A novel supported carbon nanotube composite catalyst and a preparation method thereof
By using acidified multi-walled carbon nanotube supports and controlling the Cu/Ce molar ratio to 1:4 in the CuO-CeO₂ catalyst, the problems of thermal migration and sintering of active components were solved, achieving efficient low-temperature catalytic oxidation of carbon monoxide, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202611470065.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-20
AI Technical Summary
Existing CuO-CeO₂ catalysts are prone to thermal migration and sintering of active components during preparation, resulting in insufficient low-temperature kinetic performance. Furthermore, the composition design lacks theoretical guidance, making it difficult to achieve efficient low-temperature catalytic oxidation of carbon monoxide.
Using acidified multi-walled carbon nanotubes as a carrier, and controlling the Cu/Ce molar ratio to 1:4, the oxygen-containing functional groups on the surface of the carbon nanotubes are used for chemical anchoring. Combined with equal-volume impregnation and low-temperature slow calcination processes, the active components are highly dispersed and synergistically constructed.
The catalyst achieves efficient catalytic oxidation of carbon monoxide at relatively low temperatures, exhibiting excellent low-temperature activity and structural stability, making it suitable for industrial production.
Smart Images

Figure CN123128002A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of catalyst technology, specifically relating to a novel supported carbon nanotube composite catalyst and its preparation method. Background Technology
[0002] Carbon monoxide is a common toxic gas, mainly originating from incomplete combustion of fuels, industrial exhaust emissions, and combustion processes in confined spaces. Catalytic oxidation of carbon monoxide to carbon dioxide at lower temperatures is an important technological approach in air purification, exhaust gas treatment, and safety protection.
[0003] Noble metal catalysts (such as supported Pt, Pd, and Au) exhibit high activity in the low-temperature oxidation of carbon monoxide. However, noble metal resources are scarce and expensive, and noble metal nanoparticles are prone to sintering and agglomeration under high-temperature reaction conditions, leading to a decrease in activity. Furthermore, water vapor and carbon dioxide present in the reaction atmosphere may compete with carbon monoxide for adsorption at active sites, inhibiting the catalytic reaction and affecting the long-term stability of the catalyst. Therefore, developing efficient, stable, and low-cost non-noble metal catalysts for the low-temperature oxidation of carbon monoxide is of significant research importance and practical value.
[0004] Among non-precious metal catalyst systems, Co3O4, MnO2, NiO, CuO, Fe2O3, CeO2, and their composite oxides have the advantage of low cost. Among these, the CuO-CeO2 composite oxide catalyst is considered a promising non-precious metal low-temperature carbon monoxide oxidation catalyst system due to its combination of CuO's excellent activation ability for carbon monoxide and CeO2's unique oxygen storage and release capabilities. However, for CuO-CeO2 composite oxide catalysts, the relative content of Cu to Ce is a key factor determining the dispersion state of active species and catalytic performance. Currently, there are no systematic research reports on how the Cu / Ce ratio affects the low-temperature catalytic oxidation performance of carbon monoxide in CuO-CeO2 catalysts, resulting in a lack of clear theoretical guidance for the compositional design of CuO-CeO2 catalysts. In addition, existing CuO-CeO2 catalysts are usually prepared by hydrothermal methods or deposition precipitation methods. The active component particles obtained by the above methods are prone to thermal migration and sintering during drying, calcination or reaction, which reduces the effective interface area of CuO-CeO2 and the exposure of active sites is insufficient. At the same time, some catalysts also have problems such as low specific surface area and underdeveloped pore structure, resulting in insufficient low-temperature kinetic performance. Often, higher temperatures are required to achieve the ideal carbon monoxide conversion rate.
[0005] Therefore, there is an urgent need to develop a catalyst system that, based on the study of the influence of the Cu / Ce composition ratio on catalytic performance, achieves high dispersion of active components and full construction of the CuO-CeO2 synergistic interface, thereby achieving efficient catalytic oxidation of carbon monoxide at lower temperatures. Summary of the Invention
[0006] The primary objective of this invention is to provide a novel supported carbon nanotube composite catalyst. This product achieves high dispersion of the active components and full construction of the CuO-CeO2 synergistic interface by controlling the Cu / Ce loading ratio on multi-walled carbon nanotubes, thereby exhibiting excellent carbon monoxide catalytic oxidation performance at lower temperatures.
[0007] The second objective of this invention is to provide a method for preparing the above-mentioned novel supported carbon nanotube composite catalyst, which is simple in process, mild in operating conditions, and easy to industrialize.
