A nitride hydrolysis-derived catalyst, and a method for preparing and using the same
By using a method for preparing nitride hydrolysis-derived catalysts, and combining composite supports and transition metal particles, the problems of high cost of noble metal catalysts and low catalytic activity of transition metals are solved, achieving efficient and selective hydrogenation reactions, and reducing energy consumption and environmental pollution.
Patent Information
- Application Number
- CN202510646789.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-19
- Publication Date
- 2026-11-20
AI Technical Summary
Existing noble metal supported catalysts are expensive, while transition metal-based catalysts have low catalytic activity and yield in the hydrogenation of 5-hydroxymethylfurfural to 2,5-dihydroxymethylfuran.
A nitride hydrolysis-derived catalyst is used. Through the combination of a composite support and transition metal particles, the hydrolysis characteristics of hydrolyzable nitrides are utilized to generate hydroxides that interact with the active components of transition metals to form a uniformly dispersed catalyst. The nitrogen-doped support serves as a hydrogen atom transport channel, optimizing the metal dispersion and electronic structure.
It achieves efficient catalytic selective hydrogenation of 5-hydroxymethylfurfural to 2,5-dihydroxymethylfuran under mild conditions, improving conversion rate and selectivity, reducing energy consumption and environmental pollution, and lowering cost.
Smart Images

Figure CN123128031A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of catalyst technology, specifically relating to a nitride hydrolysis derivative catalyst, its preparation method, and its application. Background Technology
[0002] With dwindling fossil fuel resources and increasingly severe global warming, the development of safe, sustainable, and environmentally friendly resources is urgently needed. Against this backdrop, biomass, as a cheap, renewable, and abundant organic carbon resource, is considered an ideal alternative to fossil fuels. Among many promising bio-based platform molecules, 5-hydroxymethylfurfural (HMF) contains a variety of chemically active functional groups, and can be transformed into various high-value-added chemicals through oxidation, hydrogenation, and other conversion processes. Specifically, HMF can be hydrogenated from the carbon-oxygen double bond to produce furan-diethanol (BHMF), an important intermediate for the production of bio-based functional polymers, pharmaceuticals, and biofuel additives. To obtain high-yield BHMF, the C=O bonds in HMF need to be hydrogenated while preventing dehydroxylation and hydrogenation of the furan ring.
[0003] Currently, noble metal supported catalysts exhibit good hydrogenation efficiency, but they suffer from high costs. Transition metals are relatively inexpensive, but transition metal-based catalysts have lower activity, exhibiting low catalytic activity and low yield in the hydrogenation of HMF to BHMF. Summary of the Invention
[0004] To solve all or part of the above-mentioned technical problems, the present invention provides the following technical solutions:
[0005] One objective of this invention is to provide a nitride hydrolysis derivatization catalyst, comprising:
[0006] A composite carrier comprising a core and a shell covering the core, wherein the core is made of a nitride containing a first element, and the shell is made of a nitride containing a first element and an oxide containing a first element, wherein the nitride containing the first element is a hydrolyzable nitride.
[0007] An active component is loaded onto the composite support, and the active component includes transition metal-based particles.
[0008] The nitride hydrolysis derivatization catalyst provided by this invention exhibits excellent catalytic activity, hydrogenation activity, and selectivity. The nitrogen-doped composite support can serve as a hydrogen atom transport channel, rapidly transferring hydrogen species from the surface of the active component to other sites on the support, thus expanding the reaction interface. This catalyst is suitable for the selective hydrogenation of 5-hydroxymethylfurfural to 2,5-dihydroxymethylfuran, achieving a high conversion rate of 5-hydroxymethylfurfural.
[0009] In some embodiments, the first element includes one or a combination of more of Al, B, and Si.
[0010] In some embodiments, the nitride containing the first element includes one or a combination of more of AlN, BN, and Si₃N₄.
[0011] In some embodiments, the oxide containing the first element includes AlO x1 (0<X1≤1.5), SiO x2 (0<X2≤2), BO x3 (0<X3≤1.5), or a combination of one or more thereof.
[0012] In some embodiments, the transition metal element contained in the transition metal-based particles includes one or a combination of more of Fe, Co, Ni, Cu, and Zn. Preferably, the transition metal element includes Cu. The 3d orbital of the copper atom overlaps with the antibonding orbital of the furan ring, and Cu metal selectively adsorbs the carbonyl group of HMF rather than the furan ring, so the copper-based catalyst exhibits more excellent selective hydrogenation catalytic performance in the reaction of hydrogenating the aldehyde group on the side chain of HMF. Certainly, the nitride-derived catalysts based on Fe, Co, Ni, and Zn provided by the present invention also exhibit better selectivity and higher conversion rates compared with the transition metal-based catalysts in the prior art that use Fe, Co, Ni, and Zn as active components.
[0013] The transition metal-based particles may be, for example, single-metal particles or multi-metal particles formed by the above-mentioned transition metal elements.
[0014] In some embodiments, the chemical formula of the nitride hydrolysis-derived catalyst is W / MO x -MN, where W represents the transition metal element contained in the transition metal-based particles, the transition metal element is selected from one or a combination of more of Fe, Co, Ni, Cu, and Zn, M represents the first element, and MO x -MN represents a composite support composed of a nitride containing the first element and an oxide containing the first element, 0<X≤2, M is selected from one or a combination of more of Al, B, and Si. The support generated by the hydrolysis-calcination process is a non-stoichiometric complex formed by partial oxidation of MN, and its surface is composed of amorphous / crystalline species (MO x ) and incompletely hydrolyzed MN.
