A w-mn3o4@f-delta-mno2 heterojunction photocatalyst and a preparation method and application thereof

CN123127982APending Publication Date: 2026-11-20SICHUAN UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611231503.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

该催化剂虽然构建了异质结结构,使表面具有丰富的氧空位,但其降解机理是光催化与热催化协同降解C3H8,在常温下仅依靠光催化过程难以实现污染物的高效去除

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123127982A_ABST
    Figure CN123127982A_ABST
Patent Text Reader

Abstract

The application discloses a W-Mn3O4@F-delta-MnO2 heterojunction photocatalyst and a preparation method and application thereof. The photocatalyst is composed of W-Mn3O4 and F-delta-MnO2 with a molar ratio of 1: (5-15), the micro-particle of the photocatalyst is a spherical structure formed on a nanoflower structure which is self-assembled by nanowire Mn3O4 inlaid in MnO2 nanosheet, and two phase interfaces form a heterojunction structure. The preparation method of the heterojunction photocatalyst is that KMnO4 powder, MnSO4.H2O powder and nanowire W-Mn3O4 powder are compounded and hydrothermally synthesized to obtain a solid-phase precipitation initial substance, and the initial substance is synthesized after calcination at a certain temperature and in an air atmosphere. The photocatalyst can effectively improve photocatalytic activity, and has the advantages of simple preparation process, controllable morphology, low cost, good operability, environmental friendliness and the like, and can be used for removal of low-concentration nitrogen oxides.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of nitrogen oxide removal technology in air pollution control, specifically relating to a W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst, its preparation method, and its application. Background Technology

[0002] Nitrogen oxides (NO) x NOx is a typical air pollutant that poses significant risks to both the environment and human health. It is commonly referred to as air pollutant. x The main pollutants are NO and NO2, with NO accounting for over 95%. NO is a major air pollutant from industrial stationary sources. x There are two main methods for NO removal: wet and dry. Dry removal methods mainly include selective catalytic reduction (SCR) and non-selective catalytic reduction (NSCR). SCR is a more widely used method, but it is not economical or suitable for treating low concentrations of NO in the atmosphere.

[0003] MnO x Due to its variable valence states and unique electronic structure, MnO possesses high application potential and exhibits excellent performance in the degradation of gaseous pollutants. However, single-component catalysts are often limited by the rapid photogenerated carrier recombination rate and specific band defects, making it difficult to simultaneously achieve excellent photoelectric properties, high efficiency in photocatalytic activity, and high stability, thus hindering the efficient removal of pollutants at room temperature. Therefore, constructing heterojunctions to modulate the electronic structure of materials has become a key approach to improving the performance of MnO. x The core approach to improving the activity and stability of basic catalysts. For example, CN121534701A discloses a Mn2O3 / Mn3O4 nanosheet heterojunction catalyst, its preparation method, and its application. This catalyst was prepared by modifying a hydrothermal method, using manganese salt as a precursor, and combining ammonia and sodium hydroxide to assist in mesoporous regulation. An oxygen-vacancy-rich Mn2O3 / Mn3O4 nanosheet heterojunction catalyst was prepared by air calcination at 300-500℃, achieving a C3H8 conversion rate of 90% at 251℃. Although this catalyst constructs a heterojunction structure, resulting in abundant oxygen vacancies on the surface, its degradation mechanism involves a synergistic degradation of C3H8 through photocatalysis and thermocatalysis. At room temperature, relying solely on photocatalysis is insufficient for achieving efficient pollutant removal. Summary of the Invention

[0004] The purpose of this invention is to solve the above-mentioned problems and provide a W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst, its preparation method, and its application. This photocatalyst is composed of MnO4 with different morphologies, phase structures, and valence states. xBy assembling, a photocatalyst with a W-Mn3O4@F-δ-MnO2 heterojunction structure in which nanowires Mn3O4 (W-Mn3O4) are embedded in nanoflower MnO2 (F-δ-MnO2) was obtained. This photocatalyst can effectively improve photocatalytic activity and has the advantages of simple preparation process, controllable morphology, low cost, good operability and environmental friendliness. It can be used for the removal of low concentration nitrogen oxides.

