A motorcycle catalyst and a method for manufacturing the same

By forming a dense oxide layer on the surface of the motorcycle catalyst carrier and controlling the particle size distribution of the coating, the problem of coating peeling under high temperature cycling and thermal shock was solved, thus improving the thermal durability and thermal shock resistance of the catalyst.

CN123127986APending Publication Date: 2026-11-20FUJIAN DERI ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611010188.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-08
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Motorcycle catalyst coatings are prone to cracking and peeling under high-temperature cycling and thermal shock, resulting in the exposure or loss of precious metals, which cannot meet the requirements of long-life emission regulations. Existing improvement methods have failed to fundamentally solve the problems of internal stress and reduced contact area caused by dense particle packing and residual volatiles after calcination.

Method used

By forming a dense oxide layer on the surface of a metal carrier and controlling the particle size distribution of the coating to be D10≤1.5μm, D90≥10μm, and D90/D10>5, the adhesion between the coating and the carrier is enhanced by nano-anchoring and macro-mechanical interlocking, thus alleviating the interfacial stress caused by the difference in thermal expansion coefficients.

Benefits of technology

This improves the thermal durability of the catalyst, perfectly adapts to the drastic fluctuations in exhaust temperature of motorcycle engines, avoids peeling of the coating due to excessive shear stress under high-temperature cycling and thermal shock, and achieves high-temperature thermal stability and thermal shock resistance of the catalyst.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The application relates to a motorcycle catalyst and a preparation method thereof, which comprises the steps of carrier pretreatment, slurry preparation, coating and calcination. Different from the prior art, the technical scheme provides the following advantages: a dense oxide layer is formed on the surface of the carrier metal, the particle size D10 of the coating layer is controlled to be less than or equal to 1.5 microns, the particle size D90 is controlled to be greater than or equal to 10 microns, D90 / D10 is greater than or equal to 5, the anchoring of the coating layer and the carrier is strengthened, the adhesion of the coating layer is improved, and the shear stress under high-temperature circulation and cold-hot impact is avoided to be too large, so that the coating layer is prevented from peeling. The preparation method can be implemented on the basis of an existing production line, does not need complex equipment modification, and is easy to popularize and promote.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of catalytic materials for purifying motor vehicle exhaust, specifically to a motorcycle catalyst and its preparation method. Background Technology

[0002] With increasingly stringent global environmental regulations, motorcycles, as an important part of urban transportation, are receiving more and more attention for exhaust emission control. Because motorcycles typically use single-cylinder engines, their exhaust temperatures are high and fluctuate wildly, and their operating conditions are far harsher than those of cars. This places extremely high demands on the thermal stability and vibration resistance of the catalysts in the exhaust system.

[0003] Currently, most motorcycle catalysts utilize metal supports (such as iron-chromium-aluminum and stainless steel supports). However, due to the surface characteristics of metal supports, the adhesion of catalyst coatings to these supports has always been a challenge in the industry. Traditional preparation methods typically aim for the narrowest possible particle size distribution in the coating, believing this improves the coating's density. However, in practical applications, it has been found that such narrowly distributed coatings are highly susceptible to cracking and peeling after experiencing the high-temperature cycling and thermal shocks characteristic of motorcycles. This leads to the exposure or loss of precious metals, rapid decline in catalyst activity, and an inability to meet long-life emission regulations.

[0004] In the existing technology, although there are some methods to improve coating adhesion, most of them focus on adding binders or changing the coating process, and fail to fundamentally solve the problems of internal stress and reduced contact area caused by dense particle packing and residual volatiles after baking. Summary of the Invention

[0005] In view of the above problems, this application provides a motorcycle catalyst in which the metal support and coating particles are firmly bonded together, and a method for preparing the same. This preparation method strengthens the support anchorage and improves the coating adhesion by controlling the substrate surface and the particle size distribution range of the coating, thus solving the problem of thermal stress spalling caused by the mismatch in the coefficients of thermal expansion between the coating and the metal substrate, and improving the thermal durability of the motorcycle catalyst.

[0006] The first aspect of this invention provides a method for preparing a motorcycle catalyst, the method comprising the following steps:

[0007] Carrier pretreatment: The metal carrier is calcined in an oxygen-containing atmosphere at 600-900℃ for 1-4 hours to obtain a metal carrier with an oxide layer on the surface.

