A molybdenum-based oxidation desulfurization catalyst, a preparation method and application thereof

CN123128047APending Publication Date: 2026-11-20WUHAN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611404474.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-10
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

然而,单一的MoOx存在易团聚、油相中分散性差、易失活和催化活性有限的缺点

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123128047A_ABST
    Figure CN123128047A_ABST
Patent Text Reader

Abstract

The present application relates to a kind of molybdenum-based oxidative desulfurization catalyst and its preparation method and application, the catalyst includes MoO3 And loaded on the hydroxyethylidene diphosphonic acid of MoO3;The hydroxyethylidene diphosphonic acid accounts for 10%-30% of the mass of the catalyst.The present application is loaded on MoO3 By hydroxyethylidene diphosphonic acid, using the active site that hydroxyethylidene diphosphonic acid has improves dispersibility and benefits the uniform dispersion of active component, to significantly promote the adsorption and conversion to sulfur-containing molecule.Result shows that the molybdenum-based oxidative desulfurization catalyst obtained by the present application has higher oxidative desulfurization activity, for dibenzothiophene, the removal rate is still above 96% for multiple cycle use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of MoO3 catalyst technology, specifically to a molybdenum-based oxidative desulfurization catalyst, its preparation method, and its application. Background Technology

[0002] Petroleum, as a natural fossil fuel, contains over 200 types of sulfur compounds, some of which remain in the finished oil during refining. These sulfides in fuels can be broadly classified into two categories: active and inert. Active sulfides have relatively simple structures and are easy to remove. Typical active sulfides include thiols, thioethers, and disulfides. Inert sulfides typically do not react directly with metals, making their removal relatively more difficult. Given that thiophene sulfides possess an aromatic skeleton and exhibit significant steric hindrance, efficient removal of them in existing desulfurization processes is challenging. Therefore, research on desulfurization processes focuses on improving the removal efficiency of thiophene compounds. Oxidative desulfurization (ODS) is an important method among many non-hydrodesulfurization technologies. Compared to hydrodesulfurization (HDS), oxidative desulfurization can be carried out at ambient temperature and pressure, consumes less energy, and does not require hydrogen during the reaction, further enhancing the safety of the desulfurization process. The core of ODS (Optical Discharge Separation) lies in converting harmful sulfides into environmentally friendly sulfones, which are then easily extracted by polar solvents or adsorbed by adsorbents, ultimately achieving separation. Due to its mild reaction conditions, high removal efficiency for thiophene sulfides, and safe operation, it has attracted widespread attention. Selecting suitable oxidants, catalysts, and extractants is a crucial component of the ODS process.

[0003] Molybdenum-based materials possess stable physicochemical properties, good electrical conductivity, and flexible valence variation capabilities (Mo). 5+ / Mo 6 + Molybdenum oxide (MoO) has been widely used in the field of catalysis. x MoO₂ has strong oxidizing power and low cost, showing promising application prospects in the ODS field. However, single MoO₂... x It has drawbacks such as easy aggregation, poor dispersibility in the oil phase, easy deactivation, and limited catalytic activity. Summary of the Invention

[0004] The purpose of this invention is to improve the dispersibility of active components by loading hydroxyethylidene diphosphonic acid onto MoO3, thereby promoting the adsorption and conversion of sulfur-containing molecules. It is also expected to stabilize oxygen vacancies and improve the performance of oxidative desulfurization cycles. Finally, it helps to achieve a synergistic effect between the support and the active components.

[0005] To achieve the above-mentioned technical objectives, the present invention provides a molybdenum-based oxidative desulfurization catalyst, comprising MoO3 and hydroxyethylidene diphosphonic acid supported on the MoO3; The hydroxyethylidene diphosphonic acid accounts for 10%-30% of the mass of the catalyst.

[0006] Furthermore, the specific surface area of ​​the catalyst is 0.8-2 m². 2 / g, pore volume of 0.0045-0.0060cm³ 3 / g, pore size is 2.0-2.45nm.