[0005] To achieve the above objectives, on the one hand, the present invention provides a W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst, which is composed of W-Mn3O4 and F-δ-MnO2 in a molar ratio of 1: (5~15). Its micro-particles are spherical structures formed by the self-assembly of nanoflower-like structures of Mn3O4 nanowires embedded in MnO2 nanosheets, and the two phase interfaces form a heterojunction structure.

[0006] The aforementioned W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst is constructed by the self-assembly of MnO2 nanosheets into F-δ-MnO2 nanoflowers, with W-Mn3O4 nanowires embedded within these nanoflowers to form W-Mn3O4@F-δ-MnO2. The two phase interfaces form a heterojunction structure, constituting a multi-coupled charge transport network and optimizing the electronic structure. This structure can be compared to a highly efficient heterojunction with chemically bonded interfaces, lowering the charge transfer energy barrier through atomic-level channels, thereby significantly improving the photocatalytic degradation efficiency of NO. The preferred molar ratio of W-Mn3O4 to F-δ-MnO2 is 1:10.

[0007] On the other hand, the present invention also provides a method for preparing a W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst, comprising the following steps:

[0008] S1. According to the set molar ratio of W-Mn3O4 and F-δ-MnO2, KMnO4 powder, MnSO4·H2O powder and W-Mn3O4 powder are simultaneously and uniformly dispersed in deionized water to form a uniform suspension.

[0009] S2. Place the suspension obtained in step S1 in a closed environment and heat it at 150~170℃ for 11~13h. After cooling it to room temperature, perform solid-liquid separation and collect the separated solid product. Wash the obtained solid product with deionized water and dry it to obtain a dry blocky solid precipitate.

[0010] S3. Grind the solid precipitate obtained in step S2 into powder and place it in a sealed environment. Calcinate it in air at 320~400℃ for 1.5~3.0 h to obtain the W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst.

[0011] In the preparation method of the above W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst, in step S1, the molar ratio of KMnO4 powder and MnSO4·H2O powder is (4~6):1.

[0012] Furthermore, by high-speed stirring, homogenization, or ultrasonic treatment, it is uniformly dispersed in the liquid to form a homogeneous suspension. The present invention preferably uses magnetic stirring to form a homogeneous suspension. The magnetic stirring time can be set according to conventional parameters.

[0013] In the preparation method of the above-mentioned W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst, the purpose of solid-liquid separation in step S2 is to obtain the separated solid product. While satisfying the purpose of solid-liquid separation, the solid-liquid separation method can be selected from conventional methods in the art, preferably centrifugal precipitation or Buchner filtration. The solid-liquid separation product is then washed with deionized water to remove unreacted material adsorbed on the surface of the solid product, and after thorough washing, it is dried at 70-90°C.

[0014] In the preparation method of the above-mentioned W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst, in step S3, the calcination heating rate can be set according to the conventional calcination heating rate in the art, preferably 5 ℃ / min.

[0015] The preparation method of the above-mentioned W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst includes the following steps:

[0016] S11. KMnO4 and (NH4)2SO4 were dissolved in deionized water under stirring at a molar ratio of (1~3):1 to obtain a dark brown suspension.

[0017] S12. Place the suspension obtained in step S11 in a closed environment and heat it at 180~200℃ for 20~28h. After cooling it to room temperature, perform solid-liquid separation and collect the separated solid product. Wash the obtained solid product with deionized water and dry it to obtain a dry blocky solid precipitate α-MnO2 intermediate.

[0018] S13. Mix solid urea and the α-MnO2 intermediate obtained in step S12 at a mass ratio of (0.6-1.0):1 and grind them to obtain a uniform mixed powder. Calcinate the mixed powder in a nitrogen atmosphere at 350-450℃ for 2-4 h to obtain W-Mn3O4.

