A monolithic structured catalyst, its preparation method and application in nonyl phenol hydrogenation reaction

By preparing a monolithic, well-structured catalyst and utilizing a TiO₂-CeO₂ composite support and a Ru-Mn-Ce synergistic catalytic system, the problems of catalyst bed pressure drop, heat transfer, and stability in the hydrogenation reaction of nonylphenol were solved, achieving high selectivity and long-term operation, making it suitable for industrial applications.

CN123127989APending Publication Date: 2026-11-20TAIXING LINGFEI CHEM TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611628658.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing fixed-bed catalysts in the hydrogenation of nonylphenol suffer from problems such as high bed pressure drop, limited mass and heat transfer, hot spot effect, and easy deactivation of the catalyst. Furthermore, monolithic catalysts lack optimization in the hydrogenation of nonylphenol, leading to coating peeling or poor heat transfer.

Method used

An integrally structured catalyst was developed using a structured support and an active coating loaded on its surface and within its pores. The coating contained composite support materials and active metal components. By optimizing the mass ratio of TiO₂ to CeO₂ and the synergistic effect of Ru, Mn, and Ce, combined with the high thermal conductivity of the FeCrAl alloy support, a catalyst with low bed pressure drop, high selectivity, and long-term stability was prepared.

Benefits of technology

It achieves low bed pressure drop, high nonylcyclohexanol selectivity and long-term stable operation. The catalyst shows no significant activity decay after more than 1000 hours, has excellent heat transfer performance, strong coating adhesion, and is suitable for both conventional and high thermal effect operating conditions, making it suitable for industrial scale-up.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123127989A_ABST
    Figure CN123127989A_ABST
Patent Text Reader

Abstract

The application discloses a monolithic regular structure catalyst, a preparation method thereof and application of the catalyst in a nonyl phenol hydrogenation reaction, and belongs to the technical field of industrial catalysis and fine chemical industry. The catalyst comprises a regular structure carrier and an active coating layer supported on the regular structure carrier. The active coating layer is composed of a TiO2-CeO2 composite carrier material and a Ru-Mn-Ce active component. By utilizing the synergistic effect of the high thermal conductivity of the metal honeycomb and the acid regulation of the coating layer, the bed layer radial temperature difference is controlled to be within 2 DEG C, the nonyl phenol conversion rate is greater than or equal to 99.5%, the nonyl cyclohexanol selectivity is greater than or equal to 99.0%, the activity does not obviously attenuate after 1000 hours of operation, the pressure drop is only 15% to 20% of that of a traditional granular catalyst, and the catalyst is especially suitable for a strong exothermic, macromolecular liquid phase continuous hydrogenation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of industrial catalysis and fine chemical technology, specifically relating to an integral structured catalyst, its preparation method, and its application in the hydrogenation reaction of nonylphenol. Background Technology

[0002] Nonylcyclohexanol is a key intermediate in the synthesis of high-performance nonionic surfactants, emulsifiers, and lubricant additives. Compared to nonylphenol, which has endocrine-disrupting effects, nonylcyclohexanol combines excellent surface activity with environmental friendliness, leading to continued growth in market demand.

[0003] Currently, the industrial production of nonylcyclohexanol mainly employs a fixed-bed continuous hydrogenation process. Existing technologies typically use nickel-based or supported noble metal (such as Pd / C, Pt / C) particulate catalysts. For example, He Hongjun et al. (Preparation of Pd / C catalyst for hydrogenation of alkylphenol to alkylcyclohexanol, Journal of Yantai University (Natural Science and Engineering Edition), Vol. 16, No. 3, 185-188, 2003) prepared a 10% Pd / C catalyst for the hydrogenation of propylphenol. Pretreatment with nitric acid solution and the addition of Ga as an auxiliary agent resulted in a one-step reduction. Under reaction conditions of 15 MPa and 160–170 °C, the conversion rate reached 89.34% after 13–15 hours. Patent CN103435449A discloses a nonylphenol conversion rate of over 99% and a selectivity of over 95% using Raney nickel as a catalyst at 5–8 MPa and 120–130 °C with the addition of an alkaline auxiliary agent. Qian Junfeng et al. (Preparation and Process Study of Ru-Ce / TiO2 Catalyst for Hydrogenation of Nonylphenol to Nonylcyclohexanol, Journal of Changzhou University (Natural Science Edition), Vol. 33, No. 3, 2021) provided a Ru-Ce / TiO2 catalyst using an excess impregnation method. Metrics of hydrated ruthenium trichloride and cerium nitrate were dissolved in deionized water, added to a TiO2 support, stirred for 2 hours, and then impregnated for another 6 hours. After drying to remove moisture, the catalyst was ground, calcined, and reduced under a H2 atmosphere to obtain the catalyst, which was used for the hydrogenation of nonylphenol. Patent CN104151134A discloses a fixed-bed nonylphenol hydrogenation method using nickel or palladium supported on TiO2-SiO2 / Al2O3, but the conversion rate is only about 85%, and the selectivity is less than 98%. Existing catalysts suffer from the following insurmountable drawbacks in practical applications: High bed pressure drop: The small random porosity formed by the accumulation of particulate catalysts results in high fluid resistance, leading to a significant increase in pressure drop in the fixed-bed reactor. This not only increases the energy consumption of the circulating compressor but also limits the increase in feed space velocity. Limited mass and heat transfer: Nonylphenol is a macromolecular compound, and its diffusion resistance within the micropores of the particulate catalyst is high, easily causing uneven distribution of reactants. This leads to excessive hydrogenation, generating byproducts such as cyclohexylcyclohexanol, reducing the selectivity of the target product. Hot spot effect and deactivation: The low radial heat transfer coefficient of the fixed bed makes it difficult to remove the heat released by the hydrogenation reaction in a timely manner, easily forming "hot spots" in the catalyst bed. This accelerates catalyst sintering and carbon deposition, shortens the catalyst's lifespan, and makes the regeneration of particulate catalysts difficult.

