A core-shell structure composite material, a catalyst and a preparation method and application thereof
By using the core-shell composite material Pd@CeO₂@NiO catalyst, the problems of activity stability and purity in the preparation of carbon nanotubes by methane cracking in the existing technology have been solved, realizing the efficient and low-cost generation of carbon nanotubes, which is suitable for industrial production.
Patent Information
- Application Number
- CN202611644350.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-23
- Publication Date
- 2026-11-20
AI Technical Summary
Existing catalysts for the preparation of carbon nanotubes from methane cracking suffer from poor activity stability, low purity of the produced carbon nanotubes, insufficient graphitization, and uneven diameter distribution. Furthermore, the preparation process is complex and costly, making it difficult to meet the requirements of high-end applications.
A multi-level core-shell structure was constructed using the core-shell composite material Pd@CeO₂@NiO through an aqueous phase synthesis method. The structure includes a Pd@CeO₂@NiO catalyst, and the synergistic effect of the CeO₂ shell and the NiO core is utilized to achieve methane cracking to generate high-quality carbon nanotubes and hydrogen.
It achieves efficient, highly active, and highly stable catalytic cracking of methane to generate bamboo-like multi-walled carbon nanotubes, reducing the amount of precious metals used and the preparation cost, making it suitable for industrial production.
Smart Images

Figure CN123128013A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of energy and environmental catalyst technology, specifically relating to a core-shell structured composite material, a catalyst, its preparation method, and its application. Background Technology
[0002] Methane catalytic cracking (MP) (CH4→C+2H2) for hydrogen production is a promising low-carbon hydrogen production route because its products do not contain carbon oxides, thus avoiding the large CO2 emissions of traditional steam reforming processes. However, the solid carbon generated in traditional cracking reactions easily deposits on the catalyst surface, leading to rapid deactivation of the active components. In current industrial practice, deactivated catalysts are often regenerated by air burning, which not only consumes the carbon byproducts as low-value fuel but also releases CO2, partially offsetting the environmental advantages of this process.
[0003] Carbon nanotubes, as one-dimensional carbon nanomaterials, possess excellent electrical and thermal conductivity and mechanical properties, making them valuable for applications in catalysis, energy storage, and electromagnetic shielding composites. Converting carbon byproducts from methane cracking into high-quality carbon nanotubes would avoid resource waste and carbon emissions associated with combustion and regeneration, while significantly enhancing the economic value of the byproducts. However, existing catalytic materials for preparing carbon nanotubes from methane cracking generally suffer from poor activity stability, low purity of the produced carbon nanotubes, insufficient graphitization, and uneven diameter distribution, failing to meet the stringent requirements for carbon material consistency in high-end applications. Furthermore, some catalysts require complex pretreatment processes, increasing process complexity and cost. Therefore, the field anticipates the development of a novel catalytic material capable of efficiently catalyzing methane cracking and simultaneously generating high-quality carbon nanotubes, meeting urgent industrial needs and possessing significant practical value.
[0004] Currently, traditional heterogeneous catalyst preparation technologies are mainly divided into two categories. One is the impregnation and loading method, in which transition metal or noble metal salts are impregnated onto the surface of a porous support. After calcination and reduction, the metal particles have a wide size distribution (typically 5-50 nm) and poor dispersion, resulting in uneven carbon nanotube diameters, low graphitization, and easy metal agglomeration, leading to insufficient active site density. The other is the pre-synthesized nanoparticle method, in which a uniform metal colloid is first synthesized in the liquid phase and then loaded. Although this can improve the uniformity of the nanoparticle diameter, the process is cumbersome, involving organic ligands, multiple centrifugation and washing, and the residues are difficult to completely remove. Uniformity is difficult to maintain during scale-up, and the cost is high. It is evident that the existing technologies for heterogeneous catalyst processes present a prominent contradiction: "simple methods have poor quality, while refined methods have high costs."
[0005] For example, Chinese patent CN122424828A discloses a hydrocarbon cracking hydrogen production molten catalyst, specifically a NiMo-Bi liquid alloy molten catalyst. This catalyst involves adding bismuth to nickel-molybdenum oxide and reducing it with high-temperature hydrogen to form a ternary liquid alloy, which is used for the cracking of low-carbon alkanes such as methane to produce hydrogen. This catalyst exhibits excellent catalytic activity and stability, and the carbon material is easily separated. However, this catalyst requires hydrogen reduction treatment at 700℃, and the temperature must be maintained above 450℃ throughout the reaction to keep the alloy in a liquid state, resulting in high energy consumption. Furthermore, the bismuth content in the catalyst is as high as 68-89.8%, requiring a large amount of low-melting-point metal, significantly increasing raw material costs and imposing high corrosion resistance requirements on the reaction equipment, which is detrimental to large-scale industrial application.
[0006] For example, the PM-FeAlO catalyst disclosed in Chinese patent CN122499788A is a FeAlO catalyst modified by gel molding combined with plasma ball milling. First, the FeAlO catalyst matrix is prepared using a gel molding process, and then the surface is synergistically activated by plasma ball milling for methane cracking to produce hydrogen and co-produce carbon nanotubes. However, the preparation process of this catalyst involves multiple steps, including gel molding, high-temperature calcination (1000-1400℃), and plasma ball milling. The operation is complex and time-consuming, and the plasma ball milling equipment requires significant investment and is difficult to scale up. Furthermore, the calcination temperature of the catalyst matrix is as high as 1350℃, resulting in extremely high energy consumption and increased manufacturing costs.
[0007] For example, Chinese patent CN122424827A discloses a nickel-based single-walled carbon nanotube catalyst supported on a hierarchical pore structure. This catalyst is a nickel-based catalyst supported on a hierarchical Al2O3-ZrO2 composite support. Through a combination of liquid-phase impregnation and gas-phase migration, molybdenum, lanthanum, and nickel are positioned in the mesopores, macropores, and micropores of the support, respectively, for catalytic cracking to prepare single-walled carbon nanotubes. However, the synthesis of this catalyst support involves the use of microporous template agents (F127) and macroporous template agents (PMMA microspheres), and requires multiple demolding operations such as Soxhlet extraction and tetrahydrofuran dissolution, supplemented by supercritical CO2 drying. The preparation process is extremely cumbersome and lengthy. Simultaneously, the gas-phase migration impregnation requires strict control of sublimation temperature and carrier gas flow rate, resulting in a narrow process window and poor reproducibility, making large-scale mass production difficult. The multiple template agents and complex operations make the catalyst expensive, limiting its industrial application prospects.
