Catalyst for wastewater treatment, preparation method and application

By setting MOF-derived carbon layers within a carbon framework and chemically bonding them with titanium metal oxide particles to form a catalyst with a hierarchical pore structure, the stability and efficiency issues of existing catalytic materials in treating organophosphorus compounds in battery immersion wastewater are solved, achieving highly efficient organophosphorus mineralization.

CN123128053APending Publication Date: 2026-11-20YICHANG BRUNP RECYCLING TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611432502.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-15
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing catalytic materials suffer from problems such as easy physical adsorption and detachment, high interfacial resistance, low pore utilization and pore blockage when treating organophosphorus compounds in battery soaking wastewater. These problems result in poor cycle stability and difficulty in effectively mineralizing organophosphorus compounds.

Method used

A catalyst with a porous carbon framework is used. The inner wall of the pores is provided with a MOF-derived carbon layer that is connected to titanium metal oxide particles through CO-Ti chemical bonds. The pore size gradually increases, and a hierarchical pore structure is formed through specific acid solution treatment and heat treatment. Combined with the in-situ growth of titanium metal MOF crystals, a stable catalyst is formed.

Benefits of technology

This improved the structural stability of the catalyst and the resistance to loss of active components, enhanced the catalytic reaction efficiency, and ensured the effective adsorption and mineralization of organic pollutants in high humidity environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123128053A_ABST
    Figure CN123128053A_ABST
Patent Text Reader

Abstract

The application discloses a catalyst for wastewater treatment, a preparation method and application. The catalyst for wastewater treatment comprises a carbon skeleton, the carbon skeleton contains a pore, the pore contains titanium metal oxide particles, a MOF derived carbon layer is arranged on the inner wall of the pore, and carbon in the MOF derived carbon layer is covalently connected with titanium in the titanium metal oxide particles through a C-O-Ti chemical bond. The catalyst for wastewater treatment has good structural stability and activity component anti-loss ability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of wastewater treatment technology, and more specifically, to catalysts for wastewater treatment, their preparation methods, and their applications. Background Technology

[0002] With the rapid development of the new energy vehicle industry, the volume of recycled and processed waste lithium batteries has increased dramatically. During battery recycling, the brine immersion method is widely used to discharge waste batteries, generating a large amount of battery immersion discharge wastewater. This wastewater has a complex composition, containing a large amount of phosphorus, a significant portion of which is organic phosphorus (such as phosphate esters), originating from solvents and additives in the battery electrolyte (such as trimethyl phosphate and triethyl phosphate). Organic phosphorus compounds are structurally stable and highly toxic to organisms, making them difficult to remove using traditional biological or chemical precipitation methods, thus posing a bottleneck to advanced wastewater treatment.

[0003] While activated carbon-supported catalytic materials and MOF-derived carbon-based materials have been extensively studied, existing technologies have fundamental technical defects for the treatment of organophosphorus compounds in battery immersion wastewater. These defects include: the physical adsorption of MOF-derived materials with activated carbon, which makes them prone to detachment during water treatment due to hydraulic scouring, resulting in poor cycle stability and high interfacial resistance that hinders electron transfer; the high crystallinity and low oxygen vacancy content of metal oxides prepared by conventional pyrolysis, which limits their efficiency in activating persulfate to generate free radicals and their insufficient mineralization capacity for stabilizing organophosphorus compounds; and the fact that active components are mostly loaded on the surface pores of the carrier, resulting in low utilization of deep pores, high mass transfer resistance, and pore blockage.

[0004] In view of this, the present invention is proposed. Summary of the Invention

[0005] The purpose of this invention is to provide a catalyst, preparation method and application for wastewater treatment, which is beneficial to improving the removal rate of organic phosphorus in wastewater.

[0006] This invention is implemented as follows: In a first aspect, the present invention provides a catalyst for wastewater treatment, the catalyst comprising a carbon skeleton containing channels containing titanium metal oxide particles, and an MOF-derived carbon layer disposed on the inner wall of the channels, wherein the carbon in the MOF-derived carbon layer and the titanium in the titanium metal oxide particles are covalently linked through CO-Ti chemical bonds.

[0007] In an optional implementation, the aperture of the channel gradually increases along the direction of increasing depth; And / or, the D50 of the titanium oxide particles is 20-100 nm; And / or, the mass fraction of titanium metal element in the catalyst is 0.5% to 5%.

[0008] Secondly, the present invention provides a method for preparing the catalyst for wastewater treatment described in the foregoing embodiments, comprising: Activated carbon is immersed in a first acid solution for the first time to obtain pre-expanded carbon; The pre-expanded carbon is immersed in a second acid solution for a second time to obtain functionalized activated carbon with a pore structure; A precursor solution is introduced into the pore structure of the functionalized activated carbon to obtain activated carbon that adsorbs titanium metal ions; the precursor solution includes a titanium metal precursor and a complexing agent. The activated carbon that adsorbs titanium metal ions is mixed with an aqueous solution of titanium metal ligand to obtain a mixture, and then titanium metal MOF crystals are grown in situ to obtain an activated carbon-supported titanium metal MOF intermediate. The activated carbon-supported titanium metal MOF intermediate was subjected to heat treatment and post-treatment in sequence to obtain the catalyst for wastewater treatment.