[0004] Monolithic catalysts, with their regular parallel channels, extremely high geometrical surface area, and extremely low fluid resistance, can significantly improve mass and heat transfer efficiency. However, there are currently no publicly reported monolithic catalysts optimized for the nonylphenol hydrogenation system, especially lacking technical solutions that can balance high activity, high selectivity, and strong coating adhesion. Furthermore, existing monolithic catalysts often employ arbitrary support selection without optimizing for the characteristics of the nonylphenol hydrogenation reaction (such as liquid phase viscosity and thermal effects), leading to problems like coating peeling or poor heat transfer during actual operation. Summary of the Invention

[0005] This invention provides a monolithic, well-structured catalyst, its preparation method, and its application in the hydrogenation reaction of nonylphenol. The catalyst achieves low bed pressure drop, high nonylcyclohexanol selectivity, long-term stable operation, and ease of industrial scale-up.

[0006] To achieve the above objectives, the present invention adopts the following technical solution:

[0007] An integral structured catalyst includes a structured support and an active coating supported on the surface and within the pores of the structured support; the active coating comprises a composite support material and an active metal component.

[0008] Based on the mass of the regular structure carrier, the coating amount of the composite carrier material is 5% to 30%;

[0009] Based on the mass of the composite carrier material, the active metal component includes the following components in mass percentage: ruthenium (Ru) 0.5%~1.5%, cerium (Ce) 0.5%~2.0%, and manganese (Mn) 1.0%~3.0%; the coating quality refers to the mass of the coating of the composite carrier material.

[0010] The composite carrier material is a composite of titanium dioxide (TiO2) and cerium dioxide (CeO2), wherein the mass ratio of TiO2 to CeO2 is 1:0.1 to 1:3.

[0011] The structured carrier is one of cordierite honeycomb ceramic, mullite honeycomb ceramic, or FeCrAl alloy metal honeycomb; the pore density of the structured carrier is 100~500 cpsi; and the geometric surface area is 1100~3160 m². 2 / m 3 .

[0012] The cordierite honeycomb ceramic has a pore density of 200~300 cpsi and a through-hole diameter of 1.5~3.0 mm. When the pore density is 200 cpsi, the through-hole diameter is preferably no more than 2.5 mm; when the pore density is 300 cpsi, the through-hole diameter is preferably no more than 2.0 mm. The thinnest wall thickness between adjacent circular holes is 0.05~1.11 mm, the geometric surface area is approximately 1100~3160 m² / m³, and the axial compressive strength is ≥12 MPa. This type of carrier is inexpensive, has good thermal shock resistance, and is suitable for most working conditions.

[0013] The FeCrAl alloy metal honeycomb has a Cr content of 15-25 wt%, an Al content of 4-8 wt%, and the balance being Fe and other trace elements. This type of carrier has extremely high thermal conductivity, which can effectively eliminate reaction hotspots and is suitable for strongly exothermic reactions.

[0014] A method for preparing a monolithic, well-structured catalyst includes the following steps:

[0015] Pretreatment of regular structure carriers: Cleaning and drying of regular structure carriers;

[0016] Slurry preparation: Titanium source precursor, cerium source precursor, binder, pore-forming agent and water are mixed and dispersed by ball milling or high-speed shearing to obtain a composite carrier coating slurry with a solid content of 20%~35% and a particle size D90 of 2~8μm.

[0017] One-time coating and firing: The composite carrier coating slurry is coated on the surface of the pretreated regular structure carrier pores, dried, and then fired in air at 400℃~600℃ for 3~5 hours to form a composite carrier coating.

[0018] Active component impregnation: Using an equal-volume impregnation method, a soluble salt solution containing ruthenium, cerium, and manganese is impregnated onto the composite carrier coating, and then allowed to stand for aging before drying;

[0019] Secondary calcination: The impregnated carrier is calcined at 300℃~500℃ under an inert atmosphere or nitrogen protection for 2~5 hours;

[0020] Reduction and activation: The calcined product is reduced in a reducing atmosphere at 250℃~350℃ for 2~5 hours to obtain the monolithic structured catalyst.

[0021] In the above-described steps, the pretreatment process of the structured carrier includes a high-temperature oxidation treatment step for metallic carriers to form a metal oxide transition layer and enhance coating adhesion.

[0022] The reducing atmosphere is hydrogen or a hydrogen-containing atmosphere.

[0023] The above-mentioned monolithic structured catalyst can be used to catalyze the hydrogenation of nonylphenol to nonylcyclohexanol in a fixed-bed reactor; the process includes the following steps: preparing nonylphenol feedstock into a liquid phase and introducing it together with hydrogen into a fixed-bed reactor packed with the catalyst; controlling the reaction temperature at 140℃~180℃, the reaction pressure at 3.0~6.0 MPa, the liquid hourly space velocity of nonylphenol at 0.2~2.0 h⁻¹, and the molar ratio of hydrogen to nonylphenol at 5:1~30:1.

