Silicon-based photoelectrocatalyst, preparation method and application thereof

By preparing silicon-based photocatalysts and utilizing the hierarchical porous structure of rare earth metal oxides and noble metal nanoparticles, the problems of high electron-hole recombination rate, single function, and poor stability of traditional photocatalytic materials were solved, achieving a highly efficient wastewater treatment effect.

CN123127987APending Publication Date: 2026-11-20GUANGDONG YOUNIJIA ENVIRONMENTAL PROTECTION TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611636529.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-22
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Traditional photocatalytic materials suffer from problems such as high recombination rate of photogenerated electron-hole pairs, low quantum efficiency, single function, difficulty in achieving integrated adsorption and catalysis, and poor stability.

Method used

A silicon-based photoelectrocatalyst was developed by adding a soluble rare earth metal salt solution to a silicon source sol and performing a hydrothermal reaction and calcination to form a hierarchical porous structure loaded with rare earth metal oxides and noble metal nanoparticles. The noble metal nanoparticles act as electron traps, while the rare earth metal oxides promote the generation of reactive oxygen species. The combination of the hierarchical porous structure provides a high specific surface area and adsorption sites.

Benefits of technology

It significantly improves quantum efficiency, enhances catalytic oxidation capacity, achieves integrated adsorption and catalysis, improves COD removal rate and color removal rate of wastewater, and has excellent stability and long lifespan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123127987A_ABST
    Figure CN123127987A_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of catalysts, and relates to a silicon-based photoelectrocatalyst as well as a preparation method and application thereof. The silicon-based photoelectrocatalyst is prepared by the following steps: S1. adding a soluble rare earth metal salt solution into a silicon source sol, performing hydrothermal reaction, and performing drying treatment to obtain a catalyst precursor; and S2. immersing the catalyst precursor obtained in the step S1 in a noble metal salt solution, performing calcination treatment in an inert atmosphere, and then performing reduction reaction in a reducing atmosphere to obtain a multi-level-pore silicon-based photoelectrocatalyst loaded with rare earth metal oxides and noble metal nanoparticles. The silicon-based photoelectrocatalyst can improve the COD removal rate and the chroma removal rate of wastewater under the synergistic conditions of photocatalysis and electrochemistry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of catalyst technology, and more specifically, to a silicon-based photoelectrocatalyst, its preparation method, and its application. Background Technology

[0002] Photocatalytic oxidation technology, as an advanced oxidation process, has broad application prospects in the field of organic wastewater treatment. However, traditional photocatalytic materials suffer from the following technical problems: (1) The photogenerated electron-hole pair recombination rate is high and the quantum efficiency is low. The electron-hole pairs generated by traditional single catalysts such as titanium dioxide after photoexcitation are very easy to recombine rapidly, resulting in a limited number of charge carriers actually participating in the catalytic reaction, and the catalytic efficiency is far lower than the theoretical value.

[0003] (2) Single function, making it difficult to achieve integrated adsorption and catalysis. Traditional catalysts usually only have catalytic function and lack the ability to pre-adsorb and enrich pollutants. They require additional adsorption units, which increases the complexity of the system and the operating cost.

[0004] (3) Poor stability and easy deactivation. Under complex water quality conditions, the catalyst surface is easily covered by by-products or undergoes structural collapse, resulting in rapid decay of catalytic activity. Summary of the Invention

[0005] The purpose of this invention is to overcome the defects and shortcomings of the above-mentioned technical problems and provide a silicon-based photocatalyst that improves the COD removal rate and color removal rate of wastewater under the synergistic conditions of photocatalysis and electrochemistry.

[0006] The above-mentioned objective of the present invention is achieved through the following technical solution: A silicon-based photocatalyst, the preparation method of which includes the following steps: S1. A soluble rare earth metal salt solution is added to a silicon source sol, followed by hydrothermal reaction and drying to obtain a catalyst precursor; S2. The catalyst precursor obtained in step S1 is impregnated in a noble metal salt solution, calcined at 300-600℃ under an inert atmosphere, kept warm, and then reduced in a reducing atmosphere to obtain a hierarchical porous silicon-based photoelectrocatalyst loaded with rare earth metal oxides and noble metal nanoparticles. In step S1, the preparation process of the silicon source sol includes the following steps: mixing tetraethyl orthosilicate, a first template agent, a second template agent and water, and undergoing a hydrolysis-condensation reaction to obtain the silicon source sol; The first template agent is one or more of ethyl cellulose, polymethyl methacrylate microspheres, or polystyrene microspheres; The second template agent is one or more of hexadecyltriethylammonium bromide, tetramethylammonium, tetrabutylphosphine bromide, or sodium laurylate; The mass ratio of the first template agent to the second template agent is 1:(1~3); The ratio of the total mass of the first template agent and the second template agent to the total mass of tetraethyl orthosilicate and water is (6~40):100.

[0007] The silicon-based photocatalyst of the present invention is a photocatalyst with a multi-level porous structure, which uses silicon dioxide as a carrier matrix and is compounded with noble metal nanoparticles and rare earth element oxides.

[0008] The hydrothermal reaction in step S1 promotes the conversion of rare earth metal salts into rare earth metal oxides.

[0009] The calcination in step S2 decomposes the noble metal salt into active metal oxides, while stabilizing the pore structure of the material.

[0010] The reduction process in step S2 reduces the noble metal oxide into metallic nanoparticles.

[0011] In the silicon-based photocatalyst of this invention, noble metals are uniformly dispersed in the form of nanoparticles on the surface and inner walls of the pores of a silicon-based support. These noble metal nanoparticles act as electron traps, effectively capturing photogenerated electrons, suppressing electron-hole recombination, and significantly improving quantum efficiency. This endows the material with excellent photocatalytic activity.

[0012] In the silicon-based photocatalyst of the present invention, rare earth metal elements are anchored to the surface of the silicon-based support in the form of oxides through chemical bonding. The rare earth element oxides have the ability to regulate oxygen vacancies, which can promote the continuous generation of reactive oxygen species (ROS) such as hydroxyl radicals and superoxide radicals, thereby enhancing the catalytic oxidation ability.

[0013] This invention mixes a first template agent and a second template agent with tetraethyl orthosilicate and water. During the hydrolysis and condensation of tetraethyl orthosilicate to form a sol, the first and second template agents form a mesoporous-macroporous framework within the sol network. After calcination, the template agents are removed, resulting in pores of different sizes, such as micropores, mesopores, or macropores, thus endowing the silicon-based photoelectrocatalyst with a high specific surface area and an ordered pore structure. The silicon-based photoelectrocatalyst of this invention has a hierarchical pore structure of micropores (0.5-2 nm), mesopores (2-50 nm), and macropores (50-500 nm) and an ultra-large specific surface area of ​​200-800 m² / g. The micropores provide a high specific surface area and adsorption sites, the mesopores provide molecular transport channels, and the macropores provide fluid channels, forming a highly efficient integrated mass transfer-adsorption-catalysis structure without the need for additional adsorption units.

