Cu-zn-zr / hzsm-5 catalyst, its preparation method and application

By loading Cu, Zn, and Zr components onto HZSM-5 molecular sieve in a stepwise manner, a highly dispersed Cu-Zn-Zr/HZSM-5 catalyst is formed, which solves the problems of high cost of precious metal catalysts and easy sintering of non-precious metal catalysts. This achieves high selectivity and long-term stability, and promotes the efficient conversion of furfural to 2-methylfuran.

CN123128041APending Publication Date: 2026-11-20PUYANG HONGYE HI-TECH DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611180935.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-05
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

In existing technologies, precious metal catalysts are expensive and have low selectivity, while non-precious metal catalysts are prone to sintering of active components and have poor acid-base site matching, which makes it difficult to improve the selectivity of 2-methylfuran and results in insufficient long-term stability, thus restricting its industrial application.

Method used

A stepwise impregnation method was used to load Cu, Zn, and Zr components onto the surface of HZSM-5 molecular sieve. After drying, calcination, and high-temperature reduction, a Cu-Zn-Zr/HZSM-5 catalyst was formed. ZrO₂ inhibited Cu particle agglomeration, and HZSM-5 provided acidic sites that synergistically complemented the active metal centers. The reaction pathway was precisely controlled by optimizing the ratio of acidic and basic sites.

Benefits of technology

This approach achieves stability of highly dispersed metal active sites and close synergy of acid-base sites, improving the selectivity of 2-methylfuran and the long-term stability of the catalyst, reducing preparation costs, and ensuring efficient conversion of furfural to 2-methylfuran.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention discloses a Cu-Zn-Zr / HZSM-5 catalyst, its preparation method, and its applications. The invention involves stepwise impregnation of Cu, Zn, and Zr components onto the surface of an HZSM-5 molecular sieve, followed by drying and calcination to form a catalyst precursor. After high-temperature reduction in a hydrogen atmosphere, the Cu species are reduced to highly dispersed metallic Cu. 0 The active sites, Zn and Zr, exist in oxide form. ZrO2 can effectively inhibit Cu particle aggregation and improve metal dispersion and structural stability. HZSM-5 provides acidic sites and shape-selective channels, forming a synergistic catalytic system with the metal active centers. The Cu-Zn-Zr / HZSM-5 catalyst prepared in this invention achieves close synergy at the nanoscale between the acidic sites provided by HZSM-5 and the basic sites provided by Zn species. The acidic sites catalyze dehydration and C-C bond formation, while the basic sites stabilize reaction intermediates and inhibit side reactions. By optimizing the acid-base site concentration ratio to 1:1.2, it can precisely guide 2-methylfuran and inhibit the formation of byproducts such as furfuryl alcohol, thereby achieving precise control of the reaction pathway.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of non-precious metal heterogeneous catalysis technology, and more specifically to a Cu-Zn-Zr / HZSM-5 catalyst, its preparation method, and its application. Background Technology

[0002] 2-Methylfuran is an important class of high-value-added chemicals, widely used as a green solvent, clean fuel additive, and pharmaceutical intermediate. Traditional preparation methods typically involve multiple reaction steps, complex processes, and low overall product yields. Direct synthesis of 2-methylfuran from biomass-based furfural via a one-step catalytic conversion offers significant advantages, including renewable raw materials, a short reaction pathway, and high atom economy, making it a crucial development direction in the fields of green catalysis and high-value utilization of biomass.

[0003] The one-step preparation of 2-methylfuran from furfural involves a complex reaction network, primarily including furfural hydrogenation to furfuryl alcohol, dehydration of the intermediate to 2-methylfuran, and byproducts such as excessive hydrogenation of the furan ring to form pentanol, as well as side reactions such as furfural self-condensation and resinification. Therefore, achieving precise control of the reaction pathway and suppressing side reactions is the core challenge of this technical route.

