Monolithic catalyst and method for its preparation and use

By preparing an integral catalyst with an iridium-based composite oxide coating, the stability and selectivity issues of dimethyl carbonate synthesis catalysts were solved, achieving higher catalytic activity and target product selectivity.

CN123128012APending Publication Date: 2026-11-20WANHUA CHEM GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611629314.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing catalysts for the synthesis of dimethyl carbonate suffer from poor stability and low selectivity.

Method used

An integral catalyst is used, including a support and an iridium-based composite oxide coating supported on the surface of the support. The coating contains iridium compounds and auxiliary components such as activated alumina or titanium dioxide. A uniform shell structure is formed by calcination, which, combined with other transition metal oxides, improves the stability and selectivity of the catalyst.

Benefits of technology

It improves the catalyst activity and product selectivity, reduces the selectivity of by-products, and enhances the catalyst stability and catalytic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present application relates to the technical field of chemical catalyst, in particular to a monolithic catalyst and its preparation method and application.The monolithic catalyst provided by the present application is composed of an iridium-based composite oxide coating and a carrier, the iridium-based composite oxide coating comprises an iridium-containing compound and an auxiliary component, the auxiliary component comprises active alumina and / or titanium dioxide; the mass percentage of iridium element in the monolithic catalyst is 0.1%-3.5%. Compared with the active component palladium in the prior art, the active component iridium in the catalyst has higher catalytic activity and product selectivity; by adding the auxiliary component, a uniform shell structure with active sites can be formed on the surface of the inert carrier, which provides a stable chemical environment for the active component iridium, so that the active component iridium is more stably and uniformly loaded on the surface of the carrier, and the selectivity of by-products is effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of chemical catalyst technology, specifically to a monolithic catalyst, its preparation method, and its application. Background Technology

[0002] Dimethyl carbonate (DMC) is a transparent liquid at room temperature with a slight odor. DMC is an important precursor for organic synthesis catalysts. Containing carbonyl, methyl, and methoxy groups, the DMC molecule exhibits excellent reactivity and can replace highly toxic phosgene, dimethyl sulfate, and chloromethane as carbonylating, methylating, and methoxylating agents. In production, it is safe, convenient, produces less pollution, and is easy to transport. Furthermore, DMC has wide applications in pesticides, pharmaceuticals, fragrances, fuel additives, solvents, and the electronics industry. In recent years, with the rapid development of the new energy vehicle industry, DMC, as a green new chemical raw material, has received attention and application in many fields, promoting the research and development of new DMC synthesis technologies. The synthesis of DMC has garnered widespread attention in the chemical industry and is currently one of the research hotspots in the field.

[0003] Currently, industrial methods for producing dimethyl carbonate include the phosgene process, transesterification, methanol oxidative carbonylation, urea alcoholysis, and direct synthesis from CO2 and methanol. Among these, the methanol gas-phase carbonylation method, with its inexpensive and readily available raw materials (methanol, CO, and oxygen), short process flow, and high atom economy, is considered a promising method for synthesizing dimethyl carbonate and is attracting increasing attention. This process uses a chlorinated copper salt as a catalyst, where carbon monoxide and methyl nitrite react via carbonylation to synthesize dimethyl carbonate, with dimethyl oxalate and methyl formate as byproducts. However, chlorinated catalysts suffer from poor stability, short lifespan, and low selectivity.

[0004] Therefore, providing a catalyst with high stability and high selectivity is of great significance for the synthesis of dimethyl carbonate. Summary of the Invention

[0005] This invention provides an integral catalyst, its preparation method, and its application, to solve the problems of poor stability and low selectivity in existing dimethyl carbonate synthesis catalysts.

[0006] In a first aspect, the present invention provides a monolithic catalyst comprising a support and an iridium-based composite oxide coating supported on at least a portion of the surface of the support. The iridium-based composite oxide coating includes an iridium-containing compound and an auxiliary component, wherein the auxiliary component includes at least one of activated alumina and titanium dioxide. The iridium content is 0.1%-3.5% by mass of the monolithic catalyst.