[0008] Therefore, the art seeks to develop a catalytic material that combines uniform dispersion of active metals with simple preparation process to overcome the shortcomings of the prior art. Summary of the Invention
[0009] The first objective of this invention is to provide a core-shell structured composite material Pd@CeO2@NiO, which can be used as a catalyst for methane cracking reaction; The second objective of this invention is to provide a core-shell structured catalyst, wherein the active component of the catalyst includes the core-shell structured composite material Pd@CeO2@NiO, and the catalyst exhibits high activity and high yield in methane cracking reaction, with high selectivity for carbon products and hydrogen in the products, making it suitable for industrial production; The third objective of this invention is to provide a method for preparing the above-mentioned core-shell composite material and catalyst, as well as their applications.
[0010] To solve the above-mentioned technical problems, the present invention provides a core-shell structured composite material, wherein the composite material includes a metallic active substance; The metal active material includes Pd@CeO2@NiO; The mass content of each element, based on the total amount of Pd@CeO2@NiO, is as follows: Pd element: 6.25-13.04 wt%; Ce element: 28.47-44.57 wt% Ni element: 28.65-44.28 wt% O element: Balance.
[0011] Preferably, in the Pd@CeO2@NiO, the mass ratio of Ni, Pd and Ce is Ni:Pd:Ce = 3.2-4.8:0.8-1.2:3.2-4.8, and more preferably Ni:Pd:Ce = 4:1:4.
[0012] Specifically, the core-shell structured composite material further includes fillers; wherein: The metal active ingredient is 1-5 wt% based on the loading amount of the filler. And / or, the filler includes Al2O3 or quartz sand.
[0013] This invention also discloses a method for preparing the core-shell structured composite material as described above, comprising the following steps: (1) Add a ligand and Ce source material to water and mix them together. Add a Pd source material and an initiator and mix them together. Then carry out the first reaction to obtain a Pd@Ce core-shell template. (2) The Pd@Ce core-shell template is dispersed in water, and Ni source material and precipitant are added and mixed, and a second reaction is carried out to obtain Pd@Ce@Ni precursor; (3) The Pd@Ce@Ni precursor is calcined to obtain the desired core-shell structure composite material.
[0014] Specifically, in the preparation method of the core-shell structure composite material: In step (1), the ligand comprises a soluble bromide salt, wherein Br - The coordination agent is preferably KBr or NaBr to limit the nuclear growth rate of Pd; And / or, in step (1), the Ce source material includes Ce(NO3)3; And / or, in step (1), the Pd source material includes Na2PdCl6 or Pd(NO3)2; And / or, in step (1), the initiator includes ammonia, which can trigger the reaction, causing Pd 2+ With Ce 3+ A redox reaction occurs, generating a core-shell structure in situ. And / or, in step (1), the temperature of the first reaction is 50-80°C; And / or, in step (1), the time for the first reaction is 0.5-2 hours; And / or, in step (2), the Ni source material includes a soluble Ni salt, preferably Ni(NO3)2; And / or, in step (2), the precipitant includes hexamethylenetetramine, ammonia, or NaOH, and the precipitant reacts with Ni. 2+ Coordination leads to precipitation; And / or, in step (2), the temperature of the second reaction is 60-90°C; And / or, in step (2), the second reaction takes 5-8 hours; And / or, in step (3), the atmosphere of the calcination step is an oxygen-containing atmosphere; And / or, in step (3), the temperature of the calcination step is 200-400℃; And / or, in step (3), the calcination step takes 1-3 hours.
[0015] Specifically, in the preparation method of the core-shell composite material, step (3) further includes dispersing the Pd@Ce@Ni precursor with water and continuing to add a selected amount of the filler for mixing and loading, collecting the reactants for calcination treatment, and obtaining the desired core-shell composite material.
[0016] The present invention also discloses the use of a core-shell structured composite material as described above or a core-shell structured composite material prepared by the method above for the preparation of a catalyst for methane cracking reaction.
[0017] The present invention also discloses a methane cracking reaction catalyst, wherein the active component of the catalyst includes the core-shell structured composite material or the core-shell structured composite material prepared by the method.
[0018] The present invention also discloses a method for catalytic methane cracking to co-produce hydrogen and carbon nanotubes, comprising a step of pretreating the catalyst in a hydrogen-containing atmosphere, and a step of introducing methane feedstock for high-temperature cracking reaction.
[0019] In the method for catalytic methane cracking and co-production of hydrogen and carbon nanotubes according to the present invention, during the pretreatment stage, the Pd core of the core-shell structure catalyst is activated by H2 and transformed into metallic Pd. 0 Furthermore, it continuously dissociates on its surface to generate active hydrogen species, thereby reducing most of the outer Ni species to metallic Ni. 0 At the pretreatment temperature, the outer Ni layer 0 Thermal migration occurs and the material diffuses towards the Pd core, forming a NiPd alloy core. Simultaneously, Ni dissolved in the CeO2 shell... 2+ In some species, because the pretreatment and reaction temperatures did not reach the ripening temperature of CeO2, CeO2 was coated on the core surface in the form of fine grains, forming a semi-constrained shell with a certain mechanical strength.
[0020] In the method for catalytic methane cracking and co-production of hydrogen and carbon nanotubes described in this invention, during the high-temperature cracking reaction, methane molecules first coordinate with unsaturated Ni on the surface of the CeO2 shell. 2+ Pre-dehydrogenation occurs at the site, generating ·CH3 radicals. These radicals further diffuse to the surface of the NiPd alloy core, forming C2 intermediates via CC coupling, and then gradually dehydrogenate to construct multilayer graphitic carbon layers. As the graphitic carbon layers thicken, accumulated compressive stress is generated between the layers and at the interface between the layers and the core. When the stress exceeds the bearing limit of the CeO2 shell, the carbon layers break through the CeO2 shell and push outward through a bottom growth mechanism, while new graphitic carbon layers continue to be deposited on the surface of the metal core. This cycle repeats, forming carbon nanotubes with a periodic bamboo-like structure.