[0004] While existing noble metal catalysts (such as Pd and Pt-based catalysts) exhibit certain catalytic activity, they suffer from problems such as high raw material costs, generally low selectivity for 2-methylfuran (typically below 90%), and the easy production of furfuryl alcohol, methylfurfural, and pentanol as byproducts. Non-noble metal Cu-based catalysts, although inexpensive, generally suffer from drawbacks such as easy sintering and agglomeration of active components, poor acid-base site matching and synergistic effects, difficulty in improving target product selectivity, and insufficient long-term operational stability, which restrict their industrial application. Summary of the Invention

[0005] The purpose of this invention is to address the problems mentioned in the background section by providing a Cu-Zn-Zr / HZSM-5 catalyst, its preparation method, and its application.

[0006] To achieve the above objectives, the present invention specifically adopts the following technical solution: A method for preparing a Cu-Zn-Zr / HZSM-5 catalyst includes the following steps: S1. Dissolve copper and zinc sources in deionized water to prepare a mixed solution with a total metal concentration of 0.7~0.9 mol / L; immerse the mixed solution on pretreated HZSM-5 molecular sieve, let it stand at room temperature, and then dry and calcine it sequentially to obtain Cu-Zn / HZSM-5 intermediate.

[0007] Furthermore, in S1, the standing time at room temperature is 12h, the drying time is 6h at 120℃, the calcination time is 4h at 450℃, and the heating rate is 2℃ / min.

[0008] Furthermore, the total metal concentration of the mixed solution is 0.8 mol / L, and the concentration of the Zr solution is 0.3 mol / L.

[0009] S2. Dissolve the zirconium source in deionized water to prepare a Zr solution with a concentration of 0.2~0.4 mol / L. Impregnate the Zr solution onto the Cu-Zn / HZSM-5 intermediate. After standing at room temperature, dry and calcine sequentially to obtain the catalyst precursor.

[0010] Furthermore, in S2, the standing time at room temperature is 10 hours, the drying time is 6 hours at 120°C, the calcination time is 5 hours at 500°C, and the heating rate is 2°C / min.

[0011] Further, the copper source includes Cu(NO3)2·3H2O or Cu(NO3)2, the zinc source includes Zn(NO3)2·6H2O or Zn(NO3)2, and the zirconium source includes ZrOCl2·8H2O or ZrO(NO3)2·2H2O.

[0012] Furthermore, the copper source is Cu(NO3)2·3H2O, the zinc source is Zn(NO3)2·6H2O, and the zirconium source is ZrOCl2·8H2O.

[0013] S3. The catalyst precursor is placed in an H2 / N2 atmosphere with a volume fraction of 9~11%, and reduced and activated at 340~360℃ for 170~190min. After natural cooling to room temperature, Cu-Zn-Zr / HZSM-5 catalyst is obtained.

[0014] Furthermore, the volume fraction of the H2 / N2 atmosphere is 10%, and the reduction and activation temperature is 350°C and the time is 180 min.

[0015] This invention involves sequentially loading Cu, Zn, and Zr components onto the surface of HZSM-5 molecular sieve via stepwise impregnation, followed by drying and calcination to form a catalyst precursor. After high-temperature reduction in a hydrogen atmosphere, the Cu species are reduced to highly dispersed metallic Cu. 0 The active sites, Zn and Zr, exist in oxide form. ZrO2 can effectively inhibit Cu particle agglomeration and improve metal dispersion and structural stability; HZSM-5 provides acidic sites and shape-selective channels, forming a synergistic catalytic system with the metal active centers, ultimately yielding the Cu-Zn-Zr / HZSM-5 catalyst.

[0016] As an inventive concept with the same technical solution described above, the present invention also claims protection for a Cu-Zn-Zr / HZSM-5 catalyst prepared by any of the preparation methods described above.

[0017] Furthermore, the Cu-Zn-Zr / HZSM-5 catalyst includes a support and an active component supported on the support. The support is the HZSM-5 molecular sieve, and the active component includes, by mass fraction of metal elements, 5.0~6.5 wt% Cu, 3.0~6.0 wt% Zn, and 1.5~2.0 wt% Zr.

