Application of nitrogen-doped copper indium sulfide xN-CuIn5S8 photothermal catalyst
By adjusting the ratio of urea and sulfur source, a nitrogen-doped copper indium sulfide (NiCuIn₅S₈) photothermal catalyst was prepared, and charge-enriched Cu-In bimetallic sites were constructed. This solved the problem of reducing CO₂ to ethanol under photothermal conditions, achieving efficient selective reduction and high activity.
Patent Information
- Application Number
- CN202611362039.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-03
- Publication Date
- 2026-11-20
AI Technical Summary
Existing photocatalysts are difficult to efficiently and selectively reduce carbon dioxide to ethanol under photothermal conditions, and traditional thermocatalysis has problems with hydrogen storage and cost.
By adjusting the ratio of urea and sulfur source, a nitrogen-doped copper indium sulfide (CuIn₅S₈) photothermal catalyst was prepared, a charge-enriched Cu-In bimetallic site was constructed, the metal microenvironment on the catalyst surface was optimized, and the coupling of CO₂ reduction and H₂O oxidation was achieved, thereby improving the adsorption capacity of CO₂.
The selective reduction of CO₂ to ethanol was achieved under photothermal conditions, which improved the activity and selectivity of the catalyst, and the ethanol yield reached 110 μmol·g⁻¹·h⁻¹.
Smart Images

Figure CN123128016A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of nitrogen-doped copper indium sulfide x N-CuIn5S8 photothermal catalytic CO2 reduction to ethanol technology, specifically involving the application of a nitrogen-doped copper indium sulfide x N-CuIn5S8 photothermal catalyst. Background Technology
[0002] The photocatalytic conversion of CO2 into valuable hydrocarbons represents a shift from solar energy to chemical energy, a win-win strategy that addresses both energy shortages and global carbon balance. However, due to the highly stable structure of CO2 and the involvement of multiple proton-coupled electron transfers, efficient photocatalytic reduction of CO2 into high-value hydrocarbons is extremely challenging from a chemical thermodynamics and kinetics perspective. Traditional thermocatalysis utilizes high-temperature thermal energy to activate CO2 molecules, promoting their reaction with H2. However, hydrogen is a light gas, difficult to compress and store, presenting technical challenges and high costs. Current research focuses on photothermal synergistic catalytic systems, leveraging light energy to excite carriers and thermal energy to accelerate surface reaction kinetics, achieving photothermal coupling to improve CO2 conversion efficiency and product selectivity. H2O, as a viable hydrogen source and electron donor in the CO2 reduction reaction, can decompose to generate O2 and H2 under the influence of photogenerated carriers. Therefore, photocatalysts need to achieve efficient separation of photogenerated electrons and holes and precise control of reaction sites to optimize the driving force of CO2 reduction rather than the hydrogen evolution side reaction. By combining the water splitting process, a hydrogen energy and water resource recycling pathway can be constructed. Photocatalytic and photothermal CO2 reduction technologies using water as a proton source provide an important approach to simultaneously addressing environmental issues and developing renewable energy. In response to society's continuous demand for carbon-based raw materials, the resource utilization of CO2 based on the carbon cycle is expected to become a core technology system with important strategic value that complements the hydrogen economy, providing key support for achieving carbon neutrality and sustainable energy supply.
[0003] Metal sulfides have become a highly regarded research system in the field of catalysis due to their advantages such as tunable structure and wide light absorption range. Compared with metal oxides, the valence band of metal sulfides is mostly composed of s 3p orbitals, which have a more negative potential, facilitating the formation of a narrower band gap for effective capture of visible light. More importantly, the conduction band bottom of these materials is mainly dominated by unoccupied metal d orbitals, providing sufficient reduction negative potential at the conduction band position, offering a good thermodynamic basis for the conversion of CO2 into high-value-added carbon-based products. Compared with conventional single-site catalysts, bimetallic or multimetallic catalytic centers exhibit particularly high catalytic activity. Traditional single-metallic site photocatalysts have weak CO2 adsorption, and the bonds between the metal and C and O atoms are easily broken, readily generating CO and hydrocarbons upon protonation; while bimetallic centers can stably adsorb CO2 through a bridging configuration, forming MCOM intermediates, raising the energy barrier for CO formation, making continuous protonation easier, and ultimately generating hydrocarbon products such as CH4 with high selectivity. Among them, bimetallic sulfides CuIn x S y The base materials exhibit excellent application potential. Combining their structural characteristics and physicochemical properties, research focusing on the selective regulation of carbon dioxide photothermal reduction products around bimetallic active centers holds significant research potential. For single-component copper-based catalysts, their unique electronic structure and surface properties effectively stabilize key CO intermediates, thereby promoting the protonation process of *CO dimerization or *CO-CHO coupling. Meanwhile, indium-based semiconductor materials possess excellent band structures, facilitating the efficient separation of photogenerated electron-hole pairs and significantly improving the efficiency of photothermal catalytic reactions. The combination of these two materials not only enables the effective utilization of visible light but also forms a matched band structure, providing an ideal material system for efficient photothermal CO2 reduction. To improve CuIn... x S y To enhance the stability of photocatalyst nanostructures and their performance in reducing carbon dioxide to hydrocarbons, various modification methods have been proposed, including morphology modulation, elemental doping, and heterojunction structures. For example, Wang et al. reported a pristine crystal-amorphous interface coupled with different forms of CuIn. 11 S 17 It possesses metal dual sites, further enhancing the photocatalytic activity and selectivity of CO2 to C2H4 release; Wang et al. reported on regulating Cu x In yThe band structure and defect sites of S photocatalysts are crucial for promoting the reduction of CO2 to C2H4. Since the C-C coupling process is highly sensitive to the catalyst structure, the design of photocatalysts, especially the construction of catalytic active sites, is particularly important. Precisely tuning the stability of *CO species adsorbed on product-specific active sites of photocatalysts and further protonating them via *CO dimerization or *CO-CHO coupling to form C-C intermediates with lower activation energies remains a challenge.