[0008] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A novel supported carbon nanotube composite catalyst comprises an acidified multi-walled carbon nanotube support and copper oxide and cerium oxide active components supported on the surface of the acidified multi-walled carbon nanotube support; the active components account for 20-60% of the total mass of the catalyst, and the molar ratio of copper to cerium in the active components is 1:4; the copper oxide and cerium oxide are partially embedded in the tube wall defects and / or tube openings of the acidified multi-walled carbon nanotubes.
[0009] According to the above-mentioned novel supported carbon nanotube composite catalyst, the acidified multi-walled carbon nanotube has an outer diameter of 10-20 nm and a length of 5-15 μm; the surface of the acidified multi-walled carbon nanotube has carboxyl and hydroxyl oxygen-containing functional groups.
[0010] Based on the aforementioned novel supported carbon nanotube composite catalyst, the catalyst is further configured such that the reaction gas composition is 1 vol% CO, 20 vol% O2, and 79 vol% N2, and the space velocity is 30000 mL·g. -1 ·h -1 At a temperature of 80 ℃, its carbon monoxide conversion rate reaches more than 50%.
[0011] A method for preparing the above-mentioned novel supported carbon nanotube composite catalyst includes the following steps: A precursor solution is obtained by dissolving copper and cerium salts in water. Under grinding conditions, the precursor solution is added dropwise to acidified multi-walled carbon nanotubes. After thorough wetting, the solution is aged, dried, dispersed, calcined, cooled, and ground to obtain the final product. The dispersion operation is gentle grinding, used to disperse the aggregated carbon nanotubes.
[0012] According to the above-described method for preparing a novel supported carbon nanotube composite catalyst, the copper salt and cerium salt are copper nitrate and cerium nitrate, respectively; the ratio of the amount of acidified multi-walled carbon nanotubes, copper salt, cerium salt and water is 2 g: (0.16-0.94) g: (1.13-6.79) g: (7-7.2) mL, and the molar ratio of copper to cerium in the copper salt and cerium salt is fixed at 1:4.
[0013] The aforementioned copper salt and cerium salt can also be other soluble copper salts or cerium salts. When they are other soluble salts, the ratio of copper element in the acidified multi-walled carbon nanotubes, copper salt, cerium element in the cerium salt, and water is 2 g: (0.66-3.9) mmol: (2.6-15.6) mmol: (7-7.2) mL.
[0014] According to the above-described method for preparing the novel supported carbon nanotube composite catalyst, the aging time is further specified as 12-16 h; the calcination temperature is 240-260 ℃, the heating rate is 2-3 ℃ / min, and the time is 2-4 h.
[0015] According to the above-described method for preparing the novel supported carbon nanotube composite catalyst, the acidified multi-walled carbon nanotubes are further prepared by the following process: Multi-walled carbon nanotubes were added to a mixed acid solution, stirred and dispersed, refluxed at a constant temperature, naturally cooled, filtered under reduced pressure, and washed with deionized water until the pH of the filtrate was 6-7. Then the solution was dried and ground to obtain acidified multi-walled carbon nanotubes.
[0016] According to the above-described method for preparing the novel supported carbon nanotube composite catalyst, the ratio of the multi-walled carbon nanotubes to the mixed acid solution is further 2.0 g: 100-120 mL.
[0017] According to the above-described method for preparing the novel supported carbon nanotube composite catalyst, the mixed acid solution further comprises 90 mL of a 6 mol / L sulfuric acid solution and 30 mL of a 6 mol / L nitric acid solution.
[0018] According to the above-described method for preparing the novel supported carbon nanotube composite catalyst, the isothermal reflux temperature is 80-85 °C and the time is 4-6 h.
[0019] The beneficial technical effects of this invention are as follows: 1. The catalyst provided by this invention uses acidified multi-walled carbon nanotubes as a support, controlling the total mass of the active component at 20-60%, and precisely controlling the Cu / Ce molar ratio in the active component to 1:4. Simultaneously, it utilizes oxygen-containing functional groups such as carboxyl and hydroxyl groups on the surface of the acidified multi-walled carbon nanotubes to chemically anchor CuO and CeO2, resulting in high dispersion of the active component at the nanoscale and the formation of abundant synergistic interfaces. This results in both excellent low-temperature catalytic activity and good structural stability. On one hand, this catalyst exhibits outstanding activity in the low-temperature oxidation of carbon monoxide, significantly reducing the reaction temperature and achieving efficient conversion under mild conditions, overcoming the shortcomings of traditional unsupported catalysts in low-temperature kinetic performance. On the other hand, the unique tubular structure of the carbon nanotube support, combined with the anchoring effect of oxygen-containing functional groups, effectively inhibits thermal migration and sintering agglomeration of the active component during preparation and reaction, ensuring that the catalyst maintains uniform dispersion of the active component and integrity of the support structure even at high loadings, thus ensuring sustained stability of catalytic performance.