[0007] Furthermore, the crystal form of the MoO3 is hexagonal.

[0008] This invention also provides a method for preparing a molybdenum-based oxidative desulfurization catalyst, comprising, MoO3 and hydroxyethylidene diphosphonic acid were mixed and ultrasonically treated to obtain a molybdenum-based oxidative desulfurization catalyst; the mass ratio of MoO3 to hydroxyethylidene diphosphonic acid was 7-9:1-3.

[0009] Furthermore, the specific surface area of ​​the MoO3 is 3-5 m². 2 / g, pore volume of 0.016-0.018cm 3 / g, pore size is 2.5-2.7nm.

[0010] Furthermore, the mixing temperature is 25-35℃ and the time is 0.5-2h.

[0011] Furthermore, the ultrasound duration is 20-60 minutes.

[0012] The present invention also provides the application of the above-mentioned molybdenum-based oxidative desulfurization catalyst in the oxidative desulfurization of petroleum.

[0013] Furthermore, the applications include, The oil to be treated is mixed with the oxidative desulfurization catalyst and heated to the reaction temperature. Hydrogen peroxide is then added for oxidative desulfurization. The upper oil phase is collected and extracted to obtain the desulfurized oil.

[0014] Furthermore, the ratio of the oil to the oxidative desulfurization catalyst is 0.001-0.003 g / mL; The reaction temperature is 40-70℃.

[0015] Compared with the prior art, the beneficial effects of the present invention include: This invention utilizes the active sites of hydroxyethylidene diphosphonic acid (HEDTA) on MoO3 to improve dispersibility and facilitate the uniform dispersion of the active components, thereby significantly promoting the adsorption and conversion of sulfur-containing molecules. Results show that the molybdenum-based oxidative desulfurization catalyst obtained in this invention exhibits high oxidative desulfurization activity, and even after multiple cycles, the removal rate of dibenzothiophene remains above 96%.

[0016] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Attached Figure Description

[0017] To more clearly illustrate the technical solutions of this application, the accompanying drawings used in this application will be briefly described below. Obviously, the drawings described below are merely some embodiments of this application. For those skilled in the art, other drawings can be obtained from these drawings without any creative effort.

[0018] Figure 1 The scanning electron microscope image and elemental distribution map of HEDP / h-MoO3-20% prepared in Example 2 of this invention are shown. Figure 1 (a) is a scanning electron microscope image. Figure 1 (b)- Figure 1 (e) are the distribution diagrams of Mo, O, P and C elements respectively; Figure 2 The XRD patterns of the catalysts prepared in Examples 1-3 of this invention, as well as HEDP and h-MoO3, are shown. Figure 3 The following are characterization diagrams of nitrogen adsorption-desorption of the catalysts prepared in Examples 1-3 of this invention and h-MoO3; Figure 4 The cycling performance diagram of HEDP / h-MoO3-20% prepared in Example 2 of the present invention is shown. Detailed Implementation

[0019] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0020] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the invention; the terms “comprising” and “having”, and any variations thereof, in the specification, claims, and foregoing description of the invention, are intended to cover non-exclusive inclusion.

[0021] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of the invention. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0022] However, existing MoO x ODS catalysts still face the following key challenges: (a) Active components are prone to aggregation MoO x Agglomeration easily occurs during the reaction, significantly limiting further improvement in catalytic performance. Agglomeration of active components leads to a reduction in effective active sites and a decrease in catalytic efficiency.

[0023] (ii) Poor dispersibility in the oil phase Molybdenum oxide exhibits poor dispersion in the oil phase, resulting in a limited number of accessible active sites and thus restricting its oxidative desulfurization activity. How to achieve MoO₂… x Uniform dispersion of active sites is a key challenge in improving the reactivity of ODS.