[0004] In recent years, constructing catalytically active centers with asymmetric structures through elemental doping (including non-metallic doping and metallic doping) has become a key method for enhancing the catalytic activity of CuIn. x S y Effective strategies for improving the catalytic performance of semiconductors include elemental doping, which can modulate the coordination environment to improve the electronic properties and surface structure of semiconductors, accelerate carrier separation, and enhance semiconductor performance. An et al. improved the local electron density and intermediate adsorption capacity by controlling the electron distribution and the distance between active centers, and utilized defect engineering to promote CC coupling, achieving efficient CO2 photocatalytic reduction to C2H4. Huang et al. constructed a Cu-In4SnS8 catalytic system with the synergistic effect of low-sulfur vacancies and Cu sites. The Cu sites effectively lower the rate-determining energy barrier between *COOH and *COH, and promote CC coupling and multi-electron transfer processes through co-adsorption and asymmetric charge distribution, thereby obtaining highly selective ethanol products. Long et al. utilized the electronegativity differences of non-metallic elements in MoS2... x Se y N z The intrinsic dipole moment and potential induced by the catalyst enhance the built-in electric field, promote carrier separation and electron accumulation around N atoms, thereby improving the adsorption of intermediates and increasing methanol production during carbon dioxide reduction. Gao et al. constructed charge-rich Cu-In bimetallic sites at the edges of CuInP2S6 nanosheets and effectively drove CC coupling through the tandem synergistic effect between the sites, achieving CO2 photocatalytic conversion with ethylene as the main product. Li et al. carefully designed a red polymer carbonitride composed of SN and Cu-N4 dual active centers. The Cu-NS structure can effectively separate photogenerated carriers, optimize CO adsorption and reduce the energy barrier for intermediate formation; at the same time, it weakens the Cu-O bond and regulates the O-Cu-C adsorption strength, making the reaction pathway biased towards ethanol rather than ethylene. This strategy provides a new idea for controlling the metal microenvironment on the catalyst surface and achieving efficient CO2 photocatalytic ethanol production. Currently, the focus is only on designing it in single-metal catalysts and applying it more in photocatalytic systems. The dynamic behavior under bimetallic and multimetallic synergistic and photothermal synergistic strategies still lacks in-depth exploration. Theoretically, controlling the oxidation state, coordination environment, and surface functional groups of Cu is crucial for achieving the reduction of CO2 to C. 2+Effective strategies for producing the product are needed. However, the adsorption strength of the key intermediate *OCHCH2OH at the Cu site affects product selectivity: the Cu-O bond is stronger than the Cu-C bond, leading to ethylene production typically outpacing ethanol production. Adjusting the chemical environment around the copper atom to weaken the Cu-O bond strength is beneficial for the selective production of ethanol. Simultaneously, the diatomic site can serve as an electron and hole trapping center, achieving efficient separation of photogenerated charges, providing a feasible approach for the efficient photocatalytic reduction of CO2 to ethanol. Developing defect semiconductors with visible light responsiveness helps improve the photoreduction activity of CO2, while designing catalysts with abundant bimetallic centers is one method to customize the selectivity of CO2 reduction products. Currently, there is still no photothermal catalyst that enables the selective reduction of CO2 to ethanol under photothermal conditions, a problem that urgently needs to be solved. Summary of the Invention
[0005] To address the shortcomings of existing technologies, this invention aims to design an xN-CuIn5S8 catalyst system by controlling the ratio of urea and sulfur source. Utilizing the electronegativity differences of non-metallic elements, the metal microenvironment on the catalyst surface is modulated, altering the electronic properties and surface structure of the semiconductor to construct charge-rich Cu-In bimetallic sites. This improves the adsorption of intermediates, enabling the coupling of CO2 reduction and H2O oxidation in a single reaction system, where H2O generates protons in situ for CO2 reduction. This invention, through catalyst design, controls the metal microenvironment on the catalyst surface, altering the surface structure and electronic properties to enhance CO2 adsorption capacity and improve the adsorption of *CO intermediates, achieving efficient photocatalytic production of ethanol from CO2.
[0006] To achieve this objective, the present invention adopts the following technical solution: In a first aspect, the present invention provides an application of a nitrogen-doped copper indium sulfide x N-CuIn5S8 photothermal catalyst, characterized in that the nitrogen-doped copper indium sulfide x N-CuIn5S8 photothermal catalyst is used for the selective reduction of carbon dioxide (CO2) to ethanol under photothermal conditions.
[0007] In some possible implementations, x in the nitrogen-doped copper indium sulfide x N-CuIn5S8 takes the value of 50, 100, 200, 300, 400 or 500, and the molar ratio of Cu, In and S is 1:5:8.
[0008] In some possible implementations, x takes the value 300.
[0009] In some possible implementations, the nitrogen-doped copper indium sulfide x N-CuIn5S8 photothermal catalyst for the selective reduction of carbon dioxide (CO2) to ethanol under photothermal conditions specifically includes the following steps: Weigh 50 mg of catalyst and measure 8 mL of ultrapure water, then add them sequentially to the reaction vessel and seal it. An unlimited number of other specific implementation methods can be obtained by preparing the catalyst and ultrapure water according to this ratio, for example: Weigh 100 mg of catalyst and measure 16 mL of ultrapure water, then add them sequentially to the reactor and seal it; or Weigh 1000 mg of catalyst and measure 160 mL of ultrapure water, add them sequentially to the reactor and seal; or Weigh 10,000 mg of catalyst and measure 1,600 mL of ultrapure water, add them sequentially to the reactor and seal it. Then, open the inlet and outlet ports simultaneously, connect a CO2 gas cylinder to the inlet port, and continuously flush the gas inside the vessel with a small amount of CO2 gas for 10-15 minutes to remove the residual air inside the vessel. Close the air outlet and adjust the pressure to 0.1 ± 0.01 MPa and maintain it for 10 ± 1 seconds; To establish adsorption equilibrium, the system was first magnetically stirred for 30 min in an environment without the xenon lamp on, and then irradiated with a 300 W xenon lamp while keeping the system temperature constant at 210 ± 2 ℃ and continuing the reaction for 4 ± 0.1 h. The specific implementation also provides gradient activity tests at various specific temperatures within the temperature range of 200-250 ℃, with the results showing that the activity is best at 210 ℃; it also provides gradient activity tests at various specific time lengths within the time range of 1-4 h of continuous reaction, with the results showing that the activity is best at 4 h.
[0010] After the reaction is complete, cool to room temperature, collect the solution in the reaction vessel, centrifuge and take the clear liquid at the top, which is a mixture of ethanol and water.
[0011] Secondly, the present invention provides a method for preparing a nitrogen-doped copper indium sulfide x N-CuIn5S8 photothermal catalyst, based on the nitrogen-doped copper indium sulfide x N-CuIn5S8 described in the first aspect, specifically including the following steps: Weigh 1 mmol of copper nitrate trihydrate (Cu(NO3)2·3H2O) and 1.2 mmol of indium chloride tetrahydrate (InCl3·4H2O) into a polytetrafluoroethylene-lined autoclave, add 35 mL of deionized water and 35 mL of ethylene glycol, and stir vigorously for 30-40 min. An unlimited number of other specific embodiments can be obtained by preparing copper nitrate trihydrate (Cu(NO3)2·3H2O), indium chloride tetrahydrate (InCl3·4H2O), deionized water, and ethylene glycol according to this ratio, for example: Weigh 5 mmol of copper nitrate trihydrate (Cu(NO3)2·3H2O) and 6 mmol of indium chloride tetrahydrate (InCl3·4H2O) into a polytetrafluoroethylene-lined autoclave, add 175 mL of deionized water and 175 mL of ethylene glycol, and stir vigorously for 30-40 min; or Weigh 10 mmol of copper nitrate trihydrate (Cu(NO3)2·3H2O) and 12 mmol of indium chloride tetrahydrate (InCl3·4H2O) into a polytetrafluoroethylene-lined autoclave, add 350 mL of deionized water and 350 mL of ethylene glycol, and stir vigorously for 30-40 min; or Weigh 100 mmol of copper nitrate trihydrate (Cu(NO3)2·3H2O) and 120 mmol of indium chloride tetrahydrate (InCl3·4H2O) into a polytetrafluoroethylene-lined autoclave, add 3500 mL of deionized water and 3500 mL of ethylene glycol, and stir vigorously for 30-40 min; or Weigh 1000 mmol of copper nitrate trihydrate (Cu(NO3)2·3H2O) and 1200 mmol of indium chloride tetrahydrate (InCl3·4H2O) into a polytetrafluoroethylene-lined autoclave, add 35000 mL of deionized water and 35000 mL of ethylene glycol, and stir vigorously for 30-40 min. Add 4 mmol of urea and thioacetamide mixture to the above transparent solution and stir for 30 min; wherein the molar ratio of urea to thioacetamide is one of 0.5, 1.0, 2.0, 3.0, 4.0 and 5.0, and the corresponding product is named xN-CuIn5S8, where X is one of 50, 100, 200, 300, 400 or 500; The turbid solution was transferred to a polytetrafluoroethylene-lined autoclave and kept at 180 ± 2 °C for 12 ± 0.3 h. After the reaction was completed, the mixture was cooled to room temperature to obtain a precipitate, which was then washed by centrifugation several times. x N-CuIn5S8 can be obtained by drying in a vacuum oven at 60 ± 2 ℃ for 12 ± 0.3 h.