[0024] Beneficial effects: This invention provides a monolithic, well-structured catalyst, its preparation method, and its application in the hydrogenation reaction of nonylphenol. Compared with the prior art, this invention has the following significant effects:

[0025] Extremely low pressure drop and high throughput: The regular structure of the parallel channel design enables the fluid to flow in a plug flow state, and the bed pressure drop is only 15% to 25% of that of traditional particulate catalysts, allowing operation at higher space velocities and significantly improving the single tower capacity.

[0026] High selectivity and low byproducts: By adjusting the mass ratio of TiO2 and CeO2 in the composite support coating and combining it with a specific ratio of Ru-Mn-Ce active components in a synergistic catalytic system (where Ru is the main active center for hydrogenation, Mn is the selectivity regulating agent, and Ce is the structural and electronic agent), the acidity and electronic environment of the catalyst surface were optimized, effectively suppressing CO bond hydrogenolysis and excessive hydrogenation of aromatic rings, achieving a nonylcyclohexanol selectivity of ≥99.0%.

[0027] High stability and long lifespan: The excellent heat transfer performance of the integral structure eliminates bed hot spots. Combined with the anti-carbon deposition effect of Mn and Ce, the catalyst can operate continuously and stably for more than 1000 hours with no significant activity decay.

[0028] Strong carrier adaptability: By limiting the specific specifications of the regular structure carrier (such as pore density and wall thickness), the catalyst can adapt to both conventional reaction conditions and extreme working conditions with high thermal effects, ensuring the reliability of industrial applications.

[0029] Strong adhesion: For well-structured metallic carriers, by limiting the chemical composition of the FeCrAl alloy and using a high-temperature oxidation process, a dense Al2O3 transition layer with strong adhesion to the substrate is grown in situ on the metal surface, solving the problem of peeling caused by the mismatch in thermal expansion coefficients between the metal carrier and the ceramic coating. Testing showed that the catalyst coating obtained by this invention exhibited a mass loss rate of ≤5% after 2 hours of ultrasonic oscillation at 40kHz; and a mass loss rate of ≤3% after 10 thermal shock cycles from 650℃ to 25℃, demonstrating excellent mechanical and thermal shock stability.

[0030] This invention utilizes a TiO2-CeO2 composite support to precisely regulate the adsorption energy of nonylphenol molecules at Ru active sites through acid-electronic dual regulation, avoiding deep hydrogenation. The oxygen storage / release capacity of CeO2 promotes H2 dissociation and adsorption, as well as active hydrogen overflow, while its oxygen vacancies anchor Ru nanoparticles, resulting in high dispersion (particle size <3 nm). MnO... x The species cover the excessively strong acid sites on the composite carrier, inhibiting the side reaction of CO bond hydrogenolysis. Ru, Mn, and Ce work synergistically, and none of them can be omitted, together achieving high activity, high selectivity, and long-term stable operation. Attached Figure Description

[0031] Figure 1 The images show (a) a cross-sectional view of the monolithic structured catalyst and (b) a partially enlarged cross-sectional view of the pore wall in the embodiments of the present invention.

[0032] Figure 2 The image shows the H2-TPR reduction spectrum of the monolithic ordered catalyst in this embodiment of the invention.

[0033] Figure 3 The XRD patterns of the monolithic, well-structured catalyst in this embodiment of the invention are compared between fresh samples and those after 1000 hours of operation. Detailed Implementation

[0034] The present invention will be further described below with reference to the accompanying drawings and specific embodiments:

[0035] Unless otherwise specified in the following examples and comparative examples, the experimental procedures or conditions can be followed according to conventional experimental procedures and conditions in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.

[0036] Example 1:

[0037] This embodiment provides the preparation of a cordierite honeycomb ceramic support catalyst:

[0038] Substrate pretreatment: Cordierite honeycomb ceramic was selected as the substrate; specifications: cross-section 50×50mm, length 100mm, pore density 200cpsi, through-hole diameter 2.0 mm, wall thickness 0.55 mm, geometric surface area approximately 1540m². 2 / m 3 The axial compressive strength is 15 MPa. It is immersed in a 10 wt% dilute nitric acid solution, treated in a water bath at 80°C for 2 hours, washed with deionized water until neutral, and dried in an oven at 120°C for 6 hours.

[0039] Slurry preparation: 80g of nano-TiO2 powder and 434g of Ce(NO3)3·6H2O crystals were prepared according to a Ti:Ce molar ratio of 1:1. 5 wt% (based on total solid mass) of polyvinyl alcohol (PVA) was added as a binder, and 5g of methylcellulose was added as a pore-forming agent. Water was added to adjust the solid content to 30%. The slurry was ball-milled for 4 hours using a planetary ball mill to obtain a stable slurry with a D90 of approximately 5μm.

[0040] One-time coating and firing: The pretreated honeycomb ceramic was immersed in the slurry and vacuum-assisted penetration was carried out for 10 minutes; after removal, the inner wall of the channel was blown with compressed air to remove excess slurry; dried at 120℃ for 12 hours, and then placed in a muffle furnace, heated to 500℃ at 2℃ / min, and fired at a constant temperature for 4 hours. After cooling, it was weighed and the coating load was calculated to be 15.2 wt%.