[0021] Specifically, in the method for catalytic methane cracking to co-produce hydrogen and carbon nanotubes: The hydrogen-containing atmosphere includes an H2 / N2 mixed atmosphere; And / or, in the hydrogen-containing atmosphere, the volume content of hydrogen is 5-15 vol.%; And / or, the flow rate of the hydrogen-containing atmosphere is 10-30 mL / min; And / or, the temperature of the pretreatment step is 600-800℃; And / or, the pretreatment step takes 0.5-2 hours; And / or, the flow rate of the methane feedstock is 3-8 mL / min; And / or, the mass hourly space velocity of the methane feedstock is 1000-6000 mL / g·h; And / or, the temperature of the high-temperature pyrolysis reaction is 600-800℃; And / or, the method further includes the step of introducing a protective gas after the reaction is complete.
[0022] The present invention also discloses a carbon nanotube product prepared by the method.
[0023] The core-shell composite material of this invention uses a small amount of highly active noble metal Pd, constructs a multi-level core-shell structure through CeO2, and modifies the Ni-based catalyst to obtain a core-shell Pd@CeO2@NiO catalytic material. The composite material can be used as a catalyst for catalytic methane cracking processes, and can co-produce hydrogen and carbon nanotubes. It can not only convert methane into bamboo-like multi-walled carbon nanotubes, but also has the advantages of high efficiency, high activity, and high stability.
[0024] The core-shell composite material described in this invention is used as a catalyst for methane cracking under relatively mild reaction conditions (600-800℃), achieving a maximum initial methane conversion rate of over 60%, effectively increasing carbon nanotube yield, and maintaining high carbon material yield and carbon production rate. This catalyst has a simple synthesis method, low metal usage, and exhibits high activity and high yield in methane cracking, with high selectivity for carbon products and hydrogen, and produces high-quality carbon nanotubes, making it suitable for industrial production.
[0025] The core-shell composite catalyst of this invention can prefabricate the core-shell structure through aqueous phase synthesis, precisely confining the initial size of the metal core. The size of the alloy core is controllable after pretreatment. Moreover, the metal content is low, with a low content of the precious metal Pd, resulting in lower catalyst cost compared to the high content of precious metals in existing technologies. In particular, the catalyst is prepared using a simple template-free synthesis strategy, eliminating the need for expensive organic ligand reagents. The synthesis method is simple, avoiding complex operations such as multi-step demolding and supercritical drying, reducing preparation difficulty and raw material costs, improving the scalability and economy of the process, and enabling large-scale synthesis with significant cost advantages.
[0026] In the core-shell composite catalyst of this invention, the physical isolation of the CeO2 shell and the synergistic effect of the Al2O3 dispersant ensure that each catalytic core is independent, effectively inhibiting the sintering and growth of metal particles at high temperatures. Furthermore, by controlling the Pd / Ni atomic ratio, the methane cracking activity and the crystallinity of the graphite carbon layer can be systematically adjusted, achieving synergistic optimization of catalytic efficiency and product quality. The Ni anchored on the outer CeO2 layer... 2+ The site has a dual function: in the early stage of the reaction, it acts as a stable dehydrogenation active center to continuously supply CH3 radicals, promoting the orderly growth of graphite carbon layers and inhibiting the formation of amorphous carbon; after the reaction starts, it assists the alloy core in activating methane molecules and improving the overall catalytic efficiency.
[0027] In the core-shell composite catalyst of the present invention, Al2O3 and other materials are used as low-cost dispersion media, which not only effectively reduces the contact probability between the catalytic cores, but also provides physical space for the longitudinal growth of carbon nanotubes, so that the product length can reach the micrometer level.
[0028] The preparation method of the core-shell composite material catalyst of the present invention can synthesize the catalyst by low-temperature calcination, without the need for high-temperature pre-reduction and melt maintenance conditions, and without the need for high-energy-consuming modification equipment such as plasma. It significantly reduces the amount of precious metals / low-melting-point metals used, simplifies the preparation process, reduces energy consumption and equipment investment, helps to reduce production costs, and is conducive to industrial-scale production. Attached Figure Description
[0029] To make the content of this invention easier to understand, the invention will be further described in detail below with reference to specific embodiments and accompanying drawings, wherein: Figure 1 TEM image of Pd@CeO2@NiO material prepared in Example 1; Figure 2 The curve shows the change in methane conversion rate with reaction time under the Pd@CeO2@NiO catalyst system. Figure 3 TEM image of Pd@CeO2@NiO catalyst after hydrogen pretreatment; Figure 4 This is a TEM image of carbon nanotubes obtained after the methane pyrolysis reaction; Figure 5 The results are Raman spectra of carbon materials obtained after methane cracking. Detailed Implementation
[0030] In the following embodiments of the present invention, in view of the problems of high cost and poor quality of carbon products in existing methane cracking catalysts, a highly efficient, highly active and highly stable catalyst material is provided, which can convert methane into bamboo-like multi-walled carbon nanotubes and hydrogen.
[0031] In the following embodiments of the present invention, a core-shell structured composite material is provided, the composite material comprising a metallic active substance; The metal active material includes Pd@CeO2@NiO; The mass content of each element, based on the total amount of Pd@CeO2@NiO, is as follows: Pd element: 6.25-13.04 wt%; Ce element: 28.47-44.57 wt% Ni element: 28.65-44.28 wt% O element: Balance.
[0032] In some specific embodiments, the mass ratio of Ni, Pd, and Ce elements in the Pd@CeO2@NiO is Ni:Pd:Ce = 3.2-4.8:0.8-1.2:3.2-4.8.
[0033] In some specific embodiments, the composite material further includes fillers for molding the composite material, which can ensure the effective dispersion and support of the metal active material.
[0034] The present invention also discloses a method for preparing the core-shell structured composite material as described above in the following embodiments, comprising the following steps: (1) Add a ligand and Ce source material to water and mix them together. Add a Pd source material and an initiator and mix them together. Then carry out the first reaction to obtain a Pd@Ce core-shell template. (2) The Pd@Ce core-shell template is dispersed in water, and Ni source material and precipitant are added and mixed, and a second reaction is carried out to obtain Pd@Ce@Ni precursor; (3) The Pd@Ce@Ni precursor is calcined to obtain the desired core-shell structure composite material.