[0007] As an example, the mass percentage of iridium, based on the mass of the monolithic catalyst, can be 0.1%, 0.5%, 0.8%, 1%, 1.3%, 1.5%, 1.7%, 2%, 2.3%, 2.5%, 2.8%, 3%, 3.5%, or within any range of the above values.

[0008] In one alternative embodiment, the mass percentage of the auxiliary component is 10%-25% based on the mass of the monolithic catalyst; as an example, the mass percentage of the auxiliary component may be 10%, 13%, 15%, 17%, 19%, 20%, 23%, 25%, or within any of the above values ​​based on the mass of the monolithic catalyst.

[0009] In one optional embodiment, the additive component comprises activated alumina and titanium dioxide in a mass ratio of 5:1 to 1:5. As an example, the mass ratio of activated alumina to titanium dioxide in the additive component can be 5:1, 4:1, 3:1, 2:1, 1:1, 1:2, 1:3, 1:4, 1:5, or within any range of these values.

[0010] In one optional embodiment, the iridium-based composite oxide coating further includes other transition metal oxides, wherein the other transition metal elements include at least one of Group VIII and Group IB metal elements, and optionally include at least one of iron, cobalt, nickel, and copper; In one alternative embodiment, the mass percentage of the other transition metal elements is 0.01%-0.5% based on the mass of the monolithic catalyst. As an example, the mass percentage of the other transition metal elements based on the mass of the monolithic catalyst may be 0.01%, 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, or within any range of the above values.

[0011] In one optional embodiment, the activated alumina includes at least one of γ-Al2O3, η-Al2O3, and δ-Al2O3; In one optional embodiment, the titanium dioxide includes at least one of anatase titanium dioxide, rutile titanium dioxide, and plate titanium dioxide, and is optionally anatase titanium dioxide; In one optional embodiment, the carrier includes at least one of α-alumina, magnesium oxide, aluminum silicate, magnesium silicate, zirconium silicate, and ceramics; optionally, it is aluminum oxide and / or aluminum silicate; in this invention, there are no special requirements for the diameter of the carrier, for example, the diameter range can be 1-3 mm.

[0012] In one alternative embodiment, the carrier is spherical, annular, or butterfly-shaped.

[0013] Secondly, the present invention provides a method for preparing an integral catalyst, comprising the following steps: S1, iridium source, additive components, binder and optionally organic ligands, optionally other transition metal compounds are mixed to obtain coating slurry; S2, the coating slurry is coated onto the surface of the carrier to obtain the catalyst precursor; S3, the catalyst precursor is calcined to obtain a monolithic catalyst.

[0014] In an optional embodiment, in S1, the organic ligand includes at least one of a nitrogen-containing aromatic ligand, a β-diketone ligand, and an organophosphorus ligand.

[0015] In one alternative embodiment, the organic ligand comprises at least one selected from 2-phenylpyridine, 2,2-bipyridine, 1,10-phenanthroline, acetylacetone, and triphenylphosphine. In one optional embodiment, the molar ratio of the organic ligand to iridium in the coating slurry is 1:1 to 5:1. As an example, the molar ratio of the organic ligand to iridium in the coating slurry can be 1:1, 2:1, 3:1, 4:1, 5:1, or within any range of these values.

[0016] In one optional embodiment, in S1, the mass percentage of the binder, based on the total solids content in the coating slurry, is 10%-20%; as an example, the mass percentage of the binder, based on the total solids content in the coating slurry, can be 10%, 12%, 14%, 15%, 17%, 19%, 20%, or within any range of the above values.

[0017] In one alternative embodiment, the adhesive includes, but is not limited to, at least one of polyvinyl acetate emulsion, a copolymer of vinyl acetate / vinyl laurate, a copolymer of vinyl acetate / acrylate, and a copolymer of vinyl acetate / ethylene.

[0018] In one optional embodiment, in S3, the roasting temperature is 250-450℃, and the roasting time is 2-6h; as an example, the roasting temperature can be 250℃, 270℃, 300℃, 330℃, 350℃, 380℃, 400℃, 430℃, 450℃, or within any range of the above values; the roasting time can be 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, or within any range of the above values.

[0019] In one alternative embodiment, the calcination is carried out in an aerobic atmosphere. Alternatively, calcination is carried out in an air atmosphere.

