain catalyst B.

[0052] Example 3

[0053] This embodiment provides a method for preparing an anti-coking catalyst for MMA synthesis, the steps of which are as follows:

[0054] (1) According to the raw material feeding mass ratio of 66:17:10:2, add pseudoboehmite (Al2O3 precursor), light magnesium oxide, monoclinic zirconium oxide and starch to a tiltable rotary granulator and stir at room temperature for 35 minutes until the mixture is uniform to obtain dry mixed material.

[0055] (2) Add 15% by mass of dilute NaOH solution to the above dry mixture (the amount added is 20% of the total mass of the dry mixture), stir at 4000 r / min for 10 min, then adjust to 1500 r / min for granulation for 18 min to obtain a particle precursor with a particle size of 3–4 mm.

[0056] (3) The particle precursor was placed in a normal pressure water vapor atmosphere and hydrothermally treated at 95°C for 50 min to obtain the carrier precursor;

[0057] (4) Cool the carrier precursor to room temperature, immerse it in 70°C deionized water, and dry it through a plate and frame filter until there is no free water. Then rinse it sequentially with 8% ammonia water for 16 min, 0.15 mol / L cesium nitrate solution (the amount of cesium nitrate solution is 1.8 times the mass of the carrier precursor) for 28 min, 8% ammonia water for 16 min, and 0.3 mol / L zirconium nitrate solution (the amount of zirconium nitrate solution is 2.0 times the mass of the carrier precursor) for 28 min. After each rinse, dry it until there are no free droplets. (Among them, cesium nitrate and zirconium nitrate are used as active component precursors and are loaded at 1.5% of the final Cs2O loading amount of ZrO2 molar amount).

[0058] (5) The washed material was dried in hot air circulation at 110℃ for 3 h, and then heated to 350℃ at a rate of 5℃ / min and calcined for 3 h to obtain catalyst C.

[0059] Example 4

[0060] This embodiment provides a method for preparing an anti-coking catalyst for MMA synthesis, the steps of which are as follows:

[0061] (1) According to the raw material feeding mass ratio of 72:16:7:1, add boehmite (Al2O3 precursor), light magnesium oxide, monoclinic zirconium oxide and starch to a tiltable rotary granulator and stir at room temperature for 40 min until the mixture is uniform to obtain dry mixed material.

[0062] (2) Add 12% dilute NaOH solution (18% of the total mass of the dry mixture) to the above dry mixture, stir at 4000 r / min for 10 min, then adjust to 1500 r / min for granulation for 22 min to obtain a particle precursor with a particle size of 4–5 mm.

[0063] (3) The particle precursor was placed in a normal pressure water vapor atmosphere and hydrothermally treated at 90°C for 45 min to obtain the carrier precursor;

[0064] (4) Cool the carrier precursor to room temperature, immerse it in 65°C deionized water, and dry it through a plate and frame filter until there is no free water. Then rinse it sequentially with 5% ammonia water for 20 min, 0.05 mol / L cesium nitrate solution (the amount of cesium nitrate solution is 3.0 times the mass of the carrier precursor) for 30 min, 5% ammonia water for 20 min, and 0.15 mol / L zirconium nitrate solution (the amount of zirconium nitrate solution is 3.0 times the mass of the carrier precursor) for 30 min. After each rinse, dry it until there are no free droplets. (Among them, cesium nitrate and zirconium nitrate are used as active component precursors and are loaded at 0.5% of the final Cs2O loading amount of ZrO2 molar amount).

[0065] (5) The washed material was dried in hot air circulation at 105℃ for 4 h, and then heated to 340℃ at a rate of 5℃ / min and calcined for 3 h to obtain catalyst D.

[0066] Example 5

[0067] This embodiment provides a method for preparing an anti-coking catalyst for MMA synthesis, the steps of which are as follows:

[0068] (1) According to the raw material feeding mass ratio of 76:15:5:1, add boehmite (Al2O3 precursor), light magnesium oxide, monoclinic zirconium oxide and starch to a tiltable rotary granulator and stir at room temperature for 45 min until the mixture is uniform to obtain dry mixed material.

[0069] (2) Add 10% by mass of dilute NaOH solution to the above dry mixture (the amount added is 15% of the total mass of the dry mixture), stir at 4000 r / min for 10 min, then adjust to 1500 r / min for granulation for 25 min to obtain a particle precursor with a particle size of 3–4 mm.

[0070] (3) The particle precursor was placed in a normal pressure water vapor atmosphere and hydrothermally treated at 110℃ for 45 min to obtain the carrier precursor;

[0071] (4) Cool the carrier precursor to room temperature, immerse it in deionized water at 80°C, and dry it through a plate and frame filter until there is no free water. Then rinse it sequentially with 10% ammonia water for 14 min, 0.1 mol / L cesium nitrate solution (the amount of cesium nitrate solution is 2.2 times the mass of the carrier precursor) for 26 min, 10% ammonia water for 14 min, and 0.2 mol / L zirconium nitrate solution (the amount of zirconium nitrate solution is 1.8 times the mass of the carrier precursor) for 26 min. After each rinse, dry it until there are no free droplets. (Among them, cesium nitrate and zirconium nitrate are used as active component precursors and are loaded at 1.0% of the final Cs2O loading amount of ZrO2 molar amount).

[0072] (5) The washed material was dried in hot air circulation at 120℃ for 2 h, and then heated to 400℃ at a rate of 5℃ / min and calcined for 2 h to obtain catalyst E.

[0073] The main chemical composition of the catalyst samples in the examples is shown in Table 1.

[0074] Table 1 Chemical composition of catalyst samples in the examples

[0075]

[0076] Comparative Example 1

[0077] The only difference from Example 1 is that no starch was added during the preparation process. The other raw material ratios, process parameters and preparation steps were the same as in Example 1, and comparative catalyst F1 was obtained.