[0012] This invention provides a nitrogen-doped copper indium sulfide (copper indium sulfide) xN-CuIn5S8 photothermal catalyst, its preparation method, and its applications. By controlling the ratio of urea and sulfur source, xN-CuIn5S8 catalysts with different nitrogen doping amounts are prepared using a one-pot hydrothermal method, achieving selective control of photothermal catalytic CO2 reduction products. Characterization results reveal that nitrogen atoms exist in the crystal lattice as dopants (N 1s = 400 eV), and through field effects, they regulate the electron density of the surrounding Cu-In-S (XPS shows that the binding energies of S, In, and Cu shift positively in sequence), optimizing the band structure and enhancing the adsorption of CO2 and intermediates (the CO2-TPD single peak becomes a double peak). Both XRD and HRTEM confirm that nitrogen doping induces lattice contraction, and this lattice strain and electronic regulation synergistically affect the electronic structure and geometry of the Cu-In active sites. Synchrotron radiation XANES, EXAFS, and wavelet transform analyses showed that the doped Cu remained predominantly +1 and highly dispersed, with no metallic Cu agglomeration. Subtle changes in the near-edge structure and coordination peaks indicated that N doping led to localized electronic perturbations and optimized the Cu-S coordination microenvironment. In pure water, 300N-CuIn5S8 exhibited excellent performance, achieving an ethanol yield of 110 μmol·g⁻¹. -1 ·h -1 This invention provides a new approach for controlling the defect chemistry of metal sulfides through non-metallic doping and achieving the selective reduction of CO2 to ethanol under photothermal conditions. Attached Figure Description
[0013] Figure 1 A simplified flow chart for the preparation of CuIn5S8 / x N-CuIn5S8 catalyst; Figure 2 (a) XRD pattern of the catalyst; (b) FT-IR spectrum of the catalyst; XPS of CuIn5S8 and 300N-CuIn5S8: (c) Cu 2p; (d) In 3d; (e) S 2p; (f) N 1s; (g) Cu K-edge XANES X in Cu foil, CuIn5S8, 300N-CuIn5S8, Cu2O and CuO; (h) Fourier transform extended X-ray absorption fine structure (FT-EXAFS); (i) Wavelet transform of K-edge XANES of copper in 300N-CuIn5S8. 3 Weighted EXAFS signal; Figure 3(a) SEM image of CuIn5S8; (b) HRTEM image of 300N-CuIn5S8; (c) SEM image of 300N-CuIn5S8; (d) HRTEM image of 300N-CuIn5S8; (e) TEM image of 300N-CuIn5S8; (f) EDS elemental mapping of 300N-CuIn5S8; Figure 4 (a) Catalytic activity of CuIn5S8 and xN-CuIn5S8 under light irradiation and 250 °C; (b) Catalytic activity of 300N-CuIn5S8 under light irradiation at different temperatures; (c) Catalytic activity of 300N-CuIn5S8 at different reaction times; (d) Catalytic activity of 300N-CuIn5S8 under different CO2 pressures; (e) Catalytic activity of 300N-CuIn5S8 with different catalyst masses; (f) Cyclic experiment; Figure 5 The image shows a magnified XRD pattern of the catalyst. Figure 6 The Raman spectrum of the catalyst; Figure 7 (ab) show the TGA tests of CuIn5S8 and 300N-CuIn5S8 catalysts, respectively; Figure 8 XPS total spectra of CuIn5S8 and 300N-CuIn5S8; Figure 9 (ab) are large-scale SEM and TEM images of CuIn5S8, and (cd) are large-scale SEM and TEM images of 300N-CuIn5S8. Figure 10 (a) Electron diffraction pattern of CuIn5S8, (b) Electron diffraction pattern of 300N-CuIn5S8; Figure 11 (a) Catalytic testing of x N-CuIn5S8 at 210 °C; (b) Catalytic testing of 300N-CuIn5S8 under illumination, no illumination (210 °C), and illumination (210 °C); (c) Catalytic testing of 300N-CuIn5S8 under different wavelengths. Figure 12 Thermal images of light sources of different wavelengths under unheated conditions; Figure 13 These are thermal images of light sources at different wavelengths under heating conditions. Figure 14 The XRD patterns of the catalyst after four cycles and the fresh catalyst sample are shown. Figure 15 TEMPO-e of (ab) CuIn5S8 and 300N-CuIn5S8 - Spectra; (cd) TEMPO-h of CuIn5S8 and 300N-CuIn5S8 + Spectroscopy; (e) Fluorescence spectrum; (f) Transient fluorescence spectrum; (g) Photocurrent response spectrum; (h) Electrochemical impedance spectroscopy; (i) Nitrogen adsorption-desorption isotherm of the catalyst; Figure 16 (a) UV-Vis DRS spectrum; (b) Band gap energy corresponding to UV-Vis DRS; (c) Mott-Schottky diagrams of CuIn5S8 and 300N-CuIn5S8; (d) Schematic diagram of band structure of different samples. Figure 17 (a) CO2-TPD experiments of CuIn5S8 and 300N-CuIn5S8; (b) XPS full spectrum of 300N-CuIn5S8 before and after in-situ illumination and reaction; (c) Cu 2p; (d) In 3d; (e) S 2p; (f) N 1s; Figure 18 (ab) Photothermal in-situ FT-IR spectrum of CuIn5S8; (cd) Photothermal in-situ FT-IR spectrum of 300N-CuIn5S8. Detailed Implementation
[0014] To make the objectives, technical solutions, and advantages of this invention clearer, the specific embodiments of this invention will be further described below with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are merely for the purpose of aiding understanding of this invention and do not constitute a limitation thereof.
[0015] The nitrogen-doped copper indium sulfide x N-CuIn5S8 (where x takes the value of 50, 100, 200, 300, 400 or 500) of the present invention is described as a specific embodiment of a high-efficiency photocatalyst, and a comparative example of pure CuIn5S8 as a photocatalyst is described below, specifically including the preparation method and experimental verification of the photocatalyst performance.
[0016] The specifications and manufacturers of the experimental drugs and reagents are as follows: Copper nitrate trihydrate (Cu(NO3)2·3H2O, 99% RG, Adamas), indium chloride tetrahydrate (InCI3·4H2O, 99% RG, Adamas), thioacetamide (CH3CSNH2, 99% RG, Adamas), urea (CO(NH2)2, 99% RG, Adamas), and ethylene glycol (C2H6O2, 99.5% AR, Greagent) were all used in this work. The water used was deionized water, and the above raw materials could be used directly without additional purification.
[0017] The main instrument names and manufacturers are as follows: Precision electronic balance (XPR404S / AC, METTLER TOLEDO), electrically heated drying oven (DHG-9023A, Shanghai Yiheng Scientific Instruments Co., Ltd.), xenon lamp light source (PLS-SXE300E, Beijing Bofei Technology Co., Ltd.), photothermal high-temperature and high-pressure reactor (100 mL, Xi'an Taikang Biotechnology Co., Ltd.), powder X-ray diffractometer (D8 ADVANCE, Bruker GmbH, Germany), scanning electron microscope (FEI Quanta 650, Thermo Scientific), transmission electron microscope (JEM-2100, JEOL), ultraviolet-visible spectrophotometer (Lambda 950, PerkinElmer, USA), Fourier transform infrared spectroscopy (Nicole iS50 FTIR, Thermo Scientific), specific surface area and pore size analyzer (ASAP 2460, McMurray Instruments Co., Ltd.), electron paramagnetic resonance spectrometer (A300, Bruker GmbH, Germany), electrochemical workstation (CHI660E, Shanghai Chenhua Instruments Co., Ltd.).
