A kind of partial flower-like structure boron nitride and its preparation method and application in propane oxidative dehydrogenation
By combining high-temperature heat treatment with potassium chloride molten salt and aqua regia treatment, a partially flower-like boron nitride structure was successfully prepared, solving the problem of insufficient exposure of catalytic active sites in the h-BN catalyst during the propane oxidative dehydrogenation reaction, and achieving improved high conversion rate and stability.
Patent Information
- Application Number
- CN202611383814.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-08
- Publication Date
- 2026-11-20
AI Technical Summary
Existing hexagonal boron nitride (h-BN) catalysts suffer from insufficient exposure of catalytic active sites in propane oxidative dehydrogenation, making it difficult to achieve both high selectivity and high stability. Furthermore, existing stripping methods may lead to structural instability.
By employing a combination of potassium chloride molten salt high-temperature heat treatment and aqua regia treatment, controllable stripping and selective etching are achieved stepwise to form partially flower-like boron nitride structures, significantly improving the exposure of catalytic active sites.
It significantly improves the propane conversion rate in the propane oxidative dehydrogenation reaction by forming a three-dimensional flower-like nanosheet structure with a thickness of about 27 nm, thereby enhancing the activity and stability of the catalyst.
Smart Images

Figure CN123128034A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of catalyst preparation and oxygen-propane oxidative dehydrogenation technology, specifically relating to a partially flower-like boron nitride obtained by potassium chloride molten salt exfoliation method, its preparation method, and its application in propane oxidative dehydrogenation. Background Technology
[0002] Oxidative dehydrogenation of propane (ODHP) is an important route for propylene production, characterized by its lack of thermodynamic equilibrium constraints and low energy consumption. However, it still faces the challenge of balancing high selectivity and high stability in catalysts. Hexagonal boron nitride (h-BN) is considered a promising ODHP catalyst due to its high olefin selectivity, but its strong basal inertness and limited exposure of active sites (such as edge sites and defects) restrict its catalytic activity. Currently, the exposure of active sites in h-BN is mainly improved through structural modulation, defect introduction, and structural stripping. However, due to the strong interlayer forces and high structural stability of h-BN (interlayer spacing of approximately 3.5 Å), effective stripping and structural modulation remain challenging. Existing studies have shown that high-temperature treatment or intercalation can achieve interlayer expansion and stripping of h-BN, thereby increasing edge sites and improving the performance of oxidative dehydrogenation. However, excessive stripping may lead to structural instability and the formation of BOx species under high-temperature and water-containing conditions, thus affecting catalytic stability. Therefore, how to maintain the stability of h-BN while appropriately modulating its structure remains a problem that needs to be solved to improve ODHP performance. Summary of the Invention
[0003] To address the problems existing in the prior art, the present invention aims to propose a partially flower-like boron nitride, its preparation method, and its application in propane oxidative dehydrogenation. By performing high-temperature thermal stripping in a specific potassium chloride molten salt environment, and in conjunction with aqua regia post-treatment, the particle size and uniformity of boron nitride are successfully reduced, forming a partially flower-like structure, which significantly improves the propane conversion rate in the propane oxidative dehydrogenation reaction.
[0004] To achieve the above-mentioned technical objectives, the present invention adopts the following technical solution: A method for preparing partially flower-like boron nitride involves first mixing bulk boron nitride with potassium chloride molten salt, then subjecting it to a high-temperature melting heat treatment, and finally treating it with aqua regia to obtain partially flower-like boron nitride.
[0005] Furthermore, the mass ratio of the bulk boron nitride to potassium chloride molten salt is 1:1~3.
[0006] Furthermore, the temperature of the melt heat treatment is 850~950 ℃, and the time is 2-6 h.
[0007] Furthermore, the aqua regia treatment process is as follows: the sample obtained after high-temperature melting heat treatment is immersed in aqua regia at 60~100℃ for 8~12 hours.
[0008] This invention also provides partially flower-shaped boron nitride structures prepared by the above-described method.
[0009] This invention also provides an application of the aforementioned partially flower-like boron nitride structure, using it in the propane oxidative dehydrogenation reaction.
