Composite catalytic particles, methods of making, and use of the catalysts in the production of single-walled carbon nanotubes
By designing composite catalytic particles and adjusting the catalytic components and surface state, the problems of component segregation and unstable transport in the preparation of single-walled carbon nanotubes by plasma arc method were solved, and the stable preparation of high-purity single-walled carbon nanotubes was achieved.
Patent Information
- Application Number
- CN202611545311.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-08
- Publication Date
- 2026-11-20
AI Technical Summary
Existing powder catalysts are prone to component segregation, unstable transport, and high-temperature agglomeration during the plasma arc method for preparing single-walled carbon nanotubes, resulting in fluctuations in product composition and making it difficult to control catalytic activity and purity.
Composite catalytic particles containing catalytic components and binders are used. By adjusting the phase composition, surface state, and metal-carbon interface state of the catalytic components, rare earth elements such as yttrium, cerium, and lanthanum, and refractory metal modifiers such as molybdenum and tungsten are used, along with sulfur and selenium to adjust the surface energy and carbon precipitation conditions of the catalytic particles, thus forming composite catalytic particles suitable for the nucleation of single-walled carbon nanotubes.
This improved the nucleation efficiency of single-walled carbon nanotubes, reduced the content of non-target carbon components and metal impurities, enhanced the stability and purity of the catalyst, and simplified subsequent purification steps.
Smart Images

Figure CN123128017A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of carbon nanomaterials, and in particular to a composite catalytic particle, a preparation method thereof, and the application of the catalyst in the preparation of single-walled carbon nanotubes by plasma arc method. Background Technology
[0002] Single-walled carbon nanotubes (SUVs) are tubular carbon materials formed by rolling up a single layer of graphene. They possess high aspect ratio, electrical conductivity, thermal conductivity, and mechanical strength, making them suitable for applications such as conductive additives, energy storage devices, composite materials, and sensors. The purity, structural integrity, diameter distribution, and metallic impurity content of SUVs directly affect their performance in these applications.
[0003] The main methods for preparing single-walled carbon nanotubes include chemical vapor deposition, laser ablation, and plasma-arc discharge. Plasma-arc discharge (PAD) is characterized by high energy density, rapid carbon source decomposition, and large throughput per unit time, making it suitable for continuous preparation of single-walled carbon nanotubes. After plasma decomposition, the carbon source forms carbon-containing active species, which are adsorbed onto the surface of composite catalytic particles and then dissolved, diffused, and precipitated to form a carbon cap structure. Under continuous carbon source supply, the carbon cap extends to form single-walled carbon nanotubes.
[0004] Iron, cobalt, and nickel provide active sites for the adsorption, dissolution, diffusion, and precipitation of carbon source pyrolysis products, and are therefore widely used as catalytic active metals for single-walled carbon nanotubes. However, single iron, cobalt, or nickel particles are prone to melting and aggregation at high temperatures, leading to increased particle size and wider distribution, which is detrimental to single-walled carbon nanotube nucleation and increases the amount of non-target carbon components such as amorphous carbon, fullerenes, coated carbon, and graphite particles. To improve the dispersibility of catalytic active metals, existing technologies use porous hard carbon, silica, and other supports to support metal catalysts. While supports can immobilize active metals, they reduce the active metal content per unit mass of catalyst and increase the steps for support removal and product purification. Another technology mixes catalysts, promoters, and carbonaceous additives and then granulates them by ball milling or calcination; however, carbonaceous additives can enter the reaction products, and the calcination process can also change the oxidation state and particle size of the metal components.
[0005] Meanwhile, in the high-temperature environment of plasma formation, the catalyst's transport stability, component uniformity, and the high-temperature state of active particles are difficult to control, easily causing fluctuations in product composition. Crude products obtained by plasma-arc methods typically contain amorphous carbon, fullerenes, coated carbon, graphite, and residual metals. Acid washing alone is insufficient to remove metal particles coated with carbon layers; oxidation alone requires balancing impurity removal with the preservation of the single-walled carbon nanotube structure. Summary of the Invention
[0006] In view of the above problems, this application provides a composite catalytic particle, a preparation method, and the application of the catalyst in the preparation of single-walled carbon nanotubes by plasma arc method, so as to solve the problems of component segregation, unstable transport and high-temperature agglomeration that easily occur in the continuous preparation of single-walled carbon nanotubes by plasma arc method of existing powder catalysts.
[0007] The first aspect of this application provides a composite catalytic particle for the preparation of single-walled carbon nanotubes, the composite catalytic particle comprising: a catalytic component and a binder; the catalytic component comprising a first catalytic component and a second catalytic component;
[0008] The first catalytic component includes at least one of iron, cobalt, and nickel, wherein the total mass of iron, cobalt, and nickel accounts for 70-98 wt% of the total mass of the catalytic component.
[0009] and
[0010] At least one of yttrium, cerium, lanthanum, molybdenum and tungsten, wherein the total mass of yttrium, cerium, lanthanum, molybdenum and tungsten accounts for 5 to 30 wt% of the total mass of the catalytic components; rare earth elements are added in the form of elements, oxides or alloys, etc., and can all inhibit metal aggregation under high plasma temperature.
[0011] The second catalytic component includes at least one of sulfur and selenium;
[0012] The ratio of the total molar amount of iron, cobalt, nickel, yttrium, cerium, lanthanum, molybdenum, and tungsten to the total molar amount of sulfur and selenium is 1:0.2 to 2. The "total molar amount of metals" mentioned in this invention refers to the sum of the molar amounts of all metal elements (iron, cobalt, nickel, yttrium, cerium, lanthanum, molybdenum, and tungsten) in the first catalytic component, regardless of whether the element is added in elemental, alloy, or oxide form, and is counted based on the molar amount of the metal element itself.
[0013] Iron, cobalt, and nickel form the main components of the composite catalytic particles. After plasma pyrolysis, the carbon source forms carbon-containing active species, which are adsorbed on the surface of the composite catalytic particles and then dissolved, diffused, and precipitated to form a carbon cap structure. Under continuous carbon source supply, the carbon cap extends to form single-walled carbon nanotubes.
[0014] Yttrium, cerium, and lanthanum, as rare earth elements, regulate the phase composition, surface state, and metal-carbon interface state of composite catalytic particles, and limit the migration and aggregation of iron, cobalt, or nickel particles during heating, reduction, and high-temperature reaction processes.
[0015] Molybdenum and tungsten, as refractory metal modifiers, are used to improve the thermal stability of composite catalytic particles, regulate the dissolution and precipitation process of carbon in composite catalytic particles, facilitate the nucleation of single-walled carbon nanotubes, maintain the active state of composite catalytic particles, and reduce the formation of non-target carbon components.
[0016] Sulfur and selenium play a role in regulating the surface energy of composite catalytic particles, affecting their melting state and carbon precipitation conditions. Insufficient sulfur and selenium content limits their regulatory effect; excessive sulfur and selenium content, on the other hand, occupies the surface of active metals, reducing the number of effective catalytic sites. Studies have found that a ratio of 1:0.2–2 between the total molar amount of iron, cobalt, nickel, yttrium, cerium, lanthanum, molybdenum, and tungsten metals and the total molar amount of sulfur and selenium can both regulate the state of the composite catalytic particles and ensure the number of catalytic sites on the metal surface.
[0017] Unlike existing technologies, yttrium, cerium, and lanthanum regulate the phase composition, surface state, and metal-carbon interface state of the composite catalytic particles, limiting their migration and aggregation. Molybdenum and tungsten are used to improve the thermal stability of the composite particles. Sulfur and selenium are used to maintain effective catalytic sites on the surface of the composite catalytic particles and regulate carbon precipitation conditions. The combination of these components is beneficial to the nucleation of single-walled carbon nanotubes and the growth of composite catalytic particles, while reducing the formation of non-target carbon components and lowering the content of heterogeneous carbon (including amorphous carbon, fullerenes, and graphite) and metal impurities in the product.