[0009] In an optional embodiment, the first acid solution is a dilute nitric acid solution with a mass fraction of 13-18%; And / or, the first soaking time is 2-3 hours; And / or, the activated carbon is selected from columnar activated carbon; And / or, the second acid solution is a mixed acid solution of nitric acid and sulfuric acid, wherein the mass fraction of nitric acid is 10-25% and the mass fraction of sulfuric acid is 5-18%; And / or, the second soaking is performed under aeration conditions for 3-5 hours; And / or, the titanium metal precursor is selected from tetrabutyl titanate; And / or, the titanium metal concentration in the precursor solution is 0.05~0.5 mol / L; And / or, the complexing agent is selected from citric acid; And / or, the molar ratio of the complexing agent to the titanium metal in the titanium metal precursor is 1:(1.8-2.2). And / or, the step of introducing a precursor solution into the pore structure of the functionalized activated carbon includes: placing the functionalized activated carbon in a container, first evacuating it to (-0.13)-(-0.17) MPa and holding it for 10-30 min; then reducing the pressure to (-0.18)-(-0.22) MPa and holding it for 10-30 min; subsequently maintaining the pressure and adding the precursor solution to soak for 4-8 h.

[0010] In an optional embodiment, the titanium metal ligand in the aqueous solution of the titanium metal ligand includes 2-methylimidazole and amino-2-methylimidazole; And / or, the total concentration of titanium metal ligands in the aqueous solution of the titanium metal ligands is 0.1~0.8 mol / L; And / or, the in-situ growth of titanium metal MOF crystals includes: first heating the mixture to 50-70°C to induce nucleation, followed by a second heating to 80-100°C for crystal growth.

[0011] In an optional embodiment, the mass fraction of amino-2-methylimidazole in the titanium metal ligand is 10%-20%; And / or, the induction of nucleation time is 1.5-2.5 h; And / or, the heating rate for the first heating is 1.8-2.2℃ / min; And / or, the crystal growth time is 6~10h; And / or, the heating rate for the second heating is 0.4-0.6℃ / min.

[0012] In an optional embodiment, the heat treatment includes a first-stage heat treatment and a second-stage heat treatment performed sequentially under a protective gas atmosphere. The temperature of the first-stage heat treatment is 280-320°C, and the holding time is 50-70 min. The temperature of the second-stage heat treatment is 550-650°C, and the holding time is 2-3 h.

[0013] In an optional embodiment, the heating rate of the heat treatment stage is 1.5-2.5℃ / min; And / or, the heating rate of the two-stage heat treatment is 0.8-1.2℃ / min; And / or, the post-processing includes: immersing the heat-treated product in a sodium hydroxide solution, followed by washing and drying.

[0014] Thirdly, the present invention provides a wastewater treatment method in which, in the presence of an oxidant, wastewater containing organophosphorus compounds with a pH of 3 to 7 is contacted with the catalyst described in any one of the foregoing embodiments to carry out a catalytic oxidation reaction, thereby obtaining wastewater containing orthophosphate.

[0015] In an optional embodiment, the oxidant is selected from persulfate; And / or, the mass ratio of the oxidant to the organic phosphorus in the wastewater to be treated is 5~10:1; And / or, the catalyst is packed in a fixed bed reaction, and the flow rate of the wastewater to be treated through the catalyst bed is 1~4 BV / h; And / or, the temperature for the catalytic oxidation reaction is 15-30℃.

[0016] The present invention has the following beneficial effects: The wastewater treatment catalyst of this application exhibits good structural stability and resistance to loss of active components. In this application, titanium metal oxide particles are chemically bonded to the MOF-derived carbon layer via CO-Ti covalent bonds. This strong chemical connection effectively inhibits the aggregation, migration, and loss of active components due to water scouring or chemical erosion during wastewater treatment, thereby ensuring the structural stability of the catalyst during long-term operation. In this application, the titanium metal oxide is connected to the MOF-derived carbon layer via CO-Ti covalent bonds. This chemical bonding helps achieve high dispersion of active components within the pores, preventing particle aggregation and exposing more effective catalytic active sites, which is beneficial for improving catalytic reaction efficiency. The MOF-derived carbon layer on the inner wall of the pores creates a hydrophobic microenvironment around the active sites of the titanium metal oxide. This microenvironment helps preferentially adsorb organic pollutant molecules in the wastewater while inhibiting competitive adsorption of water molecules and active sites, thus maintaining catalytic activity in a high humidity / aqueous environment. Attached Figure Description

[0017] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0018] Figure 1 SEM image of the wastewater treatment catalyst prepared in Example 1; Figure 2 EDS diagram of the catalyst for wastewater treatment prepared in Example 1; Figure 3 The image shows the XRD pattern of the catalyst for wastewater treatment prepared in Example 1. Detailed Implementation

[0019] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0020] This invention provides a catalyst for wastewater treatment. The catalyst includes a carbon skeleton containing channels containing titanium metal oxide particles. The inner wall of the channels is provided with an MOF-derived carbon layer, and the carbon in the MOF-derived carbon layer is covalently linked to the titanium in the titanium metal oxide particles through CO-Ti chemical bonds.

[0021] The wastewater treatment catalyst of this application exhibits good structural stability and resistance to loss of active components. In this application, titanium metal oxide particles are chemically bonded to the MOF-derived carbon layer via CO-Ti covalent bonds. This strong chemical connection effectively inhibits the aggregation, migration, and loss of active components due to water scouring or chemical erosion during wastewater treatment, thereby ensuring the structural stability of the catalyst during long-term operation. In this application, the titanium metal oxide is connected to the MOF-derived carbon layer via CO-Ti covalent bonds. This chemical bonding helps achieve high dispersion of active components within the pores, preventing particle aggregation and exposing more effective catalytic active sites, which is beneficial for improving catalytic reaction efficiency. The MOF-derived carbon layer on the inner wall of the pores creates a hydrophobic microenvironment around the active sites of the titanium metal oxide. This microenvironment helps preferentially adsorb organic pollutant molecules in the wastewater while inhibiting competitive adsorption of water molecules and active sites, thus maintaining catalytic activity in a high humidity / aqueous environment.