[0020] 2. The preparation method provided by this invention achieves precise loading and uniform dispersion of active components through the synergistic combination of three steps: equal-volume impregnation, room temperature aging, and low-temperature slow calcination. It features simple process, mild conditions, and suitability for large-scale production. First, by pre-measuring the saturated absorbent volume of the carrier and preparing a matching amount of precursor solution, the active components are uniformly loaded on the carrier surface. Combined with the room temperature aging process, metal ions are fully anchored to oxygen-containing functional group sites, effectively avoiding aggregation and segregation of the active components. Second, the method employs a low-temperature slow calcination process, which ensures sufficient decomposition of the precursor while effectively avoiding the oxidation and ablation of the carbon nanotube structure by high temperatures, maintaining the structural integrity of the carrier and the high dispersion of the active components. Attached Figure Description
[0021] Figure 1 X-ray powder diffraction patterns of cerium oxide and catalysts prepared in Comparative Examples 1-5; Figure 2 X-ray powder diffraction patterns of multi-walled carbon nanotubes and catalysts prepared in Examples 1-3 of this invention; Figure 3 These are scanning electron microscope images of the catalysts prepared in Examples 1-3 of this invention; Figure 4 Transmission electron microscope images of the catalysts prepared in Examples 1-3 of this invention; Figure 5 The graph shows the carbon monoxide conversion rate of the catalysts prepared in Comparative Examples 1-5 as a function of temperature. Figure 6 The graphs show the carbon monoxide conversion rate as a function of temperature for the catalysts prepared in Examples 1-3 and Comparative Examples 2-7. Detailed Implementation
[0022] The following is a further detailed description of the present invention in conjunction with specific preferred embodiments, and it should not be construed that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art, various simple deductions or substitutions can be made without departing from the concept of the present invention, and all such modifications and substitutions should be considered within the scope of protection of the present invention. Specific conditions not specified in the embodiments are performed according to conventional conditions or conditions recommended by the manufacturer. Unless otherwise specified, all reagents or instruments used are conventional products obtained through commercial channels.
[0023] (I) Implementation Examples Example 1 Example 1 provides a novel supported carbon nanotube composite catalyst, the catalyst comprising an acidified multi-walled carbon nanotube support and copper oxide and cerium oxide active components supported on the surface of the acidified multi-walled carbon nanotube support; the active components account for 20% of the total mass of the catalyst, and the molar ratio of copper to cerium in the active components is 1:4; the copper oxide and cerium oxide are partially embedded in the tube wall defects and / or tube openings of the acidified multi-walled carbon nanotubes.
[0024] This embodiment also provides a method for preparing a novel supported carbon nanotube composite catalyst, the specific steps of which are as follows: (1) Take 2.0 g of multi-walled carbon nanotubes and place them in a three-necked flask. Mix 90 mL of 6 mol / L sulfuric acid with 30 mL of 6 mol / L nitric acid and add the mixture to the flask. Stir at room temperature for 30 min to disperse the carbon nanotubes, and then reflux at 80℃ for 4-6 h to acidify. After the reaction is complete, allow the mixture to cool naturally and slowly pour the suspension into ice water to dilute it. Filter under reduced pressure and wash repeatedly with deionized water until the pH of the filtrate is 6-7. Dry the obtained solid at 80℃ for 12 h, grind it and pass it through a 100-mesh sieve to obtain acidified multi-walled carbon nanotubes. (2) Weigh 0.16 g Cu(NO3)2·3H2O and 1.13 g Ce(NO3)3·6H2O, dissolve them together in 7.2 mL of deionized water, stir at room temperature until clear, and obtain a precursor solution with a copper to cerium molar ratio of approximately 1:4; add the precursor solution dropwise to 2.0 g of acidified multi-walled carbon nanotube powder, grinding while adding, so that the powder is uniformly wetted. After the addition is complete, seal and age at room temperature for 12 h. The aged material is dried at 80℃ for 6 h, gently ground, and placed in a muffle furnace, heated from room temperature to 250℃ at 2℃ / min in air atmosphere, calcined at a constant temperature for 3 h, cooled naturally, and ground to obtain a novel supported carbon nanotube composite catalyst, denoted as 20% Cu2Ce8O. x / CNT.