[0014] The silicon-based photocatalyst of this invention is a catalyst with a hierarchical porous structure, high specific surface area, and dual functions of adsorption and catalysis, which can be widely used in the treatment of various organic wastewaters.

[0015] Preferably, in the first template agent, the average particle size of the polymethyl methacrylate microspheres and / or polystyrene microspheres is 50-100 nm.

[0016] Preferably, in step S1, the rare earth metal in the rare earth metal salt is one or more of cerium (Ce), lanthanum (La), gadolinium (Gd), or yttrium (Y).

[0017] Preferably, in step S2, the precious metal is one or more of platinum (Pt), palladium (Pd), rhodium (Rh) or ruthenium (Ru).

[0018] Preferably, in the silicon-based photocatalyst, the mass percentage of rare earth metal oxides is 5-25 wt%, and the mass percentage of noble metal nanoparticles is 0.5-6 wt%.

[0019] In the silicon-based photocatalyst, the mass percentage of rare earth metal oxides can be 5wt%, 10wt%, 15wt%, 20wt%, or 25wt%, and the mass percentage of noble metal nanoparticles can be 0.5wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, or 6wt%.

[0020] Preferably, in step S1, the temperature of the hydrothermal reaction is 120-200℃, and the time of the hydrothermal reaction is 12-48h.

[0021] Preferably, the mass ratio of tetraethyl orthosilicate to water is (20~30):100.

[0022] Preferably, in step S1, the temperature of the hydrothermal reaction is 120-200℃, and the time of the hydrothermal reaction is 12-48h.

[0023] In a specific embodiment, step S1, the preparation method of the silicon source sol includes the following steps: mixing tetraethyl orthosilicate, a first template agent, and a second template agent in water, adjusting the pH to 3-5, and stirring to form a homogeneous sol. After adding a soluble rare earth metal salt solution to the silicon source sol, stirring thoroughly for 2-4 hours allows the rare earth ions to be fully complexed and adsorbed into the silicon-based sol network.

[0024] In a specific embodiment, in step S1, the soluble rare earth metal salt solution can be cerium nitrate, lanthanum nitrate, gadolinium nitrate, or yttrium nitrate.

[0025] In a specific embodiment, in step S2, the concentration of the noble metal salt solution is 0.01-0.1 mol / L.

[0026] In a specific embodiment, the noble metal salt solution can be a chloroplatinic acid solution, a palladium chloride solution, a rhodium chlorochloride solution, or a ruthenium trichloride solution. The catalyst precursor obtained in step S1 is impregnated in the noble metal salt solution, which can be done using an equal-volume impregnation method, and the impregnation time can be 4-12 hours.

[0027] In a specific implementation, in step S2, the heating rate is 2-5°C / minute.

[0028] More preferably, in step S2, the calcination temperature is 400-500℃.

[0029] In a specific implementation, in step S2, the inert atmosphere is nitrogen or argon, and the heat preservation time is 2-6 hours.

[0030] In a specific embodiment, in step S2, the reducing atmosphere is a mixture of hydrogen and an inert gas, with a hydrogen volume concentration of 5%-10%. The inert gas is nitrogen or a rare gas. The rare gas is argon or helium. The reduction reaction temperature can be 200-400℃, preferably 250-350℃, and the reduction time is 1-4 hours.

[0031] The silicon-based photocatalyst prepared by the method of this invention has a high specific surface area, ranging from 200 to 800 m². 3 / g. It can provide abundant adsorption sites for organic pollutants, realizing integrated adsorption-catalysis without the need for additional adsorption units.

[0032] The preparation method of the silicon-based photoelectrocatalyst of this invention has a mature and controllable process route, which is suitable for large-scale production.

[0033] This invention also protects the application of the silicon-based photocatalyst described in any of the above claims in the photocatalytic treatment of organic pollutants in water.

[0034] Preferably, the application includes the following steps: introducing water into a photoelectrocatalytic reactor and performing photoelectrocatalytic treatment under ultraviolet light irradiation and an applied electric field; The photoelectrocatalytic reactor includes an ultraviolet light source, a cathode and an anode connected by a power source, and any one of the aforementioned silicon-based photoelectrocatalysts. The silicon-based photoelectrocatalyst is attached to the cathode surface to form a catalyst layer, and ultraviolet light emitted by the ultraviolet light source irradiates the silicon-based photoelectrocatalyst.

[0035] In a specific embodiment, the silicon-based photocatalyst can be mixed with polyvinyl alcohol (PVA) binder and water to form a slurry, which is then uniformly coated onto the anode surface and dried at 80-120°C and calcined at 300-400°C to form a catalyst layer.

[0036] Preferably, the application includes the following steps: introducing water into a photoelectrocatalytic reactor and performing photoelectrocatalytic treatment under ultraviolet light irradiation and an applied electric field; The photoelectrocatalytic reactor includes an ultraviolet light source, a cathode and an anode connected by a power source, and any of the aforementioned silicon-based photoelectrocatalysts. The silicon-based photoelectrocatalysts are filled in the photoelectrocatalytic reactor in particulate form and placed in the electric field formed by the cathode and anode. The ultraviolet light emitted by the ultraviolet light source irradiates the silicon-based photoelectrocatalysts.

[0037] In a specific embodiment, the silicon-based photocatalyst can be mixed with polyvinyl alcohol (PVA) binder and water to form a slurry, preparing particles with an average particle size of 3-8 mm. The filling height of the particles is 60%-85% of the rated height of the tank.

[0038] In the treatment of organic pollutants in water, UV light source excites silicon-based photocatalyst to generate strong oxidizing hydroxyl radicals (·OH), which rapidly break down recalcitrant organic matter, color and macromolecular pollutants in wastewater, dismantle stubborn organic structures, and complete preliminary degradation and purification.

[0039] An electrochemical oxidation-reduction reaction occurs in the reaction chamber through a high-voltage electric field, breaking the chemical bonds of organic pollutants to remove COD, ammonia nitrogen, and total nitrogen. The porous structure of the silicon-based photoelectrocatalyst can deeply retain residual trace pollutants for secondary catalytic decomposition, thus stabilizing the quality of the effluent.

[0040] The silicon-based photoelectrocatalytic wastewater treatment system of the present invention has the ability to deeply degrade recalcitrant organic matter such as polycyclic aromatic hydrocarbons and heterocyclic compounds, and the organic matter is completely mineralized into carbon dioxide and water, with no chemical sludge generated throughout the process.

[0041] In a specific embodiment, the cathode is preferably a titanium plate or 316L stainless steel.