[0018] Furthermore, the first catalytic component includes at least one of iron-nickel alloy, cobalt-nickel alloy, iron-cobalt alloy, and iron-cobalt-nickel alloy.
[0019] Furthermore, the first catalytic component includes at least one of yttrium oxide, cerium oxide, lanthanum oxide, iron-yttrium alloy, nickel-yttrium alloy, iron-cerium alloy, iron-lanthanum alloy, iron-molybdenum alloy, iron-tungsten alloy, nickel-molybdenum alloy, and nickel-tungsten alloy.
[0020] Furthermore, the composite catalytic particles include a binder, which includes at least one of carboxymethyl cellulose, polyvinyl alcohol, phenolic resin, and gelatin.
[0021] Furthermore, the mass of the binder is 0.1–3.0 wt% of the total mass of the catalytic components. The binder binds components of different sizes and densities, ensuring that the components maintain a preset ratio during storage and transportation. If the amount of binder is too low, the particle strength will be insufficient; if the amount of binder is too high, it will reduce the dispersibility of the particles in the plasma reaction region and increase the amount of non-target carbon components formed by the pyrolysis of the binder.
[0022] Furthermore, the composite catalyst particles have a particle size of 40–80 mesh. This particle size range is designed to balance the flowability required for screw conveying with the particle's disintegration, heating, and dispersion properties in the high-temperature reaction zone.
[0023] The second aspect of this application provides a method for preparing composite catalytic particles, comprising the following steps:
[0024] The catalytic components and binder are mixed and stirred for 0.5 to 4 hours to obtain a first mixture; 50 wt% ethanol aqueous solution is added to the first mixture and stirred to obtain a second mixture; the second mixture is wet granulated, sieved, and dried to obtain the composite catalytic particles; the amount of ethanol aqueous solution added is 5 to 30 wt% of the first mixture.
[0025] Unlike existing technologies, yttrium, cerium, and lanthanum regulate the phase composition, surface state, and metal-carbon interface state of the composite catalytic particles, limiting their migration and aggregation; molybdenum and tungsten improve the thermal stability of the composite catalytic particles; and sulfur and selenium regulate the surface state and carbon precipitation conditions of the composite catalytic particles. The combination of these components helps maintain composite catalytic particles suitable for single-walled carbon nanotube nucleation and growth, and reduces the formation of non-target carbon components.
[0026] This invention uses wet granulation to immobilize the main catalytic component and the second catalytic component within the same particle, reducing powder dust, agglomeration, and component segregation, and improving the stability of continuous screw conveying. Simultaneously, it eliminates the need for a large amount of solid support as a necessary component, increasing the proportion of active components per unit mass of composite catalytic particles and reducing subsequent removal steps caused by the support.
[0027] Furthermore, the D50 particle size of the first catalytic component is 100–500 nm, and the D50 particle size of the second catalytic component is 1–3 μm.
[0028] Furthermore, the amount of the ethanol aqueous solution added is 10 to 20 wt% of the first mixture.
[0029] The third aspect of this application provides a method for preparing single-walled carbon nanotubes by plasma arc method, wherein the method uses the composite catalytic particles described in the first aspect of this application.
[0030] Furthermore, the method for preparing single-walled carbon nanotubes by plasma arc method includes the following steps:
[0031] The composite catalytic particles are continuously fed into the plasma arc furnace at a rate of 10–500 g / h via a screw conveyor.
[0032] Argon, hydrogen, and a gaseous carbon source are introduced into the plasma arc furnace, wherein the volume flow rate ratio of the argon, hydrogen, and gaseous carbon source is 1:(0.1-3):(0.05-1).
[0033] The working power of the plasma arc furnace is controlled to be 50-200 kW, the temperature of the reaction zone is 1000-1500℃, and the total flow rate of the reaction gas is 100-2000 L / min;
[0034] The crude product containing single-walled carbon nanotubes is collected from the product outlet of the plasma arc furnace.
[0035] Furthermore, the gaseous carbon source includes at least one of methane, ethane, ethylene, propylene, propane, natural gas, carbon monoxide, and ethanol vapor.
[0036] Furthermore, the delivery rate of the composite catalyst particles is 50–120 g / h; the total flow rate of the reaction gas is 500–800 L / min; the operating power of the plasma arc furnace is 80–140 kW; and the temperature of the reaction zone is 1200–1350 °C.
[0037] The crude product containing single-walled carbon nanotubes can be purified according to the purity requirements of the product using conventional post-processing methods in the field, such as sequential oxidation in an oxygen atmosphere, heat treatment in an inert atmosphere, and acid washing.
[0038] Furthermore, the crude product is oxidized at 380–500°C for 30–180 min in an oxygen-containing atmosphere with an oxygen volume content of 21%; the oxidized product is then heat-treated at 800°C for 2 h in a nitrogen, argon, or helium atmosphere; followed by acid washing with 0.2–6 mol / L hydrochloric acid at 50–90°C for 1–48 h, and then washed, filtered, and dried.
[0039] The above description of the invention is merely an overview of the technical solution of this application. In order to enable those skilled in the art to better understand the technical solution of this application and to implement it based on the textual description, and to make the above-mentioned objectives and other objectives, features and advantages of this application easier to understand, the following description is provided in conjunction with the specific embodiments and accompanying drawings of this application. Attached Figure Description
[0040] The accompanying drawings are only used to illustrate the principles, implementation methods, applications, features, and effects of specific embodiments of this application and other related content, and should not be considered as limitations on this application.
[0041] In the accompanying drawings of the instruction manual:
[0042] Figure 1 This is a scanning electron microscope image of the crude single-walled carbon nanotube product obtained in Example 1.
[0043] Figure 2 This is a scanning electron microscope image of the purified single-walled carbon nanotubes obtained in Example 1.
[0044] Figure 3 This is a transmission electron microscope image of the purified single-walled carbon nanotubes obtained in Example 1.
[0045] Figure 4The image shows the Raman spectrum of the crude single-walled carbon nanotube product obtained in Example 1.
[0046] Figure 5 The image shows the Raman spectrum of the purified single-walled carbon nanotubes obtained in Example 1. Detailed Implementation
[0047] To illustrate the possible application scenarios, technical principles, implementable specific solutions, and achievable objectives and effects of this application in detail, the following description, in conjunction with the listed specific embodiments and accompanying drawings, provides a detailed explanation. The embodiments described herein are merely illustrative of the technical solutions of this application and are therefore intended to limit the scope of protection of this application.
[0048] In this document, the term "embodiment" means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The term "embodiment" appearing in various places throughout the specification does not necessarily refer to the same embodiment, nor does it specifically limit its independence or connection with other embodiments. In principle, in this application, as long as there are no technical contradictions or conflicts, the technical features mentioned in each embodiment can be combined in any way to form corresponding implementable technical solutions.
[0049] Unless otherwise defined, the technical terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the use of related terms herein is merely for the purpose of describing particular embodiments and is not intended to limit this application.
[0050] In the description of this application, the term "and / or" is used to describe the logical relationship between objects, indicating that three relationships can exist. For example, A and / or B means: A exists, B exists, and A and B exist simultaneously. Additionally, the character " / " in this document generally indicates that the preceding and following objects have an "or" logical relationship.
[0051] In this application, terms such as “first” and “second” are used only to distinguish one entity or operation from another, and do not necessarily require or imply any actual quantity, hierarchy or order relationship between these entities or operations.
[0052] Unless otherwise specified, the use of terms such as “comprising,” “including,” “having,” or other similar expressions in this application is intended to cover non-exclusive inclusion, which does not exclude the presence of additional elements in a process, method, or product that includes the stated elements, such that a process, method, or product that includes a list of elements may include not only those defined elements but also other elements not expressly listed, or elements inherent to such a process, method, or product.
[0053] In this application, expressions such as "greater than", "less than", and "exceeding" are understood to exclude the stated number; expressions such as "above", "below", and "within" are understood to include the stated number. Furthermore, in the description of the embodiments of this application, "multiple" means two or more (including two), and similar expressions related to "multiple" are also understood in this way, such as "multiple groups" and "multiple times", unless otherwise explicitly specified.