[0035] In some specific embodiments, step (3) further includes dispersing the Pd@Ce@Ni precursor with water and continuing to add a selected amount of the filler for mixing and loading, collecting the reactants for the calcination treatment, and obtaining the desired core-shell structure composite material.
[0036] As an example, the present invention also provides a method for preparing a core-shell structured composite material, comprising the following steps: (1) First, construct a Pd@Ce core-shell template. Add KBr and Ce(NO3)3·6H2O to deionized water and preheat to 60°C. Add Na2PdCl6 aqueous solution dropwise. Stir until the noble metal is fully coordinated. Then add ammonia water dropwise. After the reaction is complete, centrifuge to remove the residual unreacted raw materials. (2) Then redisperse in deionized water, add Ni(NO3)2·6H2O and hexamethylenetetramine, heat to 80°C to react fully and then centrifuge; (3) After the product is fully mixed with Al2O3 nanoparticles, the catalyst is diluted and then calcined in a muffle furnace at 300°C to obtain Pd@CeO2@NiO catalyst material.
[0037] In the following embodiments of the present invention, a method for catalytic methane cracking to co-produce hydrogen and carbon nanotubes is also provided, comprising a step of pretreating the catalyst in a hydrogen-containing atmosphere, and a step of introducing methane feedstock for a high-temperature cracking reaction.
[0038] As an example, the present invention also provides a method for catalytic methane cracking to co-produce hydrogen and carbon nanotubes, comprising: taking the catalytic material, placing it in a quartz tube, using a fixed-bed reactor, pretreating it with 10 vol.% hydrogen at 600-800°C, purging residual gas with an inert gas, then introducing pure methane at 600-800°C and a mass hourly space velocity (WHSV) of 1000-6000 mL·g. -1 ·h -1 Under the given conditions, the proportions of each component in the product were determined using an online gas chromatograph. After the reaction was complete, the carbon material was removed and weighed to determine the amount of carbon material produced.
[0039] In the following embodiments of the present invention, the gaseous byproducts of the methane cracking reaction are mainly oligomeric alkane-olefins and aromatic substances, and do not contain CO. x .
[0040] Example 1 In this embodiment, the metal active material of the composite material is Pd@CeO2@NiO; wherein, in the metal active material, the loading of Pd element is 9.08wt%, the loading of Ce element is 36.34wt%, the loading of Ni element is 36.34wt%, and the balance is O element.
[0041] In this embodiment, Na2PdCl4, Ce(NO3)3·6H2O and Ni(NO3)2·6H2O are used as metal salt precursors, and Al2O3 is used as a dispersant and structural support agent.
[0042] 294.22 mg of Na₂PdCl₄ solid powder was weighed and diluted with its deionized water to 10 mL to obtain a 0.1 M Na₂PdCl₄ aqueous solution. 100 mg of Ni(NO₃)₂·6H₂O solid powder was weighed and diluted with its deionized water to 10 mL to obtain a 10 mg / mL solution. -1 A Ni(NO3)2 aqueous solution. Measure 50 μL of saturated ammonia solution and dilute it to 20 mL of deionized water to obtain an ammonia solution with a concentration of 0.05 M.
[0043] Measure 20 mL of deionized water, add 300 mg KBr as a ligand to adjust the final Pd core size, and 86 mg Ce(NO3)3·6H2O. Heat to 60 °C and stir thoroughly for 2 h. Then, add dropwise 0.5 mL of the previously prepared Na2PdCl4 aqueous solution and stir thoroughly for 30 min. Subsequently, add dropwise 5 mL of the previously prepared ammonia solution and react for 1 h. After the reaction is complete, centrifuge to obtain a black solid, denoted as Pd@Ce.
[0044] The black solid powder obtained above was dispersed in 20 mL of deionized water. 5.8 mL of the previously prepared Ni(NO3)2·6H2O solution and 0.56 g of HMT were added to it. After stirring for 30 min, the mixture was reacted in an oil bath at 80 °C for 6 h. Subsequently, the black solid powder was obtained by centrifugation and denoted as Pd@Ce@Ni; where Ni:Pd:Ce = 4:1:4.
[0045] The Pd@Ce@Ni solid powder was dispersed in 80 mL of deionized water, and 1000 mg of Al2O3 nanoparticles were added to make the total metal loading 2.5 wt.%. After stirring thoroughly at room temperature, the mixture was filtered, and excess water was removed by rinsing with ethanol. The mixture was then dried overnight in an oven at 80°C, thoroughly ground, and calcined in a muffle furnace at 300°C for 2 hours under an air atmosphere to obtain a composite material with Pd@CeO2@NiO as the metal active material.
[0046] In this embodiment, the TEM image of the prepared Pd@CeO2@NiO composite material is attached. Figure 1 As shown, the core-shell structure has an average size of 28.9 nm, with Pd species located at the center of the material and an average size of 8.9 nm. The shell is formed by the accumulation of fine cerium oxide particles, and Ni species are widely distributed in the shell region.
[0047] In this embodiment, the catalyst material was placed in a quartz tube and pretreated with 10 vol.% hydrogen at 600-800°C using a fixed-bed reactor. After purging the residual gas with an inert gas, pure methane was introduced and the reactor was operated at 600-800°C with a mass hourly space velocity (WHSV) of 1000-6000 mL·g. -1 ·h -1 Under the specified conditions, the proportions of each component in the product were determined using an online gas chromatograph. The methane conversion rate versus time curves of the Pd@CeO2@NiO catalyst at different reaction temperatures are shown below. Figure 2 As shown.
[0048] Example 2 In this embodiment, the raw material composition and preparation method of the composite material are the same as in Example 1. The only difference is that the amount of Al2O3 added is adjusted to 500mg, and the other parameters and operation steps are the same as in Example 1.
[0049] Example 3 In this embodiment, the raw material composition and preparation method of the composite material are the same as in Example 1, except that the loading of Pd element in the metal active material is adjusted to 13.04 wt%, the loading of Ce element to 28.47 wt%, the loading of Ni element to 44.28 wt%, and the balance is O element. In the preparation method of the composite material, appropriate amounts of raw materials are selected for reaction according to the content ratio of each element.
[0050] Example 4 In this embodiment, the raw material composition and preparation method of the composite material are the same as in Example 1, except that the loading of Pd element in the metal active material is adjusted to 6.25 wt%, the loading of Ce element to 44.57 wt%, the loading of Ni element to 28.65 wt%, and the balance to O element. In the preparation method of the composite material, appropriate amounts of raw materials are selected for reaction according to the content ratio of each element.
