A low octane loss high selectivity FCC gasoline hydrodesulfurization catalyst, and a preparation method and application thereof
By using a ternary composite support and multi-metal synergistic technology, a highly selective FCC gasoline hydrodesulfurization catalyst was constructed, which solved the problems of catalyst selectivity and stability, and achieved efficient desulfurization and octane number retention, making it suitable for deep refining of FCC gasoline.
Patent Information
- Application Number
- CN202611214195.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-11
- Publication Date
- 2026-11-20
AI Technical Summary
Existing FCC gasoline hydrodesulfurization catalysts suffer from poor catalytic selectivity, excessive hydrogenation of olefins leading to significant octane number loss, poor stability, and weak resistance to poisoning and coking, making it difficult to meet the clean gasoline requirements of China VI and higher standards.
A bifunctional catalytic system was constructed by synergistic combination of ternary composite support, acidic modifier, multi-metal active component and anti-sulfur functional agent. Through the synergistic effect of anatase support, acidic site regulation by phosphoric acid, Ni-Co-Mo metal system and Mn-Ce solid solution, highly selective desulfurization and olefin isomerization were achieved, and the stability and anti-poisoning performance of the catalyst were improved.
It achieves deep desulfurization of FCC gasoline, with an octane number loss of less than 0.8 units, a catalyst life increase of 30%-50%, meets the ultra-clean gasoline standard, and reduces operation and maintenance costs.
Smart Images

Figure CN123128022A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of catalysts for petrochemical oil refining. Background Technology
[0002] FCC (fluid catalytic cracking) gasoline is a core component of the domestic refined oil gasoline pool, accounting for more than 70% of the total commercial gasoline and is the core raw material for refinery gasoline production.
[0003] However, FCC gasoline itself has the drawback of high sulfur and olefin content. The sulfur compounds mainly exist in the form of thiophene organic sulfur, and the olefin content generally reaches 30%-40%. It cannot directly meet the sulfur and olefin content requirements of China VI and higher standards for clean gasoline, and must be upgraded and refined through selective hydrodesulfurization process.
[0004] Currently, the mainstream commercial hydrodesulfurization catalyst in industry is the traditional CoMo / Catalysts, while possessing certain hydrodesulfurization activity, suffer from three major industrial shortcomings, which have become long-term technical bottlenecks in the industry: 1. Poor catalytic selectivity. While removing organic sulfur through hydrotreating, it is prone to olefin oversaturation hydrogenation reaction, causing a significant decrease in gasoline RON (Research Octane Number). Under normal industrial conditions, the octane number loss can be as high as 1.0-1.5 units, which seriously reduces gasoline quality and product added value. 2. The catalyst has poor stability and is single-element. The support is prone to hydration phase transition and pore collapse and blockage in a hydrogenated water vapor environment. At the same time, the active metal is prone to agglomeration and sintering, which leads to rapid decay of catalyst activity. 3. Weak resistance to poisoning and coking: Trace amounts of sulfides and gums in FCC gasoline can easily cause sulfur poisoning and surface coking of the catalyst, significantly shortening the catalyst's service life. The industrial service life of traditional catalysts is only about 3 years, resulting in high replacement frequency and high maintenance costs.
[0005] Existing improved catalysts mostly optimize the metal ratio or support components, which can only slightly improve desulfurization activity. They do not solve the root cause of traditional single-support catalysts' "uncontrollable acidity, poor metal dispersion, and lack of isomerization active centers" at the microscopic mechanism level. They cannot solve the core contradiction between "high desulfurization rate" and "low octane number loss" at the reaction mechanism level, and their resistance to sulfur poisoning and hydration is only slightly improved.