[0015] In some typical embodiments, the nitride hydrolysis-derived catalyst is Cu / AlO x1 -AlN, Cu / SiO x2 -Si₃N₄, Cu / BO x3 -BN, Fe / AlO x1-AlN, Co / AlO x1 -AlN, Ni / AlOx1-AlN, Zn / AlO x1 -AlN, Fe / SiO x2 -Si3N4, Co / SiO x2 -Si3N4, Ni / SiO x2 -Si3N4、Zn / SiO x2 -Si3N4、Fe / BO x3 -BN、Co / BO x3 -BN, Ni / BO x3 -BN or Zn / BO x3 -BN; where 0 < X1 ≤ 1.5, 0 < X2 ≤ 2, and 0 < X3 ≤ 1.5. Considering both the conversion rate and selectivity of HMF hydrogenation to BHMF, Cu / AlO is preferred. x1 -AlN, Cu / SiO x2 -Si3N4, Cu / BO x3 -BN, more preferably Cu / AlO x1 -AlN.
[0016] In some embodiments, the content of the active combination in the nitride hydrolysis derivatization catalyst is 0.5 to 10.0 wt%.
[0017] In some embodiments, the mass ratio of the nitride containing the first element to the oxide containing the first element in the shell is 1.5 to 2:1.
[0018] In some embodiments, the particle size of the transition metal-based particles is 3-5 nm.
[0019] A second objective of this invention is to provide a method for preparing a nitride hydrolysis derivatization catalyst, comprising:
[0020] A hydrolyzable nitride containing a first element is immersed in a solution containing an active component source, wherein the solvent of the solution includes water, to cause the surface portion of the hydrolyzable nitride to hydrolyze to form a hydroxide of the first element; wherein the active component source includes a transition metal source providing a transition metal element.
[0021] The solvent is removed from the mixture obtained by hydrolysis to obtain the precursor material;
[0022] The precursor material is calcined to obtain the intermediate material;
[0023] The intermediate material is reduced to obtain a nitride hydrolysis-derived catalyst.
[0024] In the preparation method provided by the present invention, the microstructure of the hydrolyzable nitride evolves during the hydrolysis process, and the surface layer of the hydrolyzable nitride is partially hydrolyzed to generate hydroxide (the hydrolysis reaction is: MN+H2O→M(OH) x +NH3), the generated hydroxide component is converted into oxide in the subsequent calcination process, and forms a shell layer in the form of a composite with the unhydrolyzed nitride near the surface layer, while the unhydrolyzed nitride inside constitutes the core; in the subsequent reduction treatment process, the transition metal source forms transition metal particles in-situ supported on the composite carrier, so as to obtain a catalyst with high activity and selectivity.
[0025] The preparation method provided by the present invention utilizes the hydrolysis characteristics of nitride to realize the effect of hydrolyzing while anchoring the transition metal. Since the M(OH) generated during the hydrolysis process x is generated in-situ, its surface hydroxyl group (-OH) has higher reactivity, can directly coordinate with the transition metal precursor (such as salts or complexes), and directly form a strong interaction at the atomic scale (such as M(OH) x --O--M metal bond or hydrogen bond), which optimizes the metal dispersion and electronic structure, and makes the catalyst exhibit better metal dispersion. This precise catalytic design is applicable to highly selective hydrogenation reactions. The interface formed by the in-situ dynamic formation of hydroxyl groups is more uniform than the ready-made hydroxide obtained by mechanical mixing, and avoids the agglomeration or surface passivation problems that may exist in the pre-synthesized hydroxide. Compared with the method of directly using an oxide carrier to react with a transition metal source to generate a supported catalyst, the preparation method provided by the present invention can form transition metal particles with more uniform dispersion and smaller size on the composite carrier. In addition, the nitrogen-doped carrier can act as a hydrogen atom transmission channel, rapidly transferring hydrogen species on the surface of the active metal to other sites of the carrier, thereby expanding the reaction interface.
[0026] In some embodiments, the first element includes one or a combination of more of Al, B, and Si.
[0027] In some embodiments, the hydrolyzable nitride containing the first element includes one or a combination of more of AlN, BN and Si3N4. These hydrolyzable nitrides can correspondingly generate AlO after hydrolysis and calcination treatments xi (0<X1≤1.5), SiO x2 (0<X2≤2), BO x3 (0<X3≤1.5), and finally form a shell layer in the form of a nitride and oxide composite.
[0028] In some embodiments, the transition metal element provided by the transition metal source includes one or a combination of more of Fe, Co, Ni, Cu, Zn, preferably including Cu.
[0029] In some embodiments, the transition metal source includes water-soluble salts and / or complexes of the transition metal element, such as nitrates, etc., and the present invention does not impose any particular limitation on this.
[0030] In some embodiments, the impregnation temperature is 10–30°C and the time is 6–18 hours, thereby causing hydrolysis of the surface portion of the hydrolyzable nitride.
[0031] In some embodiments, the water content in the solution reaches the saturation water absorption capacity of the hydrolyzable nitrogen compound, thereby causing sufficient hydrolysis of the surface portion of the hydrolyzable nitrogen compound.
[0032] Compared to methods that convert all hydrolyzable nitrides into hydroxides, partial hydrolysis can generate non-stoichiometric hydroxylated oxides (such as AlO(OH) or defective Al(OH)3), resulting in more surface defects. This allows for uniform anchoring of the metal precursor, and the low crystallinity can be gradually converted into oxides to form a porous structure during subsequent heat treatment. Furthermore, the thickness of the composite support shell can be adjusted by controlling the impregnation temperature and time. In some embodiments, the thickness of the shell in the composite support of the catalyst provided by this invention is approximately 5-10% of the overall size of the composite support; that is, the surface layer of the composite support is a composite of nitrides and oxides, while the internal (core) portion remains unhydrolyzed nitrides.
[0033] In some embodiments, the mass ratio of the hydrolyzable nitride to the active component source is 100:0.5-5.
