A catalyst and a method for direct conversion of carbon dioxide hydrogenation to prepare low-carbon alkanes
Patent Information
- Application Number
- CN202611109970.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-24
- Publication Date
- 2026-11-20
AI Technical Summary
[0005]本发明是为了克服现有技术CO2加氢直接制低碳烷烃的双功能催化剂对低碳烷烃选择性差、催化稳定性不佳的问题,提供一种催化剂及二氧化碳加氢直接转化制备低碳烷烃的方法,本发明采用具有SZR拓扑结构的SUZ-4分子筛与具有催化二氧化碳加氢形成含氧中间体能力的金属氧化物混合制得双功能催化剂,可催化二氧化碳和氢气直接转化生成低碳烷烃,其中低碳烷烃的选择性可以达到75~90%,副产物甲烷选择性低(<12%),且催化剂可以长期稳定运行
Smart Images

Figure CN123128044A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the technical field of low-carbon alkane preparation, and in particular to a catalyst and a method for the direct conversion of carbon dioxide hydrogenation to prepare low-carbon alkane. Background Technology
[0002] Low-carbon alkanes refer to alkanes with 4 or fewer carbon atoms (ethane, propane, and butane), and they have wide applications in civilian fuels, liquefied petroleum gas (LPG) blending components, dehydrogenation to olefins, and aromatization. Currently, the production of low-carbon alkanes mainly relies on the recovery of by-product gases from oil refineries (such as catalytic cracking and hydrocracking tail gas) and the separation of associated gases from natural gas fields. However, with the global energy structure transformation and increasingly stringent environmental regulations, the expansion of traditional refining capacity is limited, and relying solely on fossil resource by-products is no longer sufficient to meet the growing demand for high-purity low-carbon alkanes. Furthermore, traditional processes are highly dependent on oil and gas extraction, resulting in significant carbon dioxide emissions during production. Therefore, utilizing CO2 as a usable carbon resource and catalytically converting it into high-value-added low-carbon alkanes through a one-step hydrogenation reaction is of great significance for achieving closed-loop utilization of carbon resources and ensuring a clean energy supply.
[0003] Currently, research on the direct production of hydrocarbons via CO2 hydrogenation mainly focuses on low-carbon olefins, aromatics, or liquid fuels, while reports on direct catalytic conversion technologies for low-carbon alkanes are relatively few. Among existing CO2 hydrogenation technologies, the methanol-mediated route employs bifunctional catalysts combining metal oxides and molecular sieves. By selecting molecular sieves with specific topologies to limit the carbon chain growth of the products, this is currently the mainstream strategy for achieving highly selective production of specific hydrocarbons. For example, when using SAPO-34 or ZSM-5 molecular sieves with eight-membered ring channels, the reaction intermediates can be highly selectively converted into low-carbon olefins under shape-selective catalysis within the confined transition state within the channels. However, when the target product is adjusted to low-carbon alkanes, catalyst design faces a significant contradiction: on the one hand, alkane formation requires the catalyst to have stronger hydrogenation active centers to promote deep saturation of intermediates; on the other hand, if molecular sieves with stronger acidity and more stringent pore constraints are selected to suppress olefin formation, such as SSZ-13 with a CHA topology or SSZ-39 with an AEI topology, although their stronger acid centers are conducive to the hydrogen transfer reaction to produce alkanes, the excessive acidity will drastically accelerate the formation and deposition of polycyclic aromatic hydrocarbons, leading to pore blockage of the molecular sieve. The catalyst will rapidly deactivate due to severe carbon deposition, exhibiting extremely poor stability. For example, patent CN118847202A discloses a bifunctional catalyst, method, and application for CO2 hydrogenation to LPG, which uses a mixed indium zirconium composite oxide and hydrogen-form HSSZ13 molecular sieve, significantly improving CO2 conversion and LPG yield, but this technology does not consider the long-term stability of the catalyst. The contradiction between "highly selective alkane production" and "long-term stable operation" has severely restricted the development of CO2 hydrogenation technology for the direct production of low-carbon alkanes.