[0020] In one optional embodiment, the iridium source includes one or more of chloroiridic acid, sodium chloroiridate, potassium chloroiridate, iridium trichloride, and iridium acetylacetone; optionally, it is sodium chloroiridate. It should be noted that an aqueous solution containing the above-mentioned iridium source can be used, and the amount of iridium source used is measured based on the effective content without water.

[0021] In one alternative embodiment, the other transition metal compound includes a transition metal salt, optionally at least one of iron, cobalt, nickel, copper nitrate, acetate, or hydrochloride.

[0022] In one optional embodiment, the binder is present or used in the form of an aqueous dispersion (emulsion). It should be noted that the specific embodiments of the present invention use an aqueous dispersion containing the above-mentioned binder, and the amount of binder used is measured based on its effective content without water. The solid content of the aqueous dispersion of the binder is conventional in the art and is not specifically limited by the present invention.

[0023] It should be noted that, in the preparation process of the monolithic catalyst, the amounts of the iridium source, other transition metal compounds, and auxiliary components are adaptively adjusted and determined according to the content of iridium, other transition metal elements, and iridium-based composite oxide coating in the target product.

[0024] Specifically, the method for preparing the monolithic catalyst provided by the present invention may include the following steps: S1, mix the iridium source, optionally other transition metal compounds and optionally organic ligands with water to obtain material A; mix material A with the auxiliary components (activated alumina and / or titanium dioxide powder) and stir for 0.5-3 hours, then add the binder and continue stirring for 1-4 hours to obtain the iridium-based composite oxide coating slurry; In this invention, there are no special requirements for the solid content of the coating slurry, as long as it can meet the requirements of the subsequent coating process.

[0025] S2, the iridium-based composite oxide coating slurry obtained in S1 is coated onto the support in the form of an outer shell layer using a coating machine to obtain an integral catalyst precursor; the present invention can control the proportion of iridium-based composite oxide coating in the integral catalyst by adjusting the amount of iridium-based composite oxide coating slurry and support. S3, the monolithic catalyst precursor prepared in S2 is calcined at 250-450 °C for 2-6 h to obtain the monolithic catalyst.

[0026] In this invention, "optional" means that the matter or event described thereafter may or may not occur, and the description includes both the scenario in which the event occurs and the scenario in which the event does not occur.

[0027] Thirdly, the present invention provides an application of the above-described monolithic catalyst or the monolithic catalyst prepared by the above-described preparation method in the gas-phase synthesis of dimethyl carbonate from methanol.

[0028] The technical solution of this invention has the following advantages: The monolithic catalyst provided by this invention comprises an iridium-based composite oxide coating and a support. The iridium-based composite oxide coating includes an iridium-containing compound and an auxiliary component, wherein the auxiliary component includes at least one of activated alumina and titanium dioxide. The iridium content, by mass percentage, is 0.1%-3.5% of the monolithic catalyst. Compared to the active component palladium in the prior art, the iridium in this catalyst exhibits higher catalytic activity and product selectivity. By adding the auxiliary components activated alumina and / or titanium dioxide, a uniform shell structure with active sites can be formed on the surface of the inert support, providing a stable chemical environment for the active iridium, making it more stably and uniformly loaded on the support surface, and effectively reducing the selectivity of byproducts.

[0029] The monolithic catalyst provided by this invention, through the combined use of activated alumina and titanium dioxide, can further reduce the selectivity of byproducts (such as dimethyl oxalate).

[0030] The monolithic catalyst provided by this invention can improve the dispersibility of iridium oxides on the catalyst surface by adding other transition metal compounds, thereby further enhancing catalytic performance.

[0031] The monolithic catalyst preparation method provided by this invention can prepare a catalyst composed of an iridium-based composite oxide coating and a support. This method enables the active component iridium to be uniformly dispersed on the surface of the support. Finally, the binder and ligands are removed by calcination, resulting in a rich porous structure on the catalyst surface. This ensures the activity and stability of the catalyst. The preparation method is simple, easy to operate, and easy to promote and apply.

[0032] The present invention provides a method for preparing an integral catalyst, in which the addition of a suitable organic ligand can effectively improve the stability of the catalyst and further enhance the conversion rate of the raw materials and the selectivity of the target product.