[0034] In some embodiments, the calcination temperature is 450–550°C.
[0035] In some embodiments, the temperature is increased to 450-550°C at a rate of 1-3°C / min for roasting.
[0036] In some embodiments, the calcination process takes 2-6 hours. The calcination can, for example, be carried out in an air atmosphere.
[0037] In some embodiments, the reduction process includes: bringing the intermediate material into full contact with a reducing gas and performing the reduction process at a temperature of 250–550°C.
[0038] In some embodiments, the temperature is increased to 250–550°C at a rate of 2–5°C / min for reduction treatment.
[0039] In some embodiments, the reducing gas includes hydrogen.
[0040] In some embodiments, the reduction process takes 1 to 5 hours.
[0041] In some embodiments, the preparation method of the nitride hydrolysis-derived catalyst further includes calcining the hydrolyzable nitride before immersing it in a solution containing an active component source. Calcination removes surface contaminants; commercial nitrides may contain residual organic precursors, solvents, or processing aids (such as sintering aids, dispersants, etc.) during preparation. Calcination can oxidize and decompose these impurities at high temperatures, ensuring the chemical purity of the support.
[0042] In some embodiments, the calcination temperature is 500–700°C and the time is 3–5 hours.
[0043] In some embodiments, after removing the solvent from the mixture obtained by hydrolysis, the resulting precursor material is ground and then subjected to the calcination treatment. This can further break up the hard agglomeration between precursor particles (caused by solvent evaporation or condensation of hydrolysis products) and ensure more uniform contact of reactants during subsequent calcination.
[0044] The method for removing the solvent from the mixture obtained by hydrolysis can be, for example, drying, such as drying in an oven at 120°C for 12 hours. Alternatively, it can be any solvent removal method known in the art, and the present invention does not impose any particular limitation on it.
[0045] A third objective of this invention is to provide a nitride hydrolysis derivatization catalyst, which is prepared by the method described in any of the above-mentioned methods.
[0046] The nitride hydrolysis derivatization catalyst of the present invention can be prepared by the above preparation method. It includes a composite support and an active component. The composite support includes a core and a shell covering the core. The core is made of a nitride containing a first element, and the shell is made of a nitride containing a first element and an oxide containing a first element. The nitride containing the first element is a hydrolyzable nitride. The active component is loaded on the composite support and includes transition metal-based particles.
[0047] In some typical embodiments, the prepared nitride hydrolysis-derived catalyst has the chemical formula W / MO. x -MN, where W represents the transition metal element contained in the transition metal-based particles, the transition metal element being selected from one or more combinations of Fe, Co, Ni, Cu, and Zn, M representing the first element, MO x -MN represents a composite support composed of a nitride containing the first element and an oxide containing the first element, where 0 < X ≤ 2, and M is selected from one or more combinations of Al, B, and Si.
[0048] In some typical embodiments, the nitride hydrolysis derivatization catalyst is Cu / AlO. x1-AlN, Cu / SiO x2 -Si3N4, Cu / BO x3 -BN, Fe / AlO x1 -AlN, Co / AlO x1 -AlN, Ni / AlO x1 -AlN、Zn / AlO x1 -AlN, Fe / SiO x2 -Si3N4, Co / SiO x2 -Si3N4, Ni / SiO x2 -Si3N4、Zn / SiO x2 -Si3N4、Fe / BO x3 -BN、Co / BO x3 -BN, Ni / BO x3 -BN or Zn / BO x3 -BN; where 0 < X1 ≤ 1.5, 0 < X2 ≤ 2, and 0 < X3 ≤ 1.5. Considering both the conversion rate and selectivity of HMF hydrogenation to BHMF, Cu / AlO is preferred. x1 -AlN, Cu / SiO x2 -Si3N4, Cu / BO x3 -BN, more preferably Cu / AlO x1 -AlN.
[0049] A fourth objective of this invention is to provide the application of any of the nitride hydrolysis derivatization catalysts described in this invention in the catalytic hydrogenation of 5-hydroxymethylfurfural to 2,5-dihydroxymethylfuran. The catalyst provided by this invention exhibits excellent selectivity and a high conversion rate of 5-hydroxymethylfurfural in the hydrogenation reaction of 5-hydroxymethylfurfural to 2,5-dihydroxymethylfuran.
[0050] The fifth objective of this invention is to provide a method for hydrogenating 5-hydroxymethylfurfural to produce 2,5-dihydroxymethylfuran, comprising: reacting a mixed reaction system containing 5-hydroxymethylfurfural, a catalyst, and a solvent in a hydrogen-containing atmosphere to produce 2,5-dihydroxymethylfuran; wherein the catalyst comprises any one of the above-described technical solutions of the nitride hydrolysis derivatization catalyst.
[0051] In some embodiments, the reaction temperature is 60–150°C, exhibiting good conversion rate and selectivity. For example, it can be any value or a range between 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, and 150°C. The preferred reaction temperature is 110–140°C, at which point the conversion rate and selectivity are further improved.
[0052] In some embodiments, the reaction is carried out under hydrogen pressure conditions of 0.5 MPa to 5 MPa, exhibiting good conversion rate and selectivity. For example, the pressure can be any value among 0.5 MPa, 1 MPa, 2 MPa, 3 MPa, 4 MPa, and 5 MPa, or any range between two of these values. Preferably, the reaction is carried out under hydrogen pressure conditions of 1.1 MPa to 1.8 MPa, at which point the conversion rate and selectivity are further improved.
[0053] In some embodiments, the reaction time is 1 to 48 hours, for example, it can be any value or a range between 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 25 hours, 30 hours, 35 hours, 40 hours, 45 hours, and 48 hours.
[0054] In some embodiments, the catalyst content in the mixed reaction system is 10-30% of the mass of 5-hydroxymethylfurfural.