[0004] Currently, there are no reports in existing technologies regarding the application of SUZ-4 molecular sieves (with SZR topology) to the direct production of low-carbon alkanes via CO2 hydrogenation. SUZ-4 molecular sieves possess a unique structure of alternating eight-membered and ten-membered ring channels, and their channel size and acidity characteristics differ significantly from conventional molecular sieves such as SSZ-13 and SSZ-39. Theoretically, they have the potential to achieve product distribution control in CO2 hydrogenation reactions. Summary of the Invention
[0005] This invention aims to overcome the problems of poor selectivity and inadequate catalytic stability of existing bifunctional catalysts for the direct conversion of CO2 hydrogenation to low-carbon alkanes. It provides a catalyst and a method for the direct conversion of CO2 hydrogenation to low-carbon alkanes. This invention uses a SUZ-4 molecular sieve with an SZR topology mixed with a metal oxide capable of catalyzing the formation of oxygen-containing intermediates from CO2 hydrogenation to obtain a bifunctional catalyst. This catalyst can catalyze the direct conversion of CO2 and hydrogen to low-carbon alkanes, achieving a selectivity of 75-90% for low-carbon alkanes and a low selectivity for the byproduct methane (<12%). Furthermore, the catalyst can operate stably for extended periods.
[0006] To achieve the above objectives, the present invention adopts the following technical solution: A catalyst is prepared by mechanically mixing a metal oxide and a molecular sieve; the metal oxide is InZr. x O 1+1.5x ,GaZr x O 1+1.5x ZnCr x O 1+1.5x ZnAl x O 1+1.5x ZnGa x O 1+1.5x and ZnZr x O 1+1.5x At least one of them, where x ranges from 0.1 to 10; the molecular sieve is SUZ-4 molecular sieve or Me-SUZ-4 molecular sieve modified with heteroatoms Me.
[0007] This invention provides a catalyst for the direct hydrogenation of CO2 to low-carbon alkanes, exhibiting high product yield and selectivity. The SUZ-4 molecular sieve and metal oxides work together. First, a bimetallic oxide composed of elements such as In, Zr, Ga, Zn, Cr, and Al catalyzes the reaction of carbon dioxide and hydrogen to produce an active gaseous methanol intermediate. The SUZ-4 molecular sieve further converts this intermediate to obtain low-carbon olefins, which are then hydrogenated at the acidic sites of the sieve to generate low-carbon alkanes, thus achieving the direct hydrogenation of carbon dioxide to low-carbon alkanes. On one hand, the SUZ-4 molecular sieve's role in balancing the tandem reaction promotes the activation and conversion of carbon dioxide and hydrogen by the metal oxides, thereby increasing the conversion rate. On the other hand, the SUZ-4 molecular sieve possesses a three-dimensional pore structure, with its eight- and ten-membered ring pores exhibiting a unique shape-selective effect. This allows the carbon chain length of the product to be controlled within the C2-C4 range, and heteroatom modification further modulates the strong acid centers, inhibiting coking formation on the catalyst and thus improving its stability.
[0008] Preferably, the heteroatom Me is one of Ca, Fe, Ni, and Zn.
[0009] Preferably, the preparation method of the SUZ-4 molecular sieve containing heteroatom modification includes the following steps: S1. After mixing silica sol, aluminum powder, Me nitrate, potassium hydroxide, tetraethylammonium hydroxide and water, the mixture is aged, hydrothermal crystallization is carried out, and then cooled, washed, separated and dried to obtain Na-Me-SUZ-4 molecular sieve. S2. Na-Me-SUZ-4 molecular sieve is added to an aqueous solution of ammonium nitrate for ion exchange, and then dried and calcined to obtain Me-SUZ-4 molecular sieve.
[0010] Both SUZ-4 molecular sieves and heteroatom-modified SUZ-4 molecular sieves can be prepared by hydrothermal method. Referring to the preparation method of SUZ-4 molecular sieves containing heteroatom modification, the hydrothermal crystallization raw materials of SUZ-4 molecular sieves do not contain heteroatom nitrates.
[0011] Preferably, the mass ratio of the metal oxide to the molecular sieve is 0.1 to 20:1. More preferably, the mass ratio is 0.3 to 5.
[0012] Preferably, the specific surface area of the metal oxide is 100~150 m². 2 / g. The active ingredient, metal oxide, has a higher specific surface area and more active sites, which is more conducive to the catalytic reaction.
[0013] Preferably, the molecular sieve has a moderately strong acid strength, and the amount of moderately strong acid sites is 0.005~0.6 mol / kg. More preferably, the amount of moderately strong acid sites is 0.005~0.4 mol / kg, and even more preferably, the amount of moderately strong acid sites is 0.005~0.2 mol / kg.