[0024] (III) Loss and inactivation of active components Especially in continuous reactions, metal leaching and adsorption of sulfone products can lead to rapid catalyst deactivation. Studies have shown that crystalline MoO3 exhibits low activity in the reaction and is detrimental to catalyst regeneration.

[0025] Therefore, this invention is proposed.

[0026] A molybdenum-based oxidative desulfurization catalyst comprises MoO3 and hydroxyethylidene diphosphonic acid supported on the MoO3; The hydroxyethylidene diphosphonic acid accounts for 10%-30% of the mass of the catalyst.

[0027] In some preferred embodiments, the molybdenum-based oxidative desulfurization catalyst has a specific surface area of ​​0.8-2 m². 2 / g, pore volume of 0.0045-0.0060cm³ 3 / g, pore size is 2.0-2.45nm.

[0028] In some preferred embodiments, the MoO3 is in hexagonal phase, i.e., h-MoO3. h-MoO3 has a unique layered and tunnel structure, which is conducive to the diffusion and adsorption of reactant molecules; its metastable properties endow it with higher chemical activity.

[0029] Hydroxyethylidene diphosphonic acid is an organophosphonic acid component supported on the surface of h-MoO3, which plays the following dual roles: (1) as a dispersant, it improves the dispersibility of h-MoO3 in the oil phase and increases the accessible active sites; (2) as an activity regulator, it utilizes the interaction between its phosphonic acid groups and molybdenum species to regulate the surface electronic structure of h-MoO3, promote the generation of oxygen vacancies and the activation of H2O2.

[0030] The metastable crystalline structure of h-MoO3 and the phosphonic acid groups of hydroxyethylidene diphosphonic acid (HEDIA) can produce a synergistic effect: on the one hand, the loading of HEDIA can suppress the phase transition of h-MoO3 under reaction conditions, maintain the high activity of its metastable structure, and also improve its dispersion performance in the oil phase; on the other hand, the layered tunnel structure of h-MoO3 can provide abundant anchoring sites for HEDIA, achieving stable loading and uniform dispersion of HEDIA. This synergistic effect promises to achieve efficient and stable oxidative desulfurization under mild conditions.

[0031] In another invention, the present invention also provides a method for preparing a molybdenum-based oxidative desulfurization catalyst, comprising, MoO3 and hydroxyethylidene diphosphonic acid were mixed and ultrasonically treated to obtain a molybdenum-based oxidative desulfurization catalyst; the mass ratio of MoO3 to hydroxyethylidene diphosphonic acid was 7-9:1-3.

[0032] In some preferred embodiments, the specific surface area of ​​the MoO3 is 3-5 m². 2 / g, pore volume of 0.016-0.018cm 3 / g, pore size is 2.5-2.7nm.

[0033] In some preferred embodiments, the mixing temperature is 25-35°C and the time is 0.5-2 hours.

[0034] In some preferred embodiments, the ultrasound duration is 20-60 minutes.

[0035] It should be noted that the source of hydroxyethylidene diphosphonic acid is not strictly limited in this invention; it can be prepared in-house or a commercially available product purchased directly. A typical method for preparing hydroxyethylidene diphosphonic acid includes using acetyl chloride and phosphorous acid as raw materials, with excess phosphorous acid to ensure complete reaction of acetyl chloride. The mixture is stirred and heated while acetyl chloride is gradually added. After heating and holding the reaction at this temperature, a small amount of water is added to the system, and the residual intermediate is hydrolyzed by heating. The generated acetic acid is removed by vacuum distillation to obtain hydroxyethylidene diphosphonic acid. The mass ratio of acetyl chloride to phosphorous acid is 5:6; the temperature is raised to 60-100℃ and held for 2-5 hours.

[0036] The present invention will be further described in detail below through specific embodiments. It should be noted that the embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in this field or in accordance with the product instructions. Reagents or instruments used that do not specify the manufacturer are all conventional products that can be obtained commercially.