[0006] While imported high-end catalysts such as the Axens HR series outperform domestic catalysts, they suffer from high procurement costs, long delivery cycles, and poor compatibility with feedstocks in domestic refineries. Therefore, there is an urgent need for an FCC gasoline hydrodesulfurization catalyst that is independently controllable, highly selective, has low octane number loss, and a long lifespan, so as to achieve technological catch-up with imported commercial catalysts and domestic substitution. Summary of the Invention
[0007] The purpose of this invention is to provide a low-octane-loss, high-selectivity FCC gasoline hydrodesulfurization catalyst, its preparation method, and its application. This catalyst can achieve deep desulfurization of FCC gasoline while maximizing the retention of olefin components and offsetting octane-loss. It balances high desulfurization activity, high hydrodesulfurization selectivity, and high operational stability, enabling domestic substitution of the catalyst. Furthermore, it has a simple structure, is easy to use, and solves the industrial pain points of existing catalysts, such as excessive olefin hydrogenation, large octane-loss, poor structural stability, easy sulfur poisoning and coking, and short service life.
[0008] The core innovation of this invention lies in the synergistic gain effect generated by multi-dimensional technology coupling, specifically including four core innovative coupling mechanisms: (1) Synergistic mechanism of ternary carriers: Provides a large-pore framework to ensure mass transfer efficiency; anatase type This generates strong metal-support interactions, promoting the formation of type II active phases; To improve the hydrophobic stability of the carrier and suppress pore collapse and phase transition in a hydrogenated water vapor environment; (2) Mechanism of acidification by dual auxiliary agents: Phosphoric acid regulates the number of strongly acidic sites in the carrier. By passivating strong acid sites and weakening the oversaturated hydrogenation activity of olefins, the isomerization center of the olefin skeleton is precisely constructed to achieve a dual reaction balance of "desulfurization and hydrogenation" and "isomerization to maintain octane number". (3) Trimetallic synergistic mechanism: The Ni-Co-Mo molar ratio of 3:2:1 can maximize the exposure of MoS2 edge active sites, forming a highly active and selective type II metal sulfide active phase, avoiding the defect of poor selectivity of type I active phase; (4) Solid solution anti-deterioration mechanism: Mn-Ce solid solution has the ability to store and release reversible lattice oxygen, and can oxidize and decompose surface carbon and adsorbed sulfur poisons in situ, realize catalyst self-repair, and greatly improve stability and service life.
[0009] The individual components alone cannot achieve the comprehensive performance of low octane number loss, high desulfurization and high stability required in this application; it is not a simple superposition of conventional technologies.
[0010] To achieve the above objectives, the present invention provides the following technical solution: A low-octane-loss, highly selective FCC gasoline hydrodesulfurization catalyst comprises: a ternary composite support, an acid-modifying additive, a multi-metal active component, and an anti-sulfur functional additive. The ternary composite carrier is composed of Specific surface area is 320-330 m² 2 / g of pure anatase Yttrium-stabilized tetragonal zirconium oxide Composition, in which Pure anatase and The mass ratio is 70:20:10, the Used to improve the hydrophobic resistance to phase transition of the carrier; The acid-modifying auxiliaries include phosphoric acid and phosphoric acid used to synergistically regulate moderately acidic sites, construct olefin skeleton isomerization active centers, and inhibit excessive hydrogenation of olefins. ; The multi-metal active component includes a Ni, Co, and Mo composite metal for preferentially forming a stacked, highly active type II metal sulfide active phase; The anti-sulfur functional additives include Mn-Ce solid solutions used to enhance resistance to sulfur poisoning and coking.
[0011] By adopting the above technical solution, a dual-function catalytic system was constructed through the synergistic combination of ternary composite carrier, acidic modifier, multi-metal active component and anti-sulfur functional additive, achieving a balance between deep desulfurization of FCC gasoline and olefin skeleton isomerization, while efficiently removing sulfides and retaining the octane number to the maximum extent.
[0012] As a further aspect of the present invention: based on the total mass of the ternary composite carrier, it also includes pore-forming agent P123 (polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer) and pseudoboehmite, wherein the amount of P123 added is 8% and the amount of pseudoboehmite added is 5%.
[0013] By adopting the above technical solution, and by adding a specific proportion of pore-forming agent and pseudoboehmite to the carrier, the pore structure distribution and mechanical forming properties of the carrier are optimized, providing a suitable physical environment for the dispersion and loading of active components and for mass and heat transfer during the reaction process.