[0018] The characterization methods for pure CuIn5S8 and nitrogen-doped copper indium sulfide xN-CuIn5S8 (where x takes the value of 50, 100, 200, 300, 400 or 500) involved in this invention are described below: Powder X-ray diffraction (XRD) patterns were recorded on a Bruker D8 Advance X-ray diffractometer to study its crystal properties. The scanning range was 10°–80°, and the scanning rate was 10° / min. The microcrystalline structure and surface features of the samples were analyzed using scanning electron microscopy (SEM, FEI Quanta 650) and high-resolution transmission electron microscopy (HRTEM, JEM-2100). The catalyst was analyzed using UV-Vis diffuse reflectance spectroscopy with BaSO4 as a reference material using a TU-1950 visible-near-infrared spectrophotometer (TU1950, Persee). The crystal properties were further investigated using a Shimadzu AXIS SUPRA spectrophotometer. +Photoelectron spectroscopy was used to analyze the catalyst surface, detecting elemental composition and chemical state, and all binding energies were calibrated relative to the C 1s peak of 284.6 eV for amorphous carbon on the surface. The specific surface area and pore size distribution of the catalyst were measured using an automated surface area and porosity analyzer (ASAP 2460, Micromeritics, USA) based on the Brunauer-Emmet (BET) method. Photoelectrochemical tests were performed using a three-electrode electrochemical system on a CHI660E electrochemical workstation, with aqueous solutions of K3[Fe(CN)6] (0.01 M) and K4[Fe(CN)6] (0.01 M) and 0.2 M Na2SO4 as electrolytes, including characterizing the transport current response (IT), electrochemical impedance spectroscopy (EIS), and linear sweep voltammetry (LSV).
[0019] The preparation methods for synthesizing pure CuIn5S8 and nitrogen-doped copper indium sulfide x N-CuIn5S8 (where x takes the value of 50, 100, 200, 300, 400 or 500) are as follows: Figure 1 A simplified flow chart for the preparation of CuIn5S8 / x N-CuIn5S8 catalyst is shown below: (1) Preparation of CuIn5S8: It was prepared using a solvothermal method. The detailed synthesis flowchart is shown below. Figure 1 As shown. 1 mmol of copper nitrate trihydrate (Cu(NO3)2·3H2O) and 1.2 mmol of indium chloride tetrahydrate (InCl3·4H2O) were weighed into a polytetrafluoroethylene (PTFE) liner. 35 mL of deionized water and 35 mL of ethylene glycol were added, and the mixture was stirred vigorously for 30 min. Then, 4 mmol of thioacetamide was added to the clear solution, and the mixture was stirred for 30 min. The turbid solution was transferred to a PTFE-lined autoclave and kept at 180 °C for 12 h. After the reaction was complete, the mixture was cooled to room temperature to obtain the precipitate. The precipitate was washed by centrifugation several times and dried in a vacuum oven at 60 °C for 12 h to obtain the pure phase CuIn5S8.
[0020] (2) Preparation of CuIn5S8 with different N contents: For the preparation of x N-CuIn5S8, similar to the above steps, by changing the molar ratio of added urea and sulfur source (thioacetamide TAA) to 0.5, 1.0, 2.0, 3.0, 4.0 and 5.0 respectively, the resulting products are named x N-CuIn5S8 (X=50, 100, 200, 300, 400 and 500).
[0021] Photothermal catalytic CO2 reduction performance test: In a high-temperature, high-pressure, visually controlled reactor, firstly, 50 mg of catalyst was weighed and 8 mL of ultrapure water was added sequentially to the reactor using a pipette, and the reactor was sealed. Then, the inlet and outlet ports were opened simultaneously. A CO2 gas cylinder was connected to the inlet port, and a small amount of CO2 gas was continuously used to purge the gas inside the reactor for 10-15 minutes to remove residual air. The outlet port was then closed, and the pressure was adjusted to 0.1 MPa and maintained for 10 minutes. S To establish adsorption equilibrium, the system was first magnetically stirred for 30 min in an environment without the xenon lamp on, then irradiated with a 300 W xenon lamp while maintaining the system temperature at 210 °C using a temperature control program, and the reaction was continued for 4 h. After the reaction was completed, the system was cooled to room temperature, and the gaseous products were quantitatively determined using a Shimadzu GC-2014C gas chromatograph. Finally, the solution after the reaction in the reactor was collected, the supernatant was centrifuged, and quantitative analysis was performed using a gas chromatograph (FULI 9790II).
[0022] Experimental Results and Discussion: The structural and morphological characterization analysis of the catalyst is as follows: Figure 2 (a) XRD pattern of the catalyst; (b) FT-IR spectrum of the catalyst; XPS of CuIn5S8 and 300N-CuIn5S8: (c) Cu 2p; (d) In 3d; (e) S 2p; (f) N 1s; (g) Cu K-edge XANES X in Cu foil, CuIn5S8, 300N-CuIn5S8, Cu2O and CuO; (h) Fourier transform extended X-ray absorption fine structure (FT-EXAFS); (i) Wavelet transform of K-edge XANES of copper in 300N-CuIn5S8. 3 Weighted EXAFS signal.
[0023] To obtain a more accurate phase composition, the catalyst was characterized using X-ray diffraction. The X-ray diffraction patterns of CuIn5S8 and xN-CuIn5S8 samples are shown below. Figure 2 As shown in Figure a, the diffraction peaks at 14.3°, 27.7°, 33.5°, 44.0°, and 48.1° belong to the (111), (311), (400), (511), and (440) crystal planes of the CuIn5S8 phase (PFD#72-0956), respectively. After adjusting the molar ratio of urea and sulfur source, as shown in Figure a... Figure 5As shown, the diffraction peaks of the (311), (400), (511), and (440) crystal planes of the xN-CuIn5S8 sample show slight shifts. This change may be related to the addition of urea, which introduces smaller N atoms to replace S atoms in CuIn5S8. Bragg's equation states that the larger the diffraction angle, the smaller the lattice. When large-radius atoms are replaced by small-radius atoms, the crystal structure shrinks, proving that the successful doping of a small amount of N leads to lattice shrinkage. The higher the urea-mediated N doping, the broader the peaks and the lower the crystallinity, thus resulting in disorder on the material surface.
[0024] The functional groups and chemical bonds of the material were analyzed using FT-IR, and the infrared spectra are shown below. Figure 2 As shown in b, 3650~3000cm -1 The strip and 1630 cm -1 The weak absorption peaks correspond to the stretching and bending vibrations of OH groups in the surface-adsorbed water, respectively. Nitrogen-doped samples show absorption peaks in the 3000-3600 cm⁻¹ range. -1 The appearance of a broader absorption peak in the region indicates that a small amount of N doping can increase the surface active sites, enhance the adsorption of OH, and is more conducive to the adsorption and activation of CO2. Raman spectroscopy results are as follows... Figure 6 As shown, the successful preparation of N-doped CuIn5S8 samples is confirmed, with all samples reaching a thickness of ~300 cm⁻¹. -1 The characteristic peak of the out-of-plane Alg atomic vibration mode of CuIn5S8 appears at 490 cm⁻¹. -1 Nearby Cu x S-related vibrations. Thermogravimetric results are as follows: Figure 7 As shown, both catalysts exhibit slight weight loss due to water loss at around 84 °C, and their mass retention rate is higher than 95% at a reaction temperature of 210 °C, with no obvious decomposition. This indicates that CuIn5S8 and 300N-CuIn5S8 have good stability at the catalytic temperature.