[0033] Additional aspects and advantages of the invention will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Detailed Implementation

[0034] The following embodiments are provided to better understand the present invention, but the following embodiments do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the scope of protection of the present invention.

[0035] Unless otherwise specified, all experimental steps or conditions in the examples were performed according to conventional experimental procedures and conditions in the art. Reagents or instruments whose manufacturers are not specified are all commercially available products.

[0036] The present invention will now be described with reference to specific embodiments. It should be noted that these embodiments are merely descriptive and do not limit the present invention in any way.

[0037] In the following examples and comparative examples, the main sources of raw materials are as follows: Sodium chloroiridium dodecahydrate (analytical grade), 2-phenylpyridine (analytical grade), ferric nitrate (analytical grade), cobalt nitrate (analytical grade), nickel nitrate (analytical grade), and copper nitrate (analytical grade) were all purchased from Beijing Innocare Technology Co., Ltd. Methyl nitrite (purity greater than 99.5%), carbon monoxide (purity greater than 99.9%), and hydrogen chloride (HCl content 500ppm, balance nitrogen) were purchased from Dalian Date Gas Co., Ltd.

[0038] Example 1 This embodiment provides a monolithic catalyst, the specific composition of which and its preparation method are as follows: (1) Weigh 18g sodium chloroiridium dodecahydrate, 8.1g 2-phenylpyridine, 1.48g copper nitrate and mix with 350mL deionized water to prepare a mixture. (2) Weigh 20g of γ-alumina powder and 40g of anatase titanium dioxide powder, and add them to the mixture prepared in step (1). Stir at room temperature for 1 hour to obtain iridium-based composite oxide coating precursor slurry. (3) Weigh 75g of polyvinyl acetate emulsion (solid content is 55wt%) and add it to the iridium-based composite oxide coating precursor slurry prepared in step (2). Stir at room temperature for 2h to obtain the iridium-based composite oxide coating slurry. (4) The iridium-based composite oxide coating slurry obtained in step (3) is coated onto a 430g spherical α-alumina support with a diameter of about 1-3mm using a coating machine to obtain an integral catalyst precursor; (5) The monolithic catalyst obtained in step (4) is calcined at 400°C for 3 hours in an air atmosphere to obtain the monolithic catalyst.

[0039] Example 2 This embodiment provides a monolithic catalyst, the specific composition of which and its preparation method are as follows: (1) Weigh 18g sodium chloroiridium dodecahydrate, 8.1g 2-phenylpyridine, 1.56g nickel nitrate and mix with 350mL deionized water to prepare a mixture. (2) Weigh 20g of γ-alumina powder and 40g of anatase titanium dioxide powder, and add them to the mixture prepared in step (1). Stir at room temperature for 1 hour to obtain iridium-based composite oxide coating precursor slurry. (3) Weigh 75g of polyvinyl acetate emulsion (solid content is 55wt%) and add it to the iridium-based composite oxide coating precursor slurry prepared in step (2). Stir at room temperature for 2h to obtain the iridium-based composite oxide coating slurry. (4) The iridium-based composite oxide coating slurry obtained in step (3) is coated onto a 430g spherical α-alumina support with a diameter of about 1-3mm using a coating machine to obtain an integral catalyst precursor; (5) The monolithic catalyst obtained in step (4) is calcined at 400°C for 3 hours in an air atmosphere to obtain the monolithic catalyst.

[0040] Example 3 This embodiment provides an integral catalyst, which differs from Example 1 only in that an anatase titanium dioxide powder of equal mass is used instead of γ-alumina powder.

[0041] Example 4 This embodiment provides an integral catalyst, which differs from Example 1 only in that anatase titanium dioxide powder of equal mass is used instead of γ-alumina powder.