[0037] Preparation Example A method for preparing hydroxyethylidene diphosphonic acid includes the following steps: Weigh out 5g of acetyl chloride and 6g of phosphorous acid, with phosphorous acid in excess to ensure complete reaction of acetyl chloride. Add phosphorous acid to a three-necked flask, stir and heat to 60°C, gradually add acetyl chloride, then raise the temperature to 100°C and keep the reaction at this temperature for 3 hours. After the reaction is complete, add 10mL of deionized water to the system, heat to hydrolyze the residual intermediate, and remove the generated acetic acid by vacuum distillation to obtain hydroxyethylidene diphosphonic acid (HEDP).

[0038] All HEDPs described below were obtained using the same method as in this preparation example; the specific method will not be described in detail here.

[0039] Example 1 A method for preparing a molybdenum-based oxidative desulfurization catalyst includes the following steps: At 30°C, 0.1 g of HEDP was added to a beaker containing 0.9 g of h-MoO3. After impregnation for 1 h, the mixture was ultrasonically treated for 30 min. After the treatment, the insoluble material was transferred to a drying oven and dried for 12 h to obtain a molybdenum-based oxidative desulfurization catalyst, denoted as HEDP / h-MoO3-10.

[0040] Example 2 A method for preparing a molybdenum-based oxidative desulfurization catalyst includes the following steps: At 30°C, 0.2 g of HEDP was added to a beaker containing 0.8 g of h-MoO3. After impregnation for 1 h, the mixture was ultrasonically treated for 30 min. After the treatment, the insoluble material was transferred to a drying oven and dried for 12 h to obtain a molybdenum-based oxidative desulfurization catalyst, denoted as HEDP / h-MoO3-20.

[0041] Example 3 A method for preparing a molybdenum-based oxidative desulfurization catalyst includes the following steps: At 30°C, 0.3g of HEDP was added to a beaker containing 0.7g of h-MoO3. After impregnation for 1 hour, the mixture was ultrasonically treated for 30 minutes. After the treatment, the insoluble material was transferred to a drying oven and dried for 12 hours to obtain a molybdenum-based oxidative desulfurization catalyst, denoted as HEDP / h-MoO3-30.

[0042] Comparative Example 1 A method for preparing a molybdenum-based oxidative desulfurization catalyst includes the following steps: (1) Dissolve 4g of molybdic acid in 20mL of saturated HCl aqueous solution and stir for 12h to obtain a dark yellow mixed solution. Add 3mL of HNO3 to the above mixed solution and continue stirring for 4h to obtain a yellow solution. Place the obtained yellow solution in a water bath at 70℃ for 30min. After water bath treatment, transfer the solution to a single-necked flask and vacuum evaporate it at 70℃ for 2h using a rotary evaporator. Place the obtained light yellow powder in a tube furnace and calcine it at a rate of 10℃ / min to 310℃ in air atmosphere for 2h to obtain a green powder, which is monoclinic molybdenum trioxide (β-MoO3).

[0043] (2) Using (NH4)6Mo7O 24 ·4H2O and [C 12 [C] was prepared by reacting Py]3Cl in a molar ratio of 1:3. 12 Py]3(NH4)3Mo7O 24 Dissolve 2g of (NH4)6Mo7O in 30mL of water. 24 ·4H2O, then dissolve 1.406g [C] in 30mL of water. 12 [Py]3Cl, then the former solution was slowly poured into the latter solution, stirred at 25°C for 48 hours, and finally filtered to obtain a white solid substance, which was dried at 65°C for 24 hours to obtain [C 12 Py]3(NH4)3Mo7O 24 .

[0044] (3) With [C 12 Py]3(NH4)3Mo7O 24Using β-MoO3 as raw material. 0.2g of [C 12 Py]3(NH4)3Mo7O 24 The solutions were dispersed separately in DMSO. Then, these solutions were mixed with 0.8 g of β-MoO3 in a beaker, sonicated for 60 min, and the insoluble matter was collected and transferred to a vacuum drying oven at 60 °C for drying to obtain a molybdenum-based oxidative desulfurization catalyst, denoted as [C]. 12 Py]3(NH4)3Mo7O 24 / β-MoO3-20%.