[0022] In an optional embodiment, the pore size gradually increases along the direction of increasing depth; the pore inlet end is relatively narrow and gradually widens inside. The narrow pore at the inlet end can produce a confinement effect, allowing pollutant molecules to fully contact the active sites after entering the pore, thereby improving the space utilization rate of free radicals. Secondly, the gradually widening pore inside can reduce mass transfer resistance, allowing degradation products to diffuse outward smoothly and avoid pore blockage. This achieves synergistic mass transfer of efficient reactant entry and rapid product discharge, maintaining the continuous exposure of catalytic active sites.

[0023] And / or, the D50 of the titanium oxide particles is 20-100 nm, for example, 20 nm, 29 nm, 38 nm, 47 nm, 56 nm, 65 nm, 74 nm, 83 nm, 92 nm, or 100 nm. Controlling the particle size range of the titanium oxide particles to the nanoscale ensures that the particles have a high specific surface area, thereby exposing more catalytic active sites and increasing the probability of contact between active components and pollutant molecules. Simultaneously, this particle size range matches the pore structure, effectively preventing pore blockage due to excessively large particles or agglomeration due to excessively small particles with high surface energy, thus achieving a balance between dispersibility and stability.

[0024] And / or, the mass fraction of titanium metal element in the catalyst is 0.5% to 5%, for example 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%. When the titanium metal element content is less than 0.5%, the number of catalytic active sites is insufficient, making it difficult to meet the requirements of catalytic oxidation reaction; when the content is higher than 5%, it may lead to excessive accumulation or agglomeration of titanium metal oxide particles in the pores. Agglomeration of active components leads to blockage of active sites, which in turn reduces the exposure ratio of effective active sites, resulting in decreased catalytic efficiency and waste of raw materials.

[0025] This invention also provides a method for preparing the catalyst for wastewater treatment described in the foregoing embodiments, comprising: Activated carbon is first immersed in an acid solution to obtain pre-expanded pore carbon. The activated carbon is then preliminarily etched using the acid solution. Through the reaction of the acid with unstable components or impurities in the activated carbon, preliminary pore shapes are formed in the carbon framework or existing micropores are enlarged. This pre-expansion operation provides a foundation for the further construction and control of the pore structure. The pre-expanded pore carbon is immersed in a second acid solution to obtain functionalized activated carbon with a porous structure. The second acid immersion uses acid solutions of different compositions, which can further deepen and optimize the pore structure based on the pre-expanded pores. Simultaneously, acid treatment introduces oxygen-containing functional groups (such as carboxyl and hydroxyl groups) onto the carbon framework surface, achieving surface functionalization of the activated carbon. These oxygen-containing functional groups can serve as anchoring sites for subsequent titanium metal ion adsorption, enhancing the adsorption capacity for titanium metal precursors through coordination or electrostatic interactions, ensuring uniform dispersion of titanium metal ions on the inner wall of the pores, and laying the foundation for subsequent in-situ MOF growth and CO-Ti bond formation. A precursor solution is introduced into the pore structure of the functionalized activated carbon to obtain activated carbon that adsorbs titanium metal ions. The precursor solution includes a titanium metal precursor and a complexing agent. The introduction of the complexing agent allows the titanium metal ions to exist stably in the solution in the form of a complex, avoiding rapid hydrolysis and precipitation of the titanium metal precursor when it comes into contact with water or air. This ensures that the titanium metal ions are adsorbed on the inner wall of the pores of the functionalized activated carbon in a uniformly dispersed state at the molecular level. This uniform adsorption state is beneficial for the subsequent uniform nucleation and growth of MOF crystals on the inner wall of the pores, avoiding excessive crystal growth or pore blockage caused by excessively high local concentrations, and ultimately achieving a high degree of dispersion of titanium metal oxides. The activated carbon adsorbed with titanium metal ions was mixed with an aqueous solution of titanium metal ligands to obtain a mixture. Titanium metal MOF crystals were then grown in situ to obtain an activated carbon-supported titanium metal MOF intermediate. This directional in-situ growth, using pores as microreactors and anchored metals as crystal nuclei, allows the titanium metal MOF crystals to nucleate and grow directly on the inner walls of the activated carbon pores, rather than physically filling the pores with pre-synthesized MOF particles. This method ensures a tight interfacial bond between the MOF crystals and the inner walls of the activated carbon pores, resulting in better structural continuity between the MOF-derived carbon layer and the carbon framework. This facilitates the formation of strong CO-Ti covalent bonds after subsequent heat treatment, improving overall structural stability.

[0026] The activated carbon-supported titanium metal MOF intermediate was subjected to sequential heat treatment and post-treatment to obtain the catalyst for wastewater treatment. Heat treatment caused the MOF crystals to pyrolyze under an inert atmosphere or oxygen-limited conditions, transforming them into a MOF-derived carbon layer that encapsulated Ti metal oxide nanoparticles. In-situ reduction of the metal oxides under a weakly reducing atmosphere generated a large number of oxygen vacancies on the particle surface, while simultaneously... 3+ / T 4+ The formation of valence state cycle enhances catalytic activity; at high temperature, the metal oxide and the oxygen-containing functional groups on the pore wall of activated carbon undergo dehydration reaction to generate CO-Ti covalent chemical bonds, realizing interfacial chemical bonding between the active component and the support; the reducing atmosphere performs secondary etching on the activated carbon pores, widening the mesopore size and forming a hierarchical pore structure of "micropore-mesopore", which enhances mass transfer efficiency.