[0018] HZSM-5 molecular sieves not only provide a high specific surface area and a regular pore structure, but their moderately Brønsted acidic sites, regulated by the silica-alumina ratio, are also key to catalyzing the dehydration of furfuryl alcohol intermediates and further methylation to 2-methylfuran. The strength of these acidic sites is rationally designed to effectively drive dehydration and methylation reactions while avoiding excessive acidity that could lead to deep deoxygenation or carbon deposition side reactions.

[0019] The active components Cu, Zn, and Zr are highly dispersed on the surface and within the pores of the HZSM-5 molecular sieve, forming strongly interacting composite metal oxides / metal particles. Specifically, Cu is the primary hydrogenation active center. The introduction of the auxiliary agent Zn, on the one hand, forms an alloy or strong interaction with Cu, altering the electron cloud density of Cu and promoting the dissociation and activation of H2; on the other hand, the Zn species itself provides moderately basic sites, stabilizing the oxygen atoms on the furan ring and effectively suppressing the ring-opening side reaction of the furan ring under excessive hydrogenation conditions. The addition of the auxiliary agent Zr, as a structural and electronic aid, further stabilizes the Cu-Zn particles, preventing their high-temperature sintering, and modulates the redox properties of Cu through electronic interactions, enhancing its selective hydrogenation ability towards carbonyl groups (C=O).

[0020] Furthermore, the active component comprises, by mass fraction of metal elements, 5.8 wt% Cu, 3.5 wt% Zn and 1.8 wt% Zr.

[0021] Furthermore, the Cu-Zn-Zr / HZSM-5 catalyst has a specific surface area ≥450 m². 2 / g, pore volume ≥0.90cm 3 / g provides ample space for diffusion and reaction of reactants and contributes to the stable dispersion of active components.

[0022] Furthermore, the concentration ratio of acidic sites to basic sites on the surface of the Cu-Zn-Zr / HZSM-5 catalyst is 1:1.2.

[0023] The Cu-Zn-Zr / HZSM-5 catalyst provided by this invention achieves close synergy at the nanoscale between acidic sites provided by HZSM-5 and basic sites provided by Zn species. The acidic sites primarily catalyze dehydration and C / C bond formation (methylation), while the basic sites stabilize key reaction intermediates and suppress side reactions. By optimizing the acid-base site concentration ratio to 1:1.2, the reaction pathway can be precisely directed towards 2-methylfuran, inhibiting the formation of byproducts such as furfuryl alcohol, methylfurfural, and pentanol, thereby achieving precise control over the reaction pathway.

[0024] As an inventive concept with the same technical solution as the above, the present invention also claims protection for the application of Cu-Zn-Zr / HZSM-5 catalyst described above in the one-step preparation of 2-methylfuran from liquid furfural under a hydrogen atmosphere; The reaction temperature for preparing 2-methylfuran was 180–200 °C, the reaction pressure was 0.8–1.0 MPa, and the liquid hourly space velocity (LISH) of liquid furfural was 0.5–0.6 h⁻¹. -1 The molar ratio of hydrogen to furfural is 6~9:1.

[0025] Furthermore, the reaction temperature is 190°C, the reaction pressure is 0.9 MPa, and the liquid hourly space velocity (LHSV) of liquid furfural is 0.55 h⁻¹. -1 The molar ratio of hydrogen to furfural is 8:1.

[0026] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. Cu, Zn, and Zr components are sequentially loaded onto the surface of HZSM-5 molecular sieve through stepwise impregnation, followed by drying and calcination to form a catalyst precursor. After high-temperature reduction in a hydrogen atmosphere, Cu species are reduced to highly dispersed metallic Cu. 0 The active sites, Zn and Zr, exist in oxide form. ZrO2 can effectively inhibit Cu particle agglomeration and improve metal dispersion and structural stability; HZSM-5 provides acidic sites and shape-selective channels, forming a synergistic catalytic system with the metal active centers, ultimately yielding the Cu-Zn-Zr / HZSM-5 catalyst; the use of non-noble metals Cu, Zn, and Zr reduces the preparation cost; 2. The Cu-Zn-Zr / HZSM-5 catalyst prepared in this invention achieves close synergy at the nanoscale between acidic sites provided by HZSM-5 and basic sites provided by Zn species. The acidic sites primarily catalyze dehydration and C / C bond formation (methylation), while the basic sites stabilize key reaction intermediates and suppress side reactions. By optimizing the acid-base site concentration ratio to 1:1.2, the reaction pathway can be precisely directed towards 2-methylfuran, inhibiting the formation of byproducts such as furfuryl alcohol, methylfurfural, and pentanol, thereby achieving precise control over the reaction pathway. Detailed Implementation

[0027] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. The materials and instruments used in the following embodiments are all commercially available.