[0078] Comparative Example 2

[0079] The only difference from Example 1 is that no light magnesium oxide component is added to the raw materials, while the process parameters and preparation steps are the same as in Example 1, and comparative catalyst F2 is obtained.

[0080] Comparative Example 3

[0081] The only difference from Example 1 is that the atmospheric pressure steam atmosphere hydrothermal treatment process in step (3) is not performed. Instead, the obtained particulate precursor is directly subjected to subsequent impregnation, rinsing, drying and calcination operations without hydrothermal pretreatment. The other raw material ratios, process parameters and preparation steps are completely consistent with those in Example 1, and comparative catalyst F3 is obtained.

[0082] Comparative Example 4

[0083] The only difference from Example 1 is that step (4) of alternating stepwise rinsing with ammonia, cesium nitrate, ammonia, and zirconium nitrate is omitted. Instead, the cesium nitrate solution is impregnated using the traditional equal-volume impregnation method. Based on the same standard that the final Cs2O loading is 1.0% of the molar amount of ZrO2 in the support, the cesium nitrate solution is prepared to impregnate the support precursor in one go. The system retains only the ZrO2 component in the initial feed. The other raw material ratios, process parameters, and preparation steps are completely consistent with those in Example 1, and the comparative catalyst F4 is obtained.

[0084] Comparative Example 5

[0085] The only difference from Example 1 is that an industrial-grade Cs / Zr catalyst (Cs2O:ZrO2:SiO2 molar ratio of 1:5:5) was used, which is labeled as comparative catalyst F5.

[0086] Effect verification example

[0087] The prepared catalyst was continuously evaluated using a fixed-bed reactor. Specific evaluation conditions were: reaction temperature 380℃, reaction pressure 0.8 MPa, feedstock being a mixture of methyl propionate and formaldehyde in a molar ratio of 1:1.3, feed rate 0.25 g / min, catalyst addition 10 g, and mass hourly space velocity (WHSV) 1.5 h⁻¹. -1 .

[0088] The specific surface area, pore volume, and evaluation results of the catalysts in the examples and comparative examples are shown in Table 2.

[0089] Table 2

[0090]

[0091] The catalyst prepared by this invention is used in the condensation reaction of methyl propionate and formaldehyde to prepare MMA. The MMA yield is ≥88.6%, the selectivity is ≥95.5%, and the catalyst's single-pass life can reach more than 1160 hours. Its comprehensive performance is significantly better than that of existing traditional Cs / Zr catalysts.

[0092] This invention precisely controls the pore structure of the catalyst by using starch to create pores, moderately controls the alkalinity of the support surface by using MgO components, optimizes the microstructure of the support by using steam hydrothermal treatment, and precisely controls the dispersion state and distribution uniformity of the active components by using a stepwise rinsing loading method. These four key technologies work together to enhance each other and ensure that the catalyst has high catalytic activity, high product selectivity and excellent long-term operational stability.

[0093] Meanwhile, this invention can achieve an optimal balance between high catalytic activity, long service life and preparation cost by flexibly adjusting the distribution ratio of each raw material group. It can adapt to different working conditions and application needs of industrial production and has good prospects for industrial promotion.

[0094] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.

Claims

1. A coking-resistant catalyst for the synthesis of methyl methacrylate, characterized in that, Al2O3-MgO-ZrO2 is used as a ternary composite support, and Cs2O is used as the active component. In the ternary composite support, the mass ratio of Al2O3, MgO and ZrO2 is (69.5-92.7):(10-20):(3-10); and the Cs2O loading is 0.5-2.0% of the molar amount of ZrO2.

2. A method for preparing an anti-coking catalyst for the synthesis of methyl methacrylate as described in claim 1, characterized in that, Includes the following steps: (1) Mix boehmite, light magnesium oxide, monoclinic zirconium oxide and starch in a mass ratio of (60-80):(10-20):(3-10):(1-5) to obtain a dry mixture. (2) Add NaOH solution to the dry mixture, stir and granulate to obtain the precursor; (3) The precursor is placed in a water vapor atmosphere and hydrothermally treated at 90-110°C for 40-55 min to obtain the carrier precursor; (4) The carrier precursor is immersed in water, and then sequentially rinsed with a first ammonia solution, a cesium nitrate solution, a second ammonia solution, and a zirconium nitrate solution, and dried after each rinse; by adjusting the amount of cesium nitrate and zirconium nitrate added, the molar amount of Cs2O in the final anti-coking catalyst for the synthesis of methyl methacrylate is 0.5% to 2.0% of the molar amount of ZrO2; (5) The product after rinsing in step (4) is dried and then calcined at 320-400°C to obtain the anti-coking catalyst for the synthesis of methyl methacrylate.

3. The preparation method according to claim 2, characterized in that, The NaOH solution has a mass concentration of 10-20%; the amount of NaOH solution added is 15% to 25% of the total mass of the dry mixture.

4. The preparation method according to claim 2, characterized in that, The roasting time in step (5) is 2-3.5h.

5. The preparation method according to claim 2, characterized in that, The drying temperature in step (5) is 100-120℃.

6. The preparation method according to claim 2, characterized in that, In step (4), the mass fraction of the first ammonia solution and the second ammonia solution is 5% to 10%, the concentration of the cesium nitrate solution is 0.05 to 0.2 mol / L, and the concentration of the zirconium nitrate solution is 0.1 to 0.3 mol / L.

7. The preparation method according to claim 2, characterized in that, In step (4), add water at 60-80℃ for soaking.

8. A method for synthesizing methyl methacrylate, characterized in that, The anti-coking catalyst for the synthesis of methyl methacrylate as described in claim 1 is used as the catalytic medium.