[0042] The anode is preferably any one of boron-doped diamond (BDD) coated titanium-based material, titanium-based lead dioxide (Ti / PbO2) material, titanium-based ruthenium titanium binary oxide (Ti / RuO2-TiO2) material, or graphite material.

[0043] The silicon-based photoelectrocatalyst of the present invention achieves high COD removal rate and color removal rate of organic pollutants under the synergistic conditions of photocatalysis and electrochemistry.

[0044] Moreover, the silicon-based photocatalyst of the present invention exhibits a catalytic activity decay rate of less than 5% / month under continuous operation conditions, has a long service life, and low operation and maintenance costs.

[0045] Preferably, the wavelength of the ultraviolet light is 250-370 nm, for example, 254 nm and / or 365 nm.

[0046] Preferably, the voltage of the power supply is 1.5-5V.

[0047] The current density is 5-50A / m².

[0048] The silicon-based photoelectrocatalytic wastewater treatment system of the present invention is applicable to the treatment of any one or more types of industrial wastewater, including metal surface treatment wastewater, textile dyeing wastewater, landfill leachate, chemical and pharmaceutical wastewater, food and beverage wastewater, tobacco wastewater, and slaughterhouse wastewater.

[0049] This invention also protects a silicon-based photoelectrocatalytic wastewater treatment system, comprising a photoelectrocatalytic reactor, said photoelectrocatalytic reactor comprising: The tank body has a liquid inlet at the bottom; A water distribution plate is installed at the lower part of the tank body, above the liquid inlet; the water distribution plate is connected to the inner wall of the tank body. The ultraviolet light source is set on the water distribution plate and located on the central axis of the tank. The irradiation angle of the ultraviolet light source is 360 degrees, and the height of the ultraviolet light source is not lower than the liquid level of the tank's rated volume. An overflow weir is disposed around the top of the tank body, and the overflow weir is connected to the liquid outlet; The cathode is positioned around and in close contact with the inner wall of the tank. Anodes are arranged at intervals around the ultraviolet light source and close to the outer wall of the ultraviolet light source; The cathode and anode are connected to an external power source; The container contains any of the silicon-based photocatalysts described above.

[0050] It also includes a pretreatment system located upstream of the photoelectrocatalytic reactor and a gas-liquid separation system located downstream of the photoelectrocatalytic reactor, with the pretreatment system, photoelectrocatalytic reactor, and gas-liquid separation system connected in sequence.

[0051] The pretreatment system includes a filtration system and a pH adjustment system connected in sequence, wherein the pH adjustment system is used to adjust the pH of the wastewater to 3-4.

[0052] Adjusting the pH of the wastewater to 3-4 helps the silicon-based photoelectrochemical catalyst maximize the generation efficiency of free radicals.

[0053] The gas-liquid separation system can use gravity and cyclone separation technology to quickly remove CO2 gas generated in the reaction, avoiding secondary dissolution of the gas and affecting the pH value of the effluent.

[0054] Compared with existing technologies, the beneficial effects of this invention are as follows: This invention discloses a silicon-based photocatalyst, using silicon dioxide as a support matrix, and incorporating noble metal nanoparticles and rare earth element oxides, resulting in a photocatalyst with a hierarchical porous structure. In the silicon-based photocatalyst of this invention, noble metals are uniformly dispersed in the form of nanoparticles on the surface of the silicon-based support and the inner walls of the pores. The noble metal nanoparticles act as electron traps, effectively capturing photogenerated electrons, suppressing electron-hole recombination, and significantly improving quantum efficiency, thus endowing the material with excellent photocatalytic activity. Rare earth metal elements are anchored to the surface of the silicon-based support through chemical bonding in the form of oxides. These rare earth element oxides possess oxygen vacancy regulation capabilities, which can promote the continuous generation of reactive oxygen species (ROS) such as hydroxyl radicals and superoxide radicals, enhancing catalytic oxidation capacity. The silicon-based photocatalyst of this invention possesses a hierarchical pore structure comprising micropores (0.5-2 nm), mesopores (2-50 nm), and macropores (50-500 nm), and an ultra-large specific surface area of ​​200-800 m² / g. The micropores provide high specific surface area and adsorption sites, the mesopores provide molecular transport channels, and the macropores provide fluid channels, forming a highly efficient integrated mass transfer-adsorption-catalysis structure without the need for additional adsorption units. This invention also discloses a silicon-based photocatalyst with excellent stability, improving COD and color removal rates in wastewater under synergistic photocatalytic and electrochemical conditions. Attached Figure Description

[0055] Figure 1 The image shows the XRD pattern of the silicon-based photoelectrocatalyst of Example 1.

[0056] Figure 2 The images show the SEM, TEM, and EDS spectra of the silicon-based photoelectrocatalyst in Example 1.

[0057] Figure 3 The image shows the XPS spectrum of the silicon-based photoelectrocatalyst in Example 1.

[0058] Figure 4 The image shows the specific surface area and pore size distribution (BET-BJH) of the silicon-based photoelectrocatalyst in Example 1.

[0059] Figure 5 The UV-Vis DRS spectra of the silicon-based photoelectrocatalysts of Example 1 and Comparative Example 3 are shown.

[0060] Figure 6 EIS electrochemical impedance spectroscopy of the silicon-based photoelectrocatalysts of Example 1 and Comparative Example 3.

[0061] Figure 7 The photoluminescence spectra of the silicon-based photoelectrocatalysts of Example 1 and Comparative Example 3 are shown.

[0062] Figure 8 This is a schematic diagram of the structure of a photoelectrocatalytic reactor.

[0063] Figure 9 for Figure 8 A sectional view.

[0064] Figure 10 This is a schematic diagram showing how a silicon-based photoelectrocatalyst can form a three-dimensional microelectrode array inside a container.

[0065] In the diagram: 1-Tank body, 2-Water distribution plate, 3-Ultraviolet light source, 4-Overflow weir, 5-Cathode, 6-Anode, 8-Guide tube, 10-Silicon-based photoelectrocatalyst, 11-Liquid inlet, 12-Liquid outlet. Detailed Implementation

[0066] To more clearly and completely describe the technical solution of the present invention, the present invention will be further described in detail below through specific embodiments. It should be understood that the specific embodiments described herein are only for explaining the present invention and are not intended to limit the present invention. Various changes can be made within the scope of the claims of the present invention.

[0067] Ethyl cellulose 1#, manufactured by DuPont, model ETHOCEL™ Standard 20 Premium.

[0068] Ethyl cellulose 2#, manufactured by DuPont, model number ETHOCEL™ Standard 45 Premium.

[0069] Polymethyl methacrylate microspheres #1, manufactured by Alfa Chemistry, model number PL-PMMA-A117, with an average particle size of 50 nm.

[0070] Polymethyl methacrylate microspheres #2, manufactured by Alfa Chemistry, model number PL-PMMA-A118, with an average particle size of 100 nm.