[0025] Example 2 Example 2 provides a novel supported carbon nanotube composite catalyst, the catalyst comprising an acidified multi-walled carbon nanotube support and copper oxide and cerium oxide active components supported on the surface of the acidified multi-walled carbon nanotube support; the active components account for 40% of the total mass of the catalyst, and the molar ratio of copper to cerium in the active components is 1:4; the copper oxide and cerium oxide are partially embedded in the tube wall defects and / or tube openings of the acidified multi-walled carbon nanotubes.
[0026] The preparation process in this embodiment is basically the same as that in Example 1, except that the amounts of Cu(NO3)2·3H2O and Ce(NO3)3·6H2O used in step (2) are 0.42 g and 3.02 g, respectively, and the novel supported carbon nanotube composite catalyst is denoted as 40% Cu2Ce8O. x / CNT.
[0027] Example 3 Example 3 provides a novel supported carbon nanotube composite catalyst, the catalyst comprising an acidified multi-walled carbon nanotube support and copper oxide and cerium oxide active components supported on the surface of the acidified multi-walled carbon nanotube support; the active components account for 60% of the total mass of the catalyst, and the molar ratio of copper to cerium in the active components is 1:4; the copper oxide and cerium oxide are partially embedded in the tube wall defects and / or tube openings of the acidified multi-walled carbon nanotubes.
[0028] The preparation process in this embodiment is basically the same as that in Example 1, except that the amounts of Cu(NO3)2·3H2O and Ce(NO3)3·6H2O used in step (2) are 0.94 g and 6.79 g, respectively, and the novel supported carbon nanotube composite catalyst is denoted as 60% Cu2Ce8O. x / CNT.
[0029] (ii) Comparative Example Comparative Example 1 Comparative Example 1 provides a copper oxide and cerium oxide composite catalyst, denoted as Cu1Ce9O x It is prepared by the following process: Solution A was prepared by dissolving (NH4)2CO3 in water at a mass ratio of 1:41.6. Solution B was prepared by dissolving Ce(NO3)3·6H2O and Cu(NO3)2·3H2O in water at a molar ratio of 1:9. Solution A was added dropwise to solution B at a rate of 1 mL / min under stirring. After the addition was complete, stirring was continued for 2 h. The solution was centrifuged, washed with deionized water and anhydrous ethanol, dried at 60 °C, and then calcined at 550 °C at a rate of 2 °C / min for 4 h to obtain Cu1Ce9O.x .
[0030] Comparative Example 2 The preparation methods for Comparative Example 2 are basically the same as those for Comparative Example 1, except that the molar ratio of copper to cerium in Comparative Example 1 is adjusted to 2:8, denoted as Cu2Ce8O. x .
[0031] Comparative Example 3 The preparation process of Comparative Example 3 is basically the same as that of Comparative Example 1, except that the molar ratio of copper to cerium in Comparative Example 1 is adjusted to 3:7, denoted as Cu3Ce7O. x .
[0032] Comparative Example 4 The preparation process of Comparative Example 4 is basically the same as that of Comparative Example 1, except that the molar ratio of copper to cerium in Comparative Example 1 is adjusted to 4:6, denoted as Cu4Ce6O. x .
[0033] Comparative Example 5 The preparation process of Comparative Example 5 is basically the same as that of Comparative Example 1, except that the molar ratio of copper to cerium in Comparative Example 1 is adjusted to 5:5, denoted as Cu5Ce5O. x or CuCeO x .
[0034] Comparative Example 6 Comparative Example 6 is basically the same as the preparation of Example 1, except that the amounts of Cu(NO3)2·3H2O and Ce(NO3)3·6H2O used in step (2) are 0.45 g and 7.2 g, respectively, that is, the molar ratio of copper to cerium in the active components is 1:9, and the resulting composite catalyst is denoted as 60% Cu1Ce9O. x / CNT.
[0035] Comparative Example 7 Comparative Example 7 was prepared in basically the same way as Example 1, except that the amounts of Cu(NO3)2·3H2O and Ce(NO3)3·6H2O used in step (2) were 2.88 g and 5.18 g, respectively, meaning that the molar ratio of copper to cerium in the active components was 1:1. The resulting composite catalyst was designated as 60% CuCeO. x / CNT.