[0055] In some embodiments, the solvent includes water and / or an organic solvent, preferably an organic solvent.
[0056] In some embodiments, the organic solvent includes one or a combination of more of the following: tetrahydrofuran, methanol, ethanol, isopropanol, dimethyl sulfoxide, N,N-dimethylformamide, γ-valerolactone, n-hexane, and ethyl acetate.
[0057] Compared with the prior art, the present invention has at least the following beneficial effects:
[0058] (1) This invention utilizes the hydrolysis properties of hydrolyzable nitrogen compounds (MN + H₂O → M(OH)). x +NH3) modulates the surface properties of the support, and the microstructure of hydrolyzable nitrides evolves during hydrolysis, producing M(OH)2. x The components interact with the transition metal active components, thereby optimizing the metal dispersion and electronic structure. The resulting catalyst exhibits excellent hydrogenation activity and selectivity in the hydrogenation of HMF to BHMF. In this invention, the nitrogen-doped composite support acts as a hydrogen atom transport channel, rapidly transferring hydrogen species from the active metal surface to other sites on the support, thus expanding the reaction interface. Furthermore, the active sites in the catalyst can precisely select C=O bonds in HMF for hydrogenation, effectively avoiding side reactions and significantly improving the yield of BHMF. In some superior embodiments, the product yield reaches as high as 99%.
[0059] (2) The catalyst provided by this invention can achieve high-efficiency catalysis under mild conditions. Under mild conditions (e.g., 60–120°C, 0.5–1 MPa hydrogen pressure), it can catalyze the selective hydrogenation of 5-hydroxymethylfurfural to prepare 2,5-dihydroxymethylfuran. In contrast, existing transition metal-based catalysts typically require harsh reaction conditions of high temperature and high pressure to achieve high-efficiency catalysis. This means that the nitride hydrolysis catalyst provided by this invention can reduce energy consumption and environmental pollution from the selective hydrogenation of 5-hydroxymethylfurfural, aligning with the development concept of green chemistry.
[0060] (3) The preparation method provided by the present invention is simple to operate and the raw materials are readily available. The active metal is a transition metal with low cost, which solves the problem of high cost of precious metal catalysts. Attached Figure Description
[0061] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0062] Figure 1 The AlN used in Example 1 and the Cu / AlO prepared in Example 1 are used in this example. x -AlN(O), Cu / AlO x -AlN, and the XRD patterns of Al2O3 used in Comparative Example 1, Cu / Al2O3(O) prepared in Comparative Example 1, and Cu / Al2O3; wherein, Cu / AlO x -AlN(O) and Cu / Al2O3(O) represent the calcined intermediate material, i.e., the unreduced catalyst.
[0063] Figure 2 In the diagram, a and b are HADDF-STEM images of Cu / Al2O3 prepared in Example 1 at different magnifications, and c and d are Cu / Al2O3 prepared in Example 1. x -AlN HADDF-STEM images at different magnifications.
[0064] Figure 3 This is from Example 1, which describes the preparation of Cu / AlO. x - The infrared spectrum of AlN after being impregnated in copper nitrate solution during the AlN catalyst process; as a control, the infrared spectrum of AlN after being impregnated in pure water was also tested.
[0065] Figure 4 This is a reaction route diagram for the selective hydrogenation of HMF to prepare BHMF. Detailed Implementation
[0066] The technical solutions of the present invention will be described in detail below with reference to specific embodiments, so that those skilled in the art can better understand and implement the technical solutions of the present invention. The specific functional details disclosed herein should not be construed as limiting, but are merely intended to form the basis of the claims and to teach those skilled in the art to employ the representative basis of the invention in different ways in any suitable detailed embodiment.
[0067] In addition, unless otherwise specified, all raw materials used in the following embodiments can be purchased from the market or other sources, and all production and testing equipment used are known in the art, as are the testing methods used.
[0068] In the following embodiments of the present invention, the structure of the catalyst sample was characterized using a transmission electron microscope (TEM), model Talos F200x. The structure of the catalyst sample was characterized using an X-ray diffractometer (XRD), model D8 ADVANCEDAVINCI. The structure of the catalyst precursor was characterized using a Fourier transform infrared spectroscopy (FTIR), model Thermo Scientific Nicolet 6700.
[0069] The test results in the following embodiments of the present invention are all average values of three repetitions.
[0070] The conversion rate and selectivity are calculated as follows:
[0071] After the reaction was completed, gas chromatography was used to perform qualitative and quantitative analysis on the reactants and products.
[0072] The conversion rate C, selectivity S, and yield Y of furan derivatives are calculated using the external standard method according to the following formulas.
[0073]
[0074] The technical solution of the present invention will be described in detail below with reference to specific embodiments:
[0075] Example 1
[0076] This embodiment provides a Cu / AlO x -AlN catalyst and its preparation method, specifically including the following steps:
[0077] (1) Weigh a certain amount of AlN and place it in an air atmosphere in a muffle furnace, and calcine it at 600℃ for 4 hours. Dissolve Cu(NO3)2·3H2O in water to prepare a Cu(NO3)2 aqueous solution with a concentration of 0.02g Cu / mL.
[0078] (2) Taking the preparation of 2g catalyst as an example, the 4mL Cu(NO3)2 aqueous solution prepared above is dropped into a beaker containing 2g of the calcined AlN above, ensuring that the water volume is the saturated water absorption of AlN, and the mixture is stirred, sonicated, and left to stand at room temperature for 12 hours.
[0079] (3) The mixture obtained by standing was dried in an oven at 120°C for 12 hours to obtain a precursor material; the precursor material was calcined in a muffle furnace at a rate of 1°C / min to 500°C for 3 hours to obtain an intermediate material; the intermediate material was then reduced at 300°C for 3 hours in an H2 atmosphere at a rate of 2°C / min to obtain Cu / AlO x -AlN, wherein the Cu loading is 4 wt%.