[0071] Polystyrene microspheres, manufactured by Alfa Chemistry, model number PL-PS-A065, with an average particle size of 50 nm.

[0072] Example 1 A silicon-based photocatalyst, the preparation method of which includes the following steps: S1. Disperse 50g of tetraethyl orthosilicate, 20g of the first template agent ethyl cellulose 1#, and 20g of the second template agent hexadecyltriethylammonium bromide (the mass ratio of ethyl cellulose 1# to hexadecyltriethylammonium bromide is 1:1) in 200mL of water (the mass ratio of tetraethyl orthosilicate to water is 25:100, and the total mass ratio of ethyl cellulose 1# and hexadecyltriethylammonium bromide to the total mass ratio of tetraethyl orthosilicate to water is 16:100). Adjust the pH to 4 with dilute hydrochloric acid and stir magnetically for 1 hour to form a homogeneous sol. Add 7.5g of cerium nitrate (Ce(NO3)3·6H2O) to the sol and continue stirring for 3 hours. Transfer the mixture to a 500mL polytetrafluoroethylene-lined hydrothermal reactor and react hydrothermally at 160℃ for 24 hours. After the reaction, allow it to cool naturally, filter, wash three times with water, and dry under vacuum at 60℃ for 12 hours to obtain the catalyst precursor.

[0073] S2. The catalyst precursor obtained in step S1 is impregnated in a 0.05 mol / L chloroplatinic acid solution (equal volume impregnation) for 8 hours. After impregnation, the material is heated to 450°C at a heating rate of 3°C / min under a nitrogen atmosphere and calcined for 4 hours. Then, it is reduced at 300°C for 2 hours in a nitrogen-containing mixed atmosphere (10% hydrogen) to obtain a hierarchical porous silicon-based photoelectrocatalyst supported on rare earth metal oxides and noble metal nanoparticles.

[0074] The elemental content in the silicon-based photocatalyst was determined by ICP analysis. The results showed that the mass percentage of rare earth metal oxide CeO2 in the silicon-based photocatalyst was 16.3%, and the mass percentage of noble metal nanoparticles Pt was 2.17%.

[0075] Example 2 A silicon-based photocatalyst, the preparation method of which includes the following steps: S1. Disperse 50g of tetraethyl orthosilicate, 15g of the first template agent (polystyrene microspheres #1), and 45g of the second template agent (tetramethylammonium, with a mass ratio of polystyrene microspheres #1 to tetramethylammonium of 1:3) in 200mL of water (the mass ratio of tetraethyl orthosilicate to water is 25:100, and the total mass ratio of polystyrene microspheres #1 and tetramethylammonium to the total mass ratio of tetraethyl orthosilicate to water is 24:100). Adjust the pH to 4 with dilute hydrochloric acid and stir magnetically for 1 hour to form a homogeneous sol. Add 6.0g of lanthanum nitrate (La(NO3)3·6H2O) to the sol and continue stirring for 3 hours. Transfer the mixture to a 500mL polytetrafluoroethylene-lined hydrothermal reactor and react hydrothermally at 180℃ for 36 hours. After the reaction, allow it to cool naturally, filter, wash three times with water, and dry under vacuum at 60℃ for 12 hours to obtain the catalyst precursor.

[0076] S2. The catalyst precursor obtained in step S1 was impregnated in a 0.075 mol / L palladium chloride solution (equal volume impregnation) for 8 hours. After impregnation, the material was heated to 500°C at a heating rate of 3°C / min under a nitrogen atmosphere and calcined for 4 hours. Then, it was reduced at 350°C for 2 hours in a nitrogen-containing mixed atmosphere containing 10% hydrogen to obtain a hierarchical porous silicon-based photoelectrocatalyst supported on rare earth metal oxides and noble metal nanoparticles.

[0077] The elemental content in the silicon-based photocatalyst was determined by ICP analysis. The results showed that the mass percentage of rare earth metal oxide La2O3 in the silicon-based photocatalyst was 9.4%, and the mass percentage of noble metal nanoparticles Pd was 1.17%.

[0078] Example 3 A silicon-based photocatalyst, the preparation method of which includes the following steps: S1. Disperse 50g of tetraethyl orthosilicate, 15g of the first template agent (polymethyl methacrylate microspheres #1), and 30g of the second template agent (tetrabutylphosphine bromide, with a mass ratio of polymethyl methacrylate microspheres #1 to tetrabutylphosphine bromide of 1:2) in 200mL of water (the mass ratio of tetraethyl orthosilicate to water is 25:100, and the ratio of the total mass of polymethyl methacrylate microspheres #1 and tetrabutylphosphine bromide to the total mass of tetraethyl orthosilicate and water is 18:100). Adjust the pH to 4 with dilute hydrochloric acid and stir magnetically for 1 hour to form a homogeneous sol. Add 3.75g of cerium nitrate (Ce(NO3)3·6H2O) and 3.75g of lanthanum nitrate (La(NO3)3·6H2O) to the sol and continue stirring for 3 hours. Transfer the mixture to a 500mL polytetrafluoroethylene-lined hydrothermal reactor and react hydrothermally at 140℃ for 48 hours. After the reaction was completed, the mixture was allowed to cool naturally, filtered, washed three times with water, and dried under vacuum at 60°C for 12 hours to obtain the catalyst precursor.

[0079] S2. The catalyst precursor obtained in step S1 is impregnated in a 0.019 mol / L chloroplatinic acid solution (equal volume impregnation) for 8 hours, dried, and then impregnated in a 0.019 mol / L palladium chloride solution (stepwise impregnation method) for 8 hours. After impregnation, the material is heated to 400°C at a heating rate of 3°C / min under a nitrogen atmosphere and calcined for 4 hours. Then, it is reduced at 300°C for 2 hours in a nitrogen-containing mixed atmosphere containing 10% hydrogen to obtain a hierarchical porous silicon-based photoelectrocatalyst supported on rare earth metal oxides and noble metal nanoparticles.

[0080] The elemental content in the silicon-based photocatalyst was determined by ICP analysis. The results showed that the mass percentages of rare earth metal oxides CeO2 and La2O3 in the silicon-based photocatalyst were 10.93%, the mass percentage of rare earth metal oxide La2O3 was 9.4%, and the mass percentages of noble metal nanoparticles Pt and Pd were 1.64%.