[0008] Slurry preparation: Rare earth modified γ-alumina powder, cerium zirconium composite oxide powder, noble metal precursor and deionized water are mixed and then wet ball milled to obtain coating slurry; the particle size of solid particles in the coating slurry is D10≤1.5μm, D90≥10μm, and D90 / D10>5.

[0009] Coating: The coating slurry will be uniformly coated onto the surface of the metal carrier to form an oxide layer by means of dip coating or spray coating;

[0010] Calcination: After drying the coated metal carrier at 80-120℃ for 1-2 hours, it is calcined in air at 450-550℃ for 2-4 hours to obtain the motorcycle catalyst.

[0011] The inventors discovered in their research that metals conduct heat quickly and have a high coefficient of thermal expansion under high-temperature cycling and thermal shock; while the coefficient of thermal expansion of the coating is relatively low. The mismatch in the coefficients of thermal expansion between the coating and the metal substrate can lead to thermal stress spalling.

[0012] Therefore, in order to change the relatively dense surface of the original metal carrier, a pretreatment method is adopted to form a rough oxide layer on the surface of the metal carrier, which has nano- to micron-scale protrusions and pores.

[0013] Fine particles with a diameter of 10 ≤ 1.5 μm: their size is on the same order of magnitude as the microscopic roughness of the oxide layer on the carrier surface. They can effectively embed themselves in these nano / submicron-sized surface defects, achieving "nano-anchoring," which greatly increases the initial contact area and physical adhesion between the coating and the carrier, providing the first layer of protection for adhesion.

[0014] Coarse particles with D90 ≥ 10μm: Their size can create a macroscopic mechanical interlock with the large micron-level undulations or processing marks that may exist on the carrier surface, serving as the main load-bearing skeleton to bear thermal stress.

[0015] A wide D90 / D10 ratio greater than 5 ensures that small particles can fully fill the gaps between large particle skeletons, forming a dense coating. This dense structure with a continuous size gradient can uniformly disperse and buffer the enormous shear stress generated during thermal cycling due to the asynchronous expansion and contraction of the metal and coating, preventing stress concentration that could lead to coating cracking or complete peeling from the interface. Essentially, this is achieved by optimizing the microstructural mechanical properties of the coating itself to "actively adapt" to and "dissolve" thermal stress from the interface.

[0016] The dense oxide transition layer acts as a buffer layer, effectively alleviating interfacial stress caused by the difference in thermal expansion coefficients between the metal carrier and the coating. Combined with the uniform internal stress release capability of the wide-distribution coating itself, the catalyst's thermal shock resistance (resistance to rapid heating and cooling) achieves a qualitative leap, perfectly adapting to the drastic fluctuations in exhaust temperature of motorcycle engines. Rare earth-modified γ-alumina ensures the excellent high-temperature thermal stability of the coating itself.

[0017] Unlike existing technologies, the above-mentioned technical solution provides a method to strengthen the anchoring between the coating and the carrier by forming a dense oxide layer on the carrier metal surface and controlling the particle size of the coating particles (D10 ≤ 1.5 μm, D90 ≥ 10 μm, D90 / D10 ≥ 5), thereby improving coating adhesion and preventing excessive shear stress under high-temperature cycling and thermal shock, which could lead to coating peeling. This preparation method can be implemented on existing production lines without complex equipment modifications, making it easy to industrialize and promote.

[0018] In addition to wet ball milling, each raw material can be ground separately using an air jet mill to obtain a first powder with a particle size ≤1.5μm and a second powder with a particle size ≥10μm. The first and second powders are then mixed (the amount of the second powder is more than 5 times the amount of the first powder) to obtain the raw material powder. The insoluble raw material powders, soluble copper salts, and deionized water are then ultrasonically mixed to obtain the coating slurry.

[0019] Furthermore, the solid content of the coating slurry is 20-60 wt%.

[0020] Furthermore, the mass ratio of the rare earth modified γ-alumina to the cerium-zirconium composite oxide is 1-8:2.

[0021] Furthermore, a grinding aid is added during the slurry preparation step.

[0022] Furthermore, the mass ratio of the rare earth modified γ-alumina to the grinding aid is 70-95:1-5.

[0023] Furthermore, the rare earth element in the rare earth modified γ-alumina is selected from one or more of lanthanum, cerium, praseodymium, and neodymium.