[0042] Example 5 This embodiment provides a monolithic catalyst, the specific composition of which and its preparation method are as follows: (1) Weigh 54g sodium chloroiridium dodecahydrate, 60.72g 2-phenylpyridine, 0.05g copper nitrate and mix with 450mL deionized water to prepare a mixture. (2) Weigh 104g of γ-alumina powder and 20.8g of anatase titanium dioxide powder, and add them to the mixture prepared in step (1). Stir at room temperature for 3 hours to obtain iridium-based composite oxide coating precursor slurry. (3) Weigh 90.9g of polyvinyl acetate emulsion (solid content is 55wt%) and add it to the iridium-based composite oxide coating precursor slurry prepared in step (2). Stir at room temperature for 4h to obtain the iridium-based composite oxide coating slurry. (4) The iridium-based composite oxide coating slurry obtained in step (3) is coated onto a 375g spherical α-alumina support with a diameter of about 1-3mm using a coating machine to obtain an integral catalyst precursor; (5) The monolithic catalyst obtained in step (4) is calcined at 450°C for 6 hours in an air atmosphere to obtain the monolithic catalyst.

[0043] Example 6 This embodiment provides a monolithic catalyst, the specific composition of which and its preparation method are as follows: (1) Weigh 1.8g sodium chloroiridium dodecahydrate, 0.7g 2-phenylpyridine, 2.5g copper nitrate and mix with 350mL deionized water to prepare a mixture. (2) Weigh 8.4g of γ-alumina powder and 41.7g of anatase titanium dioxide powder, and add them to the mixture prepared in step (1). Stir at room temperature for 0.5h to obtain iridium-based composite oxide coating precursor slurry. (3) Weigh 181.8g of polyvinyl acetate emulsion (solid content is 55wt%) and add it to the iridium-based composite oxide coating precursor slurry prepared in step (2). Stir at room temperature for 1h to obtain the iridium-based composite oxide coating slurry. (4) The iridium-based composite oxide coating slurry obtained in step (3) is coated onto a 450g spherical α-alumina support with a diameter of about 1-3mm using a coating machine to obtain an integral catalyst precursor; (5) The monolithic catalyst obtained in step (4) is calcined at 250°C for 2 hours in an air atmosphere to obtain the monolithic catalyst.

[0044] Example 7 This embodiment provides a monolithic catalyst, the specific composition of which and its preparation method are as follows: (1) Weigh 18g of sodium chloroiridium dodecahydrate, 8.1g of 2-phenylpyridine and 350mL of deionized water and mix them to prepare a mixture. (2) Weigh 20g of γ-alumina powder and 40g of anatase titanium dioxide powder, and add them to the mixture prepared in step (1). Stir at room temperature for 1 hour to obtain iridium-based composite oxide coating precursor slurry. (3) Weigh 75g of polyvinyl acetate emulsion (solid content is 55wt%) and add it to the iridium-based composite oxide coating precursor slurry prepared in step (2). Stir at room temperature for 2h to obtain the iridium-based composite oxide coating slurry. (4) The iridium-based composite oxide coating slurry obtained in step (3) is coated onto a 430g spherical α-alumina support with a diameter of about 1-3mm using a coating machine to obtain an integral catalyst precursor; (5) The monolithic catalyst obtained in step (4) is calcined at 400°C for 3 hours in an air atmosphere to obtain the monolithic catalyst.

[0045] Example 8 This embodiment provides a monolithic catalyst, the specific composition of which and its preparation method are as follows: (1) Weigh 18g of sodium chloroiridium dodecahydrate, 8.1g of 2-phenylpyridine and 350mL of deionized water and mix them to prepare a mixture. (2) Weigh 60g of γ-alumina powder and add it to the mixture prepared in step (1). Stir at room temperature for 1h to obtain iridium-based composite oxide coating precursor slurry. (3) Weigh 75g of polyvinyl acetate emulsion (solid content is 55wt%) and add it to the iridium-based composite oxide coating precursor slurry prepared in step (2). Stir at room temperature for 2h to obtain the iridium-based composite oxide coating slurry. (4) The iridium-based composite oxide coating slurry obtained in step (3) is coated onto a 430g spherical α-alumina support with a diameter of about 1-3mm using a coating machine to obtain an integral catalyst precursor; (5) The monolithic catalyst obtained in step (4) is calcined at 400°C for 3 hours in an air atmosphere to obtain the monolithic catalyst.

[0046] Example 9 This embodiment provides an integral catalyst, which differs from Example 1 in the selection of raw materials, specifically as follows: acetylacetone is used in place of 2-phenylpyridine in equal molar amounts, γ-alumina powder is used in place of equal mass of η-Al2O3 in place of γ-alumina powder in place of equal mass of rutile titanium dioxide in place of anatase titanium dioxide ...