[0081] Example 4 A silicon-based photocatalyst, the preparation method of which includes the following steps: S1. Disperse 50g of tetraethyl orthosilicate, 25g of the first template agent ethyl cellulose 2#, and 25g of the second template agent sodium laurate (the mass ratio of ethyl cellulose 2# to sodium laurate is 1:1) in 200mL of water (the mass ratio of tetraethyl orthosilicate to water is 25:100, and the total mass ratio of ethyl cellulose 2# and sodium laurate to the total mass ratio of tetraethyl orthosilicate to water is 20:100). Adjust the pH to 4 with dilute hydrochloric acid and stir magnetically for 1 hour to form a homogeneous sol. Add 2.5g of cerium nitrate (Ce(NO3)3·6H2O) to the sol and continue stirring for 3 hours. Transfer the mixture to a 500mL polytetrafluoroethylene-lined hydrothermal reactor and react hydrothermally at 120℃ for 12 hours. After the reaction, allow it to cool naturally, filter, wash three times with water, and dry under vacuum at 60℃ for 12 hours to obtain the catalyst precursor.

[0082] S2. The catalyst precursor obtained in step S1 is impregnated in a 0.013 mol / L chloroplatinic acid solution (equal volume impregnation) for 8 hours. After impregnation, the material is heated to 300°C at a heating rate of 3°C / min under a nitrogen atmosphere and calcined for 4 hours. Then, it is reduced at 200°C for 2 hours in a nitrogen-containing mixed atmosphere containing 10% hydrogen to obtain a hierarchical porous silicon-based photoelectrocatalyst supported on rare earth metal oxides and noble metal nanoparticles.

[0083] The elemental content in the silicon-based photocatalyst was determined by ICP analysis, and the mass percentage of rare earth metal oxide CeO2 and noble metal nanoparticle Pt was calculated to be 5.5%.

[0084] Example 5 A silicon-based photocatalyst, the preparation method of which includes the following steps: S1. Disperse 50g of tetraethyl orthosilicate, 18g of the first template agent (polymethyl methacrylate microspheres #2), and 54g of the second template agent (hexadecyltriethylammonium bromide, mass ratio of polymethyl methacrylate microspheres #2 to hexadecyltriethylammonium bromide) in 200mL of water (mass ratio of tetraethyl orthosilicate to water is 25:100, and the total mass ratio of polymethyl methacrylate microspheres #2 and hexadecyltriethylammonium bromide to the total mass ratio of tetraethyl orthosilicate to water is 28.8:100). Adjust the pH to 4 with dilute hydrochloric acid and stir magnetically for 1 hour to form a homogeneous sol. Add 10.0g of cerium nitrate (Ce(NO3)3·6H2O) to the sol and continue stirring for 3 hours. Transfer the mixture to a 500mL polytetrafluoroethylene-lined hydrothermal reactor and react hydrothermally at 200℃ for 48 hours. After the reaction was completed, the mixture was allowed to cool naturally, filtered, washed three times with water, and dried under vacuum at 60°C for 12 hours to obtain the catalyst precursor.

[0085] S2. The catalyst precursor obtained in step S1 was impregnated in a 0.125 mol / L palladium chloride solution (equal volume impregnation) for 8 hours. After impregnation, the material was heated to 600°C at a heating rate of 3°C / min under a nitrogen atmosphere and calcined for 4 hours. Then, it was reduced at 400°C for 2 hours in a nitrogen-containing mixed atmosphere containing 10% hydrogen to obtain a hierarchical porous silicon-based photocatalyst supported on rare earth metal oxides and noble metal nanoparticles.

[0086] The elemental content in the silicon-based photocatalyst was determined by ICP analysis. The results showed that the mass percentage of rare earth metal oxide CeO2 in the silicon-based photocatalyst was 23.5%, and the mass percentage of noble metal nanoparticles Pd was 5.88%.

[0087] Example 6 A silicon-based photocatalyst, the preparation method of which differs from that in Example 1, is as follows: S1. Disperse 50g of tetraethyl orthosilicate, 5g of the first template agent ethyl cellulose 1# and 10g of the second template agent hexadecyltriethylammonium bromide (the mass ratio of ethyl cellulose 1# and hexadecyltriethylammonium bromide is 1:2) in 200mL of water (the mass ratio of tetraethyl orthosilicate to water is 25:100, and the ratio of the total mass of ethyl cellulose 1# and hexadecyltriethylammonium bromide to the total mass of tetraethyl orthosilicate and water is 6:100).

[0088] Example 7 A silicon-based photocatalyst, the preparation method of which differs from that in Example 1, is as follows: S1. Disperse 50g of tetraethyl orthosilicate, 50g of the first template agent ethyl cellulose 1# and 50g of the second template agent hexadecyltriethylammonium bromide (the mass ratio of ethyl cellulose 1# and hexadecyltriethylammonium bromide is 1:1) in 200mL of water (the mass ratio of tetraethyl orthosilicate to water is 25:100, and the ratio of the total mass of ethyl cellulose 1# and hexadecyltriethylammonium bromide to the total mass of tetraethyl orthosilicate and water is 40:100).

[0089] Examples 8-9 A method for photoelectrocatalytically treating organic pollutants in water includes the following steps: introducing water into a photoelectrocatalytic reactor and performing photoelectrocatalytic treatment for 5 minutes under ultraviolet light irradiation and an applied electric field. The wavelength of the ultraviolet light is 254 nm, the power is 30 W / L, and the voltage of the power supply is 1.5 V.

[0090] like Figure 8-10 As shown, a silicon-based photoelectrocatalytic wastewater treatment system includes a photoelectrocatalytic reactor, which comprises: Tank 1, with a liquid inlet 11 at the bottom; The water distribution plate 2 is located at the lower part of the tank body 1, above the liquid inlet 11; the outer edge of the water distribution plate 2 is connected to the inner wall of the tank body 1. The ultraviolet light source 3 is set on the water distribution plate 2 and located on the central axis of the tank 1. The irradiation surface of the ultraviolet light source 3 has a coverage angle of 360 degrees, and the height of the ultraviolet light source 3 is not lower than the liquid level of the rated volume of the tank 1. An overflow weir 4 is installed around the top of the tank body 1, and the overflow weir 4 is connected to the liquid outlet 12; Cathode 5 is arranged around the inner wall of tank 1 and is fitted to the inner wall. Anode 6 is arranged around ultraviolet light source 3 and at intervals near the outer wall of ultraviolet light source 3; Cathode 5 and anode 6 are connected to an external power supply; The tanks 1 of Examples 8 and 9 contain the silicon-based photocatalysts 10 of Examples 1 and 3, respectively.

[0091] The silicon-based photoelectrocatalyst 10 is granular with a particle size of 6 mm, and the filling height is 80% of the rated height of the tank. The particles form a randomly stacked three-dimensional microelectrode array in the reactor, and the contact points of adjacent particles form microelectrode pairs.

[0092] It also includes a pretreatment system located upstream of the photoelectrocatalytic reactor and a gas-liquid separation system located downstream of the photoelectrocatalytic reactor, with the pretreatment system, photoelectrocatalytic reactor, and gas-liquid separation system connected in sequence.