[0027] In an optional embodiment, the first acid solution is a dilute nitric acid solution with a mass fraction of 13-18%, such as 13%, 14%, 15%, 16%, 17%, or 18%. And / or, the first soaking time is 2-3 hours, for example 2.0 hours, 2.1 hours, 2.2 hours, 2.3 hours, 2.4 hours, 2.5 hours, 2.6 hours, 2.7 hours, 2.8 hours, 2.9 hours, or 3.0 hours; And / or, the activated carbon is selected from columnar activated carbon; And / or, the second acid solution is a mixed acid solution of nitric acid and sulfuric acid, wherein the mass fraction of nitric acid is 10-25%, for example 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 25%, and the mass fraction of sulfuric acid is 5-18%, for example 5%, 7%, 9%, 11%, 13%, 15%, 17%, 18%; And / or, the second soaking is performed under aeration conditions for 3 to 5 hours, for example, 3.0h, 3.2h, 3.4h, 3.6h, 3.8h, 4.0h, 4.2h, 4.4h, 4.6h, 4.8h, or 5.0h.

[0028] The first immersion uses dilute nitric acid for gentle etching, aiming to initially form pore structures within the carbon framework, completing pre-pore expansion and laying the structural foundation for subsequent processing. The second immersion uses a mixed acid solution of nitric acid and sulfuric acid to further deepen and optimize the pore structure based on the pre-pore expansion. At the same time, sulfuric acid is used to introduce functional groups such as sulfonic acid groups onto the carbon surface, achieving surface functionalization. This avoids the problem of sulfuric acid in the mixed acid solution interfering with the uniformity of the etching process, and also avoids the difficulty of simultaneously achieving optimal conditions for functionalization and deep etching.

[0029] And / or, the titanium metal precursor is selected from tetrabutyl titanate; as an organic titanium source, tetrabutyl titanate can gradually release titanium ions during hydrolysis. Compared with inorganic titanium salts (such as titanium tetrachloride), its hydrolysis rate is relatively controllable, which is beneficial for forming a stable precursor complex with a complexing agent. This helps to achieve uniform adsorption of titanium metal ions on the inner wall of activated carbon channels, avoiding local precipitation and uneven distribution caused by excessively rapid hydrolysis, and providing favorable conditions for the subsequent uniform in-situ growth of MOF.

[0030] And / or, the titanium metal concentration in the precursor solution is 0.05~0.5 mol / L, for example 0.05 mol / L, 0.10 mol / L, 0.15 mol / L, 0.20 mol / L, 0.25 mol / L, 0.30 mol / L, 0.35 mol / L, 0.40 mol / L, 0.45 mol / L, or 0.50 mol / L; this is beneficial for meeting the titanium metal loading requirements while avoiding localized supersaturation precipitation of titanium metal ions due to excessively high solution concentration.

[0031] And / or, the complexing agent is selected from citric acid; citric acid, as a polydentate ligand, contains multiple carboxyl and hydroxyl groups in its molecule, which can form stable chelates with titanium metal ions. Furthermore, while citric acid complexes titanium ions, its residual functional groups may participate in the formation of carbon layer structures during subsequent heat treatment, helping to introduce oxygen-containing functional groups into the MOF-derived carbon layer and providing oxygen bridging sites for the formation of CO-Ti covalent bonds.

[0032] And / or, the molar ratio of the complexing agent to the titanium metal in the titanium metal precursor is 1:(1.8-2.2), for example 1:1.80, 1:1.84, 1:1.89, 1:1.93, 1:1.98, 1:2.02, 1:2.07, 1:2.11, 1:2.16, 1:2.20; this is beneficial for forming a coordination relationship close to the stoichiometry between the complexing agent and the titanium metal ions, which is conducive to the full complexation of the titanium metal ions and reduces the hydrolysis and precipitation of free titanium ions in the solution.

[0033] And / or, the step of introducing a precursor solution into the pore structure of the functionalized activated carbon includes: placing the functionalized activated carbon in a container, first evacuating it to (-0.13)-(-0.17) MPa, for example -0.130 MPa, -0.134 MPa, -0.138 MPa, -0.142 MPa, -0.146 MPa, -0.150 MPa, -0.154 MPa, -0.158 MPa, -0.162 MPa, -0.166 MPa, -0.170 MPa and maintaining it for 10-30 min, for example 10 min, 12 min, 14 min, 16 min, 18 min, 20 min, 22 min, 24 min, 26 min, 28 min, 30 min; then reducing the pressure to (-0.18)-(-0.17) MPa. 22) MPa, for example -0.180MPa, -0.184MPa, -0.188MPa, -0.192MPa, -0.196MPa, -0.200MPa, -0.204MPa, -0.208MPa, -0.212MPa, -0.216MPa, -0.220MPa, maintain for 10-30 min, for example 10 min, 12 min, 14 min, 16 min, 18 min, 20 min, 22 min, 24 min, 26 min, 28 min, 30 min; then maintain the pressure and add precursor solution to soak for 4-8 h, for example 4.0 h, 4.4 h, 4.8 h, 5.2 h, 5.6 h, 6.0 h, 6.4 h, 6.8 h, 7.2 h, 7.6 h, 8.0 h. The stepwise vacuum impregnation process gradually reduces the pressure to first fully expel the residual gas in the activated carbon pores, and then introduces the precursor solution under negative pressure. The pressure difference drives the solution to penetrate deep into the pores, which is beneficial for titanium metal ions to be uniformly adsorbed at various depths on the inner wall of the pores, overcoming the uneven loading caused by surface adsorption alone.