[0045] Comparative Example 2 A method for preparing a molybdenum-based oxidative desulfurization catalyst includes the following steps: 70 mg ZrCl, 45 mg H2TCPP, and 2.7 g benzoic acid were weighed and dissolved in 8 mL of N,N-diethylformamide by ultrasonication. Then, 18.2 mg of molybdenum acetylacetonate was added and ultrasonically mixed for another 20 min until completely dissolved. The resulting dark green solution was then transferred to a high-pressure reactor and reacted at 130°C for 24 h. After the reaction was complete and the mixture cooled to room temperature, the crystallized product was washed 2-3 times with N,N-dimethylformamide and acetone, respectively, by centrifugation. The purple precipitate after centrifugation was vacuum dried at 80°C to obtain the molybdenum-based oxidative desulfurization catalyst, designated as 7%MoO3 / PCN-222.

[0046] Test case Figure 1 (a) shows the microstructure of the HEDP / h-MoO3-20% prepared in Example 2. The HEDP / h-MoO3-20% composite material exhibits a typical, regular rod-shaped micron crystal morphology with a smooth surface. Figure 1 (b)- Figure 1 (e) It can be seen that the Mo and O elements that constitute the main framework are highly concentrated within the bulk outline, and the C and P element signals from the HEDP molecules also highly coincide with the spatial positions of the main particles, confirming that HEDP has been successfully and uniformly loaded onto h-MoO3. These results demonstrate the uniformity of the catalyst composition and that the loading of HEDP has not damaged the structure.

[0047] Figure 2The XRD patterns of Examples 1-3, HEDP, and h-MoO3 are shown. The results show that HEDP exhibits strong diffraction peaks at 14.3°, 16.6°, and 20.2°. The catalysts prepared in Examples 1-3 show a crystal structure consistent with the characteristic peaks of the standard PDF card (PDF NO. 21-0569). The diffraction peaks at 9.6°, 17°, 19.5°, 22.3°, 25.7°, and 29.3° correspond to the (100), (110), (200), (300), and (004) crystal planes of h-MoO3, respectively, indicating that the crystal structure of h-MoO3 did not change after loading, and the intensity of the diffraction peaks belonging to HEDP increased with the increase of HEDP loading.

[0048] Figure 3 The nitrogen adsorption-desorption characterization diagrams of the catalysts prepared in Examples 1-3 of this invention are shown. It can be seen that these catalyst materials all exhibit type IV nitrogen adsorption-desorption isotherms characteristic of mesoporous materials. This characteristic is consistent with the isotherm characteristics of pure h-MoO3, indicating that after loading HEDP onto the surface of h-MoO3 using the impregnation method, the basic pore structure of the h-MoO3 catalyst did not change significantly, and its mesoporous structure was well preserved. Table 1 also gives the structural characteristics of these catalysts.

[0049] Table 1 Structural characteristics of catalysts

[0050] As shown in Table 1, the specific surface area, pore volume, and pore size of the catalyst gradually decreased with increasing HEDP loading. These phenomena indicate that HEDP was successfully loaded onto the surface and pores of the h-MoO3 catalyst, and that the loaded HEDP occupied part of the pore space of h-MoO3, leading to a corresponding decrease in its specific surface area and pore volume. This further confirms the successful preparation of the HEDP / h-MoO3 composite catalyst.

[0051] The oxidative desulfurization performance test of the catalyst included: dissolving dibenzothiophene in n-octane to prepare a simulated oil with a sulfur element concentration of 500 μg / g; adding tetradecane (2000 μg / g) as an internal standard to meet the requirements of gas chromatography quantitative analysis; adding 25 mg of catalyst, 10 mL of simulated oil, and 5 mL of acetonitrile (extractant) to a beaker; after reaching the reaction temperature, adding 30% H2O2; and taking samples at regular intervals to detect the content of each component in the gas phase by gas chromatography (GC-FID / TCD) and calculating the sulfide conversion rate. ; Where α is the desulfurization rate (%), C0 and C t The values ​​are the sulfur concentrations (µg / g) at time 0 and time t, respectively.