[0014] As a further aspect of the present invention: based on the total mass of the ternary composite carrier, the amount of phosphoric acid added is 2%, and the... The addition amount is 1%.
[0015] By adopting the above technical solution, the intensity and number of acidic sites on the catalyst surface are precisely controlled by precisely controlling the loading of acidic additives on the support surface, thereby optimizing the olefin skeleton isomerization reaction pathway and further improving the octane number retention rate.
[0016] As a further aspect of the present invention: the molar ratio of Ni, Co and Mo in the multi-metal active component is 3:2:1, and the total metal loading is 12%-15% of the total mass of the ternary composite carrier.
[0017] By adopting the above technical solution and setting a specific molar ratio of active metal components and their loading range, the hydrodesulfurization activity and hydrogenation selectivity of the catalyst are balanced, preventing the oversaturation reaction of olefins caused by excessive metal and reducing octane number loss.
[0018] As a further aspect of the present invention, the doping amount of the Mn-Ce solid solution is 3% of the total mass of the ternary composite carrier.
[0019] By adopting the above technical solution and determining the specific doping amount of the anti-sulfur additive, the catalyst is ensured to have sufficient lattice oxygen cycling capability and surface anti-carbon deposition capability, effectively resisting the attack of raw material poisons on active sites.
[0020] The present invention also discloses a method for preparing the above-mentioned catalyst, comprising the following steps: S1: Preparation of composite support: ... Pure anatase , The mixture is mixed with a pore-forming agent, and then kneaded with a binder. After molding and segmented calcination, a ternary composite carrier is obtained. S2: Acidic modification of the carrier: Using an equal-volume impregnation method, a mixture containing phosphoric acid and... The modified liquid of the precursor is loaded onto the carrier obtained in S1, and acidity regulation is completed by drying and calcination; S3: Active component loading: Prepare an active impregnation solution containing nickel nitrate, cobalt nitrate, ammonium molybdate and Mn-Ce solid solution, and co-impregnate the carrier obtained in S2; S4: Drying and calcining: The impregnated support obtained in S3 is subjected to segmented drying and calcination to obtain an oxidized catalyst precursor; S5: Sulfurization activation: The precursor is subjected to programmed temperature sulfidation in a sulfurization atmosphere to obtain the finished catalyst.
[0021] By adopting the above technical solution, through the step-by-step orderly processing of carrier preparation, acid modification, metal loading, segmented calcination and sulfurization activation, it is ensured that each functional component is stably loaded on the carrier and plays a synergistic role.
[0022] As a further aspect of the present invention: in S1, the segmented calcination process is as follows: the temperature is increased to 200°C at 2°C / min and held for 1 hour, and then increased to 550°C at 3°C / min and held for 4 hours to complete the crystal phase transformation; in S4, the segmented calcination process is as follows: the temperature is increased to 300°C at 2°C / min and held for 1 hour, and then increased to 480°C and held for 3 hours to prevent the active metal from sintering.
[0023] By adopting the above technical solution, the temperature rise program and temperature control point of the carrier preparation and subsequent calcination stages are optimized to regulate the crystal phase transformation process and framework structure stability of the carrier and precursor, thereby preventing pore collapse or active metal sintering caused by high-temperature treatment.
[0024] As a further aspect of the present invention: citric acid is added to the active impregnation solution as a complexing agent, and the amount of citric acid added is 5% of the total mass of the multi-metal active components; the co-impregnation is a closed static impregnation, and the impregnation time is 4 hours.
[0025] By adopting the above technical solution, adding a specific proportion of complexing agent and using a closed static impregnation process, the dispersion uniformity of active metal in the carrier pores is improved, local agglomeration of active components is avoided, thereby improving the utilization rate of active sites in the catalytic reaction.
[0026] As a further aspect of the present invention: the sulfidation atmosphere is air-fuel mixture, airspeed 800 The programmed temperature vulcanization process includes: first, heating to 320℃ for the first stage of vulcanization, and then heating to 380℃ for the second stage of deep vulcanization.
