A zirconium-based MOF heterojunction catalyst for pet photocatalytic degradation and a preparation method thereof
By constructing a PCN-222-based heterojunction photocatalytic system, the problems of unstable PET photocatalysis, difficulty in recycling, and harsh reaction conditions in existing technologies have been solved. This system enables efficient and selective degradation of PET at room temperature and pressure, and is suitable for visible and near-infrared light-driven processes.
Patent Information
- Application Number
- CN202611369221.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-20
AI Technical Summary
Existing technologies cannot achieve efficient photocatalytic degradation of PET at room temperature and pressure. Furthermore, the catalysts are unstable, difficult to recycle, have poor product selectivity, require harsh reaction conditions, and cannot utilize solar energy.
A heterojunction photocatalytic system based on PCN-222 was constructed. Through in-situ encapsulation of carbon dots/perovskites and type II/S heterostructures, a wide-spectrum response, efficient carrier separation, structural stability and recyclability were achieved, and PET was degraded with high selectivity under mild conditions.
It achieves efficient and selective degradation of PET at room temperature and pressure, with high carrier separation efficiency, recoverable catalyst, high product purity, mild reaction conditions, and suitability for visible and near-infrared light driving.
Smart Images

Figure CN123128050A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of PET plastic degradation technology, and in particular relates to a zirconium-based MOF heterojunction catalyst for photocatalytic degradation of PET and its preparation method. Background Technology
[0002] Global annual production of polyethylene terephthalate (PET) exceeds 38 million tons, widely used in packaging, textiles, tableware, and other fields. Its recalcitrant nature has caused serious white pollution and microplastic risks. Currently, PET recycling is mainly divided into two categories: physical recycling and chemical recycling. Physical recycling can only achieve downgrading and reuse, leaving impurities and limiting the number of cycles. Chemical recycling (hydrolysis, alcoholysis, glycolysis, hydrogenolysis), while capable of depolymerizing into monomers, generally requires high temperature and pressure, strong acids and alkalis, high energy consumption, equipment corrosion, complex products, and significant environmental pollution. Photocatalytic degradation, powered by solar energy, with mild reaction conditions and environmental friendliness, represents an ideal direction for the green resource recovery of PET.
[0003] Metal-organic frameworks (MOFs) have become a research hotspot in the field of PET photocatalysis due to their high specific surface area, tunable pores, abundant active sites, and ease of functionalization. However, existing technologies have significant drawbacks: Existing research reports the use of zirconium-based MOFs (UiO-66) for PET degradation, but this system is a high-temperature thermocatalysis requiring harsh conditions of 260℃. Furthermore, UiO-66 irreversibly transforms into MIL-140A during the reaction, resulting in crystal collapse and extremely poor recyclability, which is completely different from the room-temperature light-driven, structurally stable design of this invention. Comparative patent (CN117696101A) discloses a mesoporous molecular sieve-supported catalyst for PET degradation, which can achieve a certain depolymerization effect, but the catalyst cannot be recovered, is easily lost, and can cause secondary pollution. Comparative patent (CN116237052A) uses MOF-derived composite materials to catalyze PET, but still relies on high temperatures, has a complex preparation process, uncontrollable active sites, and low product selectivity, which is fundamentally different from the mild photocatalysis, high selectivity, and easy separation approach of this invention. The comparative patent (CN119500266A) discloses molybdenum-modified zirconium-based MOF for PET degradation, but this system can only perform thermal catalysis, has no photoresponse, no photogenerated carrier mechanism, cannot utilize solar energy, and cannot achieve near-infrared light drive.
[0004] In summary, existing technologies generally suffer from key drawbacks such as: only capable of thermal catalysis and not photocatalysis; only capable of visible light and not near-infrared light; unstable catalysts; difficult to recover; poor product selectivity; and harsh reaction conditions. To date, no effective solution has been found for MOF-based photocatalysts that can efficiently degrade PET under ambient temperature, ambient pressure, without strong acids or alkalis, with visible / near-infrared light response, oxygen resistance, recyclability, and high selectivity. Summary of the Invention
[0005] To address the technical problems in existing technologies, this invention innovatively constructs a heterojunction photocatalytic system based on PCN-222. Through in-situ encapsulation of carbon dots / perovskites and construction of type II / S heterostructures, it achieves a wide spectral response, efficient carrier separation, structural stability and recyclability, and highly selective degradation of PET under mild conditions, which is different from all existing technologies in principle and structure.