[0051] Comparative Example 1 The raw material composition and preparation method of the composite material described in this comparative example are the same as those in Example 1. The only difference is that the Pd element is not added. The composite material with CeO2@NiO structure is synthesized according to the same metal ratio. Commercial CeO2 particles are used, dispersed in deionized water, and Ni(NO3)2 solution is added. HMT is used as a precipitant for coating.
[0052] Comparative Example 2 The raw material composition and preparation method of the composite material described in this comparative example are the same as those in Example 1. The only difference is that the Ni element is not added, and the composite material with Pd@CeO2 structure is synthesized according to the same metal ratio.
[0053] Comparative Example 3 The raw material composition and preparation method of the composite material described in this comparative example are the same as those in Example 1. The only difference is that PdNi / CeO2 is synthesized by co-impregnation method, that is, metal element particles are directly loaded with commercial carrier CeO2 while keeping the mass ratio of each metal element unchanged.
[0054] Comparative Example 4 The raw material composition of the composite material described in this comparative example is the same as that in Example 1. The only difference is that the composite material is synthesized by co-impregnation method, which is based on the alumina carrier to support Pd, Ce and Ni elements. The mass ratio of each element is the same as that of the material in Example 1, and is denoted as NiPdCe / Al2O3.
[0055] Comparative Example 5 The raw material composition of the composite material described in this comparative example is the same as that in Example 1. The only difference is that the composite material directly based on the alumina carrier loaded with Ni element is synthesized by the co-impregnation method, which is denoted as Ni / Al2O3.
[0056] Comparative Example 6 The raw material composition of the composite material described in this comparative example is the same as that in Example 1. The only difference is that the composite material based on Ni and Pd elements loaded on an alumina carrier is directly synthesized by co-impregnation method, and has the same metal ratio as in Example 1, denoted as NiPd / Al2O3.
[0057] Comparative Example 7 The raw material composition of the composite material described in this comparative example is the same as that in Example 1. The only difference is that the composite material based on Pd element loaded on an alumina carrier is directly synthesized by co-impregnation method and has the same metal ratio as in Example 1, denoted as Pd / Al2O3.
[0058] Comparative Example 8 In this comparative example, the raw material composition and preparation method of the composite material are the same as in Example 1, except that the mass ratio of each element in the metal active material is adjusted to Ni:Pd:Ce = 0.5:4.5:4, that is, the loading of Pd element in the metal active material is 4.49wt%, the loading of Ce element is 35.89wt%, the loading of Ni element is 40.38wt%, and the balance is O element. In the preparation method of the composite material, an appropriate amount of raw materials is selected for reaction according to the content ratio of each element.
[0059] Comparative Example 9 In this comparative example, the raw material composition and preparation method of the composite material are the same as in Example 1, except that the mass ratio of each element in the metal active material is adjusted to Ni:Pd:Ce = 4.5:0.5:4, that is, the loading of Pd element in the metal active material is 44.75wt%, the loading of Ce element is 39.78wt%, the loading of Ni element is 4.97wt%, and the balance is O element. In the preparation method of the composite material, an appropriate amount of raw materials is selected for reaction according to the content ratio of each element.
[0060] In the following application examples of this invention, catalytic methane cracking is carried out based on the aforementioned examples and comparative catalysts. The effects of each catalyst product are observed, and the evaluation indicators include: (1) Initial methane conversion rate (i.e., initial activity): evaluate the methane conversion rate in the initial stage of the reaction. The higher the initial methane conversion rate, the better. (2) Reaction duration (i.e. stability): the time it takes for the conversion rate to drop below 10% or be forced to stop. It is used to evaluate the stability of the catalyst, and the longer it can last, the better. (3) Carbon nanotube yield: The mass of carbon material collected after the reaction is used to evaluate the specificity of the catalyst. The higher the carbon nanotube yield, the better. (4) Carbon material yield (i.e. carbon balance): Calculation formula: actual carbon production / theoretical carbon accumulation × 100%. Theoretically, the closer this yield value is to 100%, the better. (5) ID / IG ratio (i.e., the degree of graphitization of carbon materials): characterizes the intensity ratio of the D peak to the G peak in the Raman spectrum. The lower the value, the better. (6) Carbon yield (g) Carbon / g Metal ): This represents the carbon yield per unit of metal, and theoretically, the higher the value, the better; (7) Product morphology: The preparation of carbon nanotubes requires multi-walled carbon nanotubes or amorphous carbon.
[0061] Application Example 1 The composite material prepared in Example 1 was thoroughly ground, and 100 mg of the catalyst particles were weighed and placed in a fixed-bed reactor. The mixture was then heated in 20 mL of water for 1 minute. -1 Under the condition of using N2 as an inert protective gas, the temperature is raised to the pretreatment temperature of 700℃, and a certain flow rate of 20 mL / min is introduced. -1 The catalyst was subjected to a pretreatment gas of H2 / N2 (volume fraction 1 / 9) for 1 hour, followed by a 20 mL / min solution. -1 The catalyst was purged with N2 for 30 minutes to remove adsorbed H2 and avoid testing errors. In this application example, the TEM image of the Pd@CeO2@NiO catalyst after hydrogen pretreatment is attached. Figure 3 As shown, the core-shell structure has an average size of 30.4 nm, with Pd species located at the center of the material and an average size of 10.4 nm. The cerium oxide particles in the shell are coarsened, and the shell and core are no longer tightly bonded, resulting in gaps. A large number of Ni species migrate to the core, forming NiPd cores, while some remain in CeO2.
[0062] Adjust the reactor to the methane cracking reaction temperature of 700℃ and introduce 5 mL of gas. -1 Pure methane gas results in a WHSV of 3000 mL·g. -1 ·h -1 The reaction was carried out continuously at 700℃ and atmospheric pressure. During the reaction, the reaction products were analyzed online at atmospheric pressure after passing through a cold trap using a gas chromatograph equipped with a TCD, with an X13 packed column. The initial methane conversion rate was 61.8%, and after 270 min of continuous reaction, the methane conversion rate remained above 10%, before the reaction was terminated when it dropped below 10%.