[0028] In a first aspect, embodiments of the present invention provide a method for preparing a Cu-Zn-Zr / HZSM-5 catalyst, comprising the following steps: S1. Dissolve copper and zinc sources in deionized water to prepare a mixed solution with a total metal concentration of 0.7~0.9 mol / L; immerse the mixed solution on pretreated HZSM-5 molecular sieve, let it stand at room temperature, and then dry and calcine it sequentially to obtain Cu-Zn / HZSM-5 intermediate.

[0029] Furthermore, in S1, the standing time at room temperature is 12h, the drying time is 6h at 120℃, the calcination time is 4h at 450℃, and the heating rate is 2℃ / min.

[0030] Furthermore, the total metal concentration of the mixed solution is 0.8 mol / L, and the concentration of the Zr solution is 0.3 mol / L.

[0031] S2. Dissolve the zirconium source in deionized water to prepare a Zr solution with a concentration of 0.2~0.4 mol / L. Impregnate the Zr solution onto the Cu-Zn / HZSM-5 intermediate. After standing at room temperature, dry and calcine sequentially to obtain the catalyst precursor.

[0032] Furthermore, in S2, the standing time at room temperature is 10 hours, the drying time is 6 hours at 120°C, the calcination time is 5 hours at 500°C, and the heating rate is 2°C / min.

[0033] Further, the copper source includes Cu(NO3)2·3H2O or Cu(NO3)2, the zinc source includes Zn(NO3)2·6H2O or Zn(NO3)2, and the zirconium source includes ZrOCl2·8H2O or ZrO(NO3)2·2H2O.

[0034] Furthermore, the copper source is Cu(NO3)2·3H2O, the zinc source is Zn(NO3)2·6H2O, and the zirconium source is ZrOCl2·8H2O.

[0035] S3. The catalyst precursor is placed in an H2 / N2 atmosphere with a volume fraction of 9~11%, and reduced and activated at 340~360℃ for 170~190min. After natural cooling to room temperature, Cu-Zn-Zr / HZSM-5 catalyst is obtained.

[0036] Furthermore, the volume fraction of the H2 / N2 atmosphere is 10%, and the reduction and activation temperature is 350°C and the time is 180 min.

[0037] Secondly, embodiments of the present invention provide a Cu-Zn-Zr / HZSM-5 catalyst prepared by the aforementioned preparation method.

[0038] Furthermore, the Cu-Zn-Zr / HZSM-5 catalyst includes a support and an active component supported on the support. The support is the HZSM-5 molecular sieve, and the active component includes, by mass fraction of metal elements, 5.0~6.5 wt% Cu, 3.0~6.0 wt% Zn, and 1.5~2.0 wt% Zr.

[0039] Furthermore, the active component comprises, by mass fraction of metal elements, 5.8 wt% Cu, 3.5 wt% Zn and 1.8 wt% Zr.

[0040] Furthermore, the Cu-Zn-Zr / HZSM-5 catalyst has a specific surface area ≥450 m². 2 / g, pore volume ≥0.90cm 3 / g, and the concentration ratio of acidic sites to basic sites on the surface is 1:1.2.

[0041] Thirdly, embodiments of the present invention provide an application of the aforementioned Cu-Zn-Zr / HZSM-5 catalyst in the one-step preparation of 2-methylfuran from liquid furfural under a hydrogen atmosphere; The reaction temperature for preparing 2-methylfuran was 180–200 °C, the reaction pressure was 0.8–1.0 MPa, and the liquid hourly space velocity (LISH) of liquid furfural was 0.5–0.6 h⁻¹. -1 The molar ratio of hydrogen to furfural is 6~9:1.