[0034] In an optional embodiment, the titanium metal ligands in the aqueous solution of the titanium metal ligands include 2-methylimidazole and amino-2-methylimidazole; the introduction of amino groups can introduce more nitrogen doping sites into the MOF-derived carbon layer, which can serve as activity-enhancing sites, regulate the catalytic activity of titanium metal oxides through electronic effects, and help stabilize the active components.

[0035] And / or, the total concentration of titanium metal ligands in the aqueous solution of the titanium metal ligands is 0.1~0.8 mol / L, for example 0.10 mol / L, 0.18 mol / L, 0.26 mol / L, 0.34 mol / L, 0.42 mol / L, 0.50 mol / L, 0.58 mol / L, 0.66 mol / L, 0.74 mol / L, 0.80 mol / L; this is beneficial for MOF crystals to have suitable nucleation and growth rates, and to maintain MOF crystals with suitable density.

[0036] And / or, the in-situ growth of titanium MOF crystals includes: first heating the mixture to 50-70℃, for example, 50℃, 52℃, 54℃, 56℃, 58℃, 60℃, 62℃, 64℃, 66℃, 68℃, or 70℃ to induce nucleation; then performing a second heating to 80-100℃, for example, 80℃, 82℃, 84℃, 86℃, 88℃, 90℃, 92℃, 94℃, 96℃, 98℃, or 100℃ for crystal growth. Inducing nucleation at the lower temperature of 50-70℃ allows control over the number of crystal nuclei, ensuring their uniform distribution on the inner wall of the pores, which helps overcome the uneven crystal size caused by explosive nucleation at excessively high temperatures. Subsequently, heating to 80-100℃ allows for steady crystal growth based on existing nuclei, resulting in a MOF layer with uniform size and good crystallinity, laying the foundation for subsequent heat treatment to obtain a structurally uniform MOF-derived carbon layer.

[0037] In an optional embodiment, the mass fraction of amino-2-methylimidazole in the titanium metal ligand is 10%-20%, for example 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%; this is beneficial for introducing an appropriate amount of nitrogen doping sites while maintaining the basic integrity of the MOF crystal structure.

[0038] And / or, the induced nucleation time is 1.5-2.5 h, for example 1.50 h, 1.61 h, 1.72 h, 1.83 h, 1.94 h, 2.05 h, 2.16 h, 2.27 h, 2.38 h, 2.49 h, 2.50 h; And / or, the heating rate for the first heating is 1.8-2.2℃ / min, for example 1.80℃ / min, 1.90℃ / min, 2.00℃ / min, 2.10℃ / min, 2.20℃ / min; And / or, the crystal growth time is 6~10h, for example 6.0h, 6.4h, 6.8h, 7.2h, 7.6h, 8.0h, 8.4h, 8.8h, 9.2h, 9.6h, 10.0h; And / or, the heating rate for the second heating is 0.4-0.6℃ / min, for example 0.40℃ / min, 0.42℃ / min, 0.44℃ / min, 0.46℃ / min, 0.48℃ / min, 0.50℃ / min, 0.52℃ / min, 0.54℃ / min, 0.56℃ / min, 0.58℃ / min, 0.60℃ / min.

[0039] In an optional embodiment, the heat treatment includes a first-stage heat treatment and a second-stage heat treatment performed sequentially under a protective gas atmosphere. The temperature of the first-stage heat treatment is 280-320℃, for example, 280℃, 284℃, 288℃, 292℃, 296℃, 300℃, 304℃, 308℃, 312℃, 316℃, or 320℃, and the holding time is 50-70 minutes, for example, 50 minutes, 52 minutes, 54 minutes, 56 minutes, 58 minutes, 60 minutes, or 62 minutes. The heat treatment times are 64 min, 66 min, 68 min, and 70 min; the second-stage heat treatment temperature is 550~650℃, for example 550℃, 561℃, 572℃, 583℃, 594℃, 605℃, 616℃, 627℃, 638℃, 649℃, and 650℃, and the holding time is 2~3h, for example 2.0h, 2.1h, 2.2h, 2.3h, 2.4h, 2.5h, 2.6h, 2.7h, 2.8h, 2.9h, and 3.0h. The first-stage heat treatment is carried out at a lower temperature, which allows solvent molecules and unstable ligands in the MOF crystal to be removed first, initially forming a carbon framework structure, avoiding structural collapse caused by direct high-temperature treatment. The second-stage heat treatment is carried out at 550-650℃, which allows the MOF to be fully carbonized to form a stable MOF-derived carbon layer, while the titanium component is transformed into an oxide crystal form and promotes the formation of CO-Ti covalent bonds. In addition, the protective atmosphere, such as nitrogen, has reducing properties. The reducing atmosphere performs secondary etching on the activated carbon pores, widens the mesopore size, and forms a hierarchical pore structure of "surface micropores - deep mesopores". The density of oxygen-containing functional groups on the inner wall of the pores increases from the surface to the inside, providing deep anchoring points for the active components.