[0080] Example 2
[0081] Example 2 is basically the same as Example 1, except that AlN in Example 1 is replaced with Si3N4 to prepare the catalyst Cu / SiO. x -Si3N4, wherein the Cu loading is 4wt%. The rest is the same as in Example 1, and will not be repeated here.
[0082] Example 3
[0083] Example 3 is basically the same as Example 1, except that AlN in Example 1 is replaced with BN to prepare the catalyst Cu / BO. x -BN, wherein the Cu loading is 4wt%. The rest is the same as in Example 1, and will not be repeated here.
[0084] Example 4
[0085] Example 4 provides a nitride hydrolysis derivatization catalyst and its preparation method, specifically including the following steps:
[0086] (1) Dissolve Fe(NO3)3 in water to prepare an aqueous solution of Fe(NO3)3 with a concentration of 0.02 g / mL.
[0087] (2) Taking the preparation of 2g catalyst as an example, the above-prepared 4mL Fe(NO3)3 aqueous solution is dropped into a beaker containing 2g AlN, ensuring that the water volume is the saturated water absorption of AlN, and then stirred, sonicated, and left to stand at room temperature for 12 hours.
[0088] (3) The mixture obtained after standing was dried in an oven at 120℃ for 12h to obtain a precursor material; the precursor material was calcined in a muffle furnace at 500℃ for 3h to obtain an intermediate material; the intermediate material was heated to 500℃ at a rate of 2℃ / min in an H2 atmosphere and reduced at 500℃ for 3h to obtain Fe / AlO x -AlN, in which the metal Fe loading is 4%.
[0089] Example 5
[0090] Example 5 is basically the same as Example 4, except that in Example 5, Fe(NO3)3 in Example 4 is replaced with Co(NO3)2 to obtain Co / AlO. x -AlN, with a Co loading of 4%. The remaining embodiments of Example 4 are the same and will not be described again here.
[0091] Example 6
[0092] Example 6 is basically the same as Example 4, except that in Example 6, Fe(NO3)3 in Example 4 is replaced with Ni(NO3)2 to obtain Ni / AlO. x -AlN, with a Ni loading of 4%. The remaining embodiments of Example 4 are the same and will not be described again here.
[0093] Example 7
[0094] Example 7 is basically the same as Example 4, except that in Example 7, Fe(NO3)3 in Example 4 is replaced with Zn(NO3)2 to obtain Zn / AlO. x -AlN, with a Zn loading of 4%. The remaining embodiments of Example 4 are the same and will not be described again here.
[0095] Examples 8a-8h
[0096] Examples 8a to 8h are basically the same as Example 1, except that the volume of Cu(NO3)2 aqueous solution (0.02 g Cu / mL) mixed with AlN is changed to control the loading of metallic Cu in the final catalyst. Taking the preparation of 2 g catalyst as an example, the volume of Cu(NO3)2 aqueous solution used for different loadings of metallic Cu is shown in Table 1:
[0097] Table 1
[0098]
[0099] Example 9
[0100] Example 9 is basically the same as Example 1, except that the calcined intermediate material was reduced for 3 hours using H2 at a flow rate of 60 mL / min at 550°C. The rest of the procedure is the same as in Example 1 and will not be repeated here.
[0101] Example 10
[0102] Example 10 is essentially the same as Example 1, except that: the dried precursor material was calcined in a muffle furnace at a rate of 1°C / min to 500°C for 2 hours to obtain an intermediate material; then, the calcined intermediate material was reduced for 3 hours at 450°C and 550°C using H2 at a flow rate of 60 mL / min. The rest of the procedure was the same as in Example 1 and will not be repeated here.
[0103] Example 11
[0104] Example 11 is basically the same as Example 1, except that the reduction step is as follows: after calcination in a muffle furnace, the intermediate material obtained after calcination is reduced for 5 hours using H2 at a flow rate of 60 mL / min at a temperature of 250°C. The rest of the procedure is the same as in Example 1, and will not be repeated here.
[0105] Example 12
[0106] Example 12 is basically the same as Example 1, except that the reduction step is as follows: the intermediate material obtained after calcination is reduced for 1 hour using H2 at a flow rate of 60 mL / min and a temperature of 350°C. The rest is the same as in Example 1, and will not be described again here.
[0107] Example 13
[0108] The difference between Example 13 and Example 1 is that step (3) of Example 13 is as follows: the mixture obtained by standing is dried in an oven at 120°C for 12 hours to obtain a precursor material; the obtained precursor material is ground to break up the hard agglomerates between precursor particles to ensure more uniform contact of reactants during subsequent calcination; then the precursor material is calcined in a muffle furnace at a rate of 1°C / min to 500°C for 3 hours to obtain an intermediate material; in an H2 atmosphere, the temperature is increased to 300°C at a rate of 2°C / min, and the intermediate material is reduced at 300°C for 3 hours to obtain Cu / AlO. x -AlN, wherein the Cu loading is 4 wt%.
[0109] The rest is the same as in Example 1, and will not be described again here.
[0110] Comparative Example 1
[0111] Comparative Example 1 prepared a Cu / Al2O3 catalyst, specifically including the following steps:
[0112] (1) Dissolve Cu(NO3)2·3H2O in water to prepare a Cu(NO3)2 aqueous solution with a concentration of 0.02g Cu / mL.
[0113] (2) Taking the preparation of 2g catalyst as an example, 4mL of Cu(NO3)2 aqueous solution was dropped into a beaker containing 2g of commercial support Al2O3 to ensure that the water volume was the saturated water absorption of Al2O3. The mixture was stirred, sonicated, and left to stand at room temperature for 12 hours.