[0042] Furthermore, the reaction temperature is 190°C, the reaction pressure is 0.9 MPa, and the liquid hourly space velocity (LHSV) of liquid furfural is 0.55 h⁻¹. -1 The molar ratio of hydrogen to furfural is 8:1.

[0043] The present invention will be further described below with reference to specific embodiments and comparative examples.

[0044] Example 1 (1) Carrier pretreatment: Take 10.0g of HZSM-5 molecular sieve (SiO2 / Al2O3 molar ratio = 30), place it in a drying oven, dry at 120℃ for 4h, and take it out for use.

[0045] (2) Impregnation loading of Cu and Zn: Weigh Cu(NO3)2·3H2O and Zn(NO3)2·6H2O, wherein the loading of Cu element is 5.8wt% and the loading of Zn element is 3.5wt%; dissolve the two together in an appropriate amount of deionized water and stir until completely dissolved to prepare a mixed solution with a total metal concentration of 0.8mol / L.

[0046] The above mixed solution was uniformly sprayed onto the pretreated HZSM-5 support using the equal volume impregnation method. After standing at room temperature for 12 hours, it was dried at 120°C for 6 hours, then heated to 450°C in air at 2°C / min and calcined for 4 hours. After naturally cooling to room temperature, Cu-Zn / HZSM-5 intermediate was obtained.

[0047] (3) Impregnation loading of Zr additive: Weigh ZrOCl2·8H2O, which corresponds to a Zr element loading of 1.8wt%, dissolve it in an appropriate amount of deionized water, stir until completely dissolved, and prepare a Zr solution with a concentration of 0.3mol / L.

[0048] The Zr solution was uniformly sprayed onto the Cu-Zn / HZSM-5 intermediate using the equal-volume impregnation method. The mixture was allowed to stand at room temperature for 10 hours, dried at 120°C for 6 hours, and then heated to 500°C in air at a rate of 2°C / min for 5 hours. After natural cooling to room temperature, the catalyst precursor was obtained.

[0049] (4) Reduction and activation: The catalyst precursor was placed in a fixed-bed reactor, and a mixed atmosphere of H2 / N2 with a volume fraction of 10% was introduced. The temperature was increased to 350℃ at 5℃ / min, and the reduction was carried out at a constant temperature for 3h. The catalyst was then naturally cooled to room temperature to obtain a specific surface area of ​​462m². 2 / g, pore volume 0.93cm 3 / g Cu-Zn-Zr / HZSM-5 catalyst.

[0050] (5) Evaluation of Cu-Zn-Zr / HZSM-5 catalyst: 1.0 g of 40-60 mesh Cu-Zn-Zr / HZSM-5 catalyst was packed into the isothermal section of a fixed-bed reactor; hydrogen was introduced to purge and remove air and impurities, and the temperature was raised to 190℃ and stabilized; the reaction pressure was adjusted to 0.9 MPa, the molar ratio of hydrogen to furfural was controlled at 8:1, and the reaction was carried out at a liquid hourly space velocity of 0.55 h⁻¹. -1 Liquid furfural is introduced to carry out a catalytic reaction.

[0051] Samples were taken and analyzed 2 hours after the reaction stabilized. The results showed that the furfural conversion rate was 100% and the selectivity for 2-methylfuran was 100%.

[0052] After 1000 hours of continuous operation, the furfural conversion rate and 2-methylfuran selectivity remained unchanged, and the catalyst activity retention rate was 99.3%.

[0053] The catalyst specific surface area was 458 m² after 1000 h of reaction. 2 / g, pore volume 0.92cm 3 / g; NH3-TPD and CO2-TPD tests showed that the concentration ratio of acid-base sites on the catalyst was 1:1.18.

[0054] Example 2 The difference between this embodiment and Embodiment 1 is that only the metal loading is changed to 5.0 wt% Cu, 3.0 wt% Zn, and 1.5 wt% Zr.