[0006] To achieve the above-mentioned objectives, the present invention adopts the following technical solution: A zirconium-based MOF heterojunction catalyst for photocatalytic degradation of PET, wherein the heterojunction catalyst uses PCN-222 as a support, and the heterojunction catalyst is selected from any one of ternary thermosensitive catalysts, type II heterojunction catalysts, and type S heterojunction catalysts.
[0007] Another objective of this invention is to provide a method for preparing a zirconium-based MOF heterojunction catalyst for photocatalytic degradation of PET, comprising the following steps for preparing a PCN-222 support: using tetrakis(4-carboxyphenyl)porphyrin, ZrCl4 or ZrOCl2·8H2O as a metal source, adding N,N-dimethylformamide (DMF), deionized water and acetic acid, followed by sonication for 5-10 min, solvothermal reaction at 120-130℃ for 15 min-2 h, cooling, centrifugation at 8000-10000 r / min for 5-10 min, washing with ethanol 3-5 times, and vacuum drying at 50-70℃ for 10-14 h to obtain highly crystalline PCN-222.
[0008] Further, the mass ratio of the tetra(4-carboxyphenyl)porphyrin to the metal source is 3:2; the volume ratio of the N,N-dimethylformamide, deionized water, and acetic acid is 20:1:2.4; and the mass-to-volume ratio of the tetra(4-carboxyphenyl)porphyrin to acetic acid is 1:8 (g / ml).
[0009] Furthermore, it also includes the preparation steps of the ternary thermosensitive catalyst: Preparation of N-CDs: Citric acid and tris(hydroxymethyl)aminomethane were weighed and pyrolyzed at 200–250 °C for 15–30 min. After cooling, deionized water was added to dissolve the mixture, and the pH was adjusted to 7 with NaOH. After dialyzing with a 1000 Da dialysis bag for 70–74 h, the primary drying vacuum was controlled at 10–30 Pa, the temperature was -20 °C to 0 °C, and the drying time was 12–36 h. The secondary drying vacuum was controlled at 1–10 Pa, the temperature was increased to 20 °C to 50 °C, and the temperature was maintained for 12–22 h to obtain N-CDs powder. Weigh PCN-222 and ultrasonically disperse it in deionized water to prepare PCN-222 precursor solution. Add 15-25 μL of N-CDs aqueous solution from step (1) and react at 100-140 °C for 12-20 min. Centrifuge at 8000-10000 r / min for 5-10 min, wash with deionized water 3-5 times, and dry to obtain 2N-CDs@PCN-222. PNIPAM with catechol terminal group and 2N-CDs@PCN-222 from step (2) were added to N,N-dimethylformamide and mixed and stirred overnight. The mixture was centrifuged at 8000-10000 r / min for 5-10 min and washed with deionized water 2-5 times to obtain the 2N-CDs@PCN-222@PNIPAM ternary thermosensitive catalyst.
[0010] Further, in step (1), the mass ratio of citric acid to tris(hydroxymethyl)aminomethane is 4:1; the mass-to-volume ratio of citric acid to deionized water is 1:5 (g / ml); the concentration of NaOH is 1 mol / L; the concentration of N-CDs aqueous solution in step (2) is 20 mg / ml; the mass fraction of PCN-222 precursor solution is 1%; in step (3), the mass ratio of PNIPAM to 2N-CDs@PCN-222 is 1:1; and the mass-to-volume ratio of PNIPAM to N,N-dimethylformamide is 1:100 (g / ml).
[0011] Furthermore, the preparation steps of the type II heterojunction catalyst are also included: CsI and PbI2 are added to the PCN-222 ethanol dispersion, stirred at room temperature for 2-4 hours, centrifuged at 8000-10000 r / min for 5-10 minutes, washed with ethanol 3-5 times, and vacuum dried at 50-80 ℃ for 5-8 hours to obtain the CsPbI3@PCN-222 type II heterojunction catalyst.
[0012] Furthermore, the mass fraction of PCN-222 is 30-50 μmol; the mass ratio of CsI to PbI2 is 4:(6-7).
[0013] Furthermore, the preparation steps of the S-type heterojunction catalyst are also included: MAI and PbI2 are added to the DMF solution of PCN-222, ultrasonically mixed evenly, reacted in an oil bath at 70-90℃ for 3-6 hours, cooled, centrifuged at 8000-10000r / min for 5-10 minutes, washed 1-3 times with N,N-dimethylformamide and 2-5 times with methanol, and vacuum dried at 50-70℃ for 5-8 hours to obtain the MAPbI3@PCN-222 S-type heterojunction catalyst.