[0027] By adopting the above technical solution and using a specific programmed temperature rise sulfidation process, the degree of sulfidation and crystal structure of the active metal phase can be precisely controlled, so as to promote the complete transformation of the active metal into a highly active type II metal sulfide phase, thereby achieving the best catalytic performance.
[0028] This invention also discloses the application of the above-mentioned catalyst in FCC gasoline hydrodesulfurization refining, under the following operating conditions: reaction pressure 2.0-2.5 MPa, reaction temperature 260-280℃, hydrogen-to-oil volume ratio 300:1, and liquid hourly space velocity 2.0. .
[0029] By adopting the above technical solution, the specific process parameter range for the industrial application of the catalyst is defined, ensuring that under this specific operating window, the catalyst can fully exert its advantages of high desulfurization activity and high selectivity, and achieve optimal industrial refining effect.
[0030] Compared with the prior art, the beneficial effects of the present invention are: 1. The preferred catalyst of this invention has a desulfurization rate of 98.6%, which is significantly better than traditional domestic catalysts and single modified catalysts. Its performance slightly surpasses that of imported commercial catalysts. It can achieve deep desulfurization of FCC gasoline and meet the production standards of ultra-clean gasoline. 2. The acidic isomerization center constructed based on the dual-acid-adjuvant acid-adjusting mechanism effectively offsets the octane number loss caused by olefin hydrogenation. In the preferred embodiment, the RON octane number loss is as low as 0.8 units, which is superior to the mainstream domestic catalysts in the industry and fundamentally solves the industry problem of "desulfurization inevitably leads to a decrease in octane number". 3. The ternary composite support is hydrophobic and resistant to phase transformation. The Mn-Ce solid solution effectively resists sulfur poisoning and coking. There is no significant activity decay after 300 hours of long-term operation. The catalyst has a complete structure and the active metal does not agglomerate or sinter. The industrial service life is 30%-50% longer than that of traditional catalysts. 4. The preparation process of this invention is simple, the parameters are controllable and highly repeatable, there are no special and expensive raw materials, the amount of modified additives is low and the cost is controllable; it is suitable for the characteristics of FCC gasoline feedstocks in domestic refineries, which can significantly reduce the cost of refinery equipment operation and maintenance and additive replacement, and has extremely high industrialization value.
[0031] Other features and advantages of the present invention will be disclosed in detail in the following detailed description and accompanying drawings. Attached Figure Description
[0032] Figure 1 This is a schematic flowchart of the preparation method of a low-octane-loss, high-selectivity FCC gasoline hydrodesulfurization catalyst in an embodiment of the present invention. Detailed Implementation
[0033] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0034] This invention innovatively constructs a dual-functional catalytic system consisting of a "metal hydrogenation active center + acid isomerization center," employing four core technological strategies: composite support structuring, precise acidity modulation, multi-metal synergistic activation, and sulfur and coking resistance modification. With large pore capacity As the framework substrate, it is paired with a high specific surface area anatase. , Constructing a ternary composite carrier and utilizing Electron spillover effect and strong metal-support interaction (SMSI) enhance hydrodesulfurization activity, relying on The hydrophobic stability inhibits the hydration phase transition of the carrier; Through phosphoric acid and Composite modification precisely controls the medium-strength Lewis acid sites in the support to construct olefin skeleton isomerization centers, converting straight-chain low-octane hydrocarbons into branched high-octane hydrocarbons, thus offsetting the octane number loss caused by olefin saturation in situ. Introducing the Ni-Co-Mo trimetallic system forms a highly active type II metal sulfide active phase, enhancing the activity and selectivity of the hydrogenation reaction; Doping with Mn-Ce solid solution to replace traditional single metal oxide additives effectively improves the catalyst's resistance to sulfur self-healing, coking, and poisoning.