[0014] According to the NH3-TPD (ammonia temperature-programmed desorption) test, acidity can be defined by the desorption peaks of NH3, encompassing three types of acidity: weak acid, moderately strong acid, and strong acid. Under standard test conditions, the ratio of sample mass w to carrier gas flow rate f (w / f) = 100 g·h / L, the heating rate is 10℃ / min, and a thermal conductivity detector (TCD) records the thermal conductivity signal of desorbed NH3, plotting the desorption curve. Based on the peak position of the curve, the inorganic solid is classified into three acidities: weak acid refers to acidic sites with an NH3 desorption temperature below 245℃; moderately strong acid refers to acidic sites with an NH3 desorption temperature between 245 and 500℃; and strong acid refers to acidic sites with an NH3 desorption temperature above 500℃. The NH3-TPD test, by analyzing the desorption peaks at different temperatures, can characterize the acidity distribution of the sample, including the number and intensity of acidic sites. The molecular sieve of this invention, after testing, preferably contains 0.005~0.6 mol / kg of moderately strong acid sites.
[0015] Preferably, the mechanical mixing method includes one or more of mechanical stirring, ball milling, shaking table oscillation, and mechanical grinding. The required proportions of metal oxide and molecular sieve are added to a container for mechanical mixing to obtain the catalyst. The separation, crushing, and mixing are achieved by utilizing the extrusion, impact, shearing, and friction forces generated by the high-speed movement of the materials and / or the container. The conversion of mechanical energy, thermal energy, and chemical energy is achieved by adjusting the temperature and carrier gas atmosphere, further regulating the interactions between different components.
[0016] On the other hand, the present invention also provides a method for the direct conversion of carbon dioxide into low-carbon alkanes by hydrogenation, using a mixture of carbon dioxide and hydrogen as reactants, and carrying out the conversion reaction in a fixed bed or a moving bed, using the catalyst described above.
[0017] This invention uses carbon dioxide and hydrogen as reaction raw materials to directly convert low-carbon alkanes in one step. The selectivity of low-carbon alkanes can reach 83-88%, while the selectivity of the by-product methane is less than 11%, which has good application prospects.
[0018] Preferably, the temperature of the catalytic reaction is 300~500℃, and the space velocity of the mixed gas is 300~12000 mL g. -1 h -1 The pressure of the mixed gas is 0.5~10 MPa. More preferably, the temperature of the catalytic reaction is 320~450℃, and the space velocity of the mixed gas is 1000~9000 mL g. -1 h -1 The pressure of the gas mixture is 1~5 MPa. More preferably, the space velocity of the gas mixture is 3000~9000 mL g. -1 h -1 .
[0019] Preferably, the molar ratio of carbon dioxide to hydrogen is 1:0.2 to 4.5. More preferably, the molar ratio is 1:0.3 to 3.5.
[0020] Therefore, the present invention has the following beneficial effects: (1) In the catalyst of the present invention, SUZ-4 molecular sieve and metal oxide play a coupling role. The effect of molecular sieve on the equilibrium pull of series reaction can promote the activation and conversion of carbon dioxide and hydrogen by metal oxide and thus improve the conversion rate. Moreover, the eight-membered ring and ten-membered ring channel structure of SUZ-4 molecular sieve has a unique shape selection effect, which can control the carbon chain length of the product within the range of C2-C4 composition, improve the selectivity of low carbon alkanes, and the heteroatom modification can regulate the strong acid center, further inhibit the formation of carbon deposits in the catalyst, thereby improving the stability of the catalyst. (2) The preparation process of the catalyst of the present invention is simple and the conditions are mild. When used in the reaction process of direct production of low-carbon alkanes by CO2 hydrogenation, it has a high product yield and selectivity. The selectivity of low-carbon alkanes is the best, reaching 88%, and the selectivity of methane is less than 6%. The product is mainly composed of liquefied petroleum gas (LPG) components. The separation energy consumption is low and the technical economy is high. (3) This invention uses carbon dioxide as a usable carbon resource and catalytically converts it into high-value-added low-carbon alkanes in one step through hydrogenation reaction, which is of great significance for realizing the closed-loop utilization of carbon resources. Attached Figure Description
[0021] Figure 1 The image shows the X-ray diffraction pattern of SUZ-4 molecular sieve.
[0022] Figure 2 The results show the stability evaluation of the catalytic reaction in Example 2 and Comparative Example 1. Detailed Implementation
[0023] The present invention will now be further described with reference to the accompanying drawings and specific embodiments.
[0024] General Implementation Examples A catalyst is prepared by mechanically mixing a metal oxide and a molecular sieve; the metal oxide is InZr. x O 1+1.5x ,GaZr x O 1+1.5x ZnCr x O 1+1.5x ZnAl x O 1+1.5x ZnGa x O 1+1.5x and ZnZr x O 1+1.5x At least one of them, where x ranges from 0.1 to 10; the molecular sieve is SUZ-4 molecular sieve or Me-SUZ-4 molecular sieve modified with heteroatoms Me.