[0014] Furthermore, the mass fraction of PCN-222 is 30-50 μmol; the mass ratio of MAI to PbI2 is 6:(5-10).
[0015] Compared with the prior art, the beneficial effects of the present invention are as follows: This invention uses a highly stable zirconium-based porphyrin MOF (PCN-222) as the main framework, utilizing its 3.7nm large pores for in-situ encapsulation to construct three types of heterojunction catalysts: 1. Nitrogen-doped carbon dots (N-CDs) + thermosensitive PNIPAM → ternary thermosensitive photocatalyst; 2. All-inorganic perovskite CsPbI3 → type II heterojunction near-infrared response; 3. Organic-inorganic hybrid perovskite MAPbI3 → type S heterojunction strong near-infrared response. Highly efficient photogenerated electron-hole separation is achieved through heterojunction interface engineering; the photoresponse is broadened to the near-infrared region (980nm) through carbon dots / perovskite; and the hydrophilic / hydrophobic reversible transition and rapid recovery of the catalyst are achieved through the PNIPAM thermosensitive layer. Ultimately, highly efficient and selective photocatalytic degradation of PET is achieved under mild conditions.
[0016] Full-spectrum light response: Breaking through the limitation of traditional zirconium-based MOFs that only respond to visible light, it achieves efficient driving of 980nm near-infrared light.
[0017] Highly efficient carrier separation in heterojunctions: Type II / S heterostructures can significantly suppress photogenerated electron-hole recombination, and the carrier separation efficiency is significantly better than that of single-component MOF catalysts.
[0018] Green and gentle: Operates at normal temperature and pressure, non-corrosive, low / no solvents, and does not damage equipment.
[0019] High-purity product: TA selectivity ≥98%, can be directly reused.
[0020] Stable and recyclable: The framework does not collapse, it can be separated by temperature control, and its activity is basically maintained after 10 cycles. Attached Figure Description
[0021] Figure 1 The image shows the PXRD patterns of the ternary thermosensitive catalyst 2N-CDs@PCN-222@PNIPAM, N-CDs, and PCN-222 in Example 1.
[0022] Figure 2 The PXRD patterns are of the type II heterojunction catalysts CsPbI3@PCN-222, CsPbI3, and PCN-222 from Example 1.
[0023] Figure 3 Example 1: S-type heterojunction catalyst MAPbI3@PCN-222, MAPbI 3、 PXRD plot of PCN-222. Detailed Implementation
[0024] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0025] Example 1
[0026] Example 1 of this invention provides a method for preparing PCN-222, a ternary thermosensitive catalyst, a type II heterojunction catalyst, and an S-type heterojunction catalyst.
[0027] PCN-222 preparation: Weigh 0.10 g of ZrCl4 and 0.15 g of tetrakis(4-carboxyphenyl)porphyrin (H4TCPP), add 10 ml of DMF, 0.5 ml of deionized water, and 1.2 ml of acetic acid, and sonicate for 5 min; react in an oil bath at 120 ℃ for 15 min, then cool; collect the solid by centrifugation, wash three times with ethanol, and dry under vacuum at 60 ℃ for 12 h to obtain PCN-222 (see...). Figure 1 ).
[0028] Preparation of ternary thermosensitive catalysts: Preparation of N-CDs: Weigh 2.00 g of citric acid and 0.50 g of tris(hydroxymethyl)aminomethane, mix them in a crucible, and pyrolyze at 225 ℃ for 20 min; after cooling, dissolve in 10 ml of deionized water, and adjust the pH to 7 with 1 mol / L NaOH; dialyze using a 1000 Da dialysis bag for 72 h. Primary drying stage: vacuum degree controlled at 10~30 Pa, temperature set at -20℃ to 0℃, and maintained for 12 to 36 hours; secondary drying stage: vacuum degree controlled between 1~10 Pa, temperature increased to 20℃~50℃, and maintained for 12 to 24 hours; freeze-dry to obtain N-CDs powder.