[0054] Example 1
[0055] This embodiment provides a composite catalytic particle, its preparation method, and a method for preparing single-walled carbon nanotubes:
[0056] 1. Select iron-nickel alloy powder (60wt% iron, 40wt% nickel) with a D50 particle size of 500nm and lanthanum oxide powder as the first catalyst component, with a mass ratio of 85:15. Select sulfur powder with a D50 particle size of 2μm as the second catalyst component. Weigh the raw materials according to a ratio of total molar amount of metal elements to molar amount of sulfur of 1:0.2. Based on the total mass of the catalyst components, weigh 0.5 wt% of carboxymethyl cellulose.
[0057] 2. Add each catalytic component and carboxymethyl cellulose to a mixer and mix for 2 hours. Then add an ethanol aqueous solution with a mass content of 50 wt% in portions while stirring to obtain a mixture. The amount of the ethanol aqueous solution added is 15 wt% of the mass of the mixture.
[0058] 3. The mixture is granulated using a wet granulator. The granulated material is then screened using a vibrating screen to collect 40-80 mesh particles. The particles are then dried at 80℃ for 12 hours to obtain composite catalytic particles.
[0059] 4. The composite catalyst particles are added to the plasma arc furnace via a screw conveyor, with a conveying rate of 80 g / h. Argon, hydrogen, and methane are introduced into the furnace at a volumetric flow rate ratio of 1:0.5:0.1, with a total gas flow rate of 800 L / min. The plasma arc furnace operates at a power of 80 kW, and the reaction zone temperature is 1200℃.
[0060] 5. Collect the crude product containing single-walled carbon nanotubes from the product outlet of the plasma arc furnace, and oxidize the crude product at 420°C for 30 min in an oxygen-containing atmosphere with an oxygen volume content of 21%; heat-treat the oxidized product at 800°C for 2 h in a nitrogen atmosphere; acid-wash the heat-treated product with 1 mol / L hydrochloric acid at 70°C for 12 h; then wash with water, filter and dry to obtain purified single-walled carbon nanotubes.
[0061] The catalyst delivery status, the content of single-walled carbon nanotubes, heterogeneous carbon and metal impurities in the crude product, and the content of single-walled carbon nanotubes, metal impurities and Raman spectroscopy IG / ID in the purified product are listed in Table 1.
[0062] The contents of single-walled carbon nanotubes, heterogeneous carbon, and metallic impurities were determined by thermogravimetric analysis. Raman spectroscopy was performed using a 518 nm laser, and the intensity ratio of the G peak to the D peak is expressed as IG / ID.
[0063] SEM images of crude and purified single-walled carbon nanotubes are shown below. Figure 1 and Figure 2 TEM images of the purified single-walled carbon nanotubes are shown below. Figure 3 Raman spectra of crude and purified single-walled carbon nanotubes are shown in [reference needed]. Figure 4 and Figure 5 .
[0064] from Figure 1 It can be seen that the crude single-walled carbon nanotube product prepared by Example 1 contains a large number of tubular structures, indicating that the crude product has a high content of single-walled carbon nanotubes. Figure 1 The crude product contains some impurities, which are impurities formed during the growth of single-walled carbon nanotubes and residual catalyst. Figure 2 It can be seen that the impurities in the purified single-walled carbon nanotubes are significantly reduced, and the purified product has a high purity. From Figure 3 It can be seen that the purified product has a single-layer tube bundle structure and no obvious impurities were observed. This indicates that the purified single-walled carbon nanotubes have high purity. Figure 4 and Figure 5 The RBM signal peaks clearly belonging to single-walled carbon nanotubes can be observed, further confirming that the product type is single-walled carbon nanotubes. The intensity ratio of the G peak and the D peak was calculated, and the IG / ID before and after purification were 114.3 and 142.5, respectively, indicating that the purification effect was significant.
[0065] Example 2
[0066] This embodiment provides a composite catalytic particle, its preparation method, and a method for preparing single-walled carbon nanotubes:
[0067] 1. Iron powder and cerium oxide powder with a D50 particle size of 300 nm were selected as the first catalyst component, with a mass ratio of iron powder to cerium oxide powder of 90:10; sulfur powder with a D50 particle size of 1 μm was selected as the second catalyst component. The ratio of the total molar amount of metal elements to the molar amount of sulfur elements was 1:0.3. 0.5 wt% (based on the total mass of the catalyst components) of polyvinyl alcohol was weighed.
[0068] 2. Add the above components to a mixer and mix for 2 hours. Then add an ethanol aqueous solution with a mass content of 50 wt% in portions while stirring to obtain a mixture. The amount of the ethanol aqueous solution added is 15 wt% of the mass of the mixture.
[0069] 3. The mixture is granulated using a wet granulator, and the 40-80 mesh particles are collected after being screened by a vibrating screen. The particles are then dried at 80℃ for 12 hours to obtain composite catalytic particles.
[0070] 4. The composite catalyst particles are added to the plasma arc furnace via a screw conveyor, with a conveying rate of 100 g / h. Argon, hydrogen, and ethane are introduced into the furnace at a volume flow rate ratio of 1:0.5:0.1, with a total gas flow rate of 600 L / min. The plasma arc furnace operates at a power of 100 kW, and the reaction zone temperature is 1200℃.
[0071] 5. Collect the crude product containing single-walled carbon nanotubes from the product outlet of the plasma arc furnace, and oxidize the crude product at 420°C for 30 min in an oxygen-containing atmosphere with an oxygen volume content of 21%; heat-treat the oxidized product at 800°C for 2 h in a nitrogen atmosphere; acid-wash the heat-treated product with 1 mol / L hydrochloric acid at 70°C for 12 h; then wash with water, filter and dry to obtain purified single-walled carbon nanotubes.
[0072] The catalyst delivery status, the content of single-walled carbon nanotubes, heterogeneous carbon and metal impurities in the crude product, and the content of single-walled carbon nanotubes, metal impurities and Raman spectroscopy IG / ID in the purified product are listed in Table 1.
[0073] Example 3
[0074] This embodiment provides a composite catalytic particle, its preparation method, and a method for preparing single-walled carbon nanotubes:
[0075] 1. Iron-molybdenum alloy powder (50 wt% of both powder and molybdenum) with a D50 particle size of 500 nm and cerium oxide powder were selected as the first catalytic component, with a mass ratio of 80:20. Selenium powder with a D50 particle size of 2 μm was selected as the second catalytic component, with a total molar ratio of metal elements to selenium elements of 1:0.3. 0.5 wt% (based on the total mass of the catalytic components) of polyvinyl alcohol was weighed.
[0076] 2. Add the above components to a mixer and mix for 2 hours. Then add an ethanol aqueous solution with a mass content of 50 wt% in portions while stirring to obtain a mixture. The amount of the ethanol aqueous solution added is 15 wt% of the mass of the mixture.
[0077] 3. The moistened material is granulated using a wet granulator, and the 40-80 mesh particles are collected after being screened by a vibrating screen. The particles are then dried at 80℃ for 12 hours to obtain composite catalytic particles.
[0078] 4. The catalyst is added to the plasma arc furnace via a screw conveyor, with a conveying rate of 100 g / h. Argon, hydrogen, and methane are introduced into the furnace at a volumetric flow rate ratio of 1:1:0.1, with a total gas flow rate of 1000 L / min. The plasma arc furnace operates at a power of 120 kW, and the reaction zone temperature is 1250 °C.
[0079] 5. Collect the crude product containing single-walled carbon nanotubes from the product outlet of the plasma arc furnace, and oxidize the crude product at 420°C for 30 min in an oxygen-containing atmosphere with an oxygen volume content of 21%; heat-treat the oxidized product at 800°C for 2 h in a nitrogen atmosphere; acid-wash the heat-treated product with 1 mol / L hydrochloric acid at 70°C for 12 h; then wash with water, filter and dry to obtain purified single-walled carbon nanotubes.