[0025] In one specific implementation, the heteroatom Me is one of Ca, Fe, Ni, and Zn.
[0026] As a specific implementation method, the preparation method of SUZ-4 molecular sieve containing heteroatom modification includes the following steps: S1. Mixing silica sol, aluminum powder, Me nitrate, potassium hydroxide, tetraethylammonium hydroxide and water, aging the mixture, performing hydrothermal crystallization, cooling, washing, separating, and drying to obtain Na-Me-SUZ-4 molecular sieve; S2. Adding the Na-Me-SUZ-4 molecular sieve to an ammonium nitrate aqueous solution for ion exchange, followed by drying and calcination to obtain Me-SUZ-4 molecular sieve. The preparation of SUZ-4 molecular sieve also adopts a hydrothermal method, and the raw materials for the hydrothermal crystallization of SUZ-4 molecular sieve (step S1) do not contain heteroatom-modified nitrates.
[0027] In one specific implementation, the mass ratio of metal oxide to molecular sieve is 0.1 to 20:1. In a more preferred implementation, the mass ratio is 0.3 to 5.
[0028] As one specific implementation method, the specific surface area of the metal oxide is 100~150 m². 2 / g; the molecular sieve has a moderately strong acid strength, and the amount of moderately strong acid sites is 0.005~0.6 mol / kg. As a preferred embodiment, the amount of moderately strong acid sites is 0.005~0.4 mol / kg; as an optimal embodiment, the amount of moderately strong acid sites is 0.005~0.2 mol / kg.
[0029] As a specific implementation method, the preparation method of metal oxide includes the following steps: using two of zinc nitrate, chromium nitrate, aluminum nitrate, zirconium nitrate, indium nitrate, and gallium nitrate as precursors, mixing the precursors with ammonium carbonate in water at room temperature, wherein ammonium carbonate is used as a precipitant, and the molar ratio of ammonium ions to metal ions is 1:1 (or, ammonium carbonate can be in excess); aging the resulting mixture, and after aging, taking it out, washing, filtering, and drying it in sequence; calcining the resulting solid in an air atmosphere to obtain metal oxide.
[0030] As a specific implementation method, the mechanical mixing methods of metal oxides and molecular sieves include one or more of mechanical stirring, ball milling, shaking table oscillation, and mechanical grinding.
[0031] In specific embodiments of the present invention, a) mechanical stirring: In a stirring tank, a stirring rod is used to mix the metal oxide and molecular sieve. By controlling the stirring time (5~120 min) and speed (30~300 rpm), the degree of mixing and relative distance between the metal oxide and molecular sieve can be adjusted; b) ball milling: The abrasive and the metal oxide and molecular sieve are rolled at high speed in a grinding tank, generating a strong impact and crushing on the catalyst, thereby dispersing and mixing the metal oxide and molecular sieve. By controlling the mass ratio of the abrasive (material can be stainless steel, agate, or quartz, size range: 5~15 mm) to the catalyst to 20~100:1, the particle size of the catalyst can be adjusted; c) shaking table oscillation: The metal oxide and molecular sieve are premixed and loaded into a container; by controlling the reciprocating or circular oscillation of the shaking table, the mixing of the metal oxide and molecular sieve is achieved; by adjusting the oscillation speed (range: 1~70 rpm) and time (range: 5~120 rpm), the mixing degree and relative distance between the metal oxide and molecular sieve can be adjusted. (min) to achieve uniform mixing and adjust their relative distance; d) Mechanical grinding: premix the metal oxide and molecular sieve and put them into a container. Under a certain pressure (range: 5~20 kg), the mixture is subjected to relative motion with the mixed catalyst through a grinding tool (speed range: 30~300 rpm) to adjust the catalyst particle size, relative distance and achieve uniform mixing.
[0032] In one specific implementation, the metal oxide and molecular sieve are mechanically mixed in an atmosphere or directly in air at a mixing temperature of 20-100°C. In specific embodiments of the invention, the atmosphere can be selected from any of the following gases: a) nitrogen and / or an inert gas; b) a mixture of hydrogen and nitrogen and / or an inert gas, wherein the volume of hydrogen in the mixture is 5-50%; c) a mixture of CO and nitrogen and / or an inert gas, wherein the volume of CO in the mixture is 5-20%; d) a mixture of O2 and nitrogen and / or an inert gas, wherein the volume of O2 in the mixture is 5-20%. The inert gas is one or more of helium, argon, and neon.