[0093] The pretreatment system includes a filtration system and a pH adjustment system connected in sequence. The pH adjustment system is used to adjust the pH of the wastewater to 3-4.

[0094] The ultraviolet light source 3 is positioned at the central axis of tank 1. The light source emits light from the central axis of tank 1, uniformly illuminating the area radially. The light passes through the gaps between catalyst particles to reach all areas within the tank. Simultaneously, the photoelectrocatalytic reactor operates in a cross-flow mode with bottom water distribution and top overflow. The water flow direction is from bottom to top, forming an orthogonal coupling relationship with the ultraviolet light irradiation direction (radial) and the electric field direction (radial). This allows pollutants to sequentially pass through regions with different light intensities and electric field strengths during their ascent, achieving multi-stage catalytic oxidation.

[0095] Silicon-based photoelectrocatalyst particles are randomly stacked within a container to form a three-dimensional microelectrode array. The contact points of adjacent particles, under the influence of an applied electric field, constitute microelectrode pairs, each of which is an independent micro-catalytic reaction unit. This three-dimensional distributed microelectrode structure expands the two-dimensional catalytic surface of traditional planar electrodes into a three-dimensional catalytic volume, effectively increasing the catalytic area.

[0096] Overflow weir 4 is an annular thin-walled structure. The weir width is 1 / 10 to 1 / 8 of the tank's inner diameter. The water depth above the weir is controlled to not exceed 5 mm, forming a thin, uniform overflow to avoid short-flow and surface fluctuations. The water depth above the weir refers to the distance between the upper surface of the water flow and the weir crest when the water flows over it.

[0097] A transparent guide tube 8 is provided on the water distribution plate 2. The material can be selected according to actual needs; for example, in this embodiment, a guide tube 8 made of quartz glass is used. The guide tube 8 is located between the main ultraviolet light source 3 and the inner wall of the tank 1. The purpose of setting the guide tube 8 is to guide the water flow to form a uniform upward flow and avoid turbulence that would reduce the transmittance of ultraviolet light. In a further preferred embodiment, the diameter of the guide tube 8 is 1 / 3 to 1 / 2 of the inner diameter of the tank 1, and the guide tube 8 is 1 / 4 to 1 / 3 of the height of the tank 1.

[0098] Examples 10-16 A method for photoelectrocatalytically treating organic pollutants in water includes the following steps: introducing water into a photoelectrocatalytic reactor and performing photoelectrocatalytic treatment for 5 minutes under ultraviolet light irradiation and an applied electric field, wherein the wavelength of the ultraviolet light is 365 nm, the power is 30 W / L, and the voltage of the power supply is 5 V.

[0099] Unlike Examples 8-9, the silicon-based photocatalysts of Examples 1-7 were mixed with polyvinyl alcohol (PVA) binder and water to form a slurry, which was then uniformly coated on the cathode surface and dried at 100°C and calcined at 350°C to form a catalyst layer.

[0100] Comparative Example 1 A method for photoelectrocatalysis of organic pollutants in water, which differs from Example 10 in that the catalyst is titanium dioxide.

[0101] Comparative Example 2 A silicon-based photoelectrocatalyst, the preparation method of which differs from that in Example 1, does not involve the addition of rare earth metal salt solutions.

[0102] A method for photoelectrocatalytically catalyzing organic pollutants in water, differing from Example 10 in that it employs the aforementioned silicon-based photoelectrocatalyst.

[0103] Comparative Example 3 A silicon-based photoelectrocatalyst, the preparation method of which differs from that of Example 10, does not involve the addition of rare earth metal salt solutions and noble metal salt solutions.

[0104] A method for photoelectrocatalysis of organic pollutants in water, which differs from Example 10 in that it uses the aforementioned silicon-based photoelectrocatalyst.

[0105] Comparative Example 4 A silicon-based photocatalyst, the preparation method of which differs from that in Example 1, is as follows: Adjust step S1 as follows: S1. Disperse 50g of tetraethyl orthosilicate and 40g of the second template agent hexadecyltriethylammonium bromide in 200mL of water (the mass ratio of tetraethyl orthosilicate to water is 25:100, and the mass ratio of hexadecyltriethylammonium bromide to the total mass of tetraethyl orthosilicate and water is 16:100).

[0106] A method for photoelectrocatalytically catalyzing organic pollutants in water, differing from Example 10 in that it employs the aforementioned silicon-based photoelectrocatalyst.

[0107] Comparative Example 5 A silicon-based photocatalyst, the preparation method of which differs from that in Example 1, is as follows: Adjust step S1 as follows: S1. Disperse 50g of tetraethyl orthosilicate, 8g of the first template agent ethyl cellulose 1# and 32g of the second template agent hexadecyltriethylammonium bromide (the mass ratio of ethyl cellulose 1# and hexadecyltriethylammonium bromide is 1:4) in 200mL of water (the mass ratio of tetraethyl orthosilicate to water is 25:100, and the ratio of the total mass of ethyl cellulose 1# and hexadecyltriethylammonium bromide to the total mass of tetraethyl orthosilicate and water is 16:100).

[0108] A method for photoelectrocatalytically catalyzing organic pollutants in water, differing from Example 10 in that it employs the aforementioned silicon-based photoelectrocatalyst.

[0109] Comparative Example 6 A silicon-based photocatalyst, the preparation method of which differs from that in Example 1, is as follows: Adjust step S1 as follows: S1. Disperse 50g of tetraethyl orthosilicate, 27g of the first template agent ethyl cellulose 1# and 13g of the second template agent hexadecyltriethylammonium bromide (the mass ratio of ethyl cellulose 1# and hexadecyltriethylammonium bromide is 2:1) in 200mL of water (the mass ratio of tetraethyl orthosilicate to water is 25:100, and the ratio of the total mass of ethyl cellulose 1# and hexadecyltriethylammonium bromide to the total mass of tetraethyl orthosilicate and water is 16:100).

[0110] A method for photoelectrocatalytically catalyzing organic pollutants in water, differing from Example 10 in that it employs the aforementioned silicon-based photoelectrocatalyst.

[0111] Performance testing (1) XRD test: The silicon-based photoelectrocatalyst of Example 1 was analyzed by X-ray diffraction. The scanning range 2θ was 10-80 degrees. The test results are as follows: Figure 1 As shown. From Figure 1 As can be seen, 22° is the amorphous broad peak of SiO2, 28.5°, 33°, 47.5°, and 56° are characteristic peaks of CeO2 fluorite structure, and there is also a weak diffraction peak of Pt. The diffraction peaks of noble metals are weak in intensity and significantly broadened, indicating that noble metals exist in the form of highly dispersed nanoparticles rather than large-particle crystals.