[0055] After the reaction stabilized for 2 hours, samples were taken for analysis. The results showed that the furfural conversion rate was 100%, the selectivity of 2-methylfuran was 99.8%, and the main byproduct was furfuryl alcohol (0.2%).

[0056] After 1000 hours of continuous operation, the furfural conversion rate was 99.5%, the selectivity for 2-methylfuran was 99.7%, and the catalyst activity retention rate was 99.0%.

[0057] The catalyst specific surface area was 456 m² after 1000 h of reaction. 2 / g, pore volume is 0.91cm 3 / g; NH3-TPD and CO2-TPD tests showed that the concentration ratio of acid-base sites on the catalyst was 1:1.19.

[0058] Example 3 The difference between this embodiment and Embodiment 1 is that only the metal loading is changed to 6.5 wt% Cu, 4.0 wt% Zn, and 2.0 wt% Zr.

[0059] Samples were taken and analyzed 2 hours after the reaction stabilized. The results showed that the furfural conversion rate was 100%, the selectivity of 2-methylfuran was 99.5%, and the main byproduct was 0.5% methylfurfural.

[0060] After 1000 hours of continuous operation, the furfural conversion rate was 98.5%, the selectivity for 2-methylfuran was 99.5%, and the catalyst activity retention rate was 98.8%.

[0061] The catalyst specific surface area was 450 m² after 1000 h of reaction. 2 / g, pore volume 0.90cm 3 / g; NH3-TPD and CO2-TPD tests showed that the concentration ratio of acid-base sites on the catalyst was 1:1.25.

[0062] The following is a comparative analysis of Examples 1-3. The evaluation results of Examples 1-3 are shown in Table 1: Table 1 Evaluation results of Examples 1-3 Examples 1-3 only varied the metal loadings of Cu, Zn, and Zr, while the other preparation and evaluation conditions remained the same. As shown in Examples 1-3 and Table 1, the control of metal loading significantly affects the catalytic performance, structural stability, and acid-base synergistic effect of the Cu-Zn-Zr / HZSM-5 catalyst: First, the metal loading ratio in Example 1 (Cu 5.8wt%, Zn 3.5wt%, Zr 1.8wt%) is the optimal ratio, and after 1000 h of reaction, the catalyst specific surface area increased from 462 m² / h. 2 / g decreased to 458m 2 / g, a decrease of only 0.87%, and pore volume from 0.93cm 3 / g decreased to 0.92cm 3 The change in concentration was minimal, indicating that the catalyst possesses strong anti-sintering ability and structural stability, enabling long-term stable operation. Secondly, Example 1 exhibited the best acid-base site synergy, with an acid-base site concentration ratio of 1:1.18. This ratio can regulate the reaction pathway for the one-step synthesis of 2-methylfuran from furfural, effectively suppressing side reactions such as furfuryl alcohol and methylfurfural, achieving 100% furfural conversion and 100% 2-methylfuran selectivity. Finally, the catalyst demonstrated outstanding long-term catalytic stability; after 1000 hours of continuous operation, both conversion and selectivity remained unchanged, with an activity retention rate as high as 99.3%, far exceeding that of Examples 2-3. Example 2, due to its low metal loading and insufficient number of active centers, produced trace amounts of furfuryl alcohol as a byproduct, resulting in a slight decrease in activity retention rate after long-term operation. Example 3, due to its excessively high metal loading, led to easy aggregation of active components on the catalyst surface, resulting in the most significant decrease in specific surface area. Simultaneously, the acid-base site ratio became unbalanced, producing the byproduct methylfurfural, and the long-term activity retention rate dropped to 98.8%.

[0063] Comparative Example 1 The difference between this comparative example and Example 1 is that a Cu-Zn / HZSM-5 catalyst containing only 5.8 wt% Cu and 3.5 wt% Zn was prepared.

[0064] Comparative Example 2 The difference between this comparative example and Example 1 is that: no HZSM-5 acidic support was used, and neutral SiO2 was used as the support to prepare the Cu-Zn-Zr / SiO2 catalyst.