[0033] The present invention also provides a method for the direct conversion of the above-mentioned catalyst into low-carbon alkanes by hydrogenation of carbon dioxide, using a mixture of carbon dioxide and hydrogen as the reaction raw material, and carrying out the conversion reaction in a fixed bed or a moving bed.
[0034] In a specific embodiment of the present invention, the fixed-bed reactor or moving-bed reactor is equipped with a gas mass flow meter and an online product analysis chromatograph (the reactor tail gas is directly connected to the quantitative valve of the chromatograph for periodic real-time sampling and analysis). An inert gas (one or more of helium, argon, and neon) is used to replace the air in the reactor. A mixture of carbon dioxide and hydrogen is used as raw material to catalyze the reaction in contact with the catalyst. The molar ratio of carbon dioxide to hydrogen is 1:0.2~4.5, the reaction temperature is 300~500℃, the pressure of the mixed gas is 0.5~10 MPa, and the space velocity of the mixed gas is 300~12000 mLg. -1 h -1 .
[0035] In one specific implementation method, the molar ratio of carbon dioxide to hydrogen is 1:0.3~3.5, the temperature of the catalytic reaction is 320~450℃, and the space velocity of the mixed gas is 1000~9000 mL g. -1 h -1 The pressure of the gas mixture is 1~5 MPa. As a preferred embodiment, the space velocity of the gas mixture is 3000~9000 mL g. -1 h -1 .
[0036] The following specific embodiments illustrate the technical solution of the present invention, but the scope of protection of the present invention is not limited thereto. In the present invention, unless otherwise specified, all equipment and raw materials can be purchased from the market or are commonly used in the industry. Unless otherwise specified, the methods in the following embodiments are conventional methods in the art.
[0037] I. Preparation of Metal Oxides InZr₂O₄, GaZr₂O₄, ZnCr₂O₄, ZnAl₂O₄, ZnGa₂O₄, and ZnZr₂O₄ were prepared by a precipitation method, comprising the following steps: two of zinc nitrate, chromium nitrate, aluminum nitrate, zirconium nitrate, indium nitrate, and gallium nitrate were used as precursors; the precursors were mixed with ammonium carbonate in water at room temperature, wherein ammonium carbonate was used as a precipitant, and the molar ratio of ammonium ions to metal ions was 1:1; the resulting mixture was aged, and after aging, it was taken out and washed, filtered, and dried in sequence; the resulting solid was calcined in air atmosphere to obtain metal oxides; the specific preparation parameters are shown in Table 1.
[0038] Table 1 Preparation parameters of metal oxides
[0039] The remaining metal oxides, CuAl₂O₄, ZnO, and FeO, were commercially available. The 10% FeO+InZr₂O₄ catalyst was obtained by mixing ZnO and InZr₂O₄, with FeO accounting for 10% of the total mass of FeO+InZr₂O₄. As shown in Table 1, the specific surface area of the metal oxides prepared by the precipitation method was 110–140 m². 2 / g.
[0040] II. Molecular sieve preparation Both SUZ-4 molecular sieves and Me-SUZ-4 molecular sieves modified with heteroatoms were prepared by a hydrothermal method, as detailed below: (1) SUZ-4 molecular sieve The preparation method includes the following steps: Silica sol, aluminum powder, potassium hydroxide, tetraethylammonium hydroxide (templative agent), and deionized water are weighed according to the molar ratio of SiO2:Al2O3:KOH:TEAOH:H2O = 15:1.0:5:2:300. After mixing and aging at room temperature for 2 hours, the mixture is transferred to a stainless steel hydrothermal reactor and heated to 160°C at a heating rate of 2°C / min for rotary crystallization for 72 hours. After crystallization, the mixture is rapidly cooled to room temperature in a water bath and repeatedly centrifuged and washed until the pH of the supernatant is 7 at the end of the washing process. The precipitate is then dried at 120°C for 12 hours to obtain Na-SUZ-4 molecular sieve. The above Na-SUZ-4 molecular sieve powder is added to a 1.0 mol / L ammonium nitrate aqueous solution and subjected to ion exchange at 80°C for 4 hours, repeated twice. After drying and calcination at 500°C for 4 hours, conventional SUZ-4 molecular sieve is obtained.