[0019] The above-mentioned method for preparing W-Mn3O4 first involves preparing an α-MnO2 intermediate via a hydrothermal method, then mixing it with urea and calcining it to prepare W-Mn3O4 nanowires. To generate the α-MnO2 intermediate, (NH4)2SO4 is responsible for inducing the initial reduction, while a large excess of KMnO4 decomposes to release oxygen and convert it into MnO2, ensuring that the precursor is completely converted into the target product.

[0020] In step S12, the purpose of solid-liquid separation is to obtain the separated solid product. While satisfying the purpose of solid-liquid separation, the solid-liquid separation method can be a conventional method in the art, preferably centrifugal sedimentation or Buchner filtration. The solid-liquid separation product is then washed with deionized water to remove unreacted material adsorbed on the surface of the solid product. After thorough washing, it is dried at 100-110°C.

[0021] In step S13, solid urea is used as a phase change agent, and its mass ratio to the dried solid precipitate is preferably 0.8:1. The calcination heating rate can be set according to conventional calcination heating rates in the art, preferably 5℃ / min.

[0022] Furthermore, this invention also provides the application of the above-mentioned W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst in the removal of nitrogen oxides. In particular, it effectively removes low concentrations (≤100 ppm) and low flow rates (≤100 mL / min) of NO, achieving a NO conversion rate of 89% under xenon lamp irradiation while effectively suppressing NO2 formation.

[0023] The W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst, its preparation method, and its application provided by this invention have the following beneficial effects:

[0024] (1) The W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst provided by the present invention is formed by the self-assembly of nanosheet MnO2 to form nanoflower-like F-δ-MnO2, and nanowires are embedded in the nanoflowers to form W-Mn3O4@F-δ-MnO2. The two phase interfaces form a heterojunction structure. This photocatalyst is used for the photocatalytic oxidation of gaseous NO to NO3. - / NO2 - The photocatalytic activity was significantly improved, with a photocatalytic degradation efficiency of up to 89%, which is more than 10% higher than the photocatalytic denitrification efficiency of F-δ-MnO2 and W-Mn3O4 alone, and the long-term activity stability was extended.

[0025] (2) The preparation method of the W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst provided by the present invention is to prepare solid-phase precipitation initials by compounding KMnO4 powder, MnSO4·H2O powder and nanowire W-Mn3O4 powder through a hydrothermal synthesis method, and synthesize W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst after calcination at a certain temperature and air atmosphere. The preparation process does not require surfactants. The prepared W-Mn3O4@F-δ-MnO2 photocatalyst has controllable morphology, high crystallinity and no other impurities generated. The preparation process is simple, the reaction conditions are highly controllable, the equipment requirements are low, and it has the technical characteristics of low production cost, good operability and environmental friendliness.

[0026] (3) The preparation method of W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst provided by the present invention uses common chemical reagents, which are widely available, inexpensive and easy to obtain. The preparation process is simple and the equipment requirements are low. It can quickly synthesize heterojunction catalysts. The process is simple, the reaction conditions are highly controllable, the cost is low, and it is conducive to large-scale production. Attached Figure Description

[0027] Figure 1 XRD patterns of the catalyst samples prepared in Examples 1-3;

[0028] Figure 2 SEM image of the catalyst prepared in Example 2;

[0029] Figure 3 TEM image of the catalyst prepared in Example 2;

[0030] Figure 4 The relationship between the NO photodegradation efficiency and NO2 generation of the catalyst samples prepared in Examples 1-3 and time. Detailed Implementation

[0031] The technical solutions of various embodiments of the present invention will be clearly and completely described in conjunction with the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are part of the present invention.

[0032] The W-Mn3O4 powder used in the following examples was prepared in-house, while all other raw materials were purchased commercially. The W-Mn3O4 powder was prepared using the following method, specifically including the following steps:

[0033] S11. Dissolve 20 mmol KMnO4 and 10 mmol (NH4)2SO4 in 70 mL of deionized water under vigorous stirring to obtain a dark brown suspension.