[0041] Active component impregnation: Prepare a mixed aqueous solution containing RuCl3, Mn(NO3)2 and Ce(NO3)3 according to the target content of the active component, load it onto the above-mentioned coated carrier by equal volume impregnation method, let it stand at room temperature for 2 hours, and dry it at 120℃ for 6 hours.

[0042] Secondary calcination and reduction: The dried sample was placed in a tube furnace and calcined for 3 hours at 1℃ / min under N2 protection, with the temperature increased to 400℃. After natural cooling to room temperature, the temperature was switched to a 5% H2 / N2 mixture and increased to 300℃ at 1℃ / min, with constant temperature reduction for 5 hours. After cooling, the finished catalyst A1 was obtained. ICP analysis showed that catalyst A1 contained 0.82 wt% Ru, 2.05 wt% Mn, and 1.02 wt% Ce (all based on the mass of the composite carrier material coating).

[0043] Example 2:

[0044] This embodiment provides the preparation of a mullite honeycomb ceramic support catalyst:

[0045] Carrier pretreatment: Mullite honeycomb ceramic was selected as the carrier. Specifications: Cross-section 50×50 mm, length 100 mm, pore density 300 cpsi, through-hole diameter 1.5 mm, wall thickness 0.25 mm, geometric surface area approximately 2116 m². 2 / m 3 With an axial compressive strength of 15 MPa, it was immersed in a 20 wt% dilute nitric acid solution, treated in a water bath at 80°C for 2 hours, washed with deionized water until neutral, and dried in an oven at 120°C for 6 hours.

[0046] Slurry preparation: 80g of nano-TiO2 powder and 217g of Ce(NO3)3·6H2O crystals were prepared according to a Ti:Ce molar ratio of 1:0.5. 5 wt% (based on total solid mass) of polyvinyl alcohol (PVA) was added as a binder, and 4g of methylcellulose was added as a pore-forming agent. Water was added to adjust the solid content to 30%. The slurry was ball-milled for 4 hours using a planetary ball mill to obtain a stable slurry with a D90 of approximately 5 μm.

[0047] One-time coating and firing: The pretreated honeycomb ceramic was immersed in the slurry and vacuum-assisted infiltration for 10 minutes. After removal, the inner walls of the pores were purged with compressed air to remove excess slurry. It was dried at 120℃ for 12 hours, then placed in a muffle furnace and heated to 400℃ at a rate of 2℃ / min, and fired at this constant temperature for 4 hours. After cooling, it was weighed, and the coating load was calculated to be 7.4 wt%.

[0048] Active component impregnation: Prepare a mixed aqueous solution containing RuCl3, Mn(NO3)2 and Ce(NO3)3 according to the target content of the active component, load it onto the above-mentioned coated carrier by equal volume impregnation method, let it stand at room temperature for 2 hours, and dry it at 120℃ for 6 hours.

[0049] Secondary calcination and reduction: The dried sample was placed in a tube furnace and calcined for 3 hours at 1℃ / min under N2 protection, with the temperature increased to 350℃. After natural cooling to room temperature, the temperature was switched to a 5% H2 / N2 mixture and increased to 350℃ at 1℃ / min, with reduction at this constant temperature for 2 hours. After cooling, the finished catalyst A2 was obtained. ICP analysis showed that catalyst A2 contained 0.53 wt% Ru, 1.25 wt% Mn, and 0.62 wt% Ce (all based on coating weight).

[0050] Example 3:

[0051] This embodiment provides the preparation of FeCrAl alloy metal honeycomb supported catalyst:

[0052] Carrier pretreatment: FeCrAl alloy metal honeycomb was selected as the carrier, with the following specifications: cross-section 50×50mm, length 100mm, pore density 200cpsi, through-hole diameter 2.5mm, wall thickness 0.05mm, and geometric surface area approximately 1600 m². 2 / m 3 The alloy composition is: Cr 20%, Al 5%, with the balance being Fe and trace elements; it is placed in a muffle furnace and subjected to high-temperature oxidation treatment at 600℃ in air atmosphere for 2 hours to form a dense Al2O3 transition layer on its surface, which enhances the adhesion of subsequent coatings.

[0053] Slurry preparation: 80g of nano-TiO2 powder and 217g of Ce(NO3)3·6H2O crystals were prepared according to a Ti:Ce molar ratio of 1:0.5. 5 wt% (based on total solid mass) of polyvinyl alcohol (PVA) was added as a binder, and 4g of methylcellulose was added as a pore-forming agent. Water was added to adjust the solid content to 30%. The slurry was ball-milled for 4 hours using a planetary ball mill to obtain a stable slurry with a D90 of approximately 5 μm.

[0054] One-time coating and firing: The pretreated honeycomb ceramic was immersed in the slurry and vacuum-assisted infiltration for 10 minutes. After removal, the inner walls of the pores were blown with compressed air to remove excess slurry. It was dried at 120℃ for 12 hours, and then placed in a muffle furnace, heated to 500℃ at a rate of 2℃ / min, and fired at a constant temperature for 3 hours. After cooling, it was weighed, and the coating load was calculated to be 17.4wt%.

[0055] Active component impregnation: Prepare a mixed aqueous solution containing RuCl3, Mn(NO3)2, and Ce(NO3)3 according to the target content of the active component, and load it onto the above-mentioned coated carrier using an equal-volume impregnation method. Let it stand at room temperature for 2 hours, and then dry it at 120°C for 6 hours.