[0041] (2) Ca-SUZ-4 molecular sieve The preparation method includes the following steps: Silica sol, aluminum powder, calcium nitrate, potassium hydroxide, tetraethylammonium hydroxide (templative agent), and deionized water are weighed according to the molar ratio of SiO2:Al2O3:Ca:KOH:TEAOH:H2O = 15:1.0:0.01:5:2:300. After mixing and aging at room temperature for 2 h, the mixture is transferred to a stainless steel hydrothermal reactor and heated to 160°C at a heating rate of 2°C / min for rotary crystallization for 72 h. After crystallization, the mixture is rapidly cooled to room temperature in a water bath and repeatedly centrifuged and washed until the pH of the supernatant is 7 at the end of the washing process. The precipitate is dried at 120°C for 12 h to obtain Na-Ca-SUZ-4 molecular sieve. The above Na-Ca-SUZ-4 molecular sieve raw powder is added to a 1.0 mol / L ammonium nitrate aqueous solution and subjected to ion exchange at 80°C for 4 h, repeated twice. After drying and calcination at 500°C for 4 h, Ca-SUZ-4 molecular sieve is obtained.
[0042] (3) Ni-SUZ-4 molecular sieve The preparation method includes the following steps: Silica sol, aluminum powder, nickel nitrate, potassium hydroxide, tetraethylammonium hydroxide (templative agent), and deionized water are weighed according to the molar ratio of SiO2:Al2O3:Ni:KOH:TEAOH:H2O = 15:1.0:0.01:5:2:300. After mixing and aging at room temperature for 2 h, the mixture is transferred to a stainless steel hydrothermal reactor and heated to 160°C at a heating rate of 2°C / min for rotary crystallization for 72 h. After crystallization, the mixture is rapidly cooled to room temperature in a water bath and repeatedly centrifuged and washed until the pH of the supernatant is 7 at the end of the washing process. The precipitate is dried at 120°C for 12 h to obtain Na-Ni-SUZ-4 molecular sieve. The above Na-Ni-SUZ-4 molecular sieve powder is added to a 1.0 mol / L ammonium nitrate aqueous solution and subjected to ion exchange at 80°C for 4 h, repeated twice. After drying and calcination at 500°C for 4 h, Ni-SUZ-4 molecular sieve is obtained.
[0043] (4) Fe-SUZ-4 molecular sieve The preparation method includes the following steps: Silica sol, aluminum powder, ferric nitrate, potassium hydroxide, tetraethylammonium hydroxide (templative agent), and deionized water are weighed according to the molar ratio of SiO2:Al2O3:Fe:KOH:TEAOH:H2O = 15:1.0:0.01:5:2:300. After mixing and aging at room temperature for 2 h, the mixture is transferred to a stainless steel hydrothermal reactor and heated to 160°C at a heating rate of 2°C / min for rotary crystallization for 72 h. After crystallization, the mixture is rapidly cooled to room temperature in a water bath and repeatedly centrifuged and washed until the pH of the supernatant is 7 at the end of the washing process. The precipitate is dried at 120°C for 12 h to obtain Na-Fe-SUZ-4 molecular sieve. The above Na-Fe-SUZ-4 molecular sieve powder is added to a 1.0 mol / L ammonium nitrate aqueous solution and subjected to ion exchange at 80°C for 4 h, repeated twice. After drying and calcination at 500°C for 4 h, Fe-SUZ-4 molecular sieve is obtained.
[0044] (5) Zn-SUZ-4 molecular sieve The preparation method includes the following steps: Silica sol, aluminum powder, zinc nitrate, potassium hydroxide, tetraethylammonium hydroxide (templative agent), and deionized water are weighed according to the molar ratio of SiO2:Al2O3:Zn:KOH:TEAOH:H2O = 15:1.0:0.01:5:2:300. After mixing and aging at room temperature for 2 h, the mixture is transferred to a stainless steel hydrothermal reactor and heated to 160°C at a heating rate of 2°C / min for rotary crystallization for 72 h. After crystallization, the mixture is rapidly cooled to room temperature in a water bath and repeatedly centrifuged and washed until the pH of the supernatant is 7 at the end of washing. The precipitate is dried at 120°C for 12 h to obtain Na-Zn-SUZ-4 molecular sieve. The above Na-Zn-SUZ-4 molecular sieve powder is added to a 1.0 mol / L ammonium nitrate aqueous solution and subjected to ion exchange at 80°C for 4 h, repeated twice. After drying and calcination at 500°C for 4 h, Zn-SUZ-4 molecular sieve is obtained.
[0045] The remaining SSZ-13, SSZ-39, and ZSM-35 molecular sieves were commercially available. X-ray diffraction pattern analysis was performed on the prepared SUZ-4 molecular sieve, as shown... Figure 1 As shown, it exhibits diffraction peaks with a typical SZR topology, proving the successful synthesis of SUZ-4 molecular sieve.