[0114] (3) After drying the mixture obtained by standing in an oven at 120°C for 12 hours, it was calcined in a muffle furnace at a rate of 1°C / min to 500°C for 3 hours to obtain an intermediate material; then H2 was used to reduce the calcined intermediate material at 300°C for 3 hours at a rate of 2°C / min to obtain Cu / Al2O3, wherein the Cu loading was 4%.
[0115] Comparative Example 2
[0116] Comparative Example 2 used the intermediate material (Cu / Al2O3(O)) from Example 1 that was not reduced as a catalyst for the hydrogenation of HMF to BHMF.
[0117] Comparative Example 3
[0118] Comparative Example 3 provides a Fe / Al2O3 catalyst, specifically comprising the following steps:
[0119] (1) Dissolve Fe(NO3)3 in water to prepare an aqueous solution of Fe(NO3)3 with a concentration of 0.02 g / mL.
[0120] (2) Taking the preparation of 2g catalyst as an example, the above-prepared 4mL Fe(NO3)3 aqueous solution was dropped into a beaker containing 2g commercial carrier Al2O3, ensuring that the water volume was the saturated water absorption of Al2O3, and then stirred, sonicated, and left to stand at room temperature for 12 hours.
[0121] (3) The mixture obtained by standing is dried in an oven at 120°C for 12 hours to obtain a precursor material; the precursor material is calcined in a muffle furnace at 500°C for 3 hours to obtain an intermediate material; the intermediate material is heated to 500°C at a rate of 2°C / min in an H2 atmosphere and reduced at 500°C for 3 hours to obtain Fe / Al2O3, wherein the metal Fe loading is 4%.
[0122] Comparative Example 4
[0123] Comparative Example 4 is basically the same as Comparative Example 3, except that Cu(NO3)2 is replaced with an aqueous solution of Co(NO3)2 to prepare the catalyst Co / Al2O3. The rest of the procedure is the same as that of Comparative Example 3, and will not be repeated here.
[0124] Comparative Example 5
[0125] Comparative Example 5 is basically the same as Comparative Example 3, except that Cu(NO3)2 is replaced with an aqueous solution of Ni(NO3)2 to prepare the catalyst Ni / Al2O3. The rest of the procedure is the same as that of Comparative Example 3, and will not be described again here.
[0126] Comparative Example 6
[0127] Comparative Example 6 is basically the same as Comparative Example 3, except that Cu(NO3)2 is replaced with an aqueous solution of Zn(NO3)2 to prepare the catalyst Zn / Al2O3. The rest of the procedure is the same as that of Comparative Example 3, and will not be repeated here.
[0128] Comparative Example 7
[0129] The preparation method of the Cu / AlN catalyst provided in this comparative example specifically includes the following steps:
[0130] (1) Weigh a certain amount of AlN and place it in an air atmosphere in a muffle furnace, and calcine it at 600℃ for 4 hours. Dissolve Cu(NO3)2·3H2O in ethanol to prepare a Cu(NO3)2 ethanol solution with a concentration of 0.04g Cu / mL.
[0131] (2) Taking the preparation of 2g catalyst as an example, the 2mL Cu(NO3)2 aqueous solution prepared above is dropped into a beaker containing 2g of the above-mentioned calcined AlN, and stirred and sonicated. It is not necessary to let it stand overnight at room temperature.
[0132] (3) is the same as step (3) in Example 1.
[0133] Figure 1 The AlN used in Example 1 and the Cu / AlO prepared in Example 1 are used in this example. x -AlN(O), Cu / AlO x -AlN, and the XRD patterns of Al2O3 used in Comparative Example 1, Cu / Al2O3(O) prepared in Comparative Example 1, and Cu / Al2O3; wherein, Cu / AlO x -AlN(O) and Cu / Al2O3(O) represent the calcined intermediate material, i.e., the unreduced catalyst.
[0134] Figure 2In the diagram, a and b are HADDF-STEM images of Cu / Al2O3 prepared in Example 1 at different magnifications, and c and d are Cu / Al2O3 prepared in Example 1. x -AlN HADDF-STEM images at different magnifications. From Figure 2 From c and d in the figure, we can see that Cu metal particles are supported on AlO. x On the AlN composite support, and compared to Comparative Example 1, the Cu metal particles in the catalyst of Example 1 have a more uniform particle size distribution and smaller particle size, thus exhibiting superior high-selectivity catalytic hydrogenation activity. The Cu metal particle size in the catalyst of Comparative Example 1 is approximately 5.73 ± 0.19 nm, while the Cu metal particle size in the catalyst of Example 1 is approximately 4.00 ± 0.08 nm.
[0135] Figure 3 This is from Example 1, which describes the preparation of Cu / AlO. x - The infrared spectrum of AlN after being impregnated in copper nitrate solution during the AlN catalyst process; as a control, the infrared spectrum of AlN after being impregnated in pure water was also tested.
[0136] The present invention also uses the catalyst prepared above in the hydrogenation reaction of HMF to produce BHMF. Figure 4 This is a reaction route diagram for the selective hydrogenation of HMF to prepare BHMF.
[0137] 1. Conversion rate and selectivity of catalytic reaction
[0138] The catalyst prepared above was added to an ethanol solvent system with a 5-hydroxymethylfurfural concentration of 0.12M. Hydrogen gas was introduced into the reactor and the gas was replaced. The hydrogen pressure was maintained at 1-2.5 MPa and the temperature at 100-140℃. The reaction was carried out for 0.5 h. The conversion rate and selectivity of HMF to BHMF were detected. The results are shown in Table 2.