[0034] S12. Transfer the suspension obtained in step S11 to a 100 mL Teflon-lined stainless steel autoclave and seal it. Heat the autoclave at 180°C for 24 h and allow it to cool naturally to room temperature. Perform solid-liquid separation and collect the separated solid product. Add the obtained solid product to deionized water, stir thoroughly, and then centrifuge to separate the solid phase. Repeat this process three times. After washing the solid product, keep it in an oven at 105°C for 12 h to obtain a dry, blocky solid precipitate.

[0035] S13. Mix solid urea and the solid precipitate obtained in step S12 at a mass ratio of 0.8:1, grind them in a mortar to obtain a uniform mixed powder, place the mixed powder in a tube furnace, and calcine it at 400°C for 3 hours in a nitrogen atmosphere to obtain W-Mn3O4.

[0036] Example 1

[0037] The W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst of this embodiment is prepared by the following method, specifically including the following steps:

[0038] S1. Place 1.50g KMnO4, 0.28g MnSO4·H2O and 0.4578g W-Mn3O4 nanowire powder in 80 ml of deionized water and stir magnetically for about 30 minutes to form a uniform suspension.

[0039] S2. Immediately transfer the suspension obtained in step S1 to a 100 ml Teflon-lined stainless steel autoclave and seal it. Heat the mixture at 160 °C for 12 h, then allow it to cool naturally to room temperature. Centrifuge to separate the solid and liquid phases and collect the separated solid product. Wash the obtained solid product repeatedly with deionized water to remove unreacted material adsorbed on the surface of the solid product. After thorough washing, dry the solid product at 80 °C for 4 h to obtain a dry blocky solid precipitate.

[0040] S3. After grinding the solid precipitate obtained in step S2 into powder, place it in a closed muffle furnace, blow air in with an air pump, heat it to 360℃ at a heating rate of 5℃ / min, and calcine for 2h to obtain W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst, with a molar ratio of W-Mn3O4 to F-δ-MnO2 of 1:5.

[0041] Example 2

[0042] The W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst of this embodiment is prepared by the following method, specifically including the following steps:

[0043] S1. Place 1.50 g KMnO4, 0.28 g MnSO4·H2O and 0.2288 g W-Mn3O4 nanowire powder in 80 ml deionized water and stir magnetically for about 30 min to form a uniform suspension.

[0044] S2. Immediately transfer the suspension obtained in step S1 to a 100 ml Teflon-lined stainless steel autoclave and seal it. Heat the mixture at 160 °C for 12 h, then allow it to cool naturally to room temperature. Centrifuge to separate the solid and liquid phases and collect the separated solid product. Wash the obtained solid product repeatedly with deionized water to remove unreacted material adsorbed on the surface of the solid product. After thorough washing, dry the solid product at 80 °C for 4 h to obtain a dry blocky solid precipitate.

[0045] S3. After grinding the solid precipitate obtained in step S2 into powder, place it in a closed muffle furnace, blow air in with an air pump, heat it to 360℃ at a heating rate of 5℃ / min, and calcine for 2h to obtain W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst, with a molar ratio of W-Mn3O4 to F-δ-MnO2 of 1:10.

[0046] Example 3

[0047] The W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst of this embodiment is prepared by the following method, specifically including the following steps:

[0048] S1. Place 1.50 g KMnO4, 0.28 g MnSO4·H2O and 0.1525 g W-Mn3O4 nanowire powder in 80 ml deionized water and stir magnetically for about 30 min to form a uniform suspension.

[0049] S2. Immediately transfer the suspension obtained in step S1 to a 100 ml Teflon-lined stainless steel autoclave and seal it. Heat the mixture at 160 °C for 12 h, then allow it to cool naturally to room temperature. Centrifuge to separate the solid and liquid phases and collect the separated solid product. Wash the obtained solid product several times with deionized water to remove unreacted material adsorbed on the surface of the solid product. After thorough washing, dry the solid product at 80 °C for 4 h to obtain a dry blocky solid precipitate.