[0035] In this invention embodiment, a low-octane-number loss, high-selectivity FCC gasoline hydrodesulfurization catalyst, its preparation method, and its application are described in the following reference: Figure 1 As shown, it includes a ternary composite carrier, an acid-modifying agent, a multi-metal active component, and an anti-sulfur functional agent; the ternary composite carrier is composed of... Anatase , Composition; the acid-modifying agent includes phosphoric acid and The multi-metal active component is a Ni, Co, and Mo composite metal; the anti-sulfur functional additive is a Mn-Ce solid solution. By mass ratio, the ternary composite carrier : Anatase : =70:20:10; Based on the total mass of the ternary composite carrier, the amount of phosphoric acid added is 2%. The addition amount is 1%, the pore-forming agent P123 addition amount is 8%, and the pseudoboehmite addition amount is 5%; The molar ratio of the multimetallic active components Ni, Co, and Mo is 3:2:1, and the total metal loading is 12%-15% of the total mass of the ternary composite carrier. The doping amount of the Mn-Ce solid solution is 3% of the total mass of the ternary composite carrier.
[0036] In one feasible embodiment, the total loading of the multi-metal active component is preferably 13% of the total mass of the ternary composite carrier; citric acid is added as a complexing agent to the metal impregnation solution, and the amount of citric acid added is 5% of the total mass of the multi-metal active component.
[0037] In one feasible embodiment, the anatase type Specific surface area is 325 m² 2 / g, rutile type is not suitable The Yttrium-stabilized zirconium oxide is used to improve the hydrophobic stability and structural strength of the carrier.
[0038] In one feasible embodiment, the catalyst of the present invention is a preferred, pilot-scale, and feasible formulation, and the component ratio has been verified by mechanism and optimized by experiments, as follows: (1) Ternary composite carrier: : Anatase : Mass ratio = 70:20:10; (2) Carrier modification aids: Based on the total mass of the carrier, P123 pore-forming agent 8%, phosphoric acid 2%, pseudoboehmite 5%, 1%; (3) Active metal components: Ni:Co:Mo molar ratio = 3:2:1, total loading 13% (preferred value), citric acid complexing agent added at 5% of the total metal mass; (4) Functional additives: The amount of Mn-Ce solid solution doped is 3% of the total mass of the carrier.
[0039] A method for preparing a low-octane-number loss, high-selectivity FCC gasoline hydrodesulfurization catalyst employs a stepwise, controllable process involving support preparation, acid modification, metal loading, staged calcination, and programmed sulfidation. This process avoids defects such as metal agglomeration, pore collapse, and acid loss throughout, exhibiting strong process stability and high repeatability, making it suitable for industrial scale-up. The method includes the following steps: S1. Preparation of ternary composite carrier: Weigh according to the ratio. Anatase , Add P123 pore-forming agent and deionized water, and stir in a constant temperature water bath at 40℃ for 2 hours to obtain a uniform suspension slurry; add boehmite to the slurry, add 3%-5% dilute nitric acid solution dropwise and stir for 30 minutes to perform cross-linking and mixing to obtain a plastic paste material; extrude the paste material into 1.5mm strip carriers, air dry at room temperature for 2 hours, and dry at 110℃ for 4 hours; calcine using a segmented heating process: heat up to 200℃ at 2℃ / min and hold for 1 hour, heat up to 550℃ at 3℃ / min and hold for 4 hours, and then cool naturally to obtain a ternary composite carrier; S2. Pretreatment of carrier acid modification: The ternary composite carrier was impregnated with dilute phosphoric acid solution using the equal volume impregnation method, allowed to stand at room temperature for 3 hours, dried at 120℃ for 2 hours, and calcined at 500℃ for 2 hours to complete the carrier acid regulation modification. Before preparing the catalyst, Mn-Ce solid solution was first prepared: manganese nitrate and cerium nitrate were weighed in molar ratio and dissolved in deionized water. Excess