[0029] Weigh 0.10 g of PCN-222 and ultrasonically disperse it in 10 ml of deionized water to prepare PCN-222 precursor solution. Add 20 μl of N-CDs aqueous solution (20 mg / ml) to the PCN-222 precursor solution and continue to react at 120 ℃ for 15 min. After centrifugation, washing and drying, 2N-CDs@PCN-222 is obtained.
[0030] PNIPAM grafting: Weigh 0.10 g of 2N-CDs@PCN-222 and 0.10 g of terminal catechol PNIPAM, disperse them in 10 ml of DMF, and stir at room temperature for 12 h; centrifuge, wash three times with deionized water, and dry under vacuum at 40 ℃ to obtain the 2N-CDs@PCN-222@PNIPAM ternary thermosensitive catalyst (see...). Figure 1 ).
[0031] Preparation of type II heterojunction CsPbI3@PCN-222 (20 wt%): Weigh 0.10 g of PCN-222 and ultrasonically disperse it in 10 ml of ethanol; weigh 0.015 g of CsI and 0.023 g of PbI2 and add them to the above suspension; stir at room temperature in the dark for 2 h; centrifuge, wash three times with ethanol, and vacuum dry at 60 ℃ for 6 h to obtain CsPbI3@PCN-222 with a CsPbI3 loading of 20 wt% (see... Figure 2 ).
[0032] Preparation of S-type heterojunction MAPbI3@PCN-222 (10 wt%): Weigh 0.10 g of PCN-222 and disperse it in 8 ml of DMF; weigh 0.0085 g of MAI and 0.013 g of PbI2, add them and sonicate for 1 min; react in an oil bath at 80 ℃ for 4 h; cool, centrifuge, wash twice with DMF and three times with methanol, and dry under vacuum at 60 ℃ to obtain MAPbI3@PCN-222 (see...). Figure 3 ).
[0033] Experimental Example 1 Photocatalytic degradation of PET under visible light: 100 mg of PET fragments and 2 mg (2 wt%) of a ternary thermosensitive catalyst were weighed; 5 ml of anhydrous ethanol was added, and the mixture was placed in a quartz reaction tube; the mixture was stirred in the dark for 30 min to reach adsorption equilibrium; the reaction was then irradiated at 50 °C for 12 h using a 300 W xenon lamp with a 420 nm filter; after the reaction was completed, the mixture was cooled and centrifuged; the filtrate was evaporated to dryness to obtain a white solid terephthalic acid (TA); 1 ¹H NMR quantification: PET conversion rate 96%, TA selectivity 99%.
[0034] Experiment Example 2 Photocatalytic degradation of PET under 980 nm near-infrared light: 100 mg of PET fragments and 1 mg (1 wt%) of MAPbI3@PCN-222 S-type heterojunction catalyst were weighed and placed in a solvent-free system in a quartz reaction tube; the mixture was allowed to stand in the dark for 30 min; and then photocatalytic degradation was performed using a 980 nm laser (power density 0.5 W / cm²). 2 Irradiate at 80 °C for 6 h; after cooling, dissolve the product in DMSO-d6. 1 ¹H NMR quantification: PET conversion rate 95%, TA selectivity 98.5%. Experimental Example 3 Degradation of actual waste PET products (mineral water bottles / beverage bottles / polyester fabric): 100 mg of waste colorless mineral water bottle fragments were weighed; 3 mg (3 wt%) of CsPbI3@PCN-222 type II heterojunction catalyst and 5 ml of ethanol were added; the product was irradiated with visible light at 50 ℃ for 12 h; the result was a conversion rate of 78%, and the product was pure white TA with no pigment interference.
Claims
1. A zirconium-based MOF heterojunction catalyst for photocatalytic degradation of PET, characterized in that, The heterojunction catalyst uses PCN-222 as a support and is selected from any one of ternary thermosensitive catalysts, type II heterojunction catalysts, and type S heterojunction catalysts.
2. A method for preparing a zirconium-based MOF heterojunction catalyst for photocatalytic degradation of PET, characterized in that, The preparation steps of the PCN-222 support are as follows: using tetrakis(4-carboxyphenyl)porphyrin, ZrCl4 or ZrOCl2·8H2O as the metal source, adding N,N-dimethylformamide, deionized water and acetic acid, sonicating for 5 to 10 min, solvothermal reaction at 120 to 130 °C for 15 min to 2 h, cooling, centrifuging at 8000 to 10000 r / min for 5 to 10 min, washing with ethanol 3 to 5 times, and vacuum drying at 50 to 70 °C for 10 to 14 h to obtain highly crystalline PCN-222.