[0047] Example 10 This embodiment provides an integral catalyst, which differs from Example 1 in the selection of raw materials, specifically as follows: triphenylphosphine is used in place of 2-phenylpyridine in equal molar amounts, cobalt nitrate is used in place of copper nitrate in equal mass, and spherical aluminum silicate is used in place of spherical α-alumina support in equal mass.

[0048] Example 11 This embodiment provides an integral catalyst, which differs from Example 1 only in that no ligand is added in step (1).

[0049] Comparative Example 1 This comparative example provides a monolithic catalyst, the specific composition and preparation method of which are as follows: (1) Weigh 10.55g palladium acetate and 1.48g copper nitrate and dissolve them in 350mL deionized water to prepare a mixed solution; (2) Weigh 20g of γ-alumina powder and 40g of anatase titanium dioxide powder, and add them to the mixed solution prepared in step (1). Stir at room temperature for 1 hour to obtain palladium-based composite oxide coating precursor slurry. (3) Weigh 75g of polyvinyl acetate emulsion (solid content is 55wt%) and add it to the palladium-based composite oxide coating precursor slurry prepared in step (2). Stir at room temperature for 2 hours to obtain palladium-based composite oxide coating slurry. (4) The palladium-based composite oxide coating slurry obtained in step (3) is coated onto a 430g spherical α-alumina support with a diameter of about 1-3mm using a coating machine to obtain an integral catalyst precursor; (5) The monolithic catalyst obtained in step (4) is calcined at 400°C for 3 hours in an air atmosphere to obtain the monolithic catalyst.

[0050] Comparative Example 2 This comparative example provides an integral catalyst that, compared to Example 11, does not contain any active additive components and uses an equal mass of inert α-alumina instead of active γ-alumina and titanium dioxide.

[0051] Comparative Example 3 This comparative example provides an integral catalyst, which differs from Example 11 in that the amount of sodium chloroiridium dodecahydrate is adjusted to 0.18g.

[0052] Comparative Example 4 This comparative example provides an integral catalyst, which differs from Example 11 in that the amount of sodium chloroiridium dodecahydrate is adjusted to 89.8g.

[0053] Experimental Example 1 The monolithic catalysts prepared in each embodiment and comparative example were subjected to various performance tests. The specific test items and methods are as follows: (1) The specific steps for testing the content of iridium, other transition metal elements and auxiliary components are as follows: 1. Weigh 0.1g of sample and add it to a polytetrafluoroethylene digestion tube. Add 3 mL of 65% nitric acid and microwave digest at 250℃ to remove the binder.

[0054] 2. After digestion, remove the digestion tube, cool it to room temperature, add 3 mL of 40% hydrofluoric acid, heat it to completely dissolve the iridium-based composite metal oxide coating, and filter to separate the carrier.

[0055] 3. Add 1 mL of 98% sulfuric acid to the digestion solution and heat to remove excess hydrofluoric acid.

[0056] 4. Add 1 mL of 36% hydrochloric acid to stabilize the complex.

[0057] 5. After cooling to room temperature, transfer to a 100 mL volumetric flask and dilute to volume with ultrapure water.

[0058] 6. The metal elements were quantitatively analyzed using an Agilent 5800 ICP-OES spectrometer, and the mass percentage of iridium and other transition metal elements in the monolithic catalyst, as well as the mass percentage of the additive components in the iridium-based composite oxide coating, were calculated.

[0059] (2) Catalyst evaluation methods The monolithic catalysts prepared in each embodiment and comparative example were placed in a micro fixed-bed reactor with an inner diameter of 20 mm and a catalyst loading of 10 mL. The reaction was carried out at a temperature of 120 °C, a pressure of 0.60 MPaG, and a space velocity of 3000 h⁻¹. -1 The catalyst activity was evaluated under the conditions of a methyl nitrite to carbon monoxide molar ratio of 1.1:1 and an HCl concentration of 50 ppm. Samples were taken and analyzed after 100 h and 500 h of device operation. The content of each product was quantitatively analyzed using an Agilent 8890 gas chromatograph to obtain CO conversion and DMC selectivity data.