ammonia was added to adjust the pH to 10 and aged at room temperature for 2 hours. After filtration and washing with deionized water, the powder was dried at 110℃ for 12 hours and calcined at 500℃ for 4 hours to obtain Mn-Ce solid solution powder. S3. Preparation of active impregnation solution: Weigh nickel nitrate, cobalt nitrate, and ammonium molybdate according to the molar ratio of Ni:Co:Mo=3:2:1, add deionized water and citric acid complexing agent, stir at room temperature until completely dissolved to obtain a clear metal impregnation solution; add Mn-Ce solid solution powder to the impregnation solution and ultrasonically disperse for 15 min. S4. Equal volume co-impregnation: The acid-modified composite carrier is completely immersed in the impregnation solution and statically impregnated at room temperature for 4 hours in a sealed environment. S5. Segmented drying and calcination: After impregnation, the carrier is air-dried at room temperature for 1 hour, then dried at 100℃ for 3 hours; the temperature is increased to 300℃ at 2℃ / min and held for 1 hour, then the temperature is increased to 480℃ and held for 3 hours, and then cooled to obtain the oxidized catalyst precursor. S6. Programmed temperature rise sulfurization activation: The precursor is loaded into a fixed-bed reactor, and high-purity nitrogen is introduced. Purge for 30 minutes, dry at 150℃ for 1 hour; switch to 5% air-fuel mixture, airspeed 800 The temperature is increased to 320℃ at 3℃ / min for 4 hours for sulfurization, and then increased to 380℃ for deep sulfurization for 2 hours. After natural cooling and passivation, the finished catalyst is obtained.
[0040] In one feasible embodiment, silica sol binder should not be used throughout the molding process to avoid clogging the carrier's mesopores.
[0041] In one feasible embodiment, the metal impregnation process is a closed static impregnation, which should not be stirred or shaken, to ensure uniform loading of metal and additives.
[0042] An application of the catalyst in FCC gasoline hydrodesulfurization refining, wherein the operating conditions are as follows: fixed-bed reactor, reaction pressure 2.0-2.5 MPa, reaction temperature 260-280℃, hydrogen-to-oil volume ratio 300:1, and liquid hourly space velocity 2.0. .
[0043] In one feasible embodiment, the weighing mass of the metal salt in S3 is... The calculation needs to be based on the target load, and the formula is as follows:
[0044] in, For carrier quality, The target total metal loading (13%) Here are the coefficients for each metal in the molar ratio: Ni = 3, Co = 2, and Mo = 1. The molecular weight is the metal salt used. atomic weight of metallic elements Example 1 (Preferred catalyst formulation of this invention, metal loading 13%) 1. Preparation of composite carrier: Weigh precisely according to a mass ratio of 70:20:10 325m 2 / g Anatase , Add 8% P123 of the total carrier mass, add deionized water and stir in a 40℃ water bath for 2 hours; add 5% boehmite, add 4% dilute nitric acid dropwise and stir for 30 minutes to mix; extrude into 1.5mm strips, air dry at room temperature for 2 hours, dry at 110℃ for 4 hours; calcine in stages: heat at 2℃ / min to 200℃ for 1 hour, heat at 3℃ / min to 550℃ for 4 hours, and cool to obtain the composite carrier.
[0045] 2. Acid modification: Using the equal-volume impregnation method, the carrier is impregnated with a 2% phosphoric acid solution for 3 hours, dried at 120℃ for 2 hours, and calcined at 500℃ for 2 hours, while simultaneously introducing 1%... It helps to adjust acidity.
[0046] 3. Metal loading: Prepare the impregnation solution according to the molar ratio of Ni:Co:Mo=3:2:1, with a total metal loading of 13%, add 5% citric acid complexing agent; add 3% Mn-Ce solid solution, ultrasonically disperse for 15 min; and statically impregnate in a sealed environment for 4 h.
[0047] 4. Calcination and vulcanization: Dry at 100℃ for 3 hours, heat to 300℃ at 2℃ / min and hold for 1 hour, then calcine at 480℃ for 3 hours; Fixed-bed programmed vulcanization: After purging and drying, 800 Airspeed 5% The mixed gas was sulfurized at 320℃ for 4 hours and then deeply sulfurized at 380℃ for 2 hours to obtain the finished catalyst.