[0025] The photothermal reduction of CO2 is essentially affected by the Cu, In, and S elements on the catalyst surface. 2- The electron cloud density of N was modulated. X-ray photoelectron spectroscopy (XPS) was used to calibrate at C 1s (284.6 eV) to analyze the elemental valence states and existence forms of CuIn5S8 and 300N-CuIn5S8. The full spectrum (…) Figure 8 This confirmed the presence of Cu, In, S, and N elements. High-resolution photoelectron spectroscopy showed that for the original CuIn5S8 (… Figure 2 c) The high-resolution spectrum of Cu 2p shows two peaks at 951.86 eV and 931.94 eV, corresponding to 2p in a sulfide environment, respectively. 1 / 2 and 2p 3 / 2The spin orbital composition indicates the presence of Cu(I). The peaks at 452.11 and 444.48 eV in the XPS spectrum of In 3d correspond to In 3+ 3D 5 / 2 and 3D 3 / 2 state( Figure 2 d). The S 2p spectrum is unconvolved into two peaks at 162.58 eV and 161.25 eV, respectively. This is because S 2- S 2p 1 / 2 and S 2p 3 / 2 The double splitting frequency peak resulting from orbital splitting ( Figure 2 e). After nitrogen doping, the Cu 2p, In 3d, and S 2p binding energies of 300N-CuIn5S8 all shift to higher fields. This may be because the more electronegative N (3.04) atoms substitute for some S (2.58) sites, attracting electrons from neighboring Cu and In sites and enhancing the interaction of local electron clouds. Figure 2 As shown in f, a new characteristic peak appears at around 401 eV in the spectrum of 300N-CuIn5S8. This peak is an N 1s peak, and its intensity is consistent with the doping concentration. Nitrogen doping reduces the electron density at Cu / In sites, enhances the adsorption of *CO, and promotes CC coupling. 2- To achieve a stable full-shell structure, N acts as an electron acceptor, polarizing the adjacent S electrons and creating a locally positively charged region. This stabilizes the oxygen atoms in oxygen-containing intermediates (such as OCCO and *OC2H5) through electrostatic interactions, inhibiting CO bond breaking and thus redirecting the reaction pathway from ethylene to ethanol.
[0026] Through Cu K-edge XANES ( Figure 2 g), FT-EXAFS ( Figure 2 f) and Wavelet Transform Figure 2i) Analysis compared the electronic structure and coordination environment of Cu in 300N and the original CuIn5S8. XANES spectra showed that although Cu was predominantly +1 in both, the near-edge fine structure of 300N-CuIn5S8 (such as the intensity of the main peak and the oscillation characteristics at the back) differed slightly from that of CuIn5S8, indicating that nitrogen doping introduced local electronic perturbations and fine-tuned the electronic structure of Cu. In FT-EXAFS spectra, the Cu-S coordination peak intensity of 300N-CuIn5S8 was slightly lower than that of CuIn5S8, and the peak position shifted slightly towards the short-range direction, suggesting that the bond length of Cu-S bond was shortened and the coordination order was reduced after nitrogen doping. At the same time, no Cu-Cu metallic bond signal appeared, confirming that Cu still remained highly dispersed. To further verify the dispersion of copper atoms in 300N-CuIn5S8, wavelet transform (WT) analysis of Cu-K edge EXAFS was performed. The Cu-S coordination signal was more concentrated in the K space, indicating that nitrogen doping optimized the local coordination environment of Cu and enhanced the stability of the coordination structure. In summary, nitrogen doping did not change the +1 valence state of Cu or the dominant Cu-S coordination structure, but through electronic perturbation and coordination micro-tuning, it achieved precise optimization of the local structure of CuIn5S8, providing a structural basis for improving its photothermal catalytic performance.
[0027] like Figure 3 As shown, (a) SEM image of CuIn5S8; (b) HRTEM image of 300N-CuIn5S8; (c) SEM image of 300N-CuIn5S8; (d) HRTEM image of 300N-CuIn5S8; (e) TEM image of 300N-CuIn5S8; (f) EDS elemental mapping of 300N-CuIn5S8.
[0028] To fully understand the satisfactory performance of this novel nanostructured photocatalyst, its structure was analyzed, and the results were clearly shown by SEM and TEM. Figure 9 ab and Figure 3 a) CuIn5S8 exhibits a loosely spherical shape, composed of stacked nanosheets with significant gaps between large particles. High-resolution electron microscopy (HRTEM) images and electron diffraction patterns reveal the exposed crystal planes of CuIn5S8. The lattice fringe spacing of the crystal is 0.321 nm and 0.189 nm, respectively, corresponding to the (311) and (400) crystal planes of the cubic CuIn5S8 crystal. Figure 3 b and S5a). 300N-CuIn5S8 is a dense sphere, with abundant mesopores formed by the loose stacking of fine particles (b and S5a). Figure 9 cd and Figure 3c). The addition of urea generates gas under thermal decomposition, hindering grain agglomeration and growth. Gas escape leads to rough pore surfaces, and N-type doping causes slight peak broadening, consistent with XRD results. Compared to the pure phase, the lattice fringe spacing of 300N-CuIn5S8 changes slightly, to 0.314 nm and 0.184 nm respectively. Figure 3 d and Figure 10 (ab) This indicates that doping leads to minute lattice distortions, which may affect the material's electronic structure and catalytic performance. EDS spectroscopy ( Figure 3 The results (ef) show that Cu, In, S, and N are uniformly distributed on the 300N-CuIn5S8 nanoparticles, proving the successful synthesis of the material.
[0029] The photothermal catalytic performance analysis is as follows: To further investigate the photothermal catalytic performance of the catalyst, a series of experiments were conducted to compare the photothermal catalysis of CuIn5S8 with xN-CuIn5S8 with different doping contents. Figure 4 a). The liquid yield of CO2 selectively reduced to CH3CH2OH initially increases and then decreases with increasing N content in x N-CuIn5S8 (x=50, 100, 200..., 500), reaching its maximum at x=300, where the CH3CH2OH formation rate is 46.4 μmol·g. -1 ·h -1 The activity is much higher than that of CuIn5S8 (1.65 μmol·g). -1 ·h -1 However, the formation rate of C2H4 for the gaseous product xN-CuIn5S8 was lower than that for CuIn5S8 (20.83 μmol·g). -1 ·h -1 The selectivity of ethanol is greatly improved, which is beneficial for the separation of subsequent products.
[0030] like Figure 4 As shown, (a) the catalytic activity of CuIn5S8 and xN-CuIn5S8 under light irradiation and 250 °C; (b) the catalytic activity of 300N-CuIn5S8 under light irradiation at different temperatures; (c) the catalytic activity of 300N-CuIn5S8 at different reaction times; (d) the catalytic activity of 300N-CuIn5S8 under different CO2 pressures; (e) the catalytic activity of 300N-CuIn5S8 with different catalyst masses; and (f) the cyclic experiment.