[0080] The catalyst delivery status, the content of single-walled carbon nanotubes, heterogeneous carbon and metal impurities in the crude product, and the content of single-walled carbon nanotubes, metal impurities and Raman spectroscopy IG / ID in the purified product are listed in Table 1.
[0081] Example 4
[0082] This embodiment provides a composite catalytic particle, its preparation method, and a method for preparing single-walled carbon nanotubes:
[0083] 1. Nickel-yttrium alloy powder (60 wt% nickel, 40 wt% yttrium) and cerium oxide powder with a D50 particle size of 500 nm were selected as the first catalytic component. The mass ratio of nickel-yttrium alloy to cerium oxide was 80:20. Sulfur powder with a D50 particle size of 1 μm was selected as the second catalytic component. Nickel-yttrium alloy powder, cerium oxide powder, and sulfur powder were weighed according to a ratio of total molar amount of metal elements to molar amount of sulfur of 1:0.2. Based on the total mass of nickel-yttrium alloy powder, cerium oxide powder, and sulfur powder, 0.5 wt% carboxymethyl cellulose was weighed as a binder.
[0084] 2. Add the above raw materials to a mixer and mix for 2 hours. Then add an ethanol aqueous solution with a mass content of 50 wt% in portions while stirring to obtain a mixture. The amount of the ethanol aqueous solution added is 15 wt% of the mass of the mixture.
[0085] 3. Add the mixture to a wet granulator for granulation. After granulation, use a vibrating screen to sieve and collect particles of 40-80 mesh. Dry the particles at 80℃ for 12 hours to obtain composite catalytic particles.
[0086] 4. The composite catalyst particles are continuously conveyed to the plasma arc furnace via a screw conveyor, with a conveying rate of 80 g / h. Argon, hydrogen, and methane are introduced into the plasma arc furnace at a volumetric flow rate ratio of 1:0.6:0.12, and the total flow rate of the reaction gases is 600 L / min. The operating power of the plasma arc furnace is controlled at 100 kW, and the temperature of the reaction zone is 1250℃.
[0087] 5. Collect the crude product containing single-walled carbon nanotubes from the product outlet of the plasma arc furnace, and oxidize the crude product at 420°C for 30 min in an oxygen-containing atmosphere with an oxygen volume content of 21%; heat-treat the oxidized product at 800°C for 2 h in a nitrogen atmosphere; acid-wash the heat-treated product with 1 mol / L hydrochloric acid at 70°C for 12 h; then wash with water, filter and dry to obtain purified single-walled carbon nanotubes.
[0088] The catalyst delivery status, the content of single-walled carbon nanotubes, heterogeneous carbon and metal impurities in the crude product, and the content of single-walled carbon nanotubes, metal impurities and Raman spectroscopy IG / ID in the purified product are listed in Table 1.
[0089] Example 5
[0090] This embodiment provides a composite catalytic particle, its preparation method, and a method for preparing single-walled carbon nanotubes:
[0091] 1. Cobalt-nickel alloy powder (60 wt% cobalt, 40 wt% nickel) with a D50 particle size of 400 nm and lanthanum oxide powder with a D50 particle size of 300 nm were selected as the first catalyst component. The mass ratio of cobalt-nickel alloy powder to lanthanum oxide powder was 90:10. Selenium powder with a D50 particle size of 2 μm was selected as the second catalyst component. The raw materials were weighed according to a ratio of total molar amount of metal elements to molar amount of selenium elements of 1:0.3. The total molar amount of metal elements was calculated as the sum of the molar amounts of cobalt, nickel, and lanthanum. Based on the total mass of the catalyst components, 0.8 wt% of polyvinyl alcohol was weighed as a binder.
[0092] 2. Add the above raw materials to a mixer and mix for 2 hours. Then add an ethanol aqueous solution with a mass content of 50 wt% in portions while stirring to obtain a mixture. The amount of the ethanol aqueous solution added is 20 wt% of the mass of the mixture.
[0093] 3. Add the mixture to a wet granulator for granulation. After granulation, use a vibrating screen to sieve and collect particles of 40-80 mesh. Dry the particles at 80℃ for 12 hours to obtain composite catalytic particles.
[0094] 4. The composite catalyst particles are continuously conveyed to the plasma arc furnace via a screw conveyor, with a conveying rate of 100 g / h. Argon, hydrogen, and ethylene are introduced into the plasma arc furnace at a volumetric flow rate ratio of 1:0.8:0.08, and the total flow rate of the reaction gases is 700 L / min. The operating power of the plasma arc furnace is controlled at 120 kW, and the reaction zone temperature is 1300℃. The crude product containing single-walled carbon nanotubes is collected from the product outlet of the plasma arc furnace.
[0095] 5. The crude product was subjected to oxygen-containing atmosphere oxidation, nitrogen atmosphere heat treatment and hydrochloric acid washing in sequence according to the purification method described in Example 1 to obtain purified single-walled carbon nanotubes.
[0096] The catalyst delivery status, the content of single-walled carbon nanotubes, heterogeneous carbon and metal impurities in the crude product, and the content of single-walled carbon nanotubes, metal impurities and Raman spectroscopy IG / ID in the purified product are listed in Table 1.
[0097] Example 6
[0098] This embodiment provides a composite catalytic particle, its preparation method, and a method for preparing single-walled carbon nanotubes:
[0099] 1. Iron-tungsten alloy powder (85 wt% iron, 15 wt% tungsten) with a D50 particle size of 500 nm and cerium oxide powder with a D50 particle size of 300 nm were selected as the first catalytic component. The content of the iron-tungsten alloy powder was 90 wt%, and the content of the cerium oxide powder was 10 wt%. Sulfur powder and selenium powder with a D50 particle size of 2 μm were selected as the second catalytic component, with a sulfur to selenium molar ratio of 1:1. The raw materials were weighed according to a ratio of the total molar amount of metal elements to the total molar amount of sulfur and selenium elements in the second catalytic component of 1:0.25. Based on the total mass of the catalytic components, 0.5 wt% gelatin was weighed as a binder.
[0100] 2. Add the above raw materials to a mixer and mix for 2 hours. Then add an ethanol aqueous solution with a mass content of 50 wt% in portions while stirring to obtain a mixture. The amount of the ethanol aqueous solution added is 15 wt% of the mass of the mixture.
[0101] 3. Add the mixture to a wet granulator for granulation. After granulation, use a vibrating screen to sieve and collect particles of 40-80 mesh. Dry the particles at 80℃ for 12 hours to obtain composite catalytic particles.
[0102] 4. The composite catalyst particles are continuously conveyed to a plasma arc furnace via a screw conveyor, with a conveying rate of 120 g / h. Argon, hydrogen, and a mixed carbon source consisting of methane and carbon monoxide are introduced into the plasma arc furnace. The volume flow rate ratio of argon, hydrogen, and the mixed carbon source is 1:1:0.15, and the volume flow rate ratio of methane to carbon monoxide in the mixed carbon source is 2:1. The total flow rate of the reaction gases is 800 L / min. The operating power of the plasma arc furnace is controlled at 140 kW, and the reaction zone temperature is 1350℃. The crude product containing single-walled carbon nanotubes is collected from the product outlet of the plasma arc furnace.
[0103] 5. The crude product was subjected to oxygen-containing atmosphere oxidation, nitrogen atmosphere heat treatment and hydrochloric acid washing in sequence according to the purification method described in Example 1 to obtain purified single-walled carbon nanotubes.
[0104] The catalyst delivery status, the content of single-walled carbon nanotubes, heterogeneous carbon and metal impurities in the crude product, and the content of single-walled carbon nanotubes, metal impurities and Raman spectroscopy IG / ID in the purified product are listed in Table 1.