[0065] Comparative Example 3 The difference between this comparative example and Example 1 is that HZSM-5 with a SiO2 / Al2O3 molar ratio of 15 is used as the carrier.

[0066] The following is a comparative analysis of Example 1 and Comparative Examples 1-3. The evaluation results of Comparative Examples 1-3 are shown in Table 2: Table 2 Evaluation results of Comparative Examples 1-3 As shown in Example 1, Tables 1 and 2, and Comparative Example 1, Comparative Example 1, without the addition of Zr promoter, had a catalyst acid-base site concentration ratio of only 1:1.05, weakening the acid-base synergistic effect and making it impossible to precisely control the furfural hydrodeoxygenation reaction pathway. This resulted in an initial furfural conversion rate of only 98%, a 2-methylfuran selectivity of only 88%, and furfuryl alcohol as the main byproduct, along with a small amount of other impurities. After only 500 hours of long-term operation, the catalyst activity and selectivity significantly decreased, the Cu active component showed obvious sintering, poor structural stability, and overall catalytic performance far lower than that of Example 1. This indicates that the introduction of Zr promoter can effectively control the acid-base site ratio on the catalyst surface, inhibit the agglomeration and sintering of active metals, and significantly improve catalytic activity, target product selectivity, and long-term stability.

[0067] A comparison of Example 1 and Comparative Example 2 shows that Comparative Example 2, which used neutral SiO2 instead of the HZSM-5 molecular sieve support, lacked suitable acidic sites in its catalyst, exhibited no significant acid-base synergistic effect, and completely deviated from the target product formation direction. Only furfural carbonyl hydrogenation to furfuryl alcohol occurred, with zero selectivity for 2-methylfuran, failing to achieve efficient one-step synthesis of 2-methylfuran from furfural. This demonstrates that the suitable acidic sites provided by the HZSM-5 molecular sieve support are crucial for constructing an efficient acid-base synergistic catalytic system and achieving the directed hydrogenation and deoxygenation of furfural to 2-methylfuran.

[0068] A comparison of Example 1 and Comparative Example 3 reveals that Comparative Example 3, using an HZSM-5 support with a SiO2 / Al2O3 molar ratio of 15, exhibits excessive acidity. The acid-base site concentration ratio becomes unbalanced at 1:0.8. This excessive acidity easily triggers the ring-opening side reaction of furfural-furan and accelerates coke formation, leading to rapid activity decay within 200 hours, a significant decrease in conversion and selectivity, and a substantial increase in byproduct content. This further demonstrates that only by using an HZSM-5 support with a suitable silicon-to-aluminum ratio, combined with the synergistic regulation of Cu, Zn, and Zr components, can a highly efficient catalyst with a well-matched acid-base ratio, stable structure, and resistance to coke formation and sintering be constructed, achieving high conversion, high selectivity, and long-term stable synthesis of 2-methylfuran from furfural.

[0069] Example 4 The difference between this embodiment and Example 1 is that the evaluation temperature of the Cu-Zn-Zr / HZSM-5 catalyst was adjusted to 180℃.

[0070] Samples were taken and analyzed 2 hours after the reaction stabilized. The results showed that the furfural conversion rate was 99.0% and the selectivity for 2-methylfuran was 100%. The reaction rate decreased slightly, but the selectivity remained good. This indicates that the catalyst of this invention can still operate efficiently and selectively at 180℃.

[0071] Example 5 The difference between this embodiment and Embodiment 1 is that the liquid hourly space velocity of liquid furfural is increased to 0.6 h⁻¹. -1 .

[0072] Sampling and analysis were performed 2 hours after the reaction stabilized. The results showed that the furfural conversion rate was 100% and the selectivity for 2-methylfuran was 99.0%. The reaction rate decreased slightly, but the selectivity remained good. The increased space velocity meant an increase in the yield per unit Cu-Zn-Zr / HZSM-5 catalyst. Under these conditions, the Cu-Zn-Zr / HZSM-5 catalyst still maintained good performance, demonstrating its good space-time yield.