[0031] Temperature gradient activity tests were performed on 300N-CuIn5S8, and the results are as follows: Figure 4As shown in b, the catalytic activity gradually increases with increasing temperature, reaching its optimal level of ethanol yield and selectivity at 210 °C. Further heating leads to a decrease in both yield and selectivity. From a thermodynamic perspective, ethylene formation is an endothermic reaction (ΔH>0), and higher temperatures favor a shift in equilibrium towards the product. Ethanol formation involves an exothermic hydrogenation reaction, and higher temperatures are detrimental to ethanol production. Therefore, 210 °C is the optimal reaction temperature. Comparative experiments also demonstrate that at this temperature, the catalytic activity of 300N-CuIn5S8 is superior to other catalysts. Figure 11 a). Comparing the individual and synergistic effects of light and heat, it was found that, for example... Figure 11 As shown in b, the catalyst 300N-CuIn5S8 exhibits low activity under both single light irradiation (25 °C) and single heating (210 °C) conditions, but its activity significantly increases under both light irradiation and heating (210 °C) conditions, exceeding the simple sum of the activity of each alone. The photoresponse characteristics were investigated using different wavelength filters, and the results showed ( Figure 11 c. Figure 12 Compared to S13, 300N-CuIn5S8 exhibits optimal catalytic activity at approximately 550 nm. This is because the material has a higher absorption coefficient at this wavelength, allowing light energy to be effectively converted into heat energy, thus increasing the reaction temperature. Under the synergistic effect of photothermal activity, more photogenerated electrons can rapidly migrate to the surface active sites, significantly improving catalytic efficiency. Reaction time, CO2 pressure, and catalyst dosage are key factors in regulating the selectivity of CO2 catalytic reduction. Activity experiments show that the results are as follows... Figure 4 The ethanol yield, as shown by ce, gradually increased with increasing reaction time, with 4 h being the optimal time. Increased CO2 pressure enhanced catalytic activity; the catalyst surface adsorption reached saturation at 0.1 MPa, resulting in the highest activity. The optimal catalyst dosage was 50 mg; excessive addition led to decreased activity due to reaction equilibrium, site saturation, and peroxidation. Cyclic stability tests showed the results as follows: Figure 4 As shown in f, after four consecutive photothermal catalytic CO2 reduction cycles, the catalytic activity of 300N-CuIn5S8 decreased slightly, but the overall stability remained good. XRD comparison shows ( Figure 14 After cycling, the crystallinity of the catalyst increases slightly, and the surface structure becomes more regular, which affects some active sites. This is consistent with the pattern of a slight decrease in activity after cycling.
[0032] The catalytic performance was investigated as follows: like Figure 15 As shown, (ab) CuIn5S8 and 300N-CuIn5S8 have TEMPO-e - Spectra; (cd) TEMPO-h of CuIn5S8 and 300N-CuIn5S8 +Spectroscopy; (e) Fluorescence spectrum; (f) Transient fluorescence spectrum; (g) Photocurrent response spectrum; (h) Electrochemical impedance spectroscopy; (i) Nitrogen adsorption-desorption isotherm of the catalyst.
[0033] Non-metallic doping plays a crucial role in enhancing the photocatalytic reduction of CO2 and decomposition of H2O. EPR tests were used to compare monomeric CuIn5S8 and 300N-CuIn5S8 samples to investigate the ability of nitrogen doping to trap photogenerated electrons and holes. TEMPO was used as an electron trapping agent in water or acetonitrile systems, respectively. - and h + The trapping agent exhibits a classic 1:1:1 triplet. Under illumination, charge carriers generated on the catalyst surface react with TEMPO, causing the signal intensity to decrease with illumination time. After 10 min of illumination, the signal peak intensity of CuIn5S8 in TEMPO aqueous solution decreased by 26.8% (…). Figure 15 a); For 300N-CuIn5S8, the decrease was 45.2% ( Figure 15 (b) This indicates that the introduction of a small amount of nitrogen inhibits photogenerated e - and h + The recombination process retains more electrons. Similarly, when holes are captured using the TEMPO acetonitrile system, CuIn5S8 reduces the signal by only 7.8% ( Figure 15 c), 300N-CuIn5S8 decreased by 28.7% ( Figure 15 (d) indicates that it can generate more holes that can participate in the reaction. These results confirm that 300N-CuIn5S8 can effectively separate and enrich more photogenerated carriers, thereby improving photothermal catalytic performance.
[0034] Although 300N-CuIn5S8 can generate more photogenerated electrons and holes, its carrier separation and migration characteristics require further investigation. Fluorescence spectroscopy (PL) is used to investigate the separation of photogenerated carriers in the catalyst, such as... Figure 15 Figure e shows the fluorescence emission spectrum of the catalyst at an excitation wavelength of 296 nm. The fluorescence intensity of the xN-CuIn5S8 samples is generally weak. Among them, the fluorescence intensity of 300N-CuIn5S8 is the lowest, significantly lower than that of pure CuIn5S8, indicating that it has higher carrier separation efficiency and is more difficult to recombine, consistent with the EPR results. Appropriate nitrogen doping can introduce defects as carrier separation centers, while excessive nitrogen easily forms recombination centers. Transient fluorescence shows that the fluorescence lifetime of 300N-CuIn5S8 is longer (τ=2.92 ns) than that of CuIn5S8 (τ=2.62 ns). Figure 15f) indicates that charge carriers can be effectively captured and stored, rather than directly quenched. Nitrogen doping introduces electron traps and lattice defects that optimize charge transport paths and extend electron lifetime, providing a key kinetic basis for the deep multi-electron reduction of CO2 and the highly selective generation of ethanol. Electrochemical tests further confirm these conclusions. Instantaneous photocurrent response ( Figure 15 g) The results show that 300N-CuIn5S8 exhibits the highest photocurrent, indicating superior electron-hole separation efficiency. Electrochemical impedance spectroscopy (EIS) reveals that this sample has the smallest radius of curvature, lower charge transfer resistance, and faster interfacial charge transport. Overall, 300N-CuIn5S8 demonstrates excellent activity in photothermal catalytic CO2 reduction due to its superior carrier separation and transport performance. This is a result of appropriate nitrogen doping synergistically enhancing photogenerated carrier generation, suppressing recombination, and accelerating charge transfer.
[0035] The specific surface area and pore structure of a catalyst directly determine the number of active reaction sites. Nitrogen adsorption-desorption tests show that, for example... Figure 15 As shown in Table i, all six catalysts exhibit typical type IV isotherms and H2 hysteresis loops, indicating a mesoporous structure. As shown in Table 1, 300N-CuIn5S8 has the highest pore volume (0.422 cm³). 3 / g), with a moderate specific surface area (102.8 m²). 2 ( / g) provides ample active sites and substance transport channels. With increasing urea addition, the grain size decreases, and the specific surface area increases from 60.1 m² / g. 2 / g (pure phase) increased to 120.5 m 2 / g (500N), this change will cause the material surface to become disordered, consistent with the XRD results, with peak broadening and lower crystallinity. An appropriate amount of urea can regulate the pore structure and prevent dense packing. The pore size of 300N-CuIn5S8 is 10.4 nm, which is in the optimal mesoporous range, balancing the density of active sites and the mass transfer efficiency of reactants and products, thus resulting in the best catalytic performance.
[0036] Table 1. Specific surface area and pore size of catalysts like Figure 16 As shown, (a) UV-Vis DRS spectrum; (b) band gap energy corresponding to UV-Vis DRS; (c) Mott-Schottky diagrams of CuIn5S8 and 300N-CuIn5S8; (d) schematic diagram of band structure of different samples.
[0037] To explore the ultrawideband absorption of the catalyst, the optical properties of the sample were determined using UV-Vis absorption spectroscopy, which helps to understand the electronic transitions of the catalyst. For example... Figure 16As shown in ab, after N doping into CuIn5S8, the band gap decreased from 1.86 eV to 1.80 eV. This narrowing of the band gap and the redshift of the absorption edge reduce the energy required for electrons to transition from the valence band to the conduction band, making electrons easier to excite. In photothermal catalysis, the broader spectral absorption results in higher photothermal conversion efficiency. This not only improves the material's conductivity and accelerates the electron transfer rate, thereby lowering the activation energy of the reaction and enhancing the catalyst's activity.
[0038] The flat-band potentials of different samples were measured using the Mott-Shawky (MS) method. The MS curves of all samples exhibited positive slopes, indicating that they are all n-type semiconductors. According to... Figure 16 As shown in Figure c, the flat-band potentials of CuIn5S8 and 300N-CuIn5S8 are -1.32 eV and -0.97 (Vνs. Ag / AgCl), respectively. Typically, the bottom of the plateau (CB) of an n-type semiconductor is 0.1 eV negative than the flat-band potential. Therefore, the CB potentials of CuIn5S8 and 300N-CuIn5S8 are -1.22 eV and -0.87 eV, respectively. According to E... VB =E g -E CB Based on the formula and the band gap calculated above, the valence band positions of the samples are determined to be 0.64 eV and 0.93 eV respectively. Figure 16 The band structure diagrams of CuIn5S8 and 300N-CuIn5S8 were depicted, confirming that all catalysts are suitable for photothermal catalytic reduction of CO2.