[0040] In an optional embodiment, the heating rate of the heat treatment stage is 1.5-2.5℃ / min, for example 1.50℃ / min, 1.61℃ / min, 1.72℃ / min, 1.83℃ / min, 1.94℃ / min, 2.05℃ / min, 2.16℃ / min, 2.27℃ / min, 2.38℃ / min, 2.49℃ / min, or 2.50℃ / min; And / or, the heating rate of the two-stage heat treatment is 0.8-1.2℃ / min, for example 0.80℃ / min, 0.84℃ / min, 0.88℃ / min, 0.92℃ / min, 0.96℃ / min, 1.00℃ / min, 1.04℃ / min, 1.08℃ / min, 1.12℃ / min, 1.16℃ / min, 1.20℃ / min; The first heat treatment uses a faster heating rate to efficiently remove solvents and volatile components; the second heat treatment uses a slower heating rate to ensure that the MOF carbonization process proceeds smoothly and avoids uneven shrinkage of the carbon layer, cracks or damage to the pore structure caused by rapid heating. This is beneficial for obtaining a MOF-derived carbon layer with a complete structure and a tight bond with titanium metal oxide particles.

[0041] And / or, the post-treatment includes: immersing the heat-treated product in a sodium hydroxide solution, followed by washing and drying. This post-treatment step removes impurities trapped in the catalyst, ensuring unobstructed catalyst pores and full exposure of active sites to guarantee catalytic performance. For example, the post-treatment includes gently immersing the pyrolyzed catalyst in a 0.1 mol / L dilute sodium hydroxide solution for 30 minutes to remove free metal oxide particles from the surface, then washing with pure water until neutral, and drying at 60–90°C to obtain the catalyst product.

[0042] The present invention also provides a wastewater treatment method, wherein, in the presence of an oxidant, wastewater containing organophosphorus compounds with a pH of 3 to 7, such as 3.0, 3.4, 3.8, 4.2, 4.6, 5.0, 5.4, 5.8, 6.2, 6.6, or 7.0, is contacted with the catalyst described in any one of the preceding embodiments to carry out a catalytic oxidation reaction, thereby obtaining orthophosphate-containing wastewater.

[0043] A pH range of 3-7 (weakly acidic to neutral) is beneficial for maintaining the chemical stability and activity of the catalyst. This pH range also facilitates the effective decomposition of the oxidant to generate reactive oxygen species such as ·OH, which oxidize and break the CP bonds in organophosphorus compounds, converting them into orthophosphate. Orthophosphate can be further removed through subsequent precipitation or adsorption, achieving the mineralization and degradation of organophosphorus. In wastewater treatment, the catalyst first adsorbs and enriches organophosphorus in the wastewater through hierarchical pores, then efficiently activates PMS through oxygen vacancy-type heterojunctions to generate sulfate and hydroxyl radicals, completely mineralizing the organophosphorus into orthophosphate. Subsequent calcium salt precipitation of the effluent achieves compliance with total phosphorus discharge standards. The catalyst can be regenerated and reused through combined gas-water backwashing.

[0044] In an optional embodiment, the oxidant is selected from persulfate; persulfate (PMS) is a highly efficient oxidant that can be activated by a catalyst to generate sulfate radicals and ·OH. In this application, the active sites of titanium oxide within the catalyst channels can effectively activate PMS, generating strong oxidizing radicals, thereby achieving efficient oxidative degradation of organophosphorus compounds. Compared to hydrogen peroxide, PMS has better stability and is easier to store and transport.

[0045] And / or, the mass ratio of the oxidant to the organic phosphorus in the wastewater to be treated is 5~10:1, for example 5.0:1, 5.6:1, 6.1:1, 6.7:1, 7.2:1, 7.8:1, 8.3:1, 8.9:1, 9.4:1, 10.0:1; this is beneficial for the full oxidation of organic phosphorus while controlling the amount of oxidant used to reduce operating costs.

[0046] And / or, the catalyst is packed in a fixed-bed reactor, and the flow rate of the wastewater to be treated through the catalyst bed is 1~4 BV / h, for example 1.0 BV / h, 1.3 BV / h, 1.7 BV / h, 2.0 BV / h, 2.3 BV / h, 2.7 BV / h, 3.0 BV / h, 3.3 BV / h, 3.7 BV / h, 4.0 BV / h, to facilitate industrial operation.

[0047] And / or, the temperature for catalytic oxidation reactions is 15-30℃, for example 15℃, 17℃, 19℃, 21℃, 23℃, 25℃, 27℃, 29℃, 30℃.

[0048] The features and performance of the present invention will be further described in detail below with reference to embodiments.

[0049] Example 1 This embodiment provides a method for preparing a catalyst for wastewater treatment, specifically including the following steps: Gradient functionalization: Take 100g of columnar activated carbon, rinse with pure water, and soak in 15% dilute nitric acid at 25℃ for 2.5h; after washing, transfer to a mixture of 30% nitric acid and 30% sulfuric acid (volume ratio 2.5:1), and aerate in a water bath at 25℃ for 4h; wash until neutral, and dry for later use.

[0050] Vacuum coordination infusion: Prepare 0.3 mol / L tetrabutyl titanate and add citric acid to complex (citric acid / total metal molar ratio 0.5:1); first, evacuate the activated carbon to -0.15 MPa for 20 min, then reduce the pressure to -0.2 MPa for 15 min, introduce the precursor solution and then vacuum soak for 6 h; after infusion, wash with pure water to remove free metal ions on the surface and filter for later use.

[0051] In situ MOF growth: Transfer to a 0.5 mol / L mixed ligand solution (85% 2-methylimidazole and 15% amino-2-methylimidazole), and program temperature rise: 1℃ / min to 60℃ and hold for 2 h, then 0.5℃ / min to 90℃ and hold for 8 h; wash and dry.