[0050] S3. After grinding the solid precipitate obtained in step S2 into powder, place it in a closed muffle furnace, blow air in with an air pump, heat it to 360℃ at a heating rate of 5℃ / min, and calcine for 2h to obtain W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst, with a molar ratio of W-Mn3O4 to F-δ-MnO2 of 1:15.

[0051] Example 4

[0052] The W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst of this embodiment is prepared by the following method, specifically including the following steps:

[0053] S1. Place 1.50 g KMnO4, 0.28 g MnSO4·H2O and 0.2288 g W-Mn3O4 nanowire powder in 80 ml deionized water and stir magnetically for about 30 min to form a uniform suspension.

[0054] S2. Immediately transfer the suspension obtained in step S1 to a 100 ml Teflon-lined stainless steel autoclave and seal it. Heat the mixture at 150°C for 13 hours, then allow it to cool naturally to room temperature. Centrifuge to separate the solid and liquid phases and collect the separated solid product. Wash the obtained solid product several times with deionized water to remove unreacted material adsorbed on the surface of the solid product. After thorough washing, dry the solid product at 80°C for 4 hours to obtain a dry blocky solid precipitate.

[0055] S3. After grinding the solid precipitate obtained in step S2 into powder, place it in a closed muffle furnace, blow air in with an air pump, heat it to 320℃ at a heating rate of 5℃ / min, and calcine for 3h to obtain W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst, with a molar ratio of W-Mn3O4 to F-δ-MnO2 of 1:10.

[0056] Example 5

[0057] The W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst of this embodiment is prepared by the following method, specifically including the following steps:

[0058] S1. Place 1.50 g KMnO4, 0.28 g MnSO4·H2O and 0.2288 g W-Mn3O4 nanowire powder in 80 ml deionized water and stir magnetically for about 30 min to form a uniform suspension.

[0059] S2. Immediately transfer the suspension obtained in step S1 to a 100 ml Teflon-lined stainless steel autoclave and seal it. Heat the mixture at 170 °C for 11 h, then allow it to cool naturally to room temperature. Centrifuge to separate the solid and liquid phases and collect the separated solid product. Wash the obtained solid product several times with deionized water to remove unreacted material adsorbed on the surface of the solid product. After thorough washing, dry the solid product at 80 °C for 4 h to obtain a dry blocky solid precipitate.

[0060] S3. After grinding the solid precipitate obtained in step S2 into powder, place it in a closed muffle furnace, blow air in with an air pump, heat it to 400℃ at a heating rate of 5℃ / min, and calcine for 1.5h to obtain W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst, with a molar ratio of W-Mn3O4 to F-δ-MnO2 of 1:10.

[0061] Comparative Example

[0062] This comparative example provides the preparation of nanoflower δ-MnO2, specifically including the following steps:

[0063] S1, Mix 1.50 g KMnO4 and 0.28 g Mn S O4·H2O was dissolved in 80 ml of deionized water and magnetically stirred for about 30 minutes to form a uniform suspension.

[0064] S2. Immediately transfer the suspension obtained in step S1 to a 100m Teflon-lined stainless steel high-pressure reactor and seal it. Keep it at 160°C for 12 h. After the reactor cools naturally to room temperature, centrifuge to separate the solid and liquid phases and collect the separated solid product. Wash the obtained solid product several times with deionized water to remove unreacted material adsorbed on the surface of the solid product. After thorough washing, dry it at 80°C for 4 h to obtain a dry solid precipitate.

[0065] S3. The solid precipitate obtained in step S2 is placed in a closed muffle furnace, air is pumped in, and the temperature is raised to 360°C at a heating rate of 5°C / min under the flowing air atmosphere. The calcination is carried out for 2 h to obtain nanoflower δ-MnO2 (Flower-δ-MnO2), denoted as F-δ-MnO2.

[0066] The performance of the samples prepared in Examples 1-3 and the comparative examples is analyzed below.