[0039] like Figure 17 As shown, Figure 17 (a) CO2-TPD experiments of CuIn5S8 and 300N-CuIn5S8; (b) XPS full spectrum of 300N-CuIn5S8 before and after in-situ illumination and reaction; (c) Cu 2p; (d) In 3d; (e) S 2p; (f) N 1s.
[0040] CO2 is an indispensable condition in the reaction process, therefore the adsorption performance of the catalyst is studied through CO2-TPD. For example... Figure 17 As shown in the CO2-TPD spectrum, CuIn5S8 exhibits only one absorption peak for CO2, corresponding to a desorption temperature of 318.3 ℃, while 300N-CuIn5S8 shows two absorption peaks, corresponding to desorption temperatures of 318.3 and 398.2 ℃. Furthermore, the adsorption peak area is larger, indicating an increased adsorption capacity. These results suggest that N doping provides more active sites. In-situ XPS analysis ( Figure 17 b) Reveal the electron transfer patterns in the reaction process of 300N-CuIn5S8. For example... Figure 17As shown in c, the characteristic peak of Cu 2p in the original catalyst sample is Cu 2p. 1 / 2 (952.20 eV) and Cu 2p 3 / 2 (932.32 eV), after in-situ illumination, the characteristic peak of Cu 2p decreased to Cu 2p. 1 / 2 (952.12 eV) and Cu 2p 3 / 2 (932.24 eV), the shift is approximately 0.08 eV, and the characteristic peak position of Cu 2p in the post-reaction sample changes to Cu 2p. 1 / 2 (951.96 eV) and Cu 2p 3 / 2 (932.07 eV), shifting approximately 0.24 eV towards lower binding energies. The sequential shift of Cu binding energy towards lower binding energies indicates an increase in the electron cloud density around Cu, suggesting that Cu may be in an electron-rich state. Simultaneously, the characteristic peak position of In 3d can be observed at In 3d. 3 / 2 (452.56 eV) and In 3d 5 / 2 (444.94 eV) Figure 17 d) After illumination, it drops to In 3d 3 / 2 (452.34 eV) and In 3d 5 / 2 (444.72 eV), the displacement is approximately 0.22 eV; regarding the change in binding energy of the sample after the reaction, it becomes In 3d 3 / 2 (452.27 eV) and In 3d 5 / 2 (444.65 eV), shifting approximately 0.29 eV towards lower binding energies. The binding energy of In also shows a gradual decrease after illumination and reaction, indicating that the chemical environment of In changes during illumination and reaction, with an increase in electron cloud density. The double splitting frequency peaks of S are S 2p... 1 / 2 (163.23 eV) and S 2p 3 / 2 (161.90 eV) Figure 17 e), after illumination, it drops to S 2p 1 / 2 (162.85 eV) and S 2p 3 / 2 (161.61 eV), the displacement is approximately 0.38 eV; regarding the change in binding energy of the sample after the reaction, it becomes S 2p 1 / 2 (162.80 eV) and S 2p 3 / 2 (161.56 eV), shifting approximately 0.43 eV towards lower binding energy. Conversely, as... Figure 17As shown in f, the binding energy of N 1s gradually increases, indicating that N, acting as an electron acceptor, loses electrons, acts as a hole trapping center, and accumulates positive charges. In summary, electrons generated by illumination are enriched at metal and sulfur sites, while N holes are trapped, effectively suppressing carrier recombination, consistent with the EPR conclusions.
[0041] To gain a deeper understanding of the reaction mechanism of catalytic reduction of CO2 and H2O, in-situ FT-IR spectroscopic analysis was performed on the CO2 photothermal reduction process of CuIn5S8 and 300N-CuIn5S8, respectively. The dynamic evolution of intermediates during the heating process indicates a multi-step tandem reaction mechanism.
[0042] like Figure 18 As shown, (ab) is the photothermal in-situ FT-IR spectrum of CuIn5S8; (cd) is the photothermal in-situ FT-IR spectrum of 300N-CuIn5S8.
[0043] In-situ FT-IR spectroscopic analysis of CuIn5S8 catalyzed CO2 reduction is shown in Figures (8a-b). The in-situ infrared spectrum at 1647 cm⁻¹... -1 The infrared peak is attributed to the *COOH group (carboxyl group), a key initial intermediate in CO2 reduction. 1556 cm⁻¹ -1 Attributable to HOH / δ(H2O), the bending vibrations of surface-adsorbed water provide a proton source; 1200 cm -1 Belongs to *CO2 - Activated CO2. At 2077 cm⁻¹ -1 The double bond *CO intermediate (b-*CO) can be observed at 1735 cm⁻¹. -1 The absorption peak at 1716 cm⁻¹ belongs to the characteristic band of *CHO (formyl group), indicating it is a product of *CO hydrogenation. -1 *OCCHO (glyoxal group) is a C2 intermediate; at 1543 cm⁻¹ -1 The infrared peak belongs to *OCCO, which is key to C / C bond formation. 1489 cm⁻¹ -1 Belongs to *CH, chain growing, 1458 cm -1 The structure attributed to *CH2 is a structural feature of the methylene bending vibration. 1437 cm⁻¹ -1 The characteristic peak attributed to C2H4 is at 1378 cm⁻¹. -1 The peak attributable to *C2H5O (ethoxy group) is a C2 oxygen-containing intermediate. The relative intensity of this peak first increases and then decreases with increasing temperature, indicating a change in the concentration of the corresponding reaction intermediate, which will further dehydrate to form other hydrocarbons. At 1335 cm⁻¹ -1 The infrared peak is attributed to *OH (surface hydroxyl groups), which participates in dehydration; 1271 cm- 1Belongs to m-CO3 2- It is a monodentate carbonate, a byproduct or intermediate; 1090, 1043 cm⁻¹ -1 Classified as CO3 2- / ν(CO) belongs to carbonates and is a surface species.
[0044] In-situ FT-IR spectroscopic analysis of CO2 reduction catalyzed by 300N-CuIn5S8 is shown in Figures (8c-d). The in-situ infrared spectrum at 1648 cm⁻¹... -1 The infrared peak is attributed to the *COOH group (carboxyl group), a key initial intermediate in CO2 reduction; 1577 cm⁻¹ -1 The peak intensity is attributed to the *COOH group (carboxyl group) and is asymmetrically stretched. Due to the excessively high intensity of this peak, the reading is 1558 cm⁻¹. -1 The attribution to HOH / δ(H2O) is not so obvious; 1207 cm -1 It also belongs to *CO2 - Activated CO2. At 2078 cm⁻¹ - The double-bonded *CO intermediate (b-*CO) can be observed at ¹. Release of *CO leads to CO formation, while the combination of two *COs results in the formation of C2 products, which gradually increase with irradiation time. These are the initial intermediates of the reaction between gaseous CO2 and water vapor. Notably, the *OCCHO intermediate clearly increases with irradiation time at 1709 cm⁻¹. -1 The intensity at 1543 cm⁻¹ increases significantly, indicating the formation of a C₂ compound. -1 The infrared peak belongs to *OCCO, which is key to C / C bond formation. 1448 cm⁻¹ -1 It belongs to *CH3. Unlike the monomer, it does not have a 1437 cm⁻¹. -1 A characteristic peak belonging to C2H4 appears. At 1378 cm⁻¹. -1 and 1346 cm -1 The characteristic peaks are attributed to *C2H5O (ethoxy group) and *CH3CHO, which are C2 oxygen-containing intermediates. The relative intensity of these peaks gradually increases with increasing temperature, indicating changes in the concentration of the corresponding reaction intermediates. (1278 cm⁻¹) -1 Belongs to m-CO3 2- It is a monodentate carbonate, a byproduct or intermediate; at 1090 and 1036 cm⁻¹ - ¹A characteristic peak also appears, which is attributed to CO3. 2- / ν(CO) belongs to carbonates.