3. The preparation method according to claim 2, characterized in that, The mass ratio of tetra(4-carboxyphenyl)porphyrin to the metal source is 3:2; the volume ratio of N,N-dimethylformamide, deionized water, and acetic acid is 20:1:2.4; and the mass-to-volume ratio of tetra(4-carboxyphenyl)porphyrin to acetic acid is 1:8 (g / ml).
4. The preparation method according to claim 2, characterized in that, It also includes the preparation steps of ternary thermosensitive catalysts: Preparation of N-CDs: Citric acid and tris(hydroxymethyl)aminomethane were weighed and pyrolyzed at 200–250 °C for 15–30 min. After cooling, deionized water was added to dissolve the mixture, and the pH was adjusted to 7 with NaOH. After dialyzing with a 1000 Da dialysis bag for 70–74 h, the primary drying vacuum was controlled at 10–30 Pa, the temperature was -20 °C to 0 °C, and the drying time was 12–36 h. The secondary drying vacuum was controlled at 1–10 Pa, the temperature was increased to 20 °C to 50 °C, and the temperature was maintained for 12–22 h to obtain N-CDs powder. Weigh PCN-222 and ultrasonically disperse it in deionized water to prepare PCN-222 precursor solution. Add 15-25 μL of N-CDs aqueous solution from step (1), react at 100-140 °C for 12-20 min, centrifuge at 8000-10000 r / min for 5-10 min, wash with deionized water 3-5 times, and dry to obtain 2N-CDs@PCN-222. PNIPAM with catechol terminal group and 2N-CDs@PCN-222 from step (2) were added to N,N-dimethylformamide and mixed and stirred overnight. The mixture was centrifuged at 8000-10000 r / min for 5-10 min and washed with deionized water 2-5 times to obtain the 2N-CDs@PCN-222@PNIPAM ternary thermosensitive catalyst.
5. The preparation method according to claim 4, characterized in that, In step (1), the mass ratio of citric acid to tris(hydroxymethyl)aminomethane is 4:1; the mass-to-volume ratio of citric acid to deionized water is 1:5 (g / ml); the concentration of NaOH is 1 mol / L; the concentration of N-CDs aqueous solution in step (2) is 20 mg / ml; the mass fraction of PCN-222 precursor solution is 1%; in step (3), the mass ratio of PNIPAM to 2N-CDs@PCN-222 is 1:1; and the mass-to-volume ratio of PNIPAM to N,N-dimethylformamide is 1:100 (g / ml).
6. The preparation method according to claim 2, characterized in that, The preparation steps of the type II heterojunction catalyst are also included: CsI and PbI2 are added to the PCN-222 ethanol dispersion, stirred at room temperature for 2-4 hours, centrifuged at 8000-10000 r / min for 5-10 minutes, washed with ethanol 3-5 times, and vacuum dried at 50-80 ℃ for 5-8 hours to obtain the CsPbI3@PCN-222 type II heterojunction catalyst.
7. The preparation method according to claim 6, characterized in that, The amount of PCN-222 fed is 30-50 μmol; the mass ratio of CsI to PbI2 is 4:(6-7).
8. The preparation method according to claim 2, characterized in that, The preparation steps of the S-type heterojunction catalyst are also included: MAI and PbI2 are added to the DMF solution of PCN-222, ultrasonically mixed evenly, reacted in an oil bath at 70-90℃ for 3-6 hours, cooled, centrifuged at 8000-10000r / min for 5-10 minutes, washed 1-3 times with N,N-dimethylformamide and 2-5 times with methanol, and vacuum dried at 50-70℃ for 5-8 hours to obtain the MAPbI3@PCN-222 S-type heterojunction catalyst.
9. The preparation method according to claim 8, characterized in that, The amount of PCN-222 fed is 30-50 μmol; the mass ratio of MAI to PbI2 is 6:(5-10).
Citation Information
Patent Citations
Hollow nano aggregate microsphere catalyst as well as preparation method and application thereof
CN116237052A
Supported mesoporous molecular sieve type catalyst, preparation thereof and application thereof in degrading PET (Polyethylene Terephthalate) plastic
CN117696101A
Application of zirconium-based metal organic framework in PET plastic degradation, molybdenum-loaded zirconium-based metal organic framework and preparation method of molybdenum-loaded zirconium-based metal organic framework
CN119500266A