[0024] Furthermore, the precious metal is selected from one or more of platinum, palladium, rhodium, and ruthenium.

[0025] Furthermore, the precious metals include platinum, palladium, rhodium, and ruthenium; wherein rhodium accounts for 5-20 wt%, ruthenium accounts for 5-60 wt%, and platinum and palladium account for 40-70 wt%.

[0026] Since the exhaust temperature of motorcycles is relatively low (usually ≤850℃), the risk of ruthenium (Ru) volatilization and deactivation is greatly reduced within this temperature range. Therefore, partially replacing expensive rhodium (Rh) with inexpensive ruthenium (Ru) while maintaining the total precious metal load is cost-effective and has high economic value.

[0027] Meanwhile, ruthenium (Ru) exhibits good catalytic activity for NOx reduction at moderate temperatures. The quaternary combination of platinum, palladium, rhodium, and ruthenium utilizes the high oxidation activity of Pd and Pt and the reduction activity of Ru and Rh to achieve excellent synergistic purification effects of CO and HC oxidation and NOx reduction within the common low-temperature exhaust window (e.g., 300-600℃) of motorcycles, etc. Its NOx ignition temperature (T50) is superior to that of high-rhodium ternary (platinum, palladium, rhodium) catalysts with the same total loading.

[0028] Furthermore, the noble metal precursor is a noble metal soluble salt.

[0029] The second aspect of the present invention includes a motorcycle catalyst, which is prepared using the preparation method described in the first aspect of the present invention.

[0030] Furthermore, the motorcycle catalyst includes a metal carrier and a catalytic coating applied to the surface of the metal carrier.

[0031] Furthermore, the total loading of precious metals in the motorcycle catalyst is 0.5-200 g / ft. 3 .

[0032] The above description of the invention is merely an overview of the technical solution of this application. In order to enable those skilled in the art to better understand the technical solution of this application and to implement it based on the textual description, and to make the above-mentioned objectives and other objectives, features and advantages of this application easier to understand, the following description is based on the specific embodiments of this application. Detailed Implementation

[0033] To explain in detail the technical content, structural features, objectives, and effects of the technical solution, the following detailed description is provided in conjunction with specific embodiments.

[0034] To illustrate the possible application scenarios, technical principles, implementable specific solutions, and achievable objectives and effects of this application in detail, the following description is provided in conjunction with the specific embodiments listed. The embodiments described herein are merely illustrative of the technical solutions of this application and are therefore intended only as examples, not as limiting the scope of protection of this application.

[0035] In this document, the term "embodiment" means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The term "embodiment" appearing in various places throughout the specification does not necessarily refer to the same embodiment, nor does it specifically limit its independence or connection with other embodiments. In principle, in this application, as long as there are no technical contradictions or conflicts, the technical features mentioned in each embodiment can be combined in any way to form corresponding implementable technical solutions.

[0036] Unless otherwise defined, the technical terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the use of related terms herein is merely for the purpose of describing particular embodiments and is not intended to limit this application.

[0037] In the description of this application, the term "and / or" is used to describe the logical relationship between objects, indicating that three relationships can exist. For example, A and / or B means: A exists, B exists, and A and B exist simultaneously. Additionally, the character " / " in this document generally indicates that the preceding and following objects have an "or" logical relationship.

[0038] In this application, terms such as “first” and “second” are used only to distinguish one entity or operation from another, and do not necessarily require or imply any actual quantity, hierarchy or order relationship between these entities or operations.

[0039] Without further limitations, the use of terms such as “comprising,” “including,” “having,” or other similar expressions in this application is intended to cover non-exclusive inclusion, which does not exclude the presence of additional elements in a process, method, or product that includes the stated elements, such that a process, method, or product that includes a list of elements may include not only those defined elements but also other elements not expressly listed, or elements inherent to such a process, method, or product.

[0040] In this application, expressions such as "greater than", "less than", and "exceeding" are understood to exclude the stated number; expressions such as "above", "below", and "within" are understood to include the stated number. Furthermore, in the description of the embodiments of this application, "multiple" means two or more (including two), and similar expressions related to "multiple" are also understood in this way, such as "multiple groups" and "multiple times", unless otherwise explicitly specified.