[0105] Example 7:
[0106] This embodiment provides a composite catalytic particle, its preparation method, and a method for preparing single-walled carbon nanotubes:
[0107] 1. Select iron-nickel alloy powder (60wt% iron, 40wt% nickel) and lanthanum oxide powder with a D50 particle size of 500nm as the first catalyst component, with a mass ratio of iron-nickel alloy to lanthanum oxide of 85:15. Select selenium powder with a D50 particle size of 2μm as the second catalyst component. Weigh the raw materials according to a ratio of the total molar amount of iron, nickel, and lanthanum metal elements to the molar amount of selenium element of 1:0.2. Based on the total mass of the catalyst components, weigh 0.5wt% of carboxymethyl cellulose.
[0108] 2. Add each catalytic component and carboxymethyl cellulose to a mixer and mix for 2 hours. Then add an ethanol aqueous solution with a mass content of 50 wt% in portions while stirring to obtain a mixture. The amount of the ethanol aqueous solution added is 15 wt% of the mass of the mixture.
[0109] 3. The mixture is granulated using a wet granulator. The granulated material is then screened using a vibrating screen to collect 40-80 mesh particles. The particles are then dried at 80℃ for 12 hours to obtain composite catalytic particles.
[0110] 4. The composite catalyst particles are added to the plasma arc furnace via a screw conveyor, with a conveying rate of 80 g / h. Argon, hydrogen, and methane are introduced into the furnace at a volume flow ratio of 1:0.5:0.1, with a total gas flow rate of 800 L / min. The plasma arc furnace operates at a power of 80 kW, and the reaction zone temperature is 1200℃.
[0111] 5. Collect the crude product containing single-walled carbon nanotubes from the product outlet of the plasma arc furnace, oxidize the crude product at 420°C for 30 min in an oxygen-containing atmosphere with an oxygen volume content of 21%; heat-treat the oxidized product at 800°C for 2 h in a nitrogen atmosphere; acid-wash the heat-treated product with 1 mol / L hydrochloric acid at 70°C for 12 h; then wash with water, filter and dry to obtain purified single-walled carbon nanotubes.
[0112] The catalyst delivery status, the content of single-walled carbon nanotubes, heterogeneous carbon and metal impurities in the crude product, and the content of single-walled carbon nanotubes, metal impurities and Raman spectroscopy IG / ID in the purified product are listed in Table 1.
[0113] Example 8:
[0114] This embodiment provides a composite catalytic particle, its preparation method, and a method for preparing single-walled carbon nanotubes:
[0115] 1. Select iron-nickel alloy powder (60wt% iron, 40wt% nickel) and lanthanum oxide powder with a D50 particle size of 500nm as the first catalyst component, with a mass ratio of iron-nickel alloy to lanthanum oxide of 85:15. Select sulfur powder and selenium powder with a D50 particle size of 2μm as the second catalyst component, with a molar ratio of sulfur to selenium of 1:1. Weigh the raw materials according to a ratio of the total molar amount of iron, nickel, and lanthanum metal elements to the total molar amount of sulfur and selenium elements of 1:2. Based on the total mass of the catalyst components, weigh 0.5wt% of carboxymethyl cellulose.
[0116] 2. Add each catalytic component and carboxymethyl cellulose to a mixer and mix for 2 hours. Then add an ethanol aqueous solution with a mass content of 50 wt% in portions while stirring to obtain a mixture. The amount of the ethanol aqueous solution added is 15 wt% of the mass of the mixture.
[0117] 3. The mixture is granulated using a wet granulator. The granulated material is then screened using a vibrating screen to collect 40-80 mesh particles. The particles are then dried at 80℃ for 12 hours to obtain composite catalytic particles.
[0118] 4. The composite catalyst particles are added to the plasma arc furnace via a screw conveyor, with a conveying rate of 80 g / h. Argon, hydrogen, and methane are introduced into the furnace at a volume flow ratio of 1:0.5:0.1, with a total gas flow rate of 800 L / min. The plasma arc furnace operates at a power of 80 kW, and the reaction zone temperature is 1200℃.
[0119] 5. Collect the crude product containing single-walled carbon nanotubes from the product outlet of the plasma arc furnace, oxidize the crude product at 420°C for 30 min in an oxygen-containing atmosphere with an oxygen volume content of 21%; heat-treat the oxidized product at 800°C for 2 h in a nitrogen atmosphere; acid-wash the heat-treated product with 1 mol / L hydrochloric acid at 70°C for 12 h; then wash with water, filter and dry to obtain purified single-walled carbon nanotubes.
[0120] The catalyst delivery status, the content of single-walled carbon nanotubes, heterogeneous carbon and metal impurities in the crude product, and the content of single-walled carbon nanotubes, metal impurities and Raman spectroscopy IG / ID in the purified product are listed in Table 1.
[0121] Comparative Example 1:
[0122] This comparative example is used to investigate the effects of rare earth modified component lanthanum oxide on the reaction performance of composite catalytic particles and the composition of single-walled carbon nanotube products.
[0123] Except for the absence of lanthanum oxide powder in the main catalytic component, all other process conditions were the same as in Example 1.
[0124] Specifically, iron-nickel alloy powder (60 wt% iron, 40 wt% nickel) with a D50 particle size of 500 nm was selected, and sulfur powder with a D50 particle size of 2 μm was also selected. The iron-nickel alloy powder and sulfur powder were weighed according to a total molar ratio of iron and nickel to sulfur of 1:0.2. Based on the total mass of the iron-nickel alloy powder and sulfur powder, 0.5 wt% of carboxymethyl cellulose was weighed as a binder.
[0125] Iron-nickel alloy powder, sulfur powder, and carboxymethyl cellulose were added to a mixer and mixed for 2 hours. Then, an ethanol aqueous solution with a mass content of 50 wt% was added in portions while stirring to obtain a mixture. The amount of ethanol aqueous solution added was 15 wt% of the mass of the mixture.
[0126] The mixture was added to a wet granulator for granulation. The particles of 40-80 mesh were screened and collected using a vibrating screen and dried at 80°C for 12 h to obtain comparative composite catalytic particles without lanthanum oxide.
[0127] The composite catalyst particles were fed into the plasma arc furnace via a screw conveyor, with a catalyst delivery rate of 80 g / h. Argon, hydrogen, and methane were introduced into the furnace at a volumetric flow rate ratio of 1:0.5:0.1, with a total reaction gas flow rate of 500 L / min. The plasma arc furnace was operated at a power of 80 kW, and the reaction zone temperature was set to 1200℃. The crude product containing single-walled carbon nanotubes was collected from the product outlet of the plasma arc furnace.
[0128] The crude product was subjected to oxygen-containing atmosphere oxidation, nitrogen-containing atmosphere heat treatment, and hydrochloric acid washing in sequence according to the purification method described in Example 1 to obtain the purified product.
[0129] The catalyst delivery status, the content of single-walled carbon nanotubes, heterogeneous carbon and metal impurities in the crude product, and the content of single-walled carbon nanotubes, metal impurities and Raman spectroscopy IG / ID in the purified product are listed in Table 1.
[0130] This comparative example is compared with Example 1 to evaluate the effects of the lanthanum oxide modified component on the high-temperature stability of the composite catalyst particles, the composition of the crude product, and the structural integrity of the purified product.
[0131] Comparative Example 2:
[0132] This comparative example is used to investigate the effects of sulfur as a second catalytic component on the state of composite catalytic particles, the formation of single-walled carbon nanotubes, and the formation of non-target carbon components.
[0133] Except for the absence of sulfur powder, the types of raw materials, wet granulation conditions, plasma arc reaction conditions, and purification conditions are the same as in Example 1.
[0134] Specifically, iron-nickel alloy powder and lanthanum oxide powder with a D50 particle size of 500 nm were selected; the iron-nickel alloy powder contained 60 wt% iron and 40 wt% nickel; the mass ratio of iron-nickel alloy powder to lanthanum oxide powder was 85:15. Based on the total mass of iron-nickel alloy powder and lanthanum oxide powder, 0.5 wt% carboxymethyl cellulose was weighed as a binder.