[0139] Table 2. Conversion and selectivity of HMF to BHMF by hydrogenation with different catalysts
[0140]
[0141] 2. Catalyst performance in selective hydrogenation of HMF under different hydrogen pressure conditions
[0142] Cu prepared in Example 1 (4%) / AlO x Taking AlN catalyst as an example, in an ethanol system with a 5-hydroxymethylfurfural concentration of 0.12 M, Cu is added... (4%) / AlO xThe AlN catalyst was used in a reactor where hydrogen was introduced and the gas was replaced. The reaction temperature was 120℃, and the reaction time was 1 h. The hydrogen pressure was changed, and the yield of selective hydrogenation of HMF to BHMF was tested. It was found that the catalytic activity changed with the hydrogen pressure. The results are shown in Table 3.
[0143] Table 3. Conversion rate and selectivity of HMF to BHMF under different hydrogen pressures.
[0144] serial number Hydrogen pressure / MPa Conversion rate / % Selectivity / % 1 0.6 30 99.9 2 0.8 34 99.9 3 1 64 99.9 4 1.2 65 99.7 5 1.4 67 97.2 6 1.6 70 93.4 5 1.8 74 91.7 6 2 80 87.4 7 0.5 10 99.1 8 5 89 82.9
[0145] Table 3 shows that the yield of BHMF first increases and then decreases with increasing hydrogen pressure. Therefore, for the nitride hydrolysis catalyst system of the present invention, considering both conversion rate and selectivity, the hydrogen pressure is preferably 1-1.8 MPa. Within this range, the conversion rate is above 60% and the selectivity is above 90%. A more preferred hydrogen pressure is 1.2 MPa.
[0146] 3. Catalyst performance of selective hydrogenation of HMF under different temperature conditions
[0147] Cu prepared in Example 1 (4%) / AlO x Taking AlN as an example, in an ethanol system with a 5-hydroxymethylfurfural concentration of 0.12M, Cu is added... (4%) / AlO x -AlN catalyst. Hydrogen gas was introduced into the reactor and the gas was replaced. The hydrogen pressure was maintained at 1 MPa. The reactor was heated to the required temperature and stirred continuously for 1 h. Different required temperatures were selected to test the selectivity of HMF to BHMF. The results are shown in Table 4.
[0148] Table 4. Conversion and selectivity of HMF to BHMF selectively hydrogenated at different reaction temperatures.
[0149] serial number Reaction temperature / °C Conversion rate / % Selectivity / % 1 100 43 99.9 2 110 53 99.9 3 120 73 99.7 4 130 80 93.5 5 140 83 94.5 6 60 20 98.9 7 150 89 79.3
[0150] Table 4 shows that the yield of BHMF first increases and then decreases with increasing reaction temperature. For the nitride hydrolysis catalyst system of the present invention, considering both conversion and selectivity, the preferred reaction temperature is 110-140℃. Within this range, the conversion is above 50% and the selectivity is above 93%. A more preferred reaction temperature is 120℃.
[0151] 4. Catalytic performance of HMF selective hydrogenation reaction in different solvent systems
[0152] Cu prepared in Example 1 (4 % ) Taking / AlOxx-A1N as an example, in an ethanol system with a 5-hydroxymethylfurfural concentration of 0.12M, Cu is added...(4%) / AlO x -AlN catalyst. Hydrogen gas was introduced into the reactor and the gas was replaced. The hydrogen pressure was maintained at 1 MPa. The reactor was heated to 120 °C and stirred continuously for 1 h. The selectivity of HMF to BHMF was tested. The results are shown in Table 5.
[0153] Table 5. Conversion and selectivity of HMF to BHMF in different solvent systems
[0154] serial number Reaction temperature / °C Conversion rate / % Selectivity / % 1 water 2 49.9 2 ethanol 67 99.9 3 methanol 43 99.7 4 Isopropanol 30 93.5 5 n-Hexane 13 94.5 6 Ethyl acetate 5 98.9
[0155] Table 5 shows that the yield of BHMF first increases and then decreases with increasing reaction temperature. For the nitride hydrolysis catalyst system of the present invention, considering the conversion rate, selectivity and economic benefits of production, the preferred solvent is methanol or ethanol, especially ethanol.
[0156] 5. Evaluation of catalyst stability.
[0157] Cu prepared in Example 1 (4%) / AlO x Taking AlN catalyst as an example, in an ethanol system with a 5-hydroxymethylfurfural concentration of 0.12 M, Cu is added... (4%) / AlO x -AlN catalyst. Hydrogen gas was introduced into the reactor to replace the gas, maintaining a hydrogen pressure of 1 MPa and a temperature of 120 °C, and stirring was continued for 1 h. After the reaction, the catalyst was filtered, washed, dried, and recycled. The above operation was repeated 5 times to test the conversion and selectivity of HMF to BHMF. The results are shown in Table 6.
[0158] Table 6 Catalyst Cyclic Stability Test
[0159] Loop count HMF conversion rate / % BHMF Selectivity / % 1 70 99.8 2 65 99.8 3 62 99.8 4 60 99.8 5 57 99.8
[0160] As shown in Table 6, the nitride hydrolysis catalyst of the present invention has good stability.
[0161] The nitride hydrolysis catalysts prepared in other embodiments of this application were tested for hydrogenation reaction catalytic activity, selectivity, and cycle stability in accordance with the above evaluation methods. The test results showed that these products performed well.
[0162] All aspects, embodiments, features, and examples of this invention are to be regarded as illustrative in all respects and are not intended to limit the invention, the scope of which is defined only by the claims. Other embodiments, modifications, and uses will become apparent to those skilled in the art without departing from the spirit and scope of the invention as claimed.
[0163] In addition, the inventors of this case also conducted experiments with other raw materials, process operations, and process conditions described in this specification, referring to the aforementioned embodiments, and obtained relatively ideal results in all cases.