[0041] The first aspect of this invention provides a method for preparing a motorcycle catalyst, the method comprising the following steps:

[0042] Carrier pretreatment: The metal carrier is calcined in an oxygen-containing atmosphere at 600-900℃ for 1-4 hours to obtain a metal carrier with an oxide layer on the surface.

[0043] Slurry preparation: Rare earth modified γ-alumina powder, cerium zirconium composite oxide powder, noble metal precursor and deionized water are mixed and then wet ball milled to obtain coating slurry; the particle size of solid particles in the coating slurry is D10≤1.5μm, D90≥10μm, and D90 / D10>5.

[0044] Coating: The coating slurry will be uniformly coated onto the surface of the metal carrier to form an oxide layer by means of dip coating or spray coating;

[0045] Calcination: After drying the coated metal carrier at 80-120℃ for 1-2 hours, it is calcined in air at 450-550℃ for 2-4 hours to obtain the motorcycle catalyst.

[0046] The inventors discovered in their research that metals conduct heat quickly and have a high coefficient of thermal expansion under high-temperature cycling and thermal shock; while the coefficient of thermal expansion of the coating is relatively low. The mismatch in the coefficients of thermal expansion between the coating and the metal substrate can lead to thermal stress spalling.

[0047] Therefore, in order to change the relatively dense surface of the original metal carrier, a pretreatment method is adopted to form a rough oxide layer on the surface of the metal carrier, which has nano- to micron-scale protrusions and pores.

[0048] Fine particles with a diameter of 10 ≤ 1.5 μm: their size is on the same order of magnitude as the microscopic roughness of the oxide layer on the carrier surface. They can effectively embed themselves in these nano / submicron-sized surface defects, achieving "nano-anchoring," which greatly increases the initial contact area and physical adhesion between the coating and the carrier, providing the first layer of protection for adhesion.

[0049] Coarse particles with D90 ≥ 10μm: Their size can create a macroscopic mechanical interlock with the large micron-level undulations or processing marks that may exist on the carrier surface, serving as the main load-bearing skeleton to bear thermal stress.

[0050] A wide D90 / D10 ratio greater than 5 ensures that small particles can fully fill the gaps between large particle skeletons, forming a dense coating. This dense structure with a continuous size gradient can uniformly disperse and buffer the enormous shear stress generated during thermal cycling due to the asynchronous expansion and contraction of the metal and coating, preventing stress concentration that could lead to coating cracking or complete peeling from the interface. Essentially, this is achieved by optimizing the microstructural mechanical properties of the coating itself to "actively adapt" to and "dissolve" thermal stress from the interface.

[0051] The dense oxide transition layer acts as a buffer layer, effectively alleviating interfacial stress caused by the difference in thermal expansion coefficients between the metal carrier and the coating. Combined with the uniform internal stress release capability of the wide-distribution coating itself, the catalyst's thermal shock resistance (resistance to rapid heating and cooling) achieves a qualitative leap, perfectly adapting to the drastic fluctuations in exhaust temperature of motorcycle engines. Rare earth-modified γ-alumina ensures the excellent high-temperature thermal stability of the coating itself.

[0052] Unlike existing technologies, the above-mentioned technical solution provides a method to strengthen the anchoring between the coating and the carrier by forming a dense oxide layer on the carrier metal surface and controlling the particle size of the coating particles (D10 ≤ 1.5 μm, D90 ≥ 10 μm, D90 / D10 ≥ 5), thereby improving coating adhesion and preventing excessive shear stress under high-temperature cycling and thermal shock, which could lead to coating peeling. This preparation method can be implemented on existing production lines without complex equipment modifications, making it easy to industrialize and promote.

[0053] In addition to wet ball milling, each raw material can be ground separately using an air jet mill to obtain a first powder with a particle size ≤1.5μm and a second powder with a particle size ≥10μm. The first and second powders are then mixed (the amount of the second powder is more than 5 times the amount of the first powder) to obtain the raw material powder. The insoluble raw material powders, soluble copper salts, and deionized water are then ultrasonically mixed to obtain the coating slurry.

[0054] Furthermore, the solid content of the coating slurry is 20-60 wt%.

[0055] Furthermore, the mass ratio of the rare earth modified γ-alumina to the cerium-zirconium composite oxide is 1-8:2.

[0056] Furthermore, a grinding aid is added during the slurry preparation step.