[0036] (III) Test Examples Phase structure testing XRD (X-ray diffraction) tests were performed on Comparative Examples 1-5 and Examples 1-3, such as... Figure 1-2 As shown; the XRD patterns of comparative examples 1-5 and cerium oxide are shown in the figure. Figure 1 As shown, the XRD patterns of Examples 1-3 and multi-walled carbon nanotubes are as follows: Figure 2 As shown. From Figure 1 As can be seen, unsupported samples with different copper-cerium molar ratios mainly exhibit characteristic peaks of the CeO2 fluorite structure, with no obvious independent CuO phase peaks, indicating that Cu species have high dispersion or partially enter the CeO2 lattice. With changes in copper content, the positions and intensities of the CeO2-related diffraction peaks change, indicating an interaction between the copper and cerium components. Figure 2 As can be seen, multi-walled carbon nanotubes have a distinct characteristic peak at approximately 26°. As the loading of copper-cerium active components increases from 20% to 60%, the characteristic peak of carbon nanotubes weakens relatively, while the CeO2-related diffraction peaks gradually strengthen, proving that copper-cerium oxide has been loaded onto carbon nanotubes.
[0037] Surface morphology test Scanning electron microscopy and transmission electron microscopy tests were performed on Examples 1-3 as follows: Figure 3-4 As shown; where Figure 3 (a) is the 20% Cu2Ce8O prepared in Example 1. x Scanning electron microscope image of / CNT. Figure 3 (b) is the 40% Cu2Ce8O prepared in Example 2. x Scanning electron microscope image of / CNT. Figure 3 (c) is the 60% Cu2Ce8O prepared in Example 3. x Scanning electron microscope image of / CNT; Figure 4 (a) is the 20% Cu2Ce8O prepared in Example 1. x Transmission electron microscope image of / CNT. Figure 4 (b) is the 40% Cu2Ce8O prepared in Example 2. x Transmission electron microscope image of / CNT. Figure 4 (c) is the 60% Cu2Ce8O prepared in Example 3. x Transmission electron micrograph of / CNT. From Figure 3 As can be seen, copper cerium oxide particles are dispersed within the carbon nanotube network, with some particles located at defects in the tube wall or near the tube opening. From... Figure 4 As can be seen, the tubular structure of the carbon nanotubes remains intact after calcination, and the copper-cerium nanoparticles form a close contact with the carbon nanotubes. With the increase of loading, the number of active particles increases, but the overall dispersion remains good.
[0038] Performance testing The carbon monoxide oxidation activity of the catalyst was evaluated using a fixed-bed microreactor, and the temperature (T) required to achieve a carbon monoxide conversion of 15% was determined. 15) and the temperature required for a conversion rate of 50% (T) 50 The activity intensity was measured by the standard. 100 mg of each of the catalysts prepared in Examples 1-3 and Comparative Examples 1-7 were placed in a reactor. A mixture of 1 vol% CO, 20 vol% O2 and 79 vol% N2 was used as the reaction gas (total flow rate 50 mL / min). The temperature was programmed to rise from 30 °C, and the composition of the outlet gas was detected online and the carbon monoxide conversion rate was calculated.
[0039] Test results are as follows Figure 5-6 As shown, the results indicate that using a fixed ratio of copper oxide and cerium oxide to support carbon nanotubes in Examples 1-3 significantly reduced the temperature required for the catalyst to achieve the same conversion rate, and within the test range, the catalytic activity increased with increasing loading of the active component. Specifically, 60% Cu₂Ce₈O₃... x / CNT catalyst T 15 and T 50 The conversion is achieved at 47 °C and 55 °C respectively, with near-complete conversion possible at approximately 75 °C; while the non-supported Cu₂Ce₈O x T compared to catalyst 15 and T 50 Cu3Ce7O was heated to 73℃ and 84℃ respectively. x Cu4Ce6O x Cu5Ce5O x T 15 and T 50 The temperatures increased sequentially, at 86 ℃ and 100 ℃, 89 ℃ and 129 ℃, and 110 ℃ and 140 ℃ respectively; while Cu1Ce9O x The activity is the worst, T 15 and T 50 The catalytic activity reached as high as 155 °C and 190 °C, respectively. This indicates that the catalytic activity is highest when the Cu / Ce molar ratio is 1:4; when the Cu / Ce molar ratio in the active component is 1:9 (60% Cu1Ce9O), the catalytic activity is highest. x / CNT) or 1:1 (60% CuCeO) x When / CNT), the CO conversion temperature is significantly higher than that of Example 3 of this application (60% Cu2Ce8O). xThe results indicate that the CO conversion performance of both is weaker than that of Example 3 of this application. These results fully demonstrate that the present invention, by precisely controlling the Cu / Ce molar ratio in the active component to 1:4 and the total mass of the active component to 20-60%, while utilizing the oxygen-containing functional groups on the surface of acidified carbon nanotubes to chemically anchor the copper-cerium active component, combined with equal-volume impregnation and low-temperature slow calcination processes, effectively inhibits the agglomeration of active particles and increases the synergistic interface sites of copper oxide / cerium oxide. This results in the catalyst exhibiting excellent catalytic activity and rapid conversion capacity even at low temperatures, verifying the significant effectiveness of the present invention in improving the low-temperature catalytic oxidation performance of carbon monoxide.