[0056] Secondary calcination and reduction: The dried sample was placed in a tube furnace and calcined for 3 hours at 1℃ / min under N2 protection, with the temperature increased to 350℃. After natural cooling to room temperature, the temperature was switched to a 5% H2 / N2 mixture and increased to 300℃ at 1℃ / min, with constant temperature reduction for 4 hours. After cooling, the finished catalyst A3 was obtained. ICP analysis showed that catalyst A3 contained 0.55 wt% Ru, 1.63 wt% Mn, and 0.89 wt% Ce (all based on coating weight).

[0057] Example 4:

[0058] This embodiment provides the preparation of a cordierite honeycomb ceramic support catalyst:

[0059] Substrate pretreatment: Cordierite honeycomb ceramic was selected as the substrate. Specifications: Cross-section 50×50 mm, length 100 mm, pore density 100 cpsi, through-hole diameter 2.5 mm, wall thickness 1.11 mm, geometric surface area approximately 1100 m². 2 / m 3 The axial compressive strength is 15 MPa. It is immersed in a 15 wt% dilute nitric acid solution, treated in a water bath at 80°C for 2 hours, washed with deionized water until neutral, and dried in an oven at 120°C for 6 hours.

[0060] Slurry preparation: 40g of nano-TiO2 powder and 325g of Ce(NO3)3·6H2O crystals were prepared according to a Ti:Ce molar ratio of 1:3. 5wt% (based on total solid mass) of polyvinyl alcohol (PVA) was added as a binder, and 3.5g of methylcellulose was added as a pore-forming agent. Water was added to adjust the solid content to 30%. The slurry was ball-milled for 4 hours using a planetary ball mill to obtain a stable slurry with a D90 of approximately 5μm.

[0061] One-time coating and firing: The pretreated honeycomb ceramic was immersed in the slurry and vacuum-assisted infiltration for 10 minutes. After removal, the inner walls of the pores were purged with compressed air to remove excess slurry. It was dried at 120℃ for 12 hours, then placed in a muffle furnace and heated to 600℃ at a rate of 2℃ / min, and fired at this constant temperature for 4 hours. After cooling, it was weighed, and the coating load was calculated to be 28.6 wt%.

[0062] Active component impregnation: Prepare a mixed aqueous solution containing RuCl3, Mn(NO3)2, and Ce(NO3)3 according to the target content of the active component, and load it onto the above-mentioned coated carrier using an equal-volume impregnation method. Let it stand at room temperature for 2 hours, and then dry it at 120°C for 6 hours.

[0063] Secondary calcination and reduction: The dried sample was placed in a tube furnace and calcined for 3 hours at 450°C under N2 protection at a rate of 1°C / min. After natural cooling to room temperature, the temperature was switched to a 5% H2 / N2 mixture and increased to 300°C at a rate of 1°C / min, then reduced at this temperature for 5 hours. After cooling, the finished catalyst A4 was obtained. ICP analysis showed that catalyst A4 contained 1.61 wt% Ru, 2.74 wt% Mn, and 1.73 wt% Ce (all based on coating weight).

[0064] Example 5:

[0065] This embodiment provides the preparation of a cordierite honeycomb ceramic support catalyst:

[0066] Substrate pretreatment: Cordierite honeycomb ceramic was selected as the substrate. Specifications: Cross-section 50×50 mm, length 100 mm, pore density 500 cpsi, through-hole diameter 0.5 mm, wall thickness 0.72 mm, geometric surface area approximately 2330 m². 2 / m 3 The axial compressive strength is 15 MPa. It is immersed in a 10 wt% dilute nitric acid solution, treated in a water bath at 80°C for 2 hours, washed with deionized water until neutral, and dried in an oven at 120°C for 6 hours.

[0067] Slurry preparation: 40g of nano-TiO2 powder and 165g of Ce(NO3)3·6H2O crystals were prepared according to a Ti:Ce molar ratio of 1:1.5. 5 wt% (based on total solid mass) of polyvinyl alcohol (PVA) was added as a binder, and 2g of methylcellulose was added as a pore-forming agent. Water was added to adjust the solid content to 30%. The slurry was ball-milled for 4 hours using a planetary ball mill to obtain a stable slurry with a D90 of approximately 5 μm.

[0068] One-time coating and firing: The pretreated honeycomb ceramic was immersed in the slurry and vacuum-assisted infiltration for 10 minutes. After removal, the inner walls of the pores were purged with compressed air to remove excess slurry. It was dried at 120℃ for 12 hours, then placed in a muffle furnace and heated to 500℃ at a rate of 2℃ / min, and fired at this constant temperature for 4 hours. After cooling, it was weighed, and the coating load was calculated to be 5.3 wt%.

[0069] Active component impregnation: Prepare a mixed aqueous solution containing RuCl3, Mn(NO3)2, and Ce(NO3)3 according to the target content of the active component, and load it onto the above-mentioned coated carrier using an equal-volume impregnation method. Let it stand at room temperature for 2 hours, and then dry it at 120°C for 6 hours.

[0070] Secondary calcination and reduction: The dried sample was placed in a tube furnace and calcined for 5 hours under N2 protection, with the temperature increased to 300℃ at 1℃ / min. After natural cooling to room temperature, the temperature was switched to a 5% H2 / N2 mixture and increased to 300℃ at 1℃ / min, then reduced at this temperature for 5 hours. After cooling, the finished catalyst A5 was obtained. ICP analysis showed that catalyst A5 contained 0.32 wt% Ru, 2.67 wt% Mn, and 2.05 wt% Ce (all based on coating weight).