[0057] Furthermore, the mass ratio of the rare earth modified γ-alumina to the grinding aid is 70-95:1-5.

[0058] Furthermore, the rare earth element in the rare earth modified γ-alumina is selected from one or more of lanthanum, cerium, praseodymium, and neodymium.

[0059] Furthermore, the precious metal is selected from one or more of platinum, palladium, rhodium, and ruthenium.

[0060] Furthermore, the precious metals include platinum, palladium, rhodium, and ruthenium; wherein rhodium accounts for 5-20 wt%, ruthenium accounts for 5-60 wt%, and platinum and palladium account for 40-70 wt%.

[0061] Since the exhaust temperature of motorcycles is relatively low (usually ≤850℃), the risk of ruthenium (Ru) volatilization and deactivation is greatly reduced within this temperature range. Therefore, partially replacing expensive rhodium (Rh) with inexpensive ruthenium (Ru) while maintaining the total precious metal load is cost-effective and has high economic value.

[0062] Meanwhile, ruthenium (Ru) exhibits good catalytic activity for NOx reduction at moderate temperatures. The quaternary combination of platinum, palladium, rhodium, and ruthenium utilizes the high oxidation activity of Pd and Pt and the reduction activity of Ru and Rh to achieve excellent synergistic purification effects of CO and HC oxidation and NOx reduction within the common low-temperature exhaust window (e.g., 300-600℃) of motorcycles, etc. Its NOx ignition temperature (T50) is superior to that of high-rhodium ternary (platinum, palladium, rhodium) catalysts with the same total loading.

[0063] Furthermore, the noble metal precursor is a noble metal soluble salt.

[0064] The second aspect of the present invention includes a motorcycle catalyst, which is prepared using the preparation method described in the first aspect of the present invention.

[0065] Furthermore, the motorcycle catalyst includes a metal carrier and a catalytic coating applied to the surface of the metal carrier.

[0066] Furthermore, the total loading of precious metals in the motorcycle catalyst is 0.5-200 g / ft. 3 .

[0067] The metal carrier used in this embodiment is FeCrAl stainless steel.

[0068] In this embodiment, the noble metal precursors are platinum nitrate, palladium nitrate, rhodium nitrate, and ruthenium nitrite nitrate, wherein the noble metals include 50wt% palladium, 20wt% platinum, 10wt% rhodium, and 20wt% ruthenium.

[0069] The additive used in this embodiment is a grinding aid (cellulose).

[0070] The rare earth modified γ-alumina powder in this embodiment consists of 80 wt% Al2O3, 8% ZrO2, 3% La2O3, 4% BaO, and 5% MgO.

[0071] The rare earth modified γ-alumina powder in this embodiment is prepared using the following steps:

[0072] Step 1: Solution preparation

[0073] The target product (based on the mass of oxides) is composed of: 80% Al2O3, 8% ZrO2, 3% La2O3, 4% BaO, and 5% MgO. The corresponding amounts of aluminum nitrate (Al(NO3)3·9H2O), zirconium oxynitrate (ZrO(NO3)2·xH2O), lanthanum nitrate (La(NO3)3·xH2O), barium nitrate (Ba(NO3)2), and magnesium nitrate (Mg(NO3)2·6H2O) are accurately weighed.

[0074] The above salts were completely dissolved in deionized water and mixed thoroughly to prepare a mixed salt solution A with a total metal ion concentration of 1.0 mol / L.

[0075] Prepare a separate 1.5 mol / L ammonium bicarbonate (NH4HCO3) aqueous solution as precipitant solution B.

[0076] Step 2: Co-precipitation

[0077] Add mixed salt solution A to the coprecipitation reactor, and slowly add precipitant solution B to the coprecipitation reactor until the pH reaches 5 ± 0.2.

[0078] Ammonia water was then added to adjust the pH, so that the pH value of the reaction system was precisely stabilized at 8.5±0.2. After the addition was completed, the mixture was kept warm and stirred for another 30 minutes to obtain the precursor slurry.

[0079] Step 3: Aging treatment

[0080] The precursor slurry obtained in step 2 was transferred to an aging tank, heated to 70°C, and stirred continuously at this temperature for 4 hours to promote the crystallization and aging of the precipitate.

[0081] Step 4: Filtration and Washing

[0082] The aged slurry is pumped into a plate and frame filter press for filtration to obtain filter cake.