[0063] After the reaction was complete, 20 mL of the solution was bubbled through. -1An inert gas, N2, was used as a protective gas to cool the mixture to room temperature, preventing the highly reactive carbon nanotubes from spontaneously combusting upon contact with air. The solid residue after the reaction was then collected and weighed. Subtracting the 100 mg of added catalyst, the total amount of carbon nanotube material produced was determined to be 234 mg. The carbon yield was calculated as 234 mg / 2.5 mg (i.e., the total mass of Pd + Ni metal) = 93.6.
[0064] Based on the methane conversion curve of the catalyst obtained in Example 1, the theoretical amount of carbon deposited from methane was calculated by integration. Compared with the actual value, the carbon material yield was found to be 96.88%, and the byproducts were oligomeric alkane-olefins and aromatic substances.
[0065] In this application example, the obtained carbon material was characterized by TEM, and the results are shown in the appendix. Figure 4 As shown, the carbon nanotubes exhibit a periodic bamboo-like segmented structure, consistent with the aforementioned stress-driven periodic growth mechanism, with an average diameter of 12 nm.
[0066] Further Raman spectroscopy analysis was performed on the obtained carbon nanotube products, and the results are shown in the attached figure. Figure 5 As shown. It can be seen that at approximately 1580cm... -1 The presence of a strong G peak at this point corresponds to the E2g vibrational mode of the graphite structure, indicating that the product exhibits typical sp... 2 Hybrid carbon skeleton; at approximately 1350 cm -1 The appearance of peak D at approximately 2677 cm⁻¹, with an intensity ratio (ID / IG) of 0.93 compared to peak G, indicates the presence of a certain amount of structural defects in the product. Notably, at approximately 2677 cm⁻¹... -1 A significant 2D peak appears at approximately 2910 cm⁻¹, and the prominent presence of this second-order scattering characteristic peak directly indicates that the carbon layer of the product has a highly ordered graphitized structure; simultaneously, at approximately 2910 cm⁻¹... - The extremely weak D+G combined mode signal associated with the defect at point ¹ further confirms that the product has a low structural defect density.
[0067] In summary, the carbon nanotubes prepared in this embodiment have a crystal structure characterized by an ordered graphite structure and a low defect density, resulting in high product quality.
[0068] Application Example 2 In this application example, the method for catalytic methane cracking is the same as in Application Example 1, except that the pretreatment temperature of the catalyst is adjusted to 600°C, and the reaction is terminated after the methane conversion rate drops below 10% after 220 min of continuous reaction.
[0069] The initial methane conversion rate of the method in this application example was 58.9%, the carbon nanotube yield was 218 mg, the calculated carbon material yield was 96.51%, the carbon yield was 218 mg / 2.5 mg = 87.2, and the ID / IG ratio was 1.01.
[0070] Application Example 3 In this application example, the method for catalytic methane cracking is the same as in application example 1, except that the pretreatment temperature of the catalyst is adjusted to 800°C, and the reaction is terminated after the methane conversion rate drops below 10% after 190 min of continuous reaction.
[0071] The initial methane conversion rate of the method in this application example was 58.4%, the carbon nanotube yield was 188 mg, the carbon material yield was calculated to be 97.12%, the carbon yield = 188 mg / 2.5 mg = 75.2, and the ID / IG = 1.03.
[0072] Application Example 4 In this application example, the method for catalytic methane cracking is the same as in application example 1, except that the temperature of the high-temperature cracking reaction is adjusted to 600°C. After continuous reaction for 520 minutes, the test was stopped because a large amount of carbon material deposited completely blocked the gas passage and the pressure drop of the reactor exceeded 0.25 MPa.
[0073] The initial methane conversion rate of the method in this application example was 39.4%, the carbon nanotube yield was 316 mg, the carbon material yield was calculated to be 64.32%, the carbon yield was 316 mg / 2.5 mg = 126.4, and the ID / IG ratio was 1.19.
[0074] Application Example 5 In this application example, the method for catalytic methane cracking is the same as in application example 1, except that the temperature of the high-temperature cracking reaction is adjusted to 650°C, and the reaction is terminated after the methane conversion rate drops below 10% after 540 min of continuous reaction.
[0075] The initial methane conversion rate of the method in this application example was 51.3%, the carbon nanotube yield was 634 mg, the carbon material yield was 96.88%, the carbon yield was 634 mg / 2.5 mg = 253.6, and the ID / IG ratio was 0.94.
[0076] Application Example 6 In this application example, the method for catalytic methane cracking is the same as in application example 1, except that the temperature of the high-temperature cracking reaction is adjusted to 750°C, and the reaction is terminated after the methane conversion rate drops below 10% after 70 minutes of continuous reaction.
[0077] The test results showed that the initial methane conversion rate of the method in this application example was 51.9%, the carbon nanotube yield was 44 mg, the carbon material yield was 99.17%, the carbon yield was 44 mg / 2.5 mg = 17.6, and the ID / IG ratio was 0.89.
[0078] Application Example 7 In this application example, the method for catalytic methane cracking is the same as in application example 1, except that the temperature of the high-temperature cracking reaction is adjusted to 800°C, and the reaction is terminated after the methane conversion rate drops below 10% after 20 minutes of continuous reaction.
[0079] The test results showed that the initial methane conversion rate of the method in this application example was 39.5%, the carbon nanotube yield was 8 mg, the carbon material yield was 91.35%, the carbon yield was 8 mg / 2.5 mg = 3.2, and the ID / IG ratio was 1.31.
[0080] Application Example 8 In this application example, the method for catalytic methane cracking reaction is the same as in application example 1, except that the catalyst prepared in example 2 is used for the reaction, and the reaction is terminated after the methane conversion rate drops below 10% after 210 min of continuous reaction.
[0081] The initial methane conversion rate of the method in this application example was 68.3%, the carbon nanotube yield was 312 mg, the carbon material yield was 93.2%, the carbon yield was 312 mg / 5 mg = 62.4, and the ID / IG ratio was 0.94.
[0082] Comparative Application Example 1 In this comparative application example, the method for catalytic methane cracking reaction is the same as in application example 1, except that the catalyst prepared in comparative example 1 is used for the reaction, and the reaction is terminated when the methane conversion rate drops below 10%.
[0083] Testing showed that, based on CeO2@NiO as a catalyst, no catalytic activity was detected in the entire catalytic process of this application example method.