[0067] Figure 1 The XRD patterns of W-Mn3O4@F-δ-MnO2 prepared in three proportions as shown in Examples 1-3 are illustrated. All three proportions of W-Mn3O4@F-δ-MnO2 exhibit both W-Mn3O4 peaks (blue circles) and F-δ-MnO2 peaks (red squares). The blue peaks correspond to Mn3O4 (JCPDS PDF#24-0734), and the red peaks correspond to δ-MnO2 (JCPDS PDF#80-1098). XRD characterization indicates that different phases of MnO2... x There exists a heterojunction structure that can be successfully constructed from W-Mn3O4@R-α-MnO2.

[0068] Figure 2The image shows a SEM image of W-Mn3O4@F-δ-MnO2 (1:10) prepared in Example 2. It can be seen that the W-Mn3O4 nanowires are orderly inserted into the nanoflower structure of F-δ-MnO2, forming a complete spherical structure. This combination does not destroy the morphology of the previous single-phase catalyst, but rather allows the two to combine in an orderly manner, proving that they form a heterojunction.

[0069] Figure 3 The images show TEM and HTEM images of W-Mn3O4@F-δ-MnO2 (1:10) prepared in Example 2. Figures a1 and a2 are TEM images of W-Mn3O4@F-δ-MnO2 (1:10). It can be seen that its microstructure is consistent with the SEM experimental results, both being spherical structures with nanowires inserted on nanoflowers. Figure a3 shows the HRTEM image of W-Mn3O4@F-δ-MnO2 (1:10). At the junction of the nanowires and nanoflowers, two types of lattice fringes can be observed: one is a 0.70 nm lattice fringe, corresponding to the (001) crystal plane of F-δ-MnO2, and the other is a 0.30 nm lattice fringe, corresponding to the (112) crystal plane of W-Mn3O4. W-Mn3O4 exposes the (112) high-index crystal plane. In addition, the heterojunction interface formed between Mn3O4 and MnO2 constitutes a multi-coupled charge transport network. This structure can be compared with a highly efficient heterojunction with a chemically bonded interface, which reduces the energy barrier of charge transfer through atomic-level channels, thereby significantly improving the overall photocatalytic efficiency.

[0070] 300 mg of catalyst was dispersed into a sample cell with a diameter of 5 cm. The catalyst coating amount was 15.29 mg / cm². 2 The sample cell was placed in the reactor to detect photocatalytic activity. NO gas with an initial concentration of 1000 ppm was diluted to a target concentration of 100 ppm using N2 and O2, with a total flow rate of 100 mL / min. A 300 W xenon lamp was used as a simulated sunlight irradiation device to evaluate the photocatalytic performance of the prepared samples under room temperature and atmospheric pressure conditions. A photocatalytic experiment to remove 100 ppm NO was conducted in a continuous flow reactor. The reactor was a cylindrical stainless steel reactor (volume 0.2 L; diameter 8 cm; height 4 cm), with the top covered by quartz glass to ensure a sealed environment. The gas entered from the bottom of the reaction chamber and exited from the top in a spiral manner. Figure 4The removal rate of NO and the amount of NO2 generated by the three ratios of W-Mn3O4@F-δ-MnO2 catalysts prepared in Examples 1-3 were compared with those of W-Mn3O4 alone and the comparative example F-δ-MnO2 within 120 min. It can be seen that coupling F-δ-MnO2 with W-Mn3O4 can effectively improve the removal efficiency of the catalyst, and the amount of NO2 generated can be controlled below 0 ppm. In the first 50 min of the reaction, W-Mn3O4@F-δ-MnO2 (1:5) can reach a maximum removal rate of 88%, but from the 55th min onwards, the removal rate drops to 65% and then gradually rises to 70% before stabilizing. W-Mn3O4@F-δ-MnO2 (1:10) reaches a removal rate of 89% in the first 30 min of the reaction and remains stable for 2 h. The W-Mn3O4@F-δ-MnO2 (1:15) heterojunction photocatalyst achieved a removal rate of 89% in the first 75 minutes of the reaction. However, starting from the 76th minute, the removal rate dropped to around 67% and then gradually stabilized at 70%. This indicates that a molar ratio of W-Mn3O4 to F-δ-MnO2 of 1:10 is the optimal ratio for the W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst. However, excessive or insufficient ratios of W-Mn3O4 to F-δ-MnO2 will cause extreme instability of the catalyst, resulting in a decrease in the removal rate.