[0071] Example 6:

[0072] This embodiment provides the preparation of a mullite honeycomb ceramic support catalyst:

[0073] Substrate pretreatment: Mullite honeycomb ceramic was selected as the substrate. Specifications: Cross-section 50×50 mm, length 100 mm, pore density 400 cpsi, through-hole diameter 1.0 mm, wall thickness 0.36 mm, geometric surface area approximately 2210 m². 2 / m 3 The axial compressive strength is 15 MPa. It is immersed in a 25 wt% dilute nitric acid solution, treated in a water bath at 80°C for 2 hours, washed with deionized water until neutral, and dried in an oven at 120°C for 6 hours.

[0074] Slurry preparation: 80g of nano-TiO2 powder and 434g of Ce(NO3)3·6H2O crystals were prepared according to a Ti:Ce molar ratio of 1:1. 5 wt% (based on total solid mass) of polyvinyl alcohol (PVA) was added as a binder, and 5g of methylcellulose was added as a pore-forming agent. Water was added to adjust the solid content to 30%. The slurry was ball-milled for 4 hours using a planetary ball mill to obtain a stable slurry with a D90 of approximately 5 μm.

[0075] One-time coating and firing: The pretreated honeycomb ceramic was immersed in the slurry and vacuum-assisted infiltration for 10 minutes. After removal, the inner walls of the pores were blown with compressed air to remove excess slurry. It was dried at 120℃ for 12 hours, and then placed in a muffle furnace and heated to 550℃ at a rate of 2℃ / min, and fired at a constant temperature for 3 hours. After cooling, it was weighed, and the coating load was calculated to be 20.7wt%.

[0076] Active component impregnation: Prepare a mixed aqueous solution containing RuCl3, Mn(NO3)2, and Ce(NO3)3 according to the target content of the active component, and load it onto the above-mentioned coated carrier using an equal-volume impregnation method. Let it stand at room temperature for 2 hours, and then dry it at 120°C for 6 hours.

[0077] Secondary calcination and reduction: The dried sample was placed in a tube furnace and calcined for 3 hours at 500℃ under N2 protection, with the temperature increased at 1℃ / min. After natural cooling to room temperature, the temperature was switched to a 5% H2 / N2 mixture and increased to 350℃ at 1℃ / min, then reduced at this temperature for 2 hours. After cooling, the finished catalyst A6 was obtained. ICP analysis showed that catalyst A6 contained 1.31 wt% Ru, 1.03 wt% Mn, and 0.22 wt% Ce (all based on coating weight).

[0078] Example 7:

[0079] This embodiment provides the preparation of a cordierite honeycomb ceramic support catalyst:

[0080] Substrate pretreatment: Cordierite honeycomb ceramic was selected as the substrate. Specifications: Cross-section 50×50 mm, length 100 mm, pore density 400 cpsi, through-hole diameter 0.5 mm, wall thickness 0.86 mm, geometric surface area 2210 m². 2 / m 3 The axial compressive strength is 15 MPa. It is immersed in a 15 wt% dilute nitric acid solution, treated in a water bath at 80°C for 2 hours, washed with deionized water until neutral, and dried in an oven at 120°C for 6 hours.

[0081] Slurry preparation: 80g of nano-TiO2 powder and 44g of Ce(NO3)3·6H2O crystals were prepared according to a Ti:Ce molar ratio of 1:0.1. 5 wt% (based on total solid mass) of polyvinyl alcohol (PVA) was added as a binder, and 2g of methylcellulose was added as a pore-forming agent. Water was added to adjust the solid content to 30%. The slurry was ball-milled for 4 hours using a planetary ball mill to obtain a stable slurry with a D90 of approximately 5 μm.

[0082] One-time coating and firing: The pretreated honeycomb ceramic was immersed in the slurry and vacuum-assisted infiltration for 10 minutes. After removal, the inner walls of the pores were purged with compressed air to remove excess slurry. It was dried at 120℃ for 12 hours, then placed in a muffle furnace and heated to 450℃ at a rate of 2℃ / min, and fired at this constant temperature for 4 hours. After cooling, it was weighed, and the coating load was calculated to be 5.1 wt%.

[0083] Active component impregnation: Prepare a mixed aqueous solution containing RuCl3, Mn(NO3)2, and Ce(NO3)3 according to the target content of the active component, and load it onto the above-mentioned coated carrier using an equal-volume impregnation method. Let it stand at room temperature for 2 hours, and then dry it at 120°C for 6 hours.

[0084] Secondary calcination and reduction: The dried sample was placed in a tube furnace and calcined for 5 hours under N2 protection, with the temperature increased to 400℃ at 1℃ / min. After natural cooling to room temperature, the temperature was switched to a 5% H2 / N2 mixture and increased to 300℃ at 1℃ / min, then reduced at this temperature for 5 hours. After cooling, the finished catalyst A7 was obtained. ICP analysis showed that catalyst A7 contained 0.74 wt% Ru, 1.17 wt% Mn, and 0.68 wt% Ce (all based on coating weight).

[0085] Example 8: Low Mn formulation catalyst

[0086] Similar to Example 1, except that the amount of manganese nitrate in the impregnation solution was reduced, and the Mn loading of the prepared catalyst was 0.5 wt% (based on the coating mass). The remaining steps were the same as in Example 1, and the finished catalyst was designated A8.