[0052] Integrated pyrolysis: Under nitrogen atmosphere, the temperature is increased to 300℃ at 2℃ / min and held for 1 hour, then increased to 600℃ at 1℃ / min and held for 2.5 hours, followed by natural cooling.

[0053] Post-treatment: Soak in 0.1 mol / L NaOH for 30 min, wash with water until neutral, then dry at 80℃ to obtain the catalyst for wastewater treatment, such as... Figure 1-3 As shown.

[0054] Figure 1 SEM images show that the particle surface has a large number of nano- to submicron-sized micropores and mesopores, with relatively uniform pore distribution, which can provide a large specific surface area.

[0055] Figure 2 EDS analysis revealed a rough, wrinkled texture on the carbon matrix surface, with numerous nanoscale micropores, primarily ranging from 50 to 200 nm in diameter. Several clear microcracks and fracture surfaces were visible; these defects not only increased the specific surface area but also provided more anchoring sites for TiO2 particles. Some pores were interconnected, forming a three-dimensional porous network structure, which facilitates mass transfer and diffusion of reactants and products. Oxygen (O, red) was widely distributed and highly overlapped with the carbon matrix, indicating the presence of numerous oxygen-containing functional groups (such as hydroxyl and carboxyl groups) on the carbon material surface. Titanium (Ti, purple) was distributed as discrete nanoscale bright spots on the carbon matrix surface, with slight aggregation in some areas, and a relatively uniform distribution, indicating that titanium-based nanoparticles were successfully loaded onto the carbon support surface. The oxygen signal was enhanced in areas rich in titanium, indicating that the loaded particles on the carbon surface were TiO2 nanoparticles, with a size between 20 and 100 nm and an average size of approximately 50 nm. Most TiO2 particles are monodisperse and uniformly distributed on the carbon matrix surface, which is an ideal loading effect and maximizes the exposed area of ​​active sites. Most particles are nearly spherical or cubic with clear edges and good crystallinity.

[0056] Figure 3 XRD analysis showed characteristic diffraction peaks at 2θ≈25.3°(101), 37.8°(004), 48.0°(200), 54.7°(105), and 62.7°(211) that matched those of anatase TiO2, proving the formation of nano-TiO2.

[0057] Example 2 The only difference between this embodiment and Embodiment 1 is that the temperatures of the two-stage pyrolysis are 500℃ (2a), 550℃ (2b), and 650℃ (2d), respectively.

[0058] Example 3 The only difference between this embodiment and Example 1 is that the concentration of the mixed ligand solution was adjusted to 0.1 mol / L (3a), 0.3 mol / L (3b), and 0.8 mol / L (3d), respectively.

[0059] SEM observation revealed a small number of TiO2 crystal particles on the outer surface of the sample with a ligand concentration of 0.8 mol / L, indicating that some MOFs grew on the outer surface.

[0060] Example 4 The only difference between this embodiment and Example 1 is that, in the vacuum coordination infusion step, the concentration of tetrabutyl titanate is adjusted to 0.05 mol / L (4a), 0.1 mol / L (4b), 0.4 mol / L (4d), and 0.5 mol / L (4e), respectively.

[0061] Comparative Example 1 Step 1: Same as Example 1 Step 2: Pour a 0.3 mol / L tetrabutyl titanate solution into the beaker containing activated carbon from Step 1, ensuring the activated carbon is completely submerged. Stir well and soak for 6 hours. Remove the activated carbon, wash it repeatedly with pure water until the supernatant is clear, filter it, dry it at 105℃, and finally calcine it at 600℃ for 2 hours under a nitrogen atmosphere to obtain the catalyst.

[0062] Comparative Example 2 The only difference between this comparative example and Example 1 is that step (1) gradient functionalization of Example 1 is omitted, and untreated columnar activated carbon (raw carbon) is directly used for vacuum coordination infusion. The remaining steps are the same as in Example 1 to obtain the catalyst AC-TiO2 / C.

[0063] Comparative Example 3 The only difference between this comparative example and Example 1 is that the vacuum operation in step (2) of Example 1 is omitted and replaced with atmospheric pressure impregnation, that is: the functionalized activated carbon is directly immersed in tetrabutyl titanate solution and left to stand at atmospheric pressure for 6 hours. The remaining steps are the same as in Example 1 to obtain the catalyst.

[0064] Comparative Example 4 The only difference between this comparative example and Example 1 is that the mixed ligand solution in step (3) of in-situ MOF growth is replaced with pure water, while the other steps are the same as in Example 1.

[0065] Test Example 1 The mass fraction of Ti in the catalysts prepared in the above examples and comparative examples was determined by ICP, and the test results are shown in Table 1.0.

[0066] Test Example 2 The catalysts prepared in the above embodiments and comparative examples were respectively filled into fixed-bed reactors, and persulfate (PMS) was added as an oxidant at a dosage of 5 g / L. The wastewater to be treated was passed through the catalyst bed at a flow rate of 2 BV / h, and the catalytic oxidation reaction was carried out at 25°C for 60 min. The wastewater to be treated, battery soaking wastewater, was sourced from the actual production wastewater of a waste battery recycling plant, with an organic phosphorus concentration of 650 mg / L and a pH of 5. The organic phosphorus removal rates obtained are shown in Table 1.

[0067] Table 1

[0068] Combining the above embodiments and comparative examples with the data in Table 1, it can be seen that: 1. Comparing Example 1 and Comparative Example 1, the organophosphorus removal rate of Example 1 (MOF confined growth method) reached 97.9%, while that of Comparative Example 1 (conventional impregnation method) was only 52.3%, with the former being nearly twice that of the latter. This demonstrates that the present application can achieve atomic-level dispersion of metal oxides, greatly improving the utilization efficiency of active sites.