[0112] (2) Scanning electron microscopy (SEM): The surface morphology of the silicon-based photoelectrocatalyst in Example 1 was observed using a scanning electron microscope, such as... Figure 2 As shown in (a), Pt noble metal nanoparticles are uniformly dispersed on the surface of the silicon-based carrier and the inner wall of the pores. Figure 2 Image (b) shows the transmission electron microscope (TEM) image and particle size distribution diagram of the silicon-based photoelectrocatalyst in Example 1. The TEM images show that the particle size distribution of the noble metal nanoparticles ranges from 2 to 15 nm, with an average particle size of 8 nm. Energy dispersive spectroscopy (EDS) mapping confirmed the spatial distribution of elements such as Si, O, Pt, and Ce. Figure 2 (c) is the EDS surface scan distribution of Si element in the silicon-based photoelectrocatalyst of Example 1. Figure 2 (d) is the EDS surface scan distribution of the O element in the silicon-based photoelectrocatalyst of Example 1. Figure 2 (e) in the figure is the EDS surface scan distribution of Pt element in the silicon-based photoelectrocatalyst of Example 1. Figure 2 In Figure (f), the Ce element distribution of the silicon-based photocatalyst in Example 1 is shown by EDS surface scan. This demonstrates that the rare earth element oxides are uniformly dispersed on the support.

[0113] The average particle size of the noble metal in the silicon-based photoelectrocatalysts of Examples 2-5 was tested using the same method and found to be 5 nm, 6 nm, 12 nm and 4 nm.

[0114] (3) X-ray photoelectron spectroscopy (XPS): The chemical state of the surface elements of the silicon-based photoelectrocatalyst in Example 1 was analyzed using XPS. The test results are as follows: Figure 3 As shown. Figure 3 (a) in the image represents the full XPS spectrum; Figure 3 (b) in the image is the high-resolution spectrum of Pt 4f; Figure 3 (c) in the image represents the high-resolution Ce 3d spectrum; Figure 3 (d) is the O 1s high-resolution spectrum. The Pt 4f spectrum shows that Pt mainly exists in the metallic state (Pt 4f). 0 ) exists. Pt 4f 7 / 2 The binding energy is approximately 71.2 eV, confirming that the noble metal exists as metal nanoparticles after hydrogen reduction. The Ce 3d spectrum shows Ce as Ce... 3+ / Ce 4+ The presence of mixed valence states confirms that rare earth elements are anchored on the support surface in the form of oxides (CeO2). The presence of oxygen vacancy characteristic peaks in the O 1s spectrum indicates that the introduction of CeO2 has created oxygen vacancies on the material surface.

[0115] (4) Specific surface area and pore size distribution (BET-BJH) spectrum. The specific surface area of ​​the silicon-based photoelectrocatalyst in Example 1 was determined by nitrogen adsorption-desorption method, and the test results are as follows: Figure 4 As shown in (a) above. The pore size distribution of the silicon-based photoelectrocatalyst of Example 1 was determined using the nitrogen adsorption-desorption method, and the test results are shown below. Figure 4 As shown in (b) in the figure. The BET specific surface area was measured to be 520 m² / g. The pore size distribution curve shows that the material has a hierarchical pore structure with micropores (pore size 0.5-2 nm), mesopores (pore size 2-50 nm), and macropores (50-500 nm).

[0116] The specific surface areas of the silicon-based photoelectrocatalysts in Examples 2-5 were tested using the same method and were 680 m² / g, 450 m² / g, 280 m² / g, and 780 m² / g, respectively.

[0117] The specific surface areas of the silicon-based photoelectrocatalysts in Examples 6 and 7 were tested using the same method and were 330 m² / g and 220 m² / g, respectively.

[0118] The specific surface areas of the silicon-based photoelectrocatalysts in Comparative Examples 4-6 were tested using the same method and were 430 m² / g, 520 m² / g, and 330 m² / g, respectively.

[0119] (5) Ultraviolet-Vis DRS: The light absorption characteristics of the silicon-based photoelectrocatalysts of Example 1 and Comparative Example 3 were measured using UV-Vis DRS. The test results are as follows: Figure 5As shown, the vertical axis represents the Kubelka-Munk function F. This indicates that the silicon-based photocatalyst of Example 1 exhibits strong absorption in the ultraviolet region, suggesting that the introduction of noble metal nanoparticles and rare earth oxides causes a redshift in the absorption edge, thus expanding the material's photoresponse range.

[0120] (6) Electrochemical Impedance Spectroscopy (EIS): The charge transfer behavior of the silicon-based photoelectrocatalysts in Example 1 and Comparative Example 3 was analyzed using EIS. The test results are as follows: Figure 6 As shown, the horizontal axis represents the real part of the impedance Z' (Ω), and the vertical axis represents the imaginary part of the impedance -Z″ (Ω). The Nyquist radius of the silicon-based photocatalyst in Example 1 of this invention is significantly smaller than that of the silicon-based photocatalyst in Comparative Example 3, indicating that the noble metal nanoparticles, acting as electron traps, effectively promote the separation and transfer of photogenerated charges, thereby reducing the charge transfer resistance.

[0121] (7) Photoluminescence spectroscopy (PL): The photogenerated carrier recombination behavior of the silicon-based photoelectrocatalysts in Example 1 and Comparative Example 3 was analyzed using PL spectroscopy. The test results are as follows: Figure 7 As shown, the PL emission peak intensity of the silicon-based photocatalyst in Example 1 of this invention is significantly lower than that of the silicon-based photocatalyst in Comparative Example 3, indicating that the recombination of photogenerated electron-hole pairs is effectively suppressed and the carrier lifetime is extended.

[0122] (8) Photoelectrocatalysis test: The photoelectrocatalysis method for organic pollutants in water described in Example 8 was used to treat dyeing and printing wastewater with COD of 650 mg / L and a color intensity of 400 times. The photoelectrocatalysis method for organic pollutants in water described in Example 9 was used to treat dyeing and printing wastewater with COD of 450 mg / L and a color intensity of 200 times. The chemical oxygen demand (COD content) and color intensity were tested.

[0123] The COD content was tested using the dichromate method, with the testing standard being HJ 828-2017 and a detection limit of 10 mg / L.

[0124] The colorimetric method is the platinum-cobalt colorimetric method, the test standard is GB / T 11903-1989, and the detection limit is 5 degrees.

[0125] The test results are as follows: In Example 8, the COD removal rate was 94.6% and the color removal rate was 99.3% in the effluent. In Example 9, the COD removal rate was 93.3% and the color removal rate was 99.2% in the effluent.

[0126] (9) Photocatalytic test: 50 mg / L methylene blue aqueous solution was treated with the photocatalytic method for organic pollutants in water as described in Examples 10-16 and Comparative Examples 1, 2, and 4-6 respectively. After treatment for 30 minutes, the chemical oxygen demand (COD content) and color were tested.