[0087] Comparative Example 1: Traditional Particulate Catalyst

[0088] The conventional extrusion molding process was used to produce granular catalysts. TiO2 powder, CeO2 powder, RuCl3, Mn(NO3)2, Ce(NO3)3 and pseudoboehmite binder were mixed, extruded, dried, calcined at 500℃ and reduced with hydrogen at 300℃ to obtain columnar granular catalyst B1 with a diameter of 3 mm.

[0089] Comparative Example 2: Monolithic Catalyst Without Additives

[0090] A monolithic Ru / TiO2 catalyst without added Mn and Ce promoters was used. The preparation steps were the same as in Example 1, but no manganese or cerium source was added to the slurry and impregnation solution to obtain catalyst B2.

[0091] Comparative Example 3: No Ce coating (TiO2 coating only)

[0092] Similar to Example 1, except that the coating does not contain CeO2, only TiO2 is used as the coating material, the same mass of TiO2 powder as in Example 1 is used, and no Ce source is added. The remaining steps are the same as in Example 1. Catalyst B3 is obtained.

[0093] Comparative Example 4: No Mn active component (Ru-Ce only)

[0094] Similar to Example 1, except that no manganese nitrate was added to the impregnation solution, and the active components were only Ru and Ce. The remaining steps were the same as in Example 1. Catalyst B4 was obtained.

[0095] Catalyst characterization analysis

[0096] XRD analysis: such as Figure 3 As shown, the XRD pattern of the A1 catalyst exhibits characteristic peaks of the cordierite matrix, characteristic peaks of anatase TiO2 (2θ≈25.3°, 37.8°, 48.0°, 55.1°), and characteristic peaks of CeO2 fluorite structure (2θ≈28.5°, 33.1°, 47.5°, 56.3°). The characteristic peak of Ru is extremely weak, indicating that Ru exists in a highly dispersed state (particle size <3nm). The XRD pattern showed almost no change after 1000h of reaction, confirming the excellent structural stability of the catalyst.

[0097] H2-TPR analysis: such as Figure 2 As shown, the A1 catalyst exhibits two main reduction peaks at approximately 120 °C and 280 °C, which are attributed to surface RuO, respectively. x The reduction of Ru and the reduction of oxygen species on the CeO2 surface were observed. Compared with the single Ru / Al2O3 catalyst, the reduction temperature of Ru decreased by about 40 °C, indicating that the addition of CeO2 promoted the reduction of Ru and enhanced the interaction between Ru and Ce. The addition of Mn shifted the high-temperature reduction peak further to a lower temperature by about 15 °C, indicating a significant electronic synergistic effect between Ru, Ce, and Mn.

[0098] Performance Evaluation

[0099] Catalyst performance was evaluated in a micro fixed-bed continuous hydrogenation unit. The feedstock was a 20 wt% nonylphenol / cyclohexane solution. The reaction conditions were uniformly set as follows: temperature 160 °C, pressure 4.5 MPa, and liquid hourly space velocity (LHSV) 1.0 h⁻¹. -1The molar ratio of hydrogen to nonylphenol was 20:1. After the reaction stabilized for 24 hours, samples were taken, and the product composition was analyzed by gas chromatography.

[0100] Table 1 Catalyst performance evaluation results

[0101]

[0102] As can be seen from the data in the table, the catalyst of the present invention maintains extremely high conversion and selectivity while exhibiting a significantly lower bed pressure drop (only about 18% of that in Comparative Example 1). Furthermore, the addition of promoters Mn and Ce significantly improves the stability of the catalyst. It is worth noting that although the FeCrAl alloy support used in Example 3 has a thinner wall thickness, its thermal conductivity (15~30 W / (m·K)) is much higher than that of the ceramic support. This allows for strict control of the radial temperature difference in the bed during the strongly exothermic hydrogenation reaction within 2°C, fundamentally eliminating the "hot spot" phenomenon commonly found in granular beds. This is crucial for achieving stable operation of the catalyst over a long period of 1000 hours.

[0103] Catalysts A1-A3 show that cordierite, mullite, and FeCrAl alloy supports can all achieve conversion rates and selectivity of ≥99.58%. Among them, FeCrAl alloy, due to its high thermal conductivity (15-30 W / (m·K)), can control the radial temperature difference of the bed within 2℃, which is the key to achieving stable operation over a long period of 1000 h. In contrast, the conventional particulate catalyst in Comparative Example 1 has a pressure drop as high as 65 kPa (compared to only 10-13 kPa in this invention), and the activity retention rate is only 85% after 1000 h, confirming the overwhelming advantage of the regular structure in terms of pressure drop and heat transfer. The conversion rate is ≥99.47% in the pore density range of 100-500 cpsi. The lowest pore density (A4, 100 cpsi) has the lowest pressure drop (10 kPa), while the higher pore density (A5-A7, 400-500 cpsi) slightly increases the conversion rate but the pressure drop increases slightly to 13 kPa. The optimal range is 200-300 cpsi.

[0104] The TiO2 to CeO2 mass ratio maintained high activity in the range of 1:0.1 to 1:3, with 1:0.5 to 1:1.5 being the preferred range (A1 to A3, A5 to A6). Excess CeO2 (A4, 1:3) resulted in the highest selectivity (99.72%), while insufficient CeO2 (A7, 1:0.1) slightly reduced the selectivity to 99.64%. Comparative Example 3 (without Ce coating) showed a conversion rate decrease to 96.42%, confirming that CeO2 is indispensable for maintaining high activity.