[0135] Iron-nickel alloy powder, lanthanum oxide powder, and carboxymethyl cellulose were added to a mixer and mixed for 2 hours. Then, an ethanol aqueous solution with a mass content of 50 wt% was added in portions while stirring to obtain a mixture. The amount of ethanol aqueous solution added was 15 wt% of the mass of the mixture.
[0136] The mixture was added to a wet granulator for granulation. The particles of 40-80 mesh were screened and collected by a vibrating screen and dried at 80°C for 12 h to obtain comparative composite catalytic particles that do not contain sulfur as the second catalytic component.
[0137] The composite catalyst particles were fed into the plasma arc furnace via a screw conveyor, with a catalyst delivery rate of 80 g / h. Argon, hydrogen, and methane were introduced into the furnace at a volumetric flow rate ratio of 1:0.5:0.1, with a total reaction gas flow rate of 500 L / min. The plasma arc furnace was operated at a power of 80 kW, and the reaction zone temperature was set to 1200℃. The crude product containing single-walled carbon nanotubes was collected from the product outlet of the plasma arc furnace.
[0138] The crude product was subjected to oxygen-containing atmosphere oxidation, nitrogen-containing atmosphere heat treatment, and hydrochloric acid washing in sequence according to the purification method described in Example 1 to obtain the purified product.
[0139] The catalyst delivery status, the content of single-walled carbon nanotubes, heterogeneous carbon and metal impurities in the crude product, and the content of single-walled carbon nanotubes, metal impurities and Raman spectroscopy IG / ID in the purified product are listed in Table 1.
[0140] This comparative example was compared with Example 1 to evaluate the effect of sulfur as a second catalytic component on the content of single-walled carbon nanotubes, impurity carbon, residual metal content, and the structural quality of the purified product in the crude product.
[0141] Comparative Example 3:
[0142] This comparative example is used to investigate the effects of wet granulation on catalyst delivery stability, synchronous delivery of components, and the composition of single-walled carbon nanotube products.
[0143] According to the raw material types and proportions of Example 1, iron-nickel alloy powder, lanthanum oxide powder, sulfur powder, and carboxymethyl cellulose were weighed. Specifically, the iron-nickel alloy powder contained 60 wt% iron and 40 wt% nickel; the mass ratio of iron-nickel alloy powder to lanthanum oxide powder was 85:15; the ratio of the total molar amount of metal elements to the molar amount of sulfur was 1:0.2; and the amount of carboxymethyl cellulose was 0.5 wt% of the total mass of the above catalytic components.
[0144] The above raw materials were added to a mixer and mixed for 2 hours to obtain a mixed powder. Unlike Example 1, this comparative example did not add an aqueous ethanol solution, nor did it undergo wet granulation, vibrating sieving, or drying. The mixed powder was directly used as a comparative catalyst.
[0145] The comparative catalyst was added to the plasma arc furnace via a screw conveyor, with the catalyst conveying rate set at 80 g / h. During the conveying process, the conveying rate of the mixed powder fluctuated significantly, and material feeding stagnation occurred. Analysis suggests that the mixed powder has poor flowability and is prone to bridging in the hopper, thus affecting the continuity of material flow from the hopper into the screw conveyor.
[0146] Argon, hydrogen, and methane were introduced into the furnace at a volumetric flow rate ratio of 1:0.5:0.1, with a total reaction gas flow rate of 500 L / min. The plasma arc furnace was controlled at a power of 80 kW and a reaction zone temperature of 1200℃. The crude product containing single-walled carbon nanotubes was collected from the product outlet of the plasma arc furnace. Due to significant fluctuations in the actual catalyst delivery rate and unstable catalyst supply within the reaction zone, the product collection rate fluctuated.
[0147] The crude product was subjected to oxygen-containing atmosphere oxidation, nitrogen-containing atmosphere heat treatment, and hydrochloric acid washing in sequence according to the purification method described in Example 1 to obtain the purified product.
[0148] The catalyst delivery status, the content of single-walled carbon nanotubes, heterogeneous carbon and metal impurities in the crude product, and the content of single-walled carbon nanotubes, metal impurities and Raman spectroscopy IG / ID in the purified product are listed in Table 1.
[0149] This comparative example is compared with Example 1 to evaluate the effect of wet granulation on catalyst flowability, transport stability and composition of crude single-walled carbon nanotube products.
[0150] Comparative Example 4:
[0151] This comparative example is used to investigate the effect of the ratio of total molar amount of metal elements to molar amount of sulfur element being less than 1:0.2 on the reaction performance of composite catalytic particles and the composition of single-walled carbon nanotube products.
[0152] Except for the addition of the second catalytic component, sulfur powder, which was weighed according to the ratio of the total molar amount of iron, nickel, and lanthanum metal elements to the molar amount of sulfur element of 1:0.1, the other raw material types, proportions, wet granulation conditions, plasma arc reaction conditions, and purification conditions were the same as in Example 1.
[0153] Specifically, iron-nickel alloy powder (60wt% iron, 40wt% nickel) with a D50 particle size of 500nm and lanthanum oxide powder were selected as the first catalyst component, with a mass ratio of 85:15. Sulfur powder with a D50 particle size of 2μm was selected as the second catalyst component. The iron-nickel alloy powder, lanthanum oxide powder, and sulfur powder were weighed according to a molar ratio of total iron, nickel, and lanthanum metal elements to sulfur element of 1:0.1. Based on the total mass of the catalyst components, 0.5wt% of carboxymethyl cellulose was weighed as a binder.
[0154] Iron-nickel alloy powder, lanthanum oxide powder, sulfur powder, and carboxymethyl cellulose were added to a mixer and mixed for 2 hours. Then, an ethanol aqueous solution with a mass content of 50 wt% was added in portions while stirring to obtain a mixture. The amount of ethanol aqueous solution added was 15 wt% of the mass of the mixture.
[0155] The mixture was added to a wet granulator for granulation. The particles were screened and collected using a vibrating screen with a mesh size of 40-80. The particles were dried at 80°C for 12 hours to obtain the comparative composite catalytic particles.
[0156] The comparative composite catalyst particles were added to the plasma arc furnace via a screw conveyor, with the catalyst delivery rate set at 80 g / h. Argon, hydrogen, and methane were introduced into the furnace at a volumetric flow rate ratio of 1:0.5:0.1, with a total reaction gas flow rate of 800 L / min. The plasma arc furnace was controlled at a power of 80 kW and a reaction zone temperature of 1200 °C. The crude product containing single-walled carbon nanotubes was collected from the product outlet of the plasma arc furnace.
[0157] The crude product was subjected to oxygen-containing atmosphere oxidation, nitrogen-containing atmosphere heat treatment, and hydrochloric acid washing in sequence according to the purification method described in Example 1 to obtain the purified product.
[0158] The catalyst delivery status, the content of single-walled carbon nanotubes, heterogeneous carbon and metal impurities in the crude product, and the content of single-walled carbon nanotubes, metal impurities and Raman spectroscopy IG / ID in the purified product are listed in Table 1.
[0159] This comparative example is compared with Examples 1 and 8 to evaluate the effect of a ratio of total molar amount of metal elements to molar amount of sulfur elements of less than 1:0.2 on the content of single-walled carbon nanotubes, impurity carbon, residual metal content and the structural quality of purified products in the crude product.
[0160] Comparative Example 5:
[0161] This comparative example is used to investigate the effect of the ratio of total molar amount of metal elements to molar amount of sulfur element being higher than 1:2 on the reaction performance of composite catalytic particles and the composition of single-walled carbon nanotube products.
[0162] Except for the addition of the second catalytic component, sulfur powder, which was weighed according to the ratio of the total molar amount of iron, nickel, and lanthanum metal elements to the molar amount of sulfur element of 1:3, the other raw material types, proportions, wet granulation conditions, plasma arc reaction conditions, and purification conditions were the same as in Example 1.