[0073] Although embodiments of this application have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of this application, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a Cu-Zn-Zr / HZSM-5 catalyst, characterized in that, Includes the following steps: S1. Dissolve the copper source and zinc source in deionized water to prepare a mixed solution with a total metal concentration of 0.7~0.9 mol / L; The mixed solution was impregnated onto the pretreated HZSM-5 molecular sieve, and after being allowed to stand at room temperature, it was dried and calcined sequentially to obtain the Cu-Zn / HZSM-5 intermediate. S2. Dissolve the zirconium source in deionized water to prepare a Zr solution with a concentration of 0.2~0.4 mol / L. Impregnate the Zr solution onto the Cu-Zn / HZSM-5 intermediate. After standing at room temperature, dry and calcine sequentially to obtain the catalyst precursor. S3. The catalyst precursor is placed in an H2 / N2 atmosphere with a volume fraction of 9~11%, and reduced and activated at 340~360℃ for 170~190min. After natural cooling to room temperature, Cu-Zn-Zr / HZSM-5 catalyst is obtained.

2. The preparation method of the Cu-Zn-Zr / HZSM-5 catalyst as described in claim 1, characterized in that, The copper source includes Cu(NO3)2·3H2O or Cu(NO3)2, the zinc source includes Zn(NO3)2·6H2O or Zn(NO3)2, and the zirconium source includes ZrOCl2·8H2O or ZrO(NO3)2·2H2O.

3. The preparation method of the Cu-Zn-Zr / HZSM-5 catalyst as described in claim 1, characterized in that, In S1, the standing time at room temperature is 12h, the drying time is 6h at 120℃, the calcination time is 4h at 450℃, and the heating rate is 2℃ / min.

4. The method for preparing the Cu-Zn-Zr / HZSM-5 catalyst as described in claim 1, characterized in that, In S2, the standing time at room temperature is 10 hours, the drying time is 6 hours at 120°C, the calcination time is 5 hours at 500°C, and the heating rate is 2°C / min.

5. The preparation method of the Cu-Zn-Zr / HZSM-5 catalyst as described in claim 1, characterized in that, The total metal concentration of the mixed solution is 0.8 mol / L, the concentration of the Zr solution is 0.3 mol / L, the volume fraction of the H2 / N2 atmosphere is 10%, and the reduction activation temperature is 350℃ and the time is 180 min.

6. A Cu-Zn-Zr / HZSM-5 catalyst prepared by any one of the preparation methods described in claims 1 to 5.

7. The Cu-Zn-Zr / HZSM-5 catalyst as described in claim 6, characterized in that, It includes a support and an active component loaded on the support. The support is the HZSM-5 molecular sieve, and the active component includes, by mass fraction of metal elements, 5.0~6.5 wt% Cu, 3.0~6.0 wt% Zn and 1.5~2.0 wt% Zr. Among them, the Cu-Zn-Zr / HZSM-5 catalyst has a specific surface area ≥450m². 2 / g, pore volume ≥0.90cm 3 / g, and the concentration ratio of acidic sites to basic sites on the surface is 1:1.

2.

8. The Cu-Zn-Zr / HZSM-5 catalyst as described in claim 7, characterized in that, The active components comprise, by mass fraction of metal elements, 5.8 wt% Cu, 3.5 wt% Zn, and 1.8 wt% Zr.

9. The application of the Cu-Zn-Zr / HZSM-5 catalyst as described in claim 8 in the one-step preparation of 2-methylfuran from liquid furfural under a hydrogen atmosphere; in, The reaction temperature for preparing 2-methylfuran was 180–200 °C, the reaction pressure was 0.8–1.0 MPa, and the liquid hourly space velocity (LISH) of liquid furfural was 0.5–0.6 h⁻¹. -1 The molar ratio of hydrogen to furfural is 6~9:

1.

10. The application as described in claim 9, characterized in that, The reaction temperature was 190℃, the reaction pressure was 0.9MPa, and the liquid hourly space velocity (LISH) of liquid furfural was 0.55 h⁻¹. -1 The molar ratio of hydrogen to furfural is 8:1.