[0040] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them. The basic principles and main features of the present invention have been described above with specific implementation schemes. Based on the present invention, some modifications or substitutions can be made, but these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of protection claimed by the present invention.
Claims
1. A novel supported carbon nanotube composite catalyst, characterized in that, The catalyst comprises an acidified multi-walled carbon nanotube support and copper oxide and cerium oxide active components supported on the surface of the acidified multi-walled carbon nanotube support; the active components account for 20-60% of the total mass of the catalyst, and the molar ratio of copper to cerium in the active components is 1:4; the copper oxide and cerium oxide are partially embedded in the tube wall defects and / or tube openings of the acidified multi-walled carbon nanotubes.
2. The novel supported carbon nanotube composite catalyst according to claim 1, characterized in that, The acidified multi-walled carbon nanotubes have an outer diameter of 10-20 nm and a length of 5-15 μm; the surface of the acidified multi-walled carbon nanotubes has carboxyl and hydroxyl oxygen-containing functional groups.
3. The novel supported carbon nanotube composite catalyst according to claim 1, characterized in that, The catalyst was used in a reaction gas with a composition of 1 vol% CO, 20 vol% O2, and 79 vol% N2, and a space velocity of 30,000 mL·g. -1 ·h -1 At a temperature of 80 ℃, its carbon monoxide conversion rate reaches more than 50%.
4. A method for preparing a novel supported carbon nanotube composite catalyst according to any one of claims 1-3, characterized in that, Includes the following steps: Copper and cerium salts are dissolved in water to obtain a precursor solution. Under grinding conditions, the precursor solution is added dropwise to acidified multi-walled carbon nanotubes. After thorough wetting, the nanotubes are aged, dried, dispersed, calcined, cooled, and ground to obtain the final product.
5. The preparation method of the novel supported carbon nanotube composite catalyst according to claim 4, characterized in that, The copper salt and cerium salt are copper nitrate and cerium nitrate, respectively; the ratio of the acidified multi-walled carbon nanotubes, copper salt, cerium salt and water is 2 g: (0.16-0.94) g: (1.13-6.79) g: (7-7.2) mL.
6. The method for preparing the novel supported carbon nanotube composite catalyst according to claim 4, characterized in that, The aging time is 12-16 h; the calcination temperature is 240-260 ℃, the heating rate is 2-3 ℃ / min, and the time is 2-4 h.
7. The method for preparing the novel supported carbon nanotube composite catalyst according to claim 4, characterized in that, The acidified multi-walled carbon nanotubes were prepared by the following process: Multi-walled carbon nanotubes were added to a mixed acid solution, stirred and dispersed, refluxed at a constant temperature, naturally cooled, filtered under reduced pressure, and washed with deionized water until the pH of the filtrate was 6-7. Then the solution was dried and ground to obtain acidified multi-walled carbon nanotubes.
8. The method for preparing the novel supported carbon nanotube composite catalyst according to claim 7, characterized in that, The ratio of the multi-walled carbon nanotubes to the mixed acid solution is 2.0 g: 100-120 mL.
9. The method for preparing the novel supported carbon nanotube composite catalyst according to claim 7, characterized in that, The mixed acid solution consists of 90 mL of a 6 mol / L sulfuric acid solution and 30 mL of a 6 mol / L nitric acid solution.
10. The method for preparing the novel supported carbon nanotube composite catalyst according to claim 7, characterized in that, The isothermal reflux temperature is 80-85 ℃, and the time is 4-6 h.