[0163] Specifically, iron-nickel alloy powder (60wt% iron, 40wt% nickel) with a D50 particle size of 500nm and lanthanum oxide powder were selected as the first catalyst component, with a mass ratio of 85:15 between the iron-nickel alloy powder and the lanthanum oxide powder. Sulfur powder with a D50 particle size of 2μm was selected as the second catalyst component. The iron-nickel alloy powder, lanthanum oxide powder, and sulfur powder were weighed according to a molar ratio of the total molar amount of iron, nickel, and lanthanum metal elements to the molar amount of sulfur element of 1:3. Based on the total mass of the catalyst components, 0.5wt% of carboxymethyl cellulose was weighed as a binder.
[0164] Iron-nickel alloy powder, lanthanum oxide powder, sulfur powder, and carboxymethyl cellulose were added to a mixer and mixed for 2 hours. Then, an ethanol aqueous solution with a mass content of 50 wt% was added in portions while stirring to obtain a mixture. The amount of ethanol aqueous solution added was 15 wt% of the mass of the mixture.
[0165] The mixture was added to a wet granulator for granulation. The particles were screened and collected using a vibrating screen with a mesh size of 40-80. The particles were dried at 80°C for 12 hours to obtain the comparative composite catalytic particles.
[0166] The comparative composite catalyst particles were added to the plasma arc furnace via a screw conveyor, with the catalyst delivery rate set at 80 g / h. Argon, hydrogen, and methane were introduced into the furnace at a volumetric flow rate ratio of 1:0.5:0.1, with a total reaction gas flow rate of 800 L / min. The plasma arc furnace was controlled at a power of 80 kW and a reaction zone temperature of 1200 °C. The crude product containing single-walled carbon nanotubes was collected from the product outlet of the plasma arc furnace.
[0167] The crude product was subjected to oxygen-containing atmosphere oxidation, nitrogen-containing atmosphere heat treatment, and hydrochloric acid washing in sequence according to the purification method described in Example 1 to obtain the purified product.
[0168] The catalyst delivery status, the content of single-walled carbon nanotubes, heterogeneous carbon and metal impurities in the crude product, and the content of single-walled carbon nanotubes, metal impurities and Raman spectroscopy IG / ID in the purified product are listed in Table 1.
[0169] This comparative example is compared with Examples 1 and 8 to evaluate the effect of a ratio of total molar amount of metal elements to molar amount of sulfur elements higher than 1:2 on the content of single-walled carbon nanotubes, impurity carbon, residual metal content, and the structural quality of the purified product in the crude product.
[0170] Test method:
[0171] 1. The conveying stability of the composite catalyst particles was characterized using a cumulative metering method. A single counting cycle was set to 2 minutes, and the actual decrease in material (m) in the catalyst silo and the theoretical feed rate (M) of the screw conveyor were recorded during this cycle. The arithmetic mean of the conveying deviation rate (δ) over 5 counting cycles was calculated using the following formula, which was taken as the catalyst conveying rate error:
[0172]
[0173] 2. Thermogravimetric analysis (TGA) was performed according to the method specified in GB / T 32868-2016, under an air atmosphere. The mass fractions of single-walled carbon nanotubes and impurities were calculated based on the oxidation weight loss behavior of the samples in different temperature ranges; the residual mass after the TGA was taken as the mass fraction of metallic impurities. The sum of the mass fractions of single-walled carbon nanotubes, impurities, and metallic impurities was 100 wt%.
[0174] 3. Raman spectroscopy tests were performed according to the methods specified in GB / T 32871-2016:
[0175] 4. Scanning electron microscopy tests were performed according to the methods specified in GB / T 30543-2014:
[0176] 5. Transmission electron microscopy tests were performed according to the methods specified in GB / T 32869-2016:
[0177] The content of single-walled carbon nanotubes, impurity carbon, and metal content in the product, along with the Raman spectroscopy results, are shown in Table 1.
[0178] Table 1 Test Results
[0179]
[0180] Furthermore, as shown in Table 1, the catalyst delivery rate error in Examples 1-8 was 0.22%-0.38%, all significantly lower than the 18.6% error in Comparative Example 3 before granulation. The crude product contained 80.6 wt%-94.0 wt% single-walled carbon nanotubes, 3.9 wt%-11.2 wt% impurities, and 2.1 wt%-8.7 wt% metal impurities. After purification, the single-walled carbon nanotube content was 99.1 wt%-99.8 wt%, the metal impurity content was 0.2 wt%-0.9 wt%, and the IG / ID ratio was 118.6-142.5. In contrast, the crude products in Comparative Examples 1-5 contained only 32.2 wt%-64.5 wt% single-walled carbon nanotubes, 21.1 wt%-50.4 wt% impurities, and 12.9 wt%-18.9 wt% metal impurities, with a purified IG / ID ratio of only 82.6-93.5. It is evident that the composite catalytic particles of this application can significantly improve the content and purity of single-walled carbon nanotubes, reduce impurities such as mixed carbon and metals, and improve the structural integrity of the purified product in the plasma arc method.
[0181] Compared to Comparative Example 1, Example 1, under the same granulation and reaction conditions, contained lanthanum oxide as part of the first catalytic component. The crude product of Comparative Example 1 contained 62.3 wt% single-walled carbon nanotubes, 22.3 wt% impurities, and 15.4 wt% metal impurities, with an IG / ID of 92.1 after purification. In contrast, the crude product of Example 1 contained 93.6 wt% single-walled carbon nanotubes, while impurities and metal impurities decreased to 4.2 wt% and 2.2 wt%, respectively, and the IG / ID increased to 142.5 after purification. This indicates that at least one of yttrium, cerium, lanthanum, molybdenum, and tungsten in the first catalytic component, combined with at least one of iron, cobalt, and nickel, can regulate the phase composition, surface state, and metal-carbon interface state of the composite catalytic particles, inhibiting the high-temperature migration and aggregation of active metals, thereby promoting the formation of single-walled carbon nanotubes and reducing non-target carbon components.
[0182] Compared to Comparative Example 2, Example 1 contains sulfur as a second catalytic component. In the crude product of Comparative Example 2, the content of single-walled carbon nanotubes was only 48.6 wt%, the content of impure carbon was 32.5 wt%, and the content of metal impurities was 18.9 wt%, with an IG / ID of 88.4 after purification. In contrast, in the crude product of Example 1, the content of single-walled carbon nanotubes increased to 93.6 wt%, while the content of impure carbon and metal impurities decreased to 4.2 wt% and 2.2 wt%, respectively, and the IG / ID increased to 142.5 after purification. This indicates that at least one of the second catalytic components, sulfur and selenium, is necessary for regulating the surface energy of the composite catalytic particles, maintaining effective catalytic sites, and promoting carbon deposition.
[0183] Compared to Comparative Example 3, Example 1 used wet granulation to form composite catalyst particles. Comparative Example 3 directly used mixed powder, resulting in a delivery rate error as high as 18.6%. The crude product contained only 32.2 wt% single-walled carbon nanotubes, 50.4 wt% impurities, and 17.4 wt% metal impurities, with an IG / ID ratio of only 82.6 after purification. In contrast, Example 1 reduced the delivery rate error to 0.35%, increased the single-walled carbon nanotube content in the crude product to 93.6 wt%, reduced impurities and metal impurities to 4.2 wt% and 2.2 wt%, respectively, and increased the IG / ID ratio to 142.5 after purification. This demonstrates that wet granulation, which fixes the main and secondary catalyst components within the same particle, can reduce powder dust, agglomeration, and component segregation, improve the stability of continuous screw conveying, and ensure that each component participates in the reaction in a relatively stable proportion within the reaction zone.
[0184] Compared to Comparative Example 4, the ratio of total metal molar content to sulfur molar content in Example 1 was 1:0.2, while in Comparative Example 4 it was 1:0.1. The crude product of Comparative Example 4 contained only 56.2 wt% single-walled carbon nanotubes, with impurities of 30.9 wt% and 12.9 wt% respectively, and an IG / ID ratio of only 88.4 after purification. In contrast, the crude product of Example 1 contained 93.6 wt% single-walled carbon nanotubes, with impurities of 4.2 wt% and 2.2 wt% respectively, and an IG / ID ratio of 142.5 after purification. This indicates that insufficient sulfur / selenium content is insufficient to regulate the surface energy of the composite catalytic particles and the carbon precipitation conditions, making it difficult to obtain single-walled carbon nanotubes with high content and low impurities.