[0083] Step 5: Drying and roasting

[0084] The washed filter cake was placed in an oven and dried at 120°C for 12 hours.

[0085] The dried lumpy material was ground and placed in a calcining furnace. Under a ventilated atmosphere, the temperature was increased to 600°C at a rate of 5°C / min, and calcined at this temperature for 4 hours. After natural cooling, the rare earth modified γ-alumina powder of this embodiment was obtained.

[0086] Example 1: Preparation of a motorcycle catalyst

[0087] Carrier pretreatment: The metal carrier is calcined at 700℃ in an oxygen-containing atmosphere for 2 hours to obtain a metal carrier with an oxide layer on its surface; Carrier specifications: 120×60×90mm / racetrack type

[0088] Slurry preparation: Rare earth modified γ-alumina powder, cerium-zirconium composite oxide powder, noble metal precursors (platinum nitrate, palladium nitrate, rhodium nitrate, nitrosyl ruthenium nitrate, grinding aid, and deionized water) are mixed and then wet ball-milled to obtain a coating slurry; the solid content of the coating slurry is 40 wt%; the mass ratio of rare earth modified γ-alumina powder, cerium-zirconium composite oxide powder, and grinding aid is 80:40:2; the particle size of the solid particles in the coating slurry is D10≤1.5μm, D90≥10μm, and D90 / D10>5;

[0089] Coating: The coating slurry will be uniformly coated onto the surface of the metal carrier to form an oxide layer by dip coating.

[0090] Calcination: After drying the coated metal carrier at 120°C for 1 hour, it is calcined in air at 450-550°C for 2 hours to obtain the motorcycle catalyst. The total loading of precious metals in the catalyst is 50 g / ft. 3

[0091] Example 2: Preparation of a motorcycle catalyst

[0092] Carrier pretreatment: The metal carrier is calcined in an oxygen-containing atmosphere at 600℃ for 4 hours to obtain a metal carrier with an oxide layer on the surface.

[0093] Slurry preparation: Rare earth modified γ-alumina powder, cerium-zirconium composite oxide powder, noble metal precursor, grinding aid and deionized water are mixed and then wet ball milled to obtain coating slurry; the solid content of coating slurry is 20wt%; the mass ratio of rare earth modified γ-alumina powder, cerium-zirconium composite oxide powder and aid is 90:100:5; the particle size of solid particles in coating slurry is D10≤1.5μm, D90≥10μm, D90 / D10>5;

[0094] Coating: The coating slurry will be uniformly coated onto the surface of the metal carrier to form an oxide layer by spraying.

[0095] Calcination: After drying the coated metal support at 100°C for 1 hour, it is calcined in air at 450-550°C for 4 hours to obtain the motorcycle catalyst. The total loading of precious metals in the catalyst is 100 g / ft. 3 .

[0096] Example 3: Preparation of a motorcycle catalyst

[0097] Carrier pretreatment: The metal carrier is calcined in an oxygen-containing atmosphere at 900℃ for 1 hour to obtain a metal carrier with an oxide layer on the surface.

[0098] Slurry preparation: Rare earth modified γ-alumina powder, cerium-zirconium composite oxide powder, noble metal precursor, grinding aid and deionized water are mixed and then wet ball milled to obtain coating slurry; the solid content of coating slurry is 60wt%; the mass ratio of rare earth modified γ-alumina powder, cerium-zirconium composite oxide powder and aid is 70:140:1; the particle size of solid particles in coating slurry is D10≤1.5μm, D90≥10μm, D90 / D10>5;

[0099] Coating: The coating slurry will be uniformly coated onto the surface of the metal carrier to form an oxide layer by spraying.

[0100] Calcination: After drying the coated metal carrier at 100°C for 1 hour, it is calcined in air at 450-550°C for 4 hours to obtain the motorcycle catalyst. The total loading of precious metals in the catalyst is [missing information].

[0101] 1g / ft 3 .

[0102] Comparative Example 1:

[0103] The difference between Comparative Example 1 and Example 1 is that the metal carrier used in Comparative Example 1 was not pretreated, and the particle size of the solid particles in the slurry was not controlled.