[0164] Although the invention has been described with reference to illustrative embodiments, those skilled in the art will understand that various other changes, omissions, and / or additions can be made without departing from the spirit and scope of the invention, and that elements of the embodiments can be substituted with substantially equivalents. Furthermore, many modifications can be made without departing from the scope of the invention to adapt particular situations or materials to the teachings of the invention. Therefore, this invention is not intended to be limited to the specific embodiments disclosed for carrying out the invention, but rather is intended to encompass all embodiments falling within the scope of the appended claims. Moreover, unless specifically stated otherwise, any use of the terms first, second, etc., does not indicate any order or importance, but is used to distinguish one element from another.
Claims
1. A nitride hydrolysis derivatization catalyst, characterized in that, include: A composite carrier comprising a core and a shell covering the core, wherein the core is made of a nitride containing a first element, and the shell is made of a nitride containing a first element and an oxide containing a first element, wherein the nitride containing the first element is a hydrolyzable nitride. An active component is loaded onto the composite support, and the active component includes transition metal-based particles.
2. The nitride hydrolysis derivatization catalyst according to claim 1, characterized in that: The first element includes one or more of Al, B, and Si; And / or, the nitride containing the first element includes one or more combinations of AlN, BN and Si3N4; And / or, the oxide containing the first element includes AlO x1 SiO x2 BO x3 One or more combinations of 0, where 0 <X1≤1.5,0<X2≤2,0<X3≤1.5; And / or, the transition metal elements contained in the transition metal-based particles include one or more of Fe, Co, Ni, Cu, and Zn, preferably including Cu; And / or, the content of the active combination in the nitride hydrolysis derivatization catalyst is 0.5 to 10.0 wt%; And / or, in the shell, the mass ratio of the nitride containing the first element to the oxide containing the first element is 1.5 to 2:1; And / or, the particle size of the transition metal-based particles is 3-5 nm.
3. The nitride hydrolysis derivatization catalyst according to claim 1, characterized in that: The chemical formula of the nitride hydrolysis derivatization catalyst is W / MO. x -MN, where W represents the transition metal element contained in the transition metal-based particles, the transition metal element being selected from one or more combinations of Fe, Co, Ni, Cu, and Zn, M representing the first element, MO x -MN represents a composite support composed of a nitride containing the first element and an oxide containing the first element, where 0 < X ≤ 2, and M is selected from one or more combinations of Al, B, and Si.
4. A method for preparing a nitride hydrolysis derivatization catalyst, characterized in that, include: A hydrolyzable nitrogen compound containing a first element is immersed in a solution containing an active component source, wherein the solvent of the solution includes water, so that the surface portion of the hydrolyzable nitrogen compound undergoes hydrolysis to form a hydroxide of the first element. The active component source includes a transition metal source that provides transition metal elements; The solvent is removed from the mixture obtained by hydrolysis to obtain the precursor material; The precursor material is calcined to obtain the intermediate material; The intermediate material is reduced to obtain a nitride hydrolysis-derived catalyst.
5. The preparation method according to claim 4, characterized in that: The first element includes one or more of Al, B, and Si; And / or, the hydrolyzable nitride containing the first element includes one or more combinations of AlN, BN and Si3N4; And / or, the transition metal element provided by the transition metal source includes one or more of Fe, Co, Ni, Cu, and Zn, preferably including Cu; And / or, the transition metal source includes water-soluble salts and / or complexes of the transition metal element; And / or, the impregnation temperature is 10–30°C, and the time is 6–18 hours; And / or, the water content in the solution reaches the saturation water absorption capacity of the hydrolyzable nitrogen compound; And / or, the mass ratio of the hydrolyzable nitrogen compound to the active component source is 100:0.5-5.
6. The method according to claim 4, characterized in that: The calcination temperature is 450-550℃; And / or, the calcination treatment time is 2-6 hours; And / or, the reduction treatment includes: bringing the intermediate material into full contact with a reducing gas and performing the reduction treatment at a temperature of 250–550°C; preferably, the reducing gas includes hydrogen, and the reduction treatment time is 1–5 hours. And / or, further comprising: calcining the hydrolyzable nitrogen compound before immersing it in a solution containing an active component source, preferably at a temperature of 500-700°C for 3-5 hours.
7. A nitride hydrolysis derivatization catalyst, characterized in that, It is prepared by the method described in any one of claims 4-6.
8. The use of the nitride hydrolysis derivatization catalyst according to any one of claims 1, 2, 3, and 7 in the catalytic hydrogenation of 5-hydroxymethylfurfural to 2,5-dihydroxymethylfuran.
9. A method for hydrogenating 5-hydroxymethylfurfural to produce 2,5-dihydroxymethylfuran, characterized in that, include: In a hydrogen-containing atmosphere, a mixed reaction system containing 5-hydroxymethylfurfural, a catalyst, and a solvent is reacted to generate 2,5-dihydroxymethylfuran; wherein the catalyst comprises the nitride hydrolysis derivatization catalyst according to any one of claims 1, 2, 3, and 7.
10. The method for hydrogenating 5-hydroxymethylfurfural to produce 2,5-dihydroxymethylfuran according to claim 9, characterized in that: The reaction temperature is 60–150°C; And / or, the reaction is carried out under hydrogen pressure conditions of 0.5 MPa to 5 MPa; And / or, the reaction time is 0.5 to 48 hours; And / or, the content of the catalyst in the mixed reaction system is 10-30% of the mass of 5-hydroxymethylfurfural; And / or, the solvent includes an organic solvent, which includes one or more of tetrahydrofuran, methanol, ethanol, isopropanol, dimethyl sulfoxide, N,N-dimethylformamide, γ-valerolactone, n-hexane, and ethyl acetate.