[0052] Application Example 1 Take 25 mg of [C] from Comparative Example 1 12 Py]3(NH4)3Mo7O 24 Place the mixture in a beaker, add 10 mL of oil and 5 mL of acetonitrile, heat to 60 °C, then add 33 µL of H2O2 and react for 20 min.

[0053] Application Example 2 Take 60 mg of 7% MoO3 / PCN-222 from Comparative Example 2 and place it in a beaker. Add 10 mL of oil and 5 mL of acetonitrile. Heat to 60 °C and then add 33 µL of H2O2. React for 20 min.

[0054] Application Example 3 Take 25 mg of HEDP / h-MoO3-20% from Example 2 and place it in a beaker. Add 10 mL of oil and 5 mL of acetonitrile. Heat to 40 °C and then add 33 µL of H2O2 and react for 20 min.

[0055] Application Example 4 Take 25 mg of HEDP / h-MoO3-20% from Example 2 and place it in a beaker. Add 10 mL of oil and 5 mL of acetonitrile. Heat to 50 °C and then add 33 µL of H2O2 and react for 20 min.

[0056] Application Example 5 Take 25 mg of HEDP / h-MoO3-20% from Example 2 and place it in a beaker. Add 10 mL of oil and 5 mL of acetonitrile. Heat to 60 °C and then add 33 µL of H2O2 and react for 20 min.

[0057] Application Example 6 Take 25 mg of HEDP / h-MoO3-20% from Example 2 and place it in a beaker. Add 10 mL of oil and 5 mL of acetonitrile. Heat to 70 °C and then add 33 µL of H2O2 and react for 20 min.

[0058] Application Example 7 Take 25 mg of HEDP / h-MoO3-20% from Example 2 and place it in a beaker. Add 10 mL of oil and 5 mL of acetonitrile. Heat to 60 °C and then add 22 µL of H2O2. React for 20 min.

[0059] Application Example 8 Take 25 mg of HEDP / h-MoO3-20% from Example 2 and place it in a beaker. Add 10 mL of oil and 5 mL of acetonitrile. Heat to 60 °C and then add 44 µL of H2O2. React for 20 min.

[0060] Application Example 9 Take 25 mg of HEDP / h-MoO3-20% from Example 2 and place it in a beaker. Add 10 mL of oil and 5 mL of acetonitrile. Heat to 60 °C and then add 55 µL of H2O2 to react for 20 min.

[0061] Application Example 10 Take 25 mg h-MoO3 and place it in a beaker. Add 10 mL of oil and 5 mL of acetonitrile. Heat to 60 °C and then add 55 µL H2O2. React for 20 min.

[0062] Table 2 summarizes the parameter differences and sulfide conversion rates of the above application examples.

[0063] Table 2. Parameter differences and sulfide conversion rates in application examples

[0064] As can be seen from the test results in Table 2, compared with the molybdenum oxide-based catalysts using different supports in Comparative Examples 1 and 2, the HEDP / h-MoO3-20% catalyst of this invention exhibits better oxidative desulfurization performance, with a significant increase in sulfide conversion rate even at lower reaction temperatures and lower catalyst dosages. Application Examples 4-6 show that the sulfide conversion rate initially increases with increasing reaction temperature, reaching a maximum at 60°C, and then decreases with further temperature increases. This may be because at higher temperatures, H2O2 may partially decompose, leading to a slight decrease in desulfurization rate. Application Examples 5 and 7-9 show that the sulfide conversion rate initially increases and then decreases with increasing H2O2 dosage. This is because increasing H2O2 dosage produces more water, and excessive water has an adverse effect on the oxidative desulfurization process.