[0185] Compared to Comparative Example 5, the ratio of total metal molar content to total sulfur and selenium molar content in Example 8 was 1:2, while in Comparative Example 5 it was 1:3. The crude product of Comparative Example 5 contained 64.5 wt% single-walled carbon nanotubes, 21.1 wt% impurities, and 14.4 wt% metal impurities, with an IG / ID of 93.5 after purification. In contrast, the crude product of Example 8 contained 90.5 wt% single-walled carbon nanotubes, 6.0 wt% impurities, and 3.5 wt% metal impurities, with an IG / ID of 120.1 after purification. This indicates that excessively high sulfur / selenium content can occupy the surface of active metals, reducing the number of effective catalytic sites and leading to a decrease in catalytic efficiency.
[0186] As shown in Examples 2-6, different combinations of iron powder and cerium oxide, iron-molybdenum alloy and cerium oxide, nickel-yttrium alloy and cerium oxide, cobalt-nickel alloy and lanthanum oxide, and iron-tungsten alloy and cerium oxide are used as the first catalytic component. Sulfur, selenium, or a mixture of sulfur and selenium are used as the second catalytic component. Polyvinyl alcohol, carboxymethyl cellulose, or gelatin are used as the binder. Methane, ethane, ethylene, or a mixture of methane and carbon monoxide are used as the gaseous carbon source. All of these methods can produce single-walled carbon nanotubes. The single-walled carbon nanotube content in the crude products of Examples 2-6 is 80.6 wt%–90.6 wt%, and the content after purification is 99.1 wt%–99.5 wt%. The content of metal impurities after purification is 0.5 wt%–0.9 wt%, and the IG / ID ratio after purification is 120.3–136.8. This demonstrates that the first catalytic component, second catalytic component, binder, and process conditions defined in this application have a wide range of feasibility and are not limited to a specific alloy or a specific carbon source.
[0187] As shown in Example 7, when the second catalytic component is selenium and the ratio of total metal molar amount to selenium element molar amount is 1:0.2, the crude product contains 94.0 wt% single-walled carbon nanotubes, 3.9 wt% impurities, and 2.1 wt% metal impurities. The purified IG / ID ratio is 134.6, which is comparable to the effect achieved when sulfur was used in Example 1. As shown in Example 8, when the second catalytic component is a mixture of sulfur and selenium and the ratio of total metal molar amount to total sulfur and selenium molar amount is 1:2, the crude product contains 90.5 wt% single-walled carbon nanotubes, 6.0 wt% impurities, and 3.5 wt% metal impurities. The purified IG / ID ratio is 120.1. This demonstrates that the second catalytic component includes at least one of sulfur and selenium, and a mixture of sulfur and selenium can achieve the desired catalytic effect.
[0188] In summary, this application does not improve the preparation effect of single-walled carbon nanotubes solely through a single component or process condition. Instead, it achieves this through the synergistic effect of combining the active metal in the first catalytic component with at least one of yttrium, cerium, lanthanum, molybdenum, and tungsten; adjusting the second catalytic component with at least one of sulfur and selenium; maintaining a metal-to-sulfur / selenium molar ratio of 1:0.1–3; and wet granulation to form composite catalytic particles for use in the plasma arc method. This solves the problems of component segregation, unstable transport, and high-temperature agglomeration that easily occur in existing powder catalysts during the continuous plasma arc preparation of single-walled carbon nanotubes. Comparative Example 1 lacks rare earth / refractory metal modification components, Comparative Example 2 lacks sulfur / selenium as the second catalytic component, Comparative Example 3 did not undergo wet granulation, and the metal-to-sulfur / selenium molar ratios in Comparative Examples 4 and 5 deviate from the preferred range. None of these examples simultaneously yielded products with high single-walled carbon nanotube content, low impurity carbon content, low metal impurity content, and high IG / ID after purification. This demonstrates that the technical solution of this application has outstanding substantive features and significant progress.
[0189] Finally, it should be noted that although the above embodiments have been described in the text and drawings of this application, this should not limit the scope of patent protection of this application. Any technical solutions that are based on the essential concept of this application and utilize the content described in the text and drawings of this application, resulting in equivalent structural or procedural substitutions or modifications, as well as the direct or indirect application of the technical solutions of the above embodiments to other related technical fields, are all included within the scope of patent protection of this application.
Claims
1. A composite catalytic particle, characterized in that, The composite catalytic particles comprise: a catalytic component and a binder; the catalytic component comprises a first catalytic component and a second catalytic component; The first catalytic component includes at least one of iron, cobalt, and nickel, wherein the total mass of iron, cobalt, and nickel accounts for 70 wt% to 98 wt% of the total mass of the catalytic component. and At least one of yttrium, cerium, lanthanum, molybdenum, and tungsten, wherein the total mass of said yttrium, cerium, lanthanum, molybdenum, and tungsten accounts for 5 wt% to 30 wt% of the total mass of the catalytic components; The second catalytic component includes at least one of sulfur and selenium; The ratio of the total molar amount of iron, cobalt, nickel, yttrium, cerium, lanthanum, molybdenum and tungsten metals to the total molar amount of sulfur and selenium is 1:0.2 to 2.
2. The composite catalytic particles according to claim 1, characterized in that, The first catalytic component includes at least one of iron-nickel alloy, cobalt-nickel alloy, iron-cobalt alloy, and iron-cobalt-nickel alloy.
3. The composite catalytic particles according to claim 1, characterized in that, The first catalytic component includes at least one of yttrium oxide, cerium oxide, lanthanum oxide, iron-yttrium alloy, nickel-yttrium alloy, iron-cerium alloy, iron-lanthanum alloy, iron-molybdenum alloy, iron-tungsten alloy, nickel-molybdenum alloy, and nickel-tungsten alloy.
4. The composite catalytic particles according to claim 1, characterized in that, The binder includes at least one of carboxymethyl cellulose, polyvinyl alcohol, phenolic resin and gelatin; the mass of the binder is 0.1 to 3.0 wt% of the total mass of the catalytic components.
5. The composite catalytic particles according to claim 1, characterized in that, The particle size of the composite catalytic particles is 40-80 mesh.
6. The method for preparing composite catalytic particles according to any one of claims 1 to 5, characterized in that, Includes the following steps: The catalytic components and binder are mixed and stirred for 0.5 to 4 hours to obtain a first mixture; 50 wt% ethanol aqueous solution is added to the first mixture and stirred to obtain a second mixture; the second mixture is wet granulated, sieved, and dried to obtain the composite catalytic particles; the amount of ethanol aqueous solution added is 5 to 30 wt% of the first mixture.
7. The preparation method according to claim 6, characterized in that, The D50 particle size of the first catalytic component is 100–500 nm, and the D50 particle size of the second catalytic component is 1–3 μm.
8. The preparation method according to claim 6, characterized in that, The amount of the ethanol aqueous solution added is 10-20 wt% of the first mixture.
9. A method for preparing single-walled carbon nanotubes by plasma arc method, characterized in that, The method uses the composite catalytic particles described in any one of claims 1-5.
10. The method according to claim 9, characterized in that, The method includes the following steps: S1: The composite catalytic particles are continuously conveyed to the plasma arc furnace at a rate of 10-500 g / h via a screw conveyor. S2: Argon, hydrogen and gaseous carbon source are introduced into the plasma arc furnace, wherein the volume flow rate ratio of argon, hydrogen and gaseous carbon source is 1:0.1-3:0.05-1; S3: Control the working power of the plasma arc furnace to be 50-200 kW, the temperature of the reaction zone to be 1000-1500℃, and the total flow rate of the reaction gas to be 100-2000 L / min; S4: Collect the crude product containing single-walled carbon nanotubes from the product outlet of the plasma arc furnace.