[0060] The specific test results are shown in the table below: Table 1 Test Results

[0061] The test results above show that, compared with the comparative example, the embodiments of the present invention, by using the active component iridium in combination with the auxiliary component, can enable the catalyst to have higher catalytic activity and product selectivity. A comparison of Examples 3-4 with Example 1 shows that the combined use of activated alumina and titanium dioxide can further reduce the selectivity of byproducts (such as dimethyl oxalate) and improve the catalyst conversion rate and the selectivity of the target product. A comparison of Example 7 with Example 1 shows that the addition of other transition metal compounds can further enhance catalytic performance. A comparison of Example 11 with Example 1 shows that adding appropriate organic compounds during the preparation process can effectively improve the stability of the catalyst and further enhance the conversion rate of the raw materials and the selectivity of the target product.

[0062] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A monolithic catalyst, characterized in that, Includes a carrier and an iridium-based composite oxide coating loaded on at least a portion of the surface of the carrier. The iridium-based composite oxide coating includes an iridium-containing compound and an auxiliary component, wherein the auxiliary component includes at least one of activated alumina and titanium dioxide. The iridium content is 0.1%-3.5% by mass of the monolithic catalyst.

2. The monolithic catalyst according to claim 1, characterized in that, The mass percentage of the auxiliary component, based on the mass of the monolithic catalyst, is 10%-25%. And / or, the additive components include activated alumina and titanium dioxide in a mass ratio of 5:1 to 1:

5.

3. The monolithic catalyst according to claim 1, characterized in that, The iridium-based composite oxide coating also includes other transition metal oxides, wherein the other transition metal elements include at least one of Group VIII and Group IB metal elements, and optionally include at least one of iron, cobalt, nickel, and copper.

4. The monolithic catalyst according to claim 3, characterized in that, Based on the mass of the monolithic catalyst, the mass percentage of the other transition metal elements is 0.01%-0.5%; And / or, the activated alumina includes at least one of γ-Al2O3, η-Al2O3, and δ-Al2O3; And / or, the titanium dioxide includes at least one of anatase titanium dioxide, rutile titanium dioxide, and plate titanium dioxide; And / or, the carrier includes at least one of α-alumina, magnesium oxide, aluminum silicate, magnesium silicate, zirconium silicate, and ceramics; And / or, the carrier is spherical, annular, or butterfly-shaped.

5. A method for preparing an integral catalyst, characterized in that, Includes the following steps: S1, iridium source, additive components, binder and optionally organic ligands, optionally other transition metal compounds are mixed to obtain coating slurry; S2, the coating slurry is coated onto the surface of the carrier to obtain the catalyst precursor; S3, the catalyst precursor is calcined to obtain a monolithic catalyst.

6. The method for preparing the monolithic catalyst according to claim 5, characterized in that, In S1, the organic ligand includes at least one of nitrogen-containing aromatic ligands, β-diketone ligands, and organophosphine ligands.

7. The method for preparing the monolithic catalyst according to claim 6, characterized in that, The organic ligand includes at least one of 2-phenylpyridine, 2,2-bipyridine, 1,10-phenanthroline, acetylacetone, and triphenylphosphine; And / or, the molar ratio of organic ligands to iridium in the coating slurry is 1:1 to 5:

1.

8. The method for preparing the monolithic catalyst according to any one of claims 5-7, characterized in that, In S1, the adhesive has a mass percentage content of 10%-20% based on the total solids content in the coating slurry. And / or, the adhesive comprises at least one of polyvinyl acetate emulsion, a copolymer of vinyl acetate / vinyl laurate, a copolymer of vinyl acetate / acrylate, and a copolymer of vinyl acetate / ethylene.

9. The method for preparing the monolithic catalyst according to any one of claims 5-7, characterized in that, In S3, the calcination temperature is 250-450℃, and the calcination time is 2-6 hours; And / or, the calcination is carried out in an aerobic atmosphere.

10. The application of the monolithic catalyst according to any one of claims 1-4 or the monolithic catalyst prepared by the preparation method according to any one of claims 5-9 in the gas-phase synthesis of dimethyl carbonate from methanol.