[0104] Performance testing:

[0105] The ultrasonic detachment method was used. A sample was taken from the catalyst to be tested, rinsed with water, and dried until the weight stabilized. The mass m1 was then weighed using a balance with an accuracy of 0.01 g. The sample was then placed in water and subjected to ultrasonic vibration for 15 minutes. Afterward, it was removed, rinsed with water, dried, and then purged with airflow. After drying until the weight stabilized, the mass m2 was weighed using a balance with an accuracy of 0.01 g. The mass loss and coating detachment rate were calculated.

[0106] The shedding rate in Example 1 was 0.5%, while the shedding rate in Comparative Example 1 was 1.2%.

[0107] This invention employs a dual synergistic technology of "carrier pretreatment" and "wide particle size distribution in the coating." The pretreatment mechanism involves high-temperature calcination, which not only removes impurities such as oil and organic matter from the metal carrier surface but, more importantly, promotes controlled oxidation of the metal surface, forming a thin and dense transition layer of chromium oxide, aluminum oxide, or a composite oxide. This transition layer is more compatible with the subsequently applied alumina-based coating in terms of chemical properties and coefficient of thermal expansion, providing an ideal "anchoring" substrate for the coating. Simultaneously, the wide particle size distribution of the coating slurry (D90 / D10>5) enables the formation of a tightly packed structure of large-particle skeleton and small-particle filler on the optimized substrate. This combination of both approaches, addressing both "substrate optimization" and "coating structure optimization," significantly enhances coating adhesion (bonding strength), solves the problem of thermal stress spalling caused by the mismatch in coefficients of thermal expansion between the coating and the metal substrate, and improves the thermal durability of motorcycle catalysts.

[0108] Finally, it should be noted that although the above embodiments have been described in the description of this application, this should not limit the scope of patent protection of this application. Any technical solutions that are based on the essential concept of this application, utilize the content described in this application's description to make equivalent structural or procedural substitutions or modifications, or directly or indirectly implement the technical solutions of the above embodiments in other related technical fields, are all included within the scope of patent protection of this application.

Claims

1. A method for preparing a motorcycle catalyst, characterized in that, The preparation method includes the following steps: Carrier pretreatment: The metal carrier is calcined in an oxygen-containing atmosphere at 600-900℃ for 1-4 hours to obtain a metal carrier with an oxide layer on the surface. Slurry preparation: Rare earth modified γ-alumina powder, cerium zirconium composite oxide powder, noble metal precursor and deionized water are mixed and then wet ball milled to obtain coating slurry; the particle size of solid particles in the coating slurry is D10≤1.5μm, D90≥10μm, and D90 / D10>5. Coating: The coating slurry will be uniformly coated onto the surface of the metal carrier to form an oxide layer by means of dip coating or spray coating; Calcination: After drying the coated metal carrier at 80-120℃ for 1-2 hours, it is calcined in air at 450-550℃ for 2-4 hours to obtain the motorcycle catalyst.

2. The preparation method according to claim 1, characterized in that, The solid content of the coating slurry is 20-60 wt%.

3. The preparation method according to claim 1, characterized in that, The mass ratio of the rare earth modified γ-alumina to the cerium-zirconium composite oxide is 1-8:

2.

4. The preparation method according to claim 1, characterized in that, In the slurry preparation step, a grinding aid is also added; the mass ratio of rare earth modified alumina to grinding aid is 70-95:1-5.

5. The preparation method according to claim 1, characterized in that, The rare earth elements in the rare earth modified γ-alumina are selected from one or more of lanthanum, cerium, praseodymium, and neodymium.

6. The preparation method according to claim 1, characterized in that, The precious metal is selected from one or more of platinum, palladium, rhodium, and ruthenium.

7. The preparation method according to claim 6, characterized in that, The precious metals include platinum, palladium, rhodium, and ruthenium; wherein rhodium accounts for 5-20 wt%, ruthenium accounts for 5-60 wt%, and platinum and palladium account for 40-70 wt%.

8. A motorcycle catalyst, characterized in that, The motorcycle catalyst is prepared using the preparation method described in any one of claims 1-7.

9. The motorcycle catalyst according to claim 8, characterized in that, The motorcycle catalyst includes a metal carrier and a catalytic coating applied to the surface of the metal carrier.

10. The motorcycle catalyst according to claim 9, characterized in that, The total loading of noble metals in the catalyst is 0.5-200 g / ft. 3 .