[0010] This invention first utilizes the unique environment of potassium chloride molten salt to pretreat bulk boron nitride. At high temperatures, molten KCl becomes a highly efficient heat and mass transfer medium, penetrating into the interlayer space of boron nitride. This is done solely to gently loosen and weaken the van der Waals forces between the layers, creating pre-exfoliated weak layers within the crystal, rather than completely exfoliating the boron nitride into independent nanosheets. Then, aqua regia is used for further treatment. This aqua regia attacks crystal defects, edge dislocations, and areas where interlayer bonding has been weakened due to the first heat treatment, ultimately forming a petal-like layered structure on the surface of the bulk material.
[0011] The core of this invention lies in the step-by-step realization of controllable exfoliation and selective etching. These two processes are not simply superimposed; their synergistic effect is key to forming the specific flower-like structure. We discovered that using molten salt heat treatment alone only yields bulk materials with weakened intercalation; while using aqua regia alone is difficult to effectively etch due to the high stability of bulk boron nitride. Only by combining the two can the pre-exfoliated weak layer created by molten salt heat treatment make selective etching by aqua regia possible. Both are indispensable, jointly achieving the specific flower-like morphology. This, in turn, provides more catalytically active sites, thereby improving the propane conversion rate in the propane oxidative dehydrogenation reaction.
[0012] The beneficial effects of this invention are reflected in: This invention utilizes a specific potassium chloride molten salt environment for high-temperature thermal stripping, combined with aqua regia post-treatment, to successfully reduce the particle size (approximately 27 nm) and uniformity of boron nitride, forming a flower-like structure, which significantly improves the propane conversion rate in the propane oxidative dehydrogenation reaction. Attached Figure Description
[0013] Figure 1 SEM images of the samples prepared in Comparative Example 1 and Comparative Example 2.
[0014] Figure 2 SEM images of the samples obtained in Example 1 and Comparative Examples 3-4. Detailed Implementation
[0015] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments, so that those skilled in the art can better understand and implement the present invention. However, the embodiments described are not intended to limit the present invention.
[0016] The catalyst in this invention is named BN- x KCl- y hA, where x This represents the mass ratio of KCl to BN. y The value represents the melting heat treatment time, and A represents the aqua regia treatment.
[0017] The bulk hexagonal boron nitride (BN) in this invention can be prepared using existing conventional methods. For example: Bulk boron nitride (BN): In a glove box, weigh 3 g of sodium borohydride (NaBH4) and 3 g of sodium amide (NaNH2), grind them thoroughly in a nickel mortar, and transfer the uniformly ground solid mixture to a sample vial; transfer the mixture to a nickel crucible and place it in a tube furnace for high-temperature treatment under a nitrogen atmosphere. The temperature program is as follows: hold at room temperature for 1 hour; increase the temperature to 500 °C at a rate of 5 °C / min and hold at this temperature for 1 hour; continue to increase the temperature to 850 °C and hold for 2 hours; after the heating program is completed, wait for the tube furnace to cool to room temperature, remove the nickel crucible, collect the powder sample, wash it with deionized water until neutral, and then dry it in a vacuum oven to obtain BN. Figure 1 As shown, this is a block structure.
[0018] The catalytic performance of boron nitride catalyst in the oxygen oxidative dehydrogenation (ODH) of propane was evaluated in an atmospheric pressure fixed-bed reactor. 200 mg of catalyst was used to construct a catalyst bed by fixing it in a quartz reaction tube with an inner diameter of 10 mm using quartz wool. The feed gas composition was 99.9 vol.% propane (C3H8), 99.9 vol.% oxygen (O2), and nitrogen (N2) as the balance gas, with a volume ratio of C3H8 / O2 / N2 = 1 / 1.5 / 3.5. The reaction space velocity was set at 7200 mL·g⁻¹. -1 ·h -1 The operating pressure was 0.1 MPa. Before the reaction began, the system was heated to 530 °C and the catalyst was pretreated in the reaction atmosphere for 30 minutes; then it was allowed to cool naturally to room temperature. During the formal reaction, the reaction temperature was controlled between 440-530 °C, and the catalyst was held at 440, 460, 480, 500, 510, 520, and 530 °C for 20 minutes, then cooled to 500 °C and held for 5 hours to evaluate the catalyst activity and thermal stability. The reaction products were analyzed using an online gas chromatograph (HUIFEN GC-7800) equipped with an alumina packed column and a flame ionization detector (FID) to detect the reaction gas components.