[0065] After the HEDP / h-MoO3-20% catalysis was completed under the conditions of Application Example 5, the reusability of the catalyst was investigated. After the desulfurization reaction was completed, the system was transferred to a centrifuge tube and centrifuged at 6000 r / min for 10 min. The supernatant was discarded, and the lower solid layer was obtained. Acetonitrile was then added for washing and centrifugation. This operation was repeated three times. The obtained solid catalyst was then dried and recovered in a vacuum drying oven at 60℃. Figure 4 As shown, the results indicate that the catalyst maintained a 100% desulfurization rate after four cycles, and even after five cycles, 96.87% of DBT was still removed. This demonstrates that the catalyst exhibits excellent reproducibility.

[0066] In summary, this invention demonstrates that the structure of HEDP is completely preserved in the catalyst. Furthermore, the catalyst fully retains the layered and mesoporous structure of the h-MoO3 support. This enhances the mass transfer efficiency between the catalyst, oxidant, and reactants, promoting the ODS reaction.

[0067] It should be noted that when numerical ranges are involved in this invention, it should be understood that both endpoints of each numerical range, as well as any value between the two endpoints, can be selected. Since the steps and methods used are the same as in the embodiments, preferred embodiments are described here to avoid redundancy. Although preferred embodiments of this invention have been described, those skilled in the art, once they understand the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended scope of protection is intended to be interpreted as including the preferred embodiments and all changes and modifications falling within the scope of this invention.

[0068] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. Therefore, if these modifications and variations fall within the scope of protection of this invention, this invention also intends to include these modifications and variations.

Claims

1. A molybdenum-based oxidative desulfurization catalyst, characterized in that, Includes MoO3 and hydroxyethylidene diphosphonic acid supported on the MoO3; The hydroxyethylidene diphosphonic acid accounts for 10%-30% of the mass of the catalyst.

2. The molybdenum-based oxidative desulfurization catalyst according to claim 1, characterized in that, Its specific surface area is 0.8-2m². 2 / g, pore volume of 0.0045-0.0060cm³ 3 / g, pore size is 2.0-2.45nm.

3. The molybdenum-based oxidative desulfurization catalyst according to claim 1 or 2, characterized in that, The MoO3 has a hexagonal crystal structure.

4. A method for preparing a molybdenum-based oxidative desulfurization catalyst, characterized in that, include, MoO3 and hydroxyethylidene diphosphonic acid were mixed and ultrasonically treated to obtain a molybdenum-based oxidative desulfurization catalyst; the mass ratio of MoO3 to hydroxyethylidene diphosphonic acid was 7-9:1-3.

5. The method for preparing the molybdenum-based oxidative desulfurization catalyst according to claim 4, characterized in that, The specific surface area of ​​the MoO3 is 3-5 m². 2 / g, pore volume of 0.016-0.018cm 3 / g, pore size is 2.5-2.7nm.

6. The method for preparing the molybdenum-based oxidative desulfurization catalyst according to claim 4, characterized in that, The mixing temperature is 25-35℃ and the time is 0.5-2h.

7. The method for preparing the molybdenum-based oxidative desulfurization catalyst according to claim 4, characterized in that, The ultrasonic power is 200W, and the ultrasonic time is 20-60min.

8. The application of a molybdenum-based oxidative desulfurization catalyst as described in any one of claims 1-3 in the oxidative desulfurization of petroleum.

9. The application according to claim 8, characterized in that, include, The oil to be treated is mixed with the oxidative desulfurization catalyst and heated to the reaction temperature. Hydrogen peroxide is then added for oxidative desulfurization. The upper oil phase is collected and extracted to obtain the desulfurized oil.

10. The application according to claim 9, characterized in that, The ratio of the oil to the oxidative desulfurization catalyst is 0.001-0.003 g / mL; The reaction temperature is 40-70℃.