[0048] Performance test results: Hydrodesulfurization rate 98.6%, RON octane number loss 0.8 units, olefin retention rate 61.2%, no obvious deactivation after 300 hours of continuous operation, low coking amount on catalyst surface, and no sulfur poisoning.
[0049] Microscopic characterization shows that the pore volume of the BET test carrier reaches 0.85 cm³. 3 / g, pyridine infrared spectroscopy confirmed the formation of abundant medium-strong acid sites, HRTEM observation confirmed the formation of a typical stacked type II MoS2 active phase, and TG test showed that the carbon deposition rate was only 2.1% after 300h of operation.
[0050] Example 2 (12% metal loading) In this embodiment, only the total multi-metal loading was adjusted to 12%, while the rest of the formulation and preparation process were completely consistent with Example 1.
[0051] Performance test results: hydrodesulfurization rate 98.1%, RON octane number loss 0.9 units, olefin retention rate 59.8%, and stable performance during 300 hours of continuous operation.
[0052] Example 3 (15% metal loading) In this embodiment, only the total multi-metal loading is adjusted to 15%, while the rest of the formulation and preparation process are completely consistent with Example 1.
[0053] Performance test results: Hydrodesulfurization rate 98.8%, RON octane number loss 1.0 unit, olefin retention rate 58.5%, desulfurization activity slightly improved, octane number loss slightly increased, still meeting the industry's preferred indicators.
[0054] Comparative examples (existing technology and univariate control catalysts) Comparative Example 1: Traditional Industrial CoMo / Commercial catalysts (without composite supports, acid modification, or anti-sulfur additives) Comparative Example 2: Removal Example 1 Catalyst (only the support was replaced with pure (The rest is the same as in Example 1) Comparative Example 3: Catalyst of Example 1 with Mn-Ce promoter removed (only without the addition of Mn-Ce solid solution, otherwise the same as in Example 1) Comparative Example 4: Removal Example 1 of the additives: catalyst (only without additives) (The rest is the same as in Example 1) Comparative Example 5: Imported Axens HR series commercial catalysts All comparative catalysts were evaluated under the same conditions as those in the examples, and their core performance indicators were tested uniformly. The performance comparison data are shown in the table below:
[0055] Based on the univariate comparison data above, we can conclude that: Comparative Example 1, due to the use of a single carrier and the absence of isomerization centers, resulted in excessive hydrogenation of the olefin, leading to significant octane number loss and easy coking. Comparative Example 2 only removes Subsequently, the carrier lacked hydrophobic stability, and after 300 hours of operation, it exhibited hydration pulverization and activity degradation, proving that... Its crucial role in structural stability; In Comparative Example 3, after removing only the Mn-Ce additive, the catalyst's anti-sulfur self-healing ability decreased, and the amount of coking during operation increased significantly, demonstrating the necessity of Mn-Ce solid solution to combat degradation. Comparative Example 4 only removes Subsequently, the strong acid sites were not effectively passivated, leading to excessive hydrogenation of the olefin and an increase in octane number loss to 1.3, proving that... Its central role in adjusting acidity and maintaining octane number; Although Comparative Example 5 showed stable performance, its olefin retention rate and octane number loss were slightly inferior to those of the present invention.
[0056] Embodiment 1 of this invention demonstrates the synergistic and non-obvious effects of the indispensable innovative components through the synergistic coupling of four major technologies.
[0057] This invention provides a low-octane-number-loss, high-selectivity FCC gasoline hydrodesulfurization catalyst, its preparation method, and its application. It can achieve deep desulfurization of FCC gasoline while maximizing the retention of olefin components and offsetting octane-number loss, taking into account high desulfurization activity, high hydrodesulfurization selectivity, and high operational stability, thus realizing the domestic substitution of catalysts.
[0058] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No reference numerals in the claims should be construed as limiting the scope of the claims.