[0019] Example 1
[0020] Boron nitride (BN) and molten KCl were mixed at a mass ratio of 1:2 and ground in a mortar for 10 minutes to obtain a homogeneous BN / KCl mixture. This mixture was placed in a microreactor under a nitrogen atmosphere and heated to 900 °C at a heating rate of 5 °C / min, and held at this temperature for 2 hours. After heat treatment, the resulting sample was immersed in aqua regia (prepared from concentrated hydrochloric acid and concentrated nitric acid at a volume ratio of 3:1) for 10 hours, and then repeatedly washed with deionized water until the pH of the filtrate was close to neutral. The resulting boron nitride product was dried overnight in an oven at 65 °C and designated as BN-2KCl-2h-A.
[0021] like Figure 2 As shown, a distinct petal structure is formed on the surface of the block.
[0022] The test showed that the propane conversion rate was 37.63% after reacting at 500 °C for 300 min.
[0023] Example 2
[0024] Boron nitride (BN) and molten KCl were mixed at a mass ratio of 1:4 and ground in a mortar for 10 minutes to obtain a homogeneous BN / KCl mixture. This mixture was placed in a microreactor under a nitrogen atmosphere and heated to 900 °C at a heating rate of 5 °C / min, and held at this temperature for 2 hours. After heat treatment, the resulting sample was immersed in aqua regia (prepared from concentrated hydrochloric acid and concentrated nitric acid at a volume ratio of 3:1) for 10 hours, and then repeatedly washed with deionized water until the pH of the filtrate was close to neutral. The resulting boron nitride product was dried overnight in an oven at 65 °C and designated as BN-2KCl-4h-A.
[0025] The test showed that the propane conversion rate was 45.55% after reacting at 500 °C for 300 min.
[0026] Example 3
[0027] Boron nitride (BN) and molten KCl were mixed at a mass ratio of 1:6 and ground in a mortar for 10 minutes to obtain a homogeneous BN / KCl mixture. This mixture was placed in a microreactor under a nitrogen atmosphere and heated to 900 °C at a heating rate of 5 °C / min, and held at this temperature for 2 hours. After heat treatment, the resulting sample was immersed in aqua regia (prepared from concentrated hydrochloric acid and concentrated nitric acid at a volume ratio of 3:1) for 10 hours, and then repeatedly washed with deionized water until the pH of the filtrate was close to neutral. The resulting boron nitride product was dried overnight in an oven at 65 °C and designated as BN-2KCl-6h-A.
[0028] The test showed that the propane conversion rate was 35.88% after reacting at 500 °C for 300 min.
[0029] Comparative Example 1 Using BN directly as a catalyst, the propane conversion rate was tested to be 22.36% after reacting at 500 °C for 300 min.
[0030] Comparative Example 2 BN was soaked in aqua regia (prepared from concentrated hydrochloric acid and concentrated nitric acid in a volume ratio of 3:1) for 10 h, and then repeatedly washed with deionized water until the pH of the filtrate was close to neutral. The resulting boron nitride product was dried overnight in an oven at 65 °C and denoted as BN-A.
[0031] like Figure 1 As shown, BN-A is almost indistinguishable from the original bulk BN in morphology, maintaining its dense, angular, blocky shape. However, it should be noted that under high magnification, some weak etching pits appear on the surface of BN-A, but there are no lamellar lifts or flower-like structures. This demonstrates that aqua nitride alone is insufficient to remove bulk boron nitride. Because boron nitride is extremely chemically inert, aqua nitride can only wash away surface impurities or minor corrosion defects, but cannot overcome the van der Waals forces between layers.
[0032] The test showed that the propane conversion rate was 22.39% after reacting at 500 °C for 300 min.
[0033] Comparative Example 3 BN and molten salt KCl were mixed at a mass ratio of 1:2 and ground in a mortar for 10 minutes to obtain a homogeneous BN / KCl mixture. This mixture was placed in a microreactor under a nitrogen atmosphere and heated to 900 °C at a heating rate of 5 °C / min, and held at this temperature for 2 hours. The resulting boron nitride product was denoted as BN-2KCl-2h.