[0084] Comparative Application Example 2 In this comparative application example, the method for catalytic methane cracking reaction is the same as in application example 1, except that the catalyst prepared in comparative example 2 is used for the reaction, and the reaction is terminated when the methane conversion rate drops below 10% after the Pd@CeO2 sample reacts continuously for 30 min.
[0085] The initial methane conversion rate of the method in this application example was 28.82%, the multi-walled carbon nanotube yield was 20 mg, the carbon material yield was 94.6%, the carbon yield was 20 mg / 0.5 mg (i.e., the total mass of Pd metal) = 40, and the ID / IG ratio was 1.37.
[0086] Comparative Application Example 3 In this comparative application example, the method for catalytic methane cracking is the same as in application example 1, except that the catalyst prepared in comparative example 3 is used for the reaction.
[0087] The initial methane conversion rate of the method in this application example was 29.33%, but it was immediately deactivated within 5 minutes of the reaction, and no effective carbon material was obtained.
[0088] Comparative Application Example 4 In this comparative application example, the method for catalytic methane cracking is the same as in application example 1, except that the catalyst prepared in comparative example 4 is used for the reaction, and the reaction is terminated after the methane conversion rate drops below 10% after 10 min of continuous catalytic reaction of NiPdCe / Al2O3.
[0089] The initial methane conversion rate of this application example method was tested to be 55.12%, the carbon material yield was 5 mg, the carbon material recovery rate was 92.1%, the carbon yield was calculated as 5 mg / 2.5 mg (i.e., the total mass of Pd + Ni metal) = 2, and the ID / IG ratio was 1.53. The obtained carbon materials were identified as including multi-walled carbon nanotubes and amorphous carbon materials.
[0090] Comparative Application Example 5 In this comparative application example, the method for catalytic methane cracking is the same as in application example 1, except that the catalyst Ni / Al2O3 prepared in comparative example 5 is used for the reaction.
[0091] The initial methane conversion rate of the method in this application example was 22.32%, but it was immediately deactivated within 5 minutes, and no effective carbon material was obtained.
[0092] Comparative Application Example 6 In this comparative application example, the method for catalytic methane cracking is the same as in application example 1, except that the catalyst prepared in comparative example 6 is used for the reaction, and the reaction is terminated after the methane conversion rate drops below 10% after 15 min of continuous catalytic reaction with NiPd / Al2O3.
[0093] The test results showed that the initial methane conversion rate of the method in this application example was 44.51%, the multi-walled carbon nanotube yield was 9 mg, the carbon material yield was 96.2%, the carbon yield was 9 mg / 2.5 mg (i.e., the total mass of Pd+NI metal) = 3.6, and the ID / IG ratio was 1.12.
[0094] Comparative Application Example 7 In this comparative application example, the method for catalytic methane cracking is the same as in application example 1, except that the catalyst prepared in comparative example 7 is used for the reaction, and the reaction is terminated after the methane conversion rate drops below 10% after continuous catalytic reaction of Pd / Al2O3 for 35 min.
[0095] The initial methane conversion rate of the method in this application example was 33.96%, the multi-walled carbon nanotube yield was 40 mg, the carbon material yield was 90.9%, the carbon yield was 40 mg / 0.5 mg (i.e., the total mass of Pd metal) = 80, and the ID / IG ratio was 1.33.
[0096] Comparative Application Example 8 In this application example, the method for catalytic methane cracking is the same as in application example 1, except that the catalyst prepared in comparative example 8 is used for the reaction, and the reaction is terminated when the methane conversion rate drops below 10% after 30 minutes of continuous reaction.
[0097] The test results showed that the initial methane conversion rate of the method in this application example was 70.1%, the carbon nanotube yield was 12 mg, the carbon material yield was 98.32%, the carbon yield = 12 mg / 2.5 mg (i.e., the total mass of Pd + Ni metal) = 4.8, and the ID / IG = 2.15. It is evident that the catalyst deactivates too quickly, the carbon nanotube yield is low, and the carbon nanotubes have many defects and a low degree of graphitization.
[0098] Comparative Application Example 9 In this application example, the method for catalytic methane cracking is the same as in application example 1, except that the catalyst prepared in comparative example 9 is used for the reaction, and the reaction is terminated when the methane conversion rate drops below 10% after 110 min of continuous reaction.
[0099] The test results showed that the initial methane conversion rate of the method in this application example was 53.2%, the carbon nanotube yield was 64 mg, the carbon material yield was 97.21%, the carbon yield = 64 mg / 2.5 mg (i.e., the total mass of Pd + Ni metal) = 25.6, and the ID / IG = 0.98. It is evident that the catalyst deactivates too quickly, resulting in low carbon nanotube yield.
[0100] It is evident that the catalyst described in this invention can effectively catalyze the cracking of methane to produce hydrogen and carbon nanotubes. The catalyst not only has high catalytic activity but also a long catalytic time, resulting in a high yield of carbon nanotubes.
[0101] As can be seen from the application examples above, in the process of catalytic methane cracking for co-production of hydrogen and carbon nanotubes, the pretreatment temperature of the catalyst described in this invention affects the overall process performance. Pretreatment at 600-800℃ yields better results, with 700℃ showing the best activation effect. If the pretreatment temperature is too low, Ni reduction will be insufficient and NiPd alloying will be incomplete; if the temperature is too high, it may cause partial ripening of the CeO2 shell or growth of metal particles, leading to a reduction in active sites and a decrease in carbon nanotube quality.
[0102] As can be seen from the application examples above, in the process of catalytic methane cracking for co-production of hydrogen and carbon nanotubes, the temperature of the high-temperature cracking reaction of the catalyst described in this invention has a certain impact on the overall process effect, with 650-700℃ being the optimal reaction window. At low temperatures, methane cracking produces more byproducts, leading to a decrease in carbon yield; at high temperatures, the carbon deposition rate is too fast, causing rapid catalyst deactivation, and higher reaction temperatures exacerbate the partial ripening of the CeO2 shell or the growth of metal particles.
[0103] As can be seen from the data in the above application examples, the ratio of metal elements in the catalyst, i.e., the Ni / Pd / Ce ratio, has a certain impact on the performance of the catalyst. If there is too much Pd, methane activation will be too fast, carbon deposits will quickly cover the active sites, and the graphitization degree of carbon nanotubes will be poor; if there is too much Ni, the NiPd alloying degree will be low, which will lead to increased carbon resistance, making the carbon nanotube growth process difficult, and both activity and stability will decrease.