[0127] The test results of the photoelectrocatalytic method for removing organic pollutants in water in Examples 10-16 and Comparative Examples 1, 2, and 4-6 are shown in Table 1 below.

[0128] Table 1: Test results of the photoelectrocatalytic method for removing organic pollutants in water in each embodiment and comparative example

[0129] As can be seen from Table 1 above, the silicon-based photocatalyst of the present invention has both adsorption and catalytic functions. Under the synergistic conditions of photocatalysis and electrochemistry, the COD removal rate of the organic pollutant methylene blue is greater than 90%, reaching 92~94.6%, and the color removal rate is as high as 99.3~99.8%.

[0130] As can be seen from Comparative Examples 1 and 2, under the same photoelectrocatalytic conditions, the COD removal rate and color removal rate are significantly lower than those of the present invention.

[0131] As can be seen from Examples and Comparative Example 4, in the preparation method of silicon-based photoelectrocatalyst, excluding the first template agent, the prepared silicon-based photoelectrocatalyst has too low COD removal rate and color removal rate.

[0132] As can be seen from Examples and Comparative Example 5, in the preparation method of silicon-based photoelectrocatalyst, if the mass ratio of the first template agent and the second template agent is too small, the resulting silicon-based photoelectrocatalyst will have a low COD removal rate and a low color removal rate.

[0133] As can be seen from Examples and Comparative Example 6, in the preparation method of silicon-based photoelectrocatalyst, if the mass ratio of the first template agent and the second template agent is too large, the resulting silicon-based photoelectrocatalyst will have excessively low COD removal rate and color removal rate.

[0134] (9) Stability test: The silicon-based photoelectrocatalyst of Example 1 was used to conduct stability tests in a continuous flow reactor using the photoelectrocatalytic method for organic pollutants in water described in Example 8. The influent was simulated dyeing and printing wastewater with a COD of 500 mg / L, the flow rate was 10 mL / min, and the reactor was run continuously for 30 days.

[0135] Test results: COD removal rate was 93.2% on day 1, 92.1% on day 15, and 91.5% on day 30. The catalytic activity decay rate within 30 days was only 1.7%, indicating that the silicon-based photoelectrocatalyst of this invention has excellent long-term operational stability, long service life, low operating and maintenance costs, and produces no sludge.

[0136] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation of the present invention. Those skilled in the art can make other variations or modifications based on the above description. It is neither necessary nor possible to exhaustively describe all embodiments here. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the claims of the present invention.

Claims

1. A silicon-based photocatalyst, characterized in that, The preparation method of the silicon-based photocatalyst includes the following steps: S1. A soluble rare earth metal salt solution is added to a silicon source sol, followed by hydrothermal reaction and drying to obtain a catalyst precursor; S2. The catalyst precursor obtained in step S1 is impregnated in a noble metal salt solution, calcined at 300-600℃ under an inert atmosphere, kept warm, and then reduced in a reducing atmosphere to obtain a hierarchical porous silicon-based photoelectrocatalyst loaded with rare earth metal oxides and noble metal nanoparticles. In step S1, the preparation process of the silicon source sol includes the following steps: mixing tetraethyl orthosilicate, a first template agent, a second template agent and water, and undergoing a hydrolysis-condensation reaction to obtain the silicon source sol; The first template agent is one or more of ethyl cellulose, polymethyl methacrylate microspheres, or polystyrene microspheres; The second template agent is one or more of hexadecyltriethylammonium bromide, tetramethylammonium, tetrabutylphosphine bromide, or sodium laurylate; The mass ratio of the first template agent to the second template agent is 1:(1~3); The ratio of the total mass of the first template agent and the second template agent to the total mass of tetraethyl orthosilicate and water is (6~40):

100.

2. The silicon-based photocatalyst according to claim 1, characterized in that, In step S1, the rare earth metal in the rare earth metal salt is one or more of cerium, lanthanum, gadolinium, or yttrium.

3. The silicon-based photocatalyst according to claim 1, characterized in that, In step S2, the precious metal is one or more of platinum, palladium, rhodium or ruthenium.

4. The silicon-based photocatalyst according to claim 1, characterized in that, In the silicon-based photocatalyst, the mass percentage of rare earth metal oxides is 5-25 wt%, and the mass percentage of noble metal nanoparticles is 0.5-6 wt%.

5. The silicon-based photocatalyst according to claim 1, characterized in that, In step S1, the hydrothermal reaction temperature is 120-200℃ and the hydrothermal reaction time is 12-48h.

6. The application of the silicon-based photocatalyst according to any one of claims 1 to 5 in the photocatalytic removal of organic pollutants in water.

7. The application according to claim 6, characterized in that, The application includes the following steps: introducing water into a photoelectrocatalytic reactor and performing photoelectrocatalytic treatment under ultraviolet light irradiation and an applied electric field; The photoelectrocatalytic reactor includes an ultraviolet light source, a cathode and an anode connected by a power source, and a silicon-based photoelectrocatalyst as described in any one of claims 1 to 3. The silicon-based photoelectrocatalyst is attached to the surface of the cathode to form a catalyst layer, and the ultraviolet light emitted by the ultraviolet light source irradiates the silicon-based photoelectrocatalyst.

8. The application according to claim 6, characterized in that, The application includes the following steps: introducing water into a photoelectrocatalytic reactor and performing photoelectrocatalytic treatment under ultraviolet light irradiation and an applied electric field; The photoelectrocatalytic reactor includes an ultraviolet light source, a cathode and an anode connected by a power source, and a silicon-based photoelectrocatalyst as described in any one of claims 1 to 3. The silicon-based photoelectrocatalyst is filled in the photoelectrocatalytic reactor in particulate form and is placed in the electric field formed by the cathode and the anode. The ultraviolet light emitted by the ultraviolet light source irradiates the silicon-based photoelectrocatalyst.

9. The application according to claim 7 or 8, characterized in that, The voltage of the power supply is 1.5-5V.

10. A silicon-based photoelectrocatalytic wastewater treatment system, characterized in that, Includes a photoelectrocatalytic reactor, said photoelectrocatalytic reactor comprising: The tank body has a liquid inlet at the bottom; A water distribution plate is installed at the lower part of the tank body, above the liquid inlet; the water distribution plate is connected to the inner wall of the tank body. The ultraviolet light source is set on the water distribution plate and located on the central axis of the tank. The irradiation angle of the ultraviolet light source is 360 degrees, and the height of the ultraviolet light source is not lower than the liquid level of the tank's rated volume. An overflow weir is disposed around the top of the tank body, and the overflow weir is connected to the liquid outlet; The cathode is positioned around and in close contact with the inner wall of the tank. Anodes are arranged at intervals around the ultraviolet light source and close to the outer wall of the ultraviolet light source; The cathode and anode are connected to an external power source; The container contains the silicon-based photocatalyst according to any one of claims 1 to 5.