[0046] III. Catalyst Preparation The catalysts in Examples 1-10 and Comparative Examples 1-8 were obtained by mechanically mixing metal oxides and molecular sieves in the required proportions in a container. The mechanical mixing methods included: a) mechanical stirring: mixing the metal oxides and molecular sieves in a stirring tank using a stirring rod, controlling the stirring time and rate; b) ball milling: mixing the metal oxides and molecular sieves at high speed in a grinding jar using abrasive materials, controlling the mass ratio of the abrasive material and size to the catalyst; c) shaking table oscillation: pre-mixing the metal oxides and molecular sieves and placing them in a container, controlling the oscillation speed and time of the shaking table; d) mechanical grinding: pre-mixing the metal oxides and molecular sieves and placing them in a container, using a grinding tool to move relative to the mixture, controlling the pressure and relative motion rate to achieve final mixing. Specific catalyst preparation methods and their parameter characteristics are shown in Table 2.
[0047] Table 2. Preparation parameters of catalysts in Examples 1-10 and Comparative Examples 1-8
[0048] IV. Catalytic Reaction Catalytic reactions were carried out using carbon dioxide and hydrogen as raw materials, in contact with the catalysts of Examples 1-10 and Comparative Examples 1-8. 2 g of catalyst was placed in a fixed-bed reactor, the air in the reactor was purged with argon, and then the temperature was raised to 300°C in an H2 atmosphere. A mixture of carbon dioxide and hydrogen (H2 / CO2 molar ratio = 0.2~4.5) was switched, the pressure of the mixture was 0.5~10 MPa, and the temperature was raised to the reaction temperature of 300~500°C. The gas hourly space velocity (GHSV) of the mixture was adjusted to 300~12000 mL g. -1 h -1 The specific reaction parameters for different catalysts are shown in Table 3, and the products were analyzed by online chromatography.
[0049] Table 3 Catalytic reaction parameters used in Examples 1-10 and Comparative Examples 1-8
[0050] The application effects of the catalysts of Examples 1-10 and Comparative Examples 1-8 in the catalytic production of low-carbon alkanes from CO2 were determined and are shown in Table 4, including the initial CO2 conversion rate, CO2 conversion rate after 30 h of reaction, low-carbon alkane selectivity, and methane selectivity. Among them, the CO2 conversion rates of Examples 2 and Comparative Example 1 after 30 h of catalytic reaction are as follows: Figure 2 As shown.
[0051] Table 4. Application effects of catalysts in Examples 1-10 and Comparative Examples 1-8 (30h)
[0052] As shown in Table 4, Examples 1-10 demonstrate that by changing the temperature, pressure, space velocity, and the molar ratio of H2 / CO2 in the catalytic reaction, the final catalytic effect will vary, but the overall catalytic activity, selectivity, and stability are high. After 30 h of reaction, the CO2 conversion rate can still reach 30-40%, and after 30 h of reaction, the selectivity of low-carbon alkanes (one or more of ethane, propane, and butane) in hydrocarbon products can reach 83-88%, while the methane selectivity is less than 11%.
[0053] The comparative results of Comparative Example 1 and Example 2, Comparative Example 2 and Example 3, and Comparative Example 3 and Example 2 show that molecular sieves with different topologies significantly modulate the product selectivity. The molecular sieves used in Comparative Examples 1 and 2 were commercially available SSZ-13 and SSZ-39 catalysts, both possessing three-dimensional intersecting channels, eight-membered ring pore diameters, and pore sizes of 3.8 Å, suitable for C2-C4 hydrocarbons. However, due to the strong acidity of the catalysts, deactivation was relatively significant (e.g., ...). Figure 2Furthermore, the selectivity for low-carbon alkanes was only 72-73%, and the selectivity for methane was 13-14%. In Comparative Example 3, the molecular sieve used in the catalyst was the commercially available ZSM-35, which has two-dimensional ten-membered ring and eight-membered ring channels. The selectivity for low-carbon alkanes in the product was significantly reduced to only 45%, while the selectivity for hydrocarbons of C5 and above increased. At the same time, the catalyst was significantly deactivated.