[0104] The data from the above application examples show that the amount of filler added to the catalyst product also has a certain impact on the catalyst performance. Taking the amount of Al2O3 added as an example, an appropriate amount of Al2O3 helps to improve carbon yield and stability; while reducing Al2O3 slightly increases activity and carbon production, but decreases carbon yield, indicating that insufficient dispersant leads to the deactivation of some sites, and the long-term stability decreases slightly.
[0105] As can be seen from the application examples above, the catalyst of this invention, employing a core-shell structure and a superior elemental combination, can effectively catalyze the cracking of methane to produce hydrogen and carbon nanotubes. The core-shell structure (Pd@CeO2@NiO) of the catalyst is an indispensable feature. Compared with the comparative application examples, the lack of Pd, the absence of Ni, or the use of a co-impregnation method all result in low activity, short lifespan, and poor carbon nanotube quality. The CeO2 shell provides physical confinement, and Ni... 2+ Anchoring and stress accumulation functions; Pd core promotes H2 dissociation and NiPd alloying; Ni provides active sites for carbon nanotube growth.
[0106] In summary, the core-shell composite material Pd@CeO2@NiO described in this invention can be used as a catalyst in the catalytic methane cracking process, and can co-produce hydrogen and carbon nanotubes. It can not only convert methane into bamboo-like multi-walled carbon nanotubes, but also has the advantages of high efficiency, high activity and high stability.
[0107] The embodiments of the present invention have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only for the purpose of helping to understand the method and core ideas of the present invention. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of the present invention. Therefore, the content of this specification should not be construed as a limitation of the present invention.
Claims
1. A core-shell structured composite material, characterized in that, The composite material includes metallic active substances; The metal active material includes Pd@CeO2@NiO; The mass content of each element, based on the total amount of Pd@CeO2@NiO, is as follows: Pd element: 6.25-13.04 wt%; Ce element: 28.47-44.57 wt% Ni element: 28.65-44.28 wt% O element: Balance.
2. The core-shell composite material according to claim 1, characterized in that, The composite material further includes fillers; wherein: The metal active ingredient is 1-5 wt% based on the loading amount of the filler. And / or, the filler comprises Al2O3 or quartz sand.
3. A method for preparing a core-shell structured composite material as described in claim 1 or 2, characterized in that, Includes the following steps: (1) Add a ligand and Ce source material to water and mix them together. Add a Pd source material and an initiator and mix them together. Then carry out the first reaction to obtain a Pd@Ce core-shell template. (2) The Pd@Ce core-shell template is dispersed in water, and Ni source material and precipitant are added and mixed, and a second reaction is carried out to obtain Pd@Ce@Ni precursor; (3) The Pd@Ce@Ni precursor is calcined to obtain the desired core-shell structure composite material.
4. The method for preparing the core-shell composite material according to claim 3, characterized in that: In step (1), the ligand comprises a soluble bromide salt; And / or, in step (1), the Ce source material includes Ce(NO3)3; And / or, in step (1), the Pd source material includes Na2PdCl6 or Pd(NO3)2; And / or, in step (1), the initiator includes ammonia, NaOH, or hexamethylenetetramine; And / or, in step (1), the temperature of the first reaction is 50-80°C; And / or, in step (1), the time for the first reaction is 0.5-2 hours; And / or, in step (2), the Ni source material includes a soluble Ni salt; And / or, in step (2), the precipitant includes hexamethylenetetramine, ammonia, or NaOH; And / or, in step (2), the temperature of the second reaction is 60-90°C; And / or, in step (2), the second reaction takes 5-8 hours; And / or, in step (3), the atmosphere of the calcination step is an oxygen-containing atmosphere; And / or, in step (3), the temperature of the calcination step is 200-400℃; And / or, in step (3), the calcination step takes 1-3 hours.
5. The method for preparing the core-shell composite material according to claim 3 or 4, characterized in that, Step (3) further includes dispersing the Pd@Ce@Ni precursor with water and continuing to add a selected amount of the filler for mixing and loading, collecting the reactants for calcination treatment, and obtaining the desired core-shell structure composite material.
6. Use of a core-shell structured composite material as described in claim 1 or 2, or a core-shell structured composite material prepared by the method of any one of claims 3-5, for the preparation of a methane cracking reaction catalyst.
7. A catalyst for methane cracking reaction, characterized in that, The active component of the catalyst includes the core-shell composite material of claim 1 or 2, or the core-shell composite material prepared by the method of any one of claims 3-5.
8. A method for catalytic methane cracking to co-produce hydrogen and carbon nanotubes, characterized in that, The method includes the step of pretreating the catalyst of claim 7 in a hydrogen-containing atmosphere, and the step of introducing methane feedstock for a high-temperature cracking reaction.
9. The method for catalytic methane cracking and co-production of hydrogen and carbon nanotubes according to claim 8, characterized in that: The hydrogen-containing atmosphere includes an H2 / N2 mixed atmosphere; And / or, in the hydrogen-containing atmosphere, the volume content of hydrogen is 5-15 vol.%; And / or, the flow rate of the hydrogen-containing atmosphere is 10-30 mL / min; And / or, the temperature of the pretreatment step is 600-800℃; And / or, the pretreatment step takes 0.5-2 hours; And / or, the flow rate of the methane feedstock is 3-8 mL / min; And / or, the mass hourly space velocity of the methane feedstock is 1000-6000 mL / g·h; And / or, the temperature of the high-temperature pyrolysis reaction is 600-800℃; And / or, the method further includes the step of introducing a protective gas after the reaction is complete.
10. A carbon nanotube product prepared by the method of claim 8 or 9, characterized in that, The carbon nanotubes include bamboo-like multi-walled carbon nanotubes.
Citation Information
Patent Citations
Nickel-based single-walled carbon nanotube catalyst based on hierarchical porous channel loading and preparation method of nickel-based single-walled carbon nanotube catalyst
CN122424827A
Preparation method and application of hydrocarbon cracking hydrogen production melting catalyst
CN122424828A
PM-FeAlO3 catalyst as well as preparation method and application thereof
CN122499788A