[0071] Those skilled in the art will recognize that the embodiments described herein are intended to help the reader understand the principles of the invention, and should be understood that the scope of protection of the invention is not limited to such specific statements and embodiments. Those skilled in the art can make various other specific modifications and combinations based on the technical teachings disclosed in this invention without departing from the spirit of the invention, and these modifications and combinations are still within the scope of protection of this invention.

Claims

1. A W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst, characterized in that: The photocatalyst is composed of W-Mn3O4 and F-δ-MnO2 in a molar ratio of 1: (5~15). Its micro-particles are spherical structures formed by the self-assembly of nanowires Mn3O4 embedded in MnO2 nanosheets into a nanoflower-like structure. The two phase interfaces form a heterojunction structure.

2. The W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst according to claim 1, characterized in that: The molar ratio of W-Mn3O4 to F-δ-MnO2 is 1:

10.

3. A method for preparing the W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst according to claim 1 or 2, characterized in that: Includes the following steps: S1. According to the set molar ratio of W-Mn3O4 and F-δ-MnO2, KMnO4 powder, MnSO4·H2O powder and W-Mn3O4 powder are simultaneously and uniformly dispersed in deionized water to form a uniform suspension. S2. Place the suspension obtained in step S1 in a closed environment and heat it at 150~170℃ for 11~13h. After cooling it to room temperature, perform solid-liquid separation and collect the separated solid product. Wash the obtained solid product with deionized water and dry it to obtain a dry blocky solid precipitate. S3. Grind the solid precipitate obtained in step S2 into powder and place it in a sealed environment. Calcinate it in air at 320~400℃ for 1.5~3.0 h to obtain the W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst.

4. The preparation method of the W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst according to claim 3, characterized in that: In step S1, the molar ratio of KMnO4 powder to MnSO4·H2O powder is (4~6):

1.

5. The preparation method of the W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst according to claim 3, characterized in that: The preparation method of W-Mn3O4 includes the following steps: S11. KMnO4 and (NH4)2SO4 were dissolved in deionized water under stirring at a molar ratio of (1~3):1 to obtain a dark brown suspension. S12. Place the suspension obtained in step S11 in a closed environment and heat it at 180~200℃ for 20~28h. After cooling it to room temperature, perform solid-liquid separation and collect the separated solid product. Wash the obtained solid product with deionized water and dry it to obtain a dry blocky solid precipitate α-MnO2 intermediate. S13. Mix solid urea and the α-MnO2 intermediate obtained in step S12 at a mass ratio of (0.6-1.0):1 and grind them to obtain a uniform mixed powder. Calcinate the mixed powder in a nitrogen atmosphere at 350-450℃ for 2-4 h to obtain W-Mn3O4.

6. The preparation method of the W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst according to claim 4, characterized in that: In step S2, the solid-liquid separation is performed by centrifugal sedimentation or Buchner filtration; the drying temperature is 70~90℃. In step S12, the solid-liquid separation is carried out by centrifugal sedimentation or Buchner filtration; the drying temperature is 100~110℃.

7. The preparation method of the W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst according to claim 4, characterized in that: In step S13, the mass ratio of the solid urea to the dried solid precipitate is 0.8:

1.

8. The preparation method of the W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst according to claim 4, characterized in that: In step S13, the calcination heating rate is 5 °C / min.

9. The method for preparing the W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst according to any one of claims 3-8, characterized in that: In step S3, the calcination heating rate is 5 °C / min.

10. The application of the W-Mn3O4@F-δ-MnO2 heterojunction photocatalyst according to claim 1 or 2 in the removal of nitrogen oxides.

Citation Information

Patent Citations

  • Mn2O3 / Mn3O4 nanosheet heterojunction catalyst as well as preparation method and application thereof

    CN121534701A