[0034] like Figure 2 As shown, obvious layered lifting and unevenness begin to appear on the surface of the block, but the layers are still stuck together and stacked, without forming an independently extending petal structure.
[0035] The test showed that the propane conversion rate was 12.74% after reacting at 500 °C for 300 min.
[0036] Comparative Example 4 Boron nitride (BN) and molten KCl were mixed at a mass ratio of 1:6 and ground in a mortar for 10 minutes to obtain a homogeneous BN / KCl mixture. This mixture was placed in a microreactor under a nitrogen atmosphere and heated to 900 °C at a heating rate of 5 °C / min, and held at this temperature for 2 hours. After heat treatment, the resulting sample was immersed in aqua regia (prepared from concentrated hydrochloric acid and concentrated nitric acid at a volume ratio of 3:1) for 10 hours, and then repeatedly washed with deionized water until the pH of the filtrate was close to neutral. The resulting boron nitride product was dried overnight in an oven at 65 °C and designated as BN-6KCl-2h-A.
[0037] like Figure 2 As shown, there are no discernible flaky protrusions or independent layers; it remains a block.
[0038] The test showed that the propane conversion rate was 28.32% after reacting at 500 ℃ for 300 min.
[0039] From the above, we can see that: 1. The original bulk boron nitride (BN) surface is dense, smooth, and structurally intact; the sample treated with aqua regia alone (BN-A) showed no significant morphological changes at either the macroscopic or microscopic scale. This fully demonstrates that due to the extremely high chemical inertness and stable interlayer van der Waals forces of boron nitride, aqua regia itself does not have the ability to peel off or destroy bulk boron nitride. Under these conditions, the effect of aqua regia is limited to the removal of surface impurities, rather than structural modification.
[0040] 2. The sample treated only with potassium chloride molten salt (BN-2KCl-2h) showed significant lamellar warping and microcracks on its surface, indicating a marked weakening of interlayer bonding and a pre-exfoliation intermediate structure. However, at this stage, the lamellar layers remained adhered and stacked, not yet fully opened to form an independent three-dimensional structure. This demonstrates that the core function of molten salt heat treatment is to utilize the penetration and intercalation effects of high-temperature molten salt to create the necessary conditions for subsequent structural modification.
[0041] 3. After treatment with aqua regia (BN-2KCl-2h-A), the originally adhered pre-exfoliated layers were selectively etched and fully released, forming well-defined, three-dimensional flower-like nanosheets with a significantly reduced thickness of approximately 27 nm. This indicates that the role of aqua regia here is not a conventional washing action, but rather a precise identification and preferential etching of grain boundary defects and weak interlayer regions created by molten salt heat treatment, transforming the pre-exfoliation into the final flower-like morphology.
[0042] In summary, the synergistic effect of KCl molten salt heat treatment and aqua regia selective etching in this invention successfully processed micron-sized bulk boron nitride into a three-dimensional flower-like structure with nanosheets of approximately 27 nm thickness, thereby significantly improving the catalytic activity of propane oxidative dehydrogenation.
Claims
1. A method for preparing partially flower-like boron nitride, characterized in that: First, bulk boron nitride is mixed with potassium chloride molten salt, then subjected to a high-temperature melting heat treatment, and finally treated with aqua regia to obtain flower-shaped boron nitride.
2. The preparation method according to claim 1, characterized in that: The mass ratio of the bulk boron nitride to potassium chloride molten salt is 1:1~3.
3. The preparation method according to claim 1, characterized in that: The melting heat treatment is performed at a temperature of 850~950℃ for 2-6 hours.
4. The preparation method according to claim 1, characterized in that: The process of aqua regia treatment is as follows: the sample obtained after high-temperature melting heat treatment is immersed in aqua regia at 60~100 ℃ for 8~12 h.
5. Partially flower-shaped boron nitride prepared by the preparation method according to any one of claims 1-4.
6. The application of the partially flower-like boron nitride structure as described in claim 5, characterized in that: It was used in the oxidative dehydrogenation reaction of propane.