[0059] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A low-octane-loss, high-selectivity FCC gasoline hydrodesulfurization catalyst, characterized in that, include: Ternary composite carrier, acid-modifying additive, multi-metal active component and anti-sulfur functional additive; The ternary composite carrier is composed of Specific surface area is 320-330 m² 2 / g of pure anatase Yttrium-stabilized tetragonal zirconium oxide Composition, in which Pure anatase and The mass ratio is 70:20:10, the Used to improve the hydrophobic resistance to phase transition of the carrier; The acid-modifying auxiliaries include phosphoric acid and phosphoric acid used to synergistically regulate moderately acidic sites, construct olefin skeleton isomerization active centers, and inhibit excessive hydrogenation of olefins. ; The multi-metal active component includes a Ni, Co, and Mo composite metal for preferentially forming a stacked, highly active type II metal sulfide active phase; The anti-sulfur functional additives include Mn-Ce solid solutions used to enhance resistance to sulfur poisoning and coking.
2. The catalyst according to claim 1, characterized in that, Based on the total mass of the ternary composite carrier, it also includes pore-forming agent P123 and pseudoboehmite, wherein the amount of P123 added is 8% and the amount of pseudoboehmite added is 5%.
3. The catalyst according to claim 1, characterized in that, Based on the total mass of the ternary composite carrier, the amount of phosphoric acid added is 2%. The addition amount is 1%.
4. The catalyst according to claim 1, characterized in that, The molar ratio of Ni, Co, and Mo in the multi-metal active component is 3:2:1, and the total metal loading is 12%-15% of the total mass of the ternary composite carrier.
5. The catalyst according to claim 1, characterized in that, The doping amount of the Mn-Ce solid solution is 3% of the total mass of the ternary composite carrier.
6. A method for preparing the catalyst according to claim 1, characterized in that, Includes the following steps: S1: Preparation of composite support: ... Pure anatase , The mixture is mixed with a pore-forming agent, and a binder is added for compounding. The mixture is then molded and calcined in stages to obtain a ternary composite carrier. S2: Acidic modification of the carrier: Using an equal-volume impregnation method, a mixture containing phosphoric acid and... The modified precursor liquid is loaded onto the carrier obtained in S1, and acidity regulation is completed by drying and calcination; S3: Active component loading: Prepare an active impregnation solution containing nickel nitrate, cobalt nitrate, ammonium molybdate and Mn-Ce solid solution, and co-impregnate the carrier obtained in S2; S4: Drying and calcining: The impregnated support obtained in S3 is subjected to segmented drying and calcination to obtain an oxidized catalyst precursor; S5: Sulfurization activation: The precursor is subjected to programmed temperature sulfidation in a sulfurization atmosphere to obtain the finished catalyst.
7. The preparation method according to claim 6, characterized in that, In S1, the segmented calcination process is as follows: the temperature is increased to 200℃ at 2℃ / min and held for 1 hour, and then increased to 550℃ at 3℃ / min and held for 4 hours to complete the crystal phase transformation; in S4, the segmented calcination process is as follows: the temperature is increased to 300℃ at 2℃ / min and held for 1 hour, and then increased to 480℃ and held for 3 hours to prevent the active metal from sintering.
8. The preparation method according to claim 6, characterized in that, In step S3, citric acid is added to the active impregnation solution as a complexing agent, and the amount of citric acid added is 5% of the total mass of the multi-metal active components; the co-impregnation is a closed static impregnation, and the impregnation time is 4 hours.
9. The preparation method according to claim 6, characterized in that, In S5, the sulfidation atmosphere is air-fuel mixture, airspeed 800 The programmed temperature vulcanization process includes: first, heating to 320℃ for the first stage of vulcanization, and then heating to 380℃ for the second stage of deep vulcanization.
10. The application of the catalyst according to claim 1 in the hydrodesulfurization refining of FCC gasoline, characterized in that, The operating conditions are as follows: reaction pressure 2.0-2.5 MPa, reaction temperature 260-280℃, hydrogen-to-oil volume ratio 300:1, and liquid hourly space velocity 2.
0. .