[0105] In the active components, the Ru loading range of 0.32% to 1.61% met the activity requirements. Decreasing the Mn content (A8, 0.5 wt%) reduced the selectivity to 99.11%, and in Comparative Example 4 (without Mn), it further decreased to 96.63%, indicating that Mn is a key auxiliary agent for inhibiting CO bond hydrogenolysis and maintaining high selectivity. Ce also functions as an electronic auxiliary agent in the active components; when its content is too low (A6, 0.22 wt%), the selectivity slightly decreases (to 99.37%). Comparative Example 2 (Ru / TiO2 without auxiliary agent) showed a conversion rate of only 95.31%, further confirming the necessity of the Ru-Mn-Ce ternary synergy.

[0106] Coating adhesion test:

[0107] Catalyst A1 prepared in Example 1 and catalyst A3 prepared in Example 3 were used to test the coating adhesion according to the relevant standard (scratch test*: test method for adhesion of fine ceramic coatings (current national standard, under the jurisdiction of the National Technical Committee on Standardization of Industrial Ceramics; specific operation: diamond indenter is used to scratch until the critical load (N) of coating peeling off, suitable for ceramic, wear-resistant and other hard coatings). The results showed that after 2 hours of ultrasonic oscillation at 40 kHz, the coating mass loss rate of A1 was 3.2%; after the same test, the mass loss rate of A3 was 2.8%. A1 and A3 were placed in a muffle furnace and quickly removed from 650°C and placed in air at 25°C. This cycle was repeated 10 times. The coating mass loss rate of A1 was 2.1%, and the coating mass loss rate of A3 was 1.6%, indicating that the coating and the carrier are extremely firmly bonded, exhibiting excellent mechanical stability and thermal shock stability.

[0108] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention, such as fine-tuning of the element substitution ratio, reasonable changes in sintering temperature, or adjustment of cooling rate, should all be covered within the scope of protection of the present invention.

Claims

1. A monolithic, well-structured catalyst, characterized in that, It includes a regular structure carrier and an active coating loaded on the surface and pores of the regular structure carrier; the active coating comprises a composite carrier material and an active metal component; based on the mass of the composite carrier material, the active metal component comprises the following components in mass percentage: ruthenium 0.5%~1.5%, cerium 0.5%~2.0%, and manganese 1.0%~3.0%.

2. The monolithic structured catalyst according to claim 1, characterized in that, Based on the mass of the regular structure carrier, the coating amount of the composite carrier material is 5% to 30%.

3. The monolithic structured catalyst according to claim 1 or 2, characterized in that, The composite carrier material is a composite of TiO2 and CeO2, wherein the mass ratio of TiO2 to CeO2 is 1:0.1 to 1:

3.

4. The monolithic structured catalyst according to claim 1 or 2, characterized in that, The regular structural carrier is one of cordierite honeycomb ceramic, mullite honeycomb ceramic, or FeCrAl alloy metal honeycomb.

5. The monolithic structured catalyst according to claim 4, characterized in that, The honeycomb ceramic carrier is cordierite honeycomb ceramic with a pore density of 200-300 cpsi and a pore diameter of 1.5-3.0 mm; the thinnest wall thickness between adjacent pores is 0.05-1.11 mm, and the geometric surface area is 1100-3160 m². 2 / m 3 The geometric surface area is calculated based on the inner wall area of ​​the through hole, excluding the end face.

6. The monolithic structured catalyst according to claim 4, characterized in that, The FeCrAl alloy metal honeycomb has a Cr content of 15%~25%, an Al content of 4%~8%, and the balance being unavoidable Fe impurities.

7. A method for preparing a monolithic, well-structured catalyst according to any one of claims 1-6, characterized in that, Includes the following steps: Pretreatment of regular structural carriers; A composite carrier coating slurry is prepared by mixing titanium source precursor, cerium source precursor, binder, pore-forming agent and water, followed by dispersion treatment. The composite carrier coating slurry is coated onto the surface of the pretreated regular structure carrier channels, dried, and then calcined in air at 400℃~600℃ for 3~5 hours to form a composite carrier coating. The composite carrier coating was impregnated with a soluble salt solution containing ruthenium, cerium, and manganese using an equal-volume impregnation method, and then allowed to stand for aging before drying. The impregnated carrier is calcined in a protective atmosphere at 300℃~500℃ for 2~5 hours; The calcined product was reduced in a reducing atmosphere at 250℃~350℃ for 2~5 hours to obtain the monolithic structured catalyst.

8. The method for preparing the monolithic structured catalyst according to claim 7, characterized in that, In the pretreatment process of the regular structure carrier, for metal carriers, a high-temperature oxidation treatment step is also included to form a metal oxide transition layer and enhance the adhesion of the coating.

9. The method for preparing the monolithic structured catalyst according to claim 7, characterized in that, The reducing atmosphere is hydrogen or a hydrogen-containing atmosphere.

10. The application of the monolithic, well-structured catalyst according to any one of claims 1-6, characterized in that, The monolithic, structured catalyst is used to catalyze the hydrogenation of nonylphenol to nonylcyclohexanol in a fixed-bed reactor.

Citation Information

Patent Citations

  • Method for preparing p-nonyl cyclohexanol with hydrogenating p-nonyl phenol

    CN103435449A

  • Method for continuously preparing nonyl cyclohexanol through catalytic hydrogenation of nonyl phenol

    CN104151134A