[0054] Comparing Comparative Examples 4-5 with Example 1, Comparative Example 4 used a catalyst containing only metal oxides and no molecular sieves, resulting in a very low reaction conversion rate and products mainly consisting of dimethyl ether, methane, and other byproducts, with almost no low-carbon alkanes generated. Comparative Example 5 used a catalyst containing only molecular sieves and no metal oxides; since molecular sieves lack the ability to activate CO2, the catalytic reaction had almost no activity. Comparative Examples 4-5 demonstrate that the catalytic reaction effect is poor when only metal oxides or molecular sieves are used, completely lacking the excellent reaction performance described in this invention.
[0055] Comparing Comparative Example 6 and Example 4, the catalyst used in Comparative Example 6 was a Cu-based oxide, resulting in a very low conversion rate (8.3%), and the main products were byproducts such as methane, with very low selectivity for low-carbon alkanes (10%). Comparing Comparative Example 7 and Example 5, the catalyst used in Comparative Example 7 was a single-component ZnO, which had a large grain size and low specific surface area (<1 m²). 2 The catalyst in Comparative Example 8 (g) lacked partially reduced O-defect structures on its surface, resulting in a very low conversion rate and significant hydrogenation, with methane being the predominant product. Comparing Comparative Example 8 with Example 1, the catalyst in Comparative Example 8 contained 10% FeO in its oxide component, and the reaction product was mainly methane, with a significantly lower selectivity for low-carbon alkanes (25%) compared to Example 1 (86%). This is because the FeO in the catalyst was reduced during the reaction to form iron carbide, thus transforming the reaction process into the traditional Fischer-Tropsch synthesis route. The product distribution followed the ASF distribution, no longer meeting the requirements of this invention and failing to achieve the technical effects of this invention. The reaction results of Comparative Examples 6-8 demonstrate that the oxide component in the catalyst used is crucial for the preparation of highly selective low-carbon alkanes.
[0056] In summary, the catalyst prepared by mechanically mixing the specific metal oxide and SUZ-4 molecular sieve of this invention can be successfully used for the direct conversion of carbon dioxide hydrogenation to low-carbon alkanes, achieving high CO2 conversion rate and low-carbon alkane selectivity, and high low-carbon alkane yield.
Claims
1. A catalyst, prepared by mechanically mixing a metal oxide and a molecular sieve; characterized in that, The metal oxide is InZr. x O 1+1.5x ,GaZr x O 1+1.5x ZnCr x O 1+1.5x ZnAl x O 1+1.5x ZnGa x O 1+1.5x and ZnZr x O 1+1.5x At least one of them, where x ranges from 0.1 to 10; the molecular sieve is SUZ-4 molecular sieve or Me-SUZ-4 molecular sieve modified with heteroatoms Me.
2. The catalyst according to claim 1, characterized in that, The heteroatom Me is one of Ca, Fe, Ni, and Zn.
3. The catalyst according to claim 1 or 2, characterized in that, The preparation method of the SUZ-4 molecular sieve containing heteroatom modification includes the following steps: S1. After mixing silica sol, aluminum powder, Me nitrate, potassium hydroxide, tetraethylammonium hydroxide and water, the mixture is aged, hydrothermal crystallization is carried out, and then cooled, washed, separated and dried to obtain Na-Me-SUZ-4 molecular sieve. S2. Na-Me-SUZ-4 molecular sieve is added to an aqueous solution of ammonium nitrate for ion exchange, and then dried and calcined to obtain Me-SUZ-4 molecular sieve.
4. The catalyst according to claim 1, characterized in that, The mass ratio between the metal oxide and the molecular sieve is 0.1 to 20:
1.
5. The catalyst according to claim 1, characterized in that, The specific surface area of the metal oxide is 100~150m². 2 / g.
6. The catalyst according to claim 1, characterized in that, The molecular sieve has a moderately strong acid strength, and the amount of moderately strong acid sites is 0.005~0.6 mol / kg.
7. The catalyst according to claim 1, characterized in that, The mechanical mixing method includes one or more of mechanical stirring, ball milling, shaking table oscillation, and mechanical grinding.
8. A method for the direct conversion of carbon dioxide to low-carbon alkanes via hydrogenation, characterized in that, The method uses a mixture of carbon dioxide and hydrogen as the reaction raw material and carries out the conversion reaction in a fixed bed or a moving bed. The catalyst used is the catalyst described in any one of claims 1 to 7.
9. The method according to claim 8, characterized in that, The catalytic reaction is carried out at a temperature of 300–500 °C, and the space velocity of the mixed gas is 300–12000 mL g. -1 h -1 The pressure of the mixed gas is 0.5~10 MPa.
10. The method according to claim 8 or 9, characterized in that, The molar ratio of carbon dioxide to hydrogen is 1:0.2~4.5.