[0045] Based on the above analysis, we propose a possible catalytic mechanism for the photothermal selective reduction of CO2 in a non-metallic N-doped CuIn5S8 system.
[0046] The first step is CO2 activation and protonation. At 1647 / 1648 cm⁻¹ -1 The infrared peak is attributed to *COOH (carboxyl group), where CO2 accepts the first proton, forming the key C1 intermediate, 1556 / 1558 cm⁻¹. -1 Attributable to HOH / δ(H2O), the bending vibration of surface-adsorbed water provides a proton source; 1200 / 1207 cm⁻¹ -1 Belongs to *CO2 - CO2 radical anion, activated CO2.
[0047] CO2 + hv (light energy) → CO2* (activated state) CO2* + H + + e - → *CO2 - CO2+ H + + e - → *COOH The second step is the reduction of the C1 intermediate. At 2077 / 2078 cm⁻¹ -1 The infrared peak is attributed to *CO (linearly adsorbed CO), which is a CC coupling precursor; 1735 / 1738 cm⁻¹ -1 The group classified as *CHO (formyl group) is a hydrogenation product of *CO and can be further reduced; *COOH + H + + e - → CO + H₂O *CO + H + + e - → *CHO The third step is the evolution of C-C coupling and the C2 intermediate. At 1543 cm... -1 The infrared peaks belong to *OCCO, which is key to C / C bond formation. (1716 / 1709 cm⁻¹) -1 The *OCCHO (glyoxal) group is a C2 intermediate, formed by CO dimerization or *CHO coupling. 1489 cm -1 Belongs to *CH, chain growing, 1458 cm -1 The *CH2 group is a structural feature of the methylene bending vibration. Reaction: *COOH → *CO → *CHO → *CH2 → *CH3 (methane pathway, suppressed). 1437 cm⁻¹ -1 Characteristic peaks attributable to C2H4, 1378 / 1380 cm⁻¹ -1 It belongs to *C2H5O (ethoxy group) and is a C2 oxygen-containing intermediate and a dehydration precursor. CC coupling mechanism: *CO + *CO → *OCCO (CC symmetric coupling, the peak intensity is stronger in the CuIn5S8 spectrum). *OCCO + H + + e - → *OCCHO (glyoxal, 1716 cm⁻¹) -1 ) *CO + *CHO → *OCCHO (CC asymmetric coupling, the peak intensity is stronger in the 300N spectrum).
[0048] *OCCHO + H + + e - → *CHOHCO *OCCHO + H + + e - → *CHCO + H2O *CHCO + H + + e - → *CHCHO *CHCHO + H + + e - → *CCH + H2O *CCH + H + + e - → *CHCH *CHCH + H + + e - → *CH2CH *CH2CH + H + + e - → *CH2CH2 *CHCO + 2H + + 2e - → *CH2CHO *CH2CO + H + + e - → *CH3CHO *CH3CHO + H + + e - → *CH3CH2O *CH3CH2O + H + + e - → CH3CH2OH This invention achieves multi-dimensional optimization from morphology to electronic structure, and from photophysics to electrochemistry, through the in-situ synthesis of N-doped CuIn5S8 mediated by urea. The core of this strategy lies in utilizing the high electronegativity of N and the thermal decomposition properties of urea to simultaneously optimize grain nanostructuring, mesoporous structure construction, band structure modulation, and carrier separation. The resulting 300N sample exhibited excellent ethanol selectivity in the photothermal catalytic reduction of CO2 + H2O, demonstrating the effectiveness of the synergistic strategy of "structural nanostructuring—electron deprivation—kinetic optimization" in complex multi-electron catalytic reactions, and providing a universal approach for designing highly efficient CO2 reduction catalysts.
[0049] Obviously, those skilled in the art can make various modifications and variations to the embodiments of the present invention without departing from the spirit and scope of the invention. Therefore, if these modifications and variations fall within the scope of the claims of the present invention and their equivalents, the present invention also intends to include these modifications and variations.
Claims
1. The application of a nitrogen-doped copper indium sulfide x N-CuIn5S8 photothermal catalyst, characterized in that, The nitrogen-doped copper indium sulfide xN-CuIn5S8 photothermal catalyst is used for the selective reduction of carbon dioxide to ethanol under photothermal conditions.
2. The application of the nitrogen-doped copper indium sulfide x N-CuIn5S8 photothermal catalyst according to claim 1, characterized in that, In the nitrogen-doped copper indium sulfide x N-CuIn5S8, x takes the value of 50, 100, 200, 300, 400 or 500, and the molar ratio of Cu, In and S is 1:5:
8.
3. The application of the nitrogen-doped copper indium sulfide x N-CuIn5S8 photothermal catalyst according to claim 2, characterized in that, The value of x is 300.
4. The application of the nitrogen-doped copper indium sulfide x N-CuIn5S8 photothermal catalyst according to any one of claims 1-3, characterized in that, The nitrogen-doped copper indium sulfide x N-CuIn5S8 photothermal catalyst for the selective reduction of CO2 to ethanol under photothermal conditions specifically includes the following steps: Weigh 50 mg of catalyst and measure 8 mL of ultrapure water, add them sequentially to the reaction vessel and seal it; Then, open the inlet and outlet ports simultaneously, connect a CO2 gas cylinder to the inlet port, and continuously flush the gas inside the vessel with a small amount of CO2 gas for 10-15 minutes to remove the residual air inside the vessel. Close the air outlet and adjust the pressure to 0.1 ± 0.01 MPa and maintain it for 10 ± 1 s; To establish adsorption equilibrium, the system was first magnetically stirred for 30 min in an environment without the xenon lamp on, and then irradiated with a 300 W xenon lamp while keeping the system temperature constant at 210 ± 2 ℃ and continuing the reaction for 4 ± 0.1 h. After the reaction is complete, cool to room temperature, collect the solution in the reaction vessel, centrifuge and take the clear liquid at the top, which is a mixture of ethanol and water.
5. A method for preparing a nitrogen-doped copper indium sulfide x N-CuIn5S8 photothermal catalyst, based on the nitrogen-doped copper indium sulfide x N-CuIn5S8 according to any one of claims 4, characterized in that, Specifically, the steps include the following: Weigh 1 mmol of copper nitrate trihydrate (Cu(NO3)2·3H2O) and 1.2 mmol of indium chloride tetrahydrate (InCl3·4H2O) into a polytetrafluoroethylene-lined autoclave, add 35 mL of deionized water and 35 mL of ethylene glycol, and stir vigorously for 30-40 min. Add 4 mmol of a mixture of urea and thioacetamide to the above transparent solution and stir for 30 ± 1 min; wherein the molar ratio of urea to thioacetamide is one of 0.5, 1.0, 2.0, 3.0, 4.0 and 5.0, and the corresponding product is named xN-CuIn5S8, where X is one of 50, 100, 200, 300, 400 or 500; The turbid solution was transferred to a polytetrafluoroethylene-lined autoclave and kept at 180 ± 2 °C for 12 ± 0.3 h. After the reaction was completed, the mixture was cooled to room temperature to obtain a precipitate, which was then washed by centrifugation several times. x N-CuIn5S8 can be obtained by drying in a vacuum oven at 60 ± 2 ℃ for 12 ± 0.3 h.