[0069] 2. Comparing Example 1 and Comparative Example 2, the organophosphorus removal rate of Comparative Example 2 (non-pore functionalized) was only 61.5%, significantly lower than that of Example 1 (97.9%). This demonstrates that gradient pores are beneficial for organophosphorus removal.

[0070] 3. Comparing Example 1 and Comparative Example 3 (without vacuum infusion), the organophosphorus removal rate of Comparative Example 3 was 67.8%, which was lower than that of Example 1. This demonstrates that vacuum infusion can penetrate metal ions deep into the pores, improving the loading capacity and distribution uniformity.

[0071] 4. Comparing Example 1 and Comparative Example 4, the organophosphorus removal rate of Comparative Example 4 was 63.4%, which proves that the organic ligand can promote the in-situ growth of MOF crystals by metal ions in the confined space of the pores, and obtain activated carbon-MOF composite intermediate.

[0072] 5. Comparing Example 1 and Example 2, the optimal pyrolysis temperature is 600℃. If the temperature is too low, the MOF carbonization is incomplete and the active sites are not fully exposed; if the temperature is too high, the TiO2 particles grow or even volatilize, and the activity decreases.

[0073] 6. Comparing Example 1 and Example 3, the optimal ligand concentration is 0.5 mol / L. When the concentration is too low (0.1 mol / L), the MOF growth is incomplete and the loading is low; when the concentration is too high (0.8 mol / L), the MOF grows explosively on the outer surface, which makes the active component easy to detach.

[0074] 7. Comparing Example 1 and Example 4, the activity increases with increasing metal loading within the range of 1-3%. However, the activity decreases when the metal loading exceeds 3% due to pore blockage and particle agglomeration.

[0075] II. Catalyst stability test (taking Example 1 AC-TiO2 / C as an example) The catalyst prepared in Example 1 was reused 10 times under the experimental conditions of Test Example 2. After each reaction, the catalyst surface was rinsed with pure water, and the next round of reaction was carried out directly without any regeneration treatment. The results are shown in Table 2.

[0076] Table 2 Recycling performance of AC-TiO2 / C catalyst

[0077] Note: The titanium leaching amount in the table refers to the concentration of titanium in the treated wastewater.

[0078] After 10 cycles of use, the removal rate of organic phosphorus remained above 90%, and the titanium leaching amount was consistently below 0.05 mg / L (national standard limit), proving that the catalyst of this invention has excellent stability and anti-leakage performance.

[0079] This invention successfully prepared a MOF-derived metal oxide-carbon composite material supported on columnar activated carbon. This catalyst exhibits excellent catalytic degradation performance of recalcitrant phosphorus in battery immersion wastewater, achieving an organophosphorus removal rate of over 97.9% under optimal conditions. Compared with existing technologies, this invention eliminates the need for precious metals (such as Re) and external electric fields, resulting in lower costs, simpler operation, and good catalyst stability and reusability, demonstrating promising prospects for industrial applications.

[0080] In summary, this application has the following superior effects: The pyrolysis process of this invention is not an independent unit operation, but rather relies on the preconditions of prior gradient functionalization, bimetallic infusion, and in-situ MOF growth to simultaneously achieve four functions: carbonization, bonding, vacancy generation, and pore etching. These four functions are interdependent: without a gradient-anchored MOF distribution, uniform interfacial covalent bonds cannot be formed; without N doping introduced by amino ligands, the stability of oxygen vacancies decreases significantly; and without secondary etching in a reducing atmosphere, hierarchical pores cannot be formed.

[0081] This invention generates COM covalent bonds through interfacial chemical reactions, increasing the binding force by an order of magnitude and completely solving the problem of active component detachment under water erosion. Simultaneously, the covalent bonds significantly reduce interfacial electron transfer resistance, increasing the catalytic reaction rate by over 30%. Cyclic testing demonstrates that after 5 cycles, the activity retention rate remains above 95%, far superior to conventional supported materials; this effect cannot be achieved through conventional process stacking.

[0082] The oxygen vacancies generated through in-situ reduction, in synergy with Ti, can efficiently activate persulfate to produce a variety of active species, exhibiting a bond-breaking mineralization ability for phosphate ester organophosphorus compounds that is far superior to that of single-metal oxides. For high-concentration battery-immersed organophosphorus wastewater, the removal rate is significantly higher than the performance level of existing conventional catalysts.

[0083] The gradient pore structure ensures deep loading of active components and enhances mass transfer efficiency through hierarchical structure. Organophosphorus molecules are first adsorbed and enriched by micropores, and then degraded in situ at active sites in mesopores, forming a synergistic effect of "adsorption and enrichment-in situ catalysis", which is especially suitable for treating low-concentration recalcitrant organophosphorus wastewater.

[0084] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A catalyst for wastewater treatment, characterized in that, The catalyst comprises a carbon framework containing channels containing titanium metal oxide particles. The inner wall of the channels is provided with an MOF-derived carbon layer, and the carbon in the MOF-derived carbon layer is covalently connected to the titanium in the titanium metal oxide particles through CO-Ti chemical bonds.

2. The catalyst for wastewater treatment according to claim 1, characterized in that, The diameter of the channel gradually increases along the direction of increasing depth; And / or, the D50 of the titanium oxide particles is 20-100 nm; And / or, the mass fraction of titanium metal element in the catalyst is 0.5% to 5%.

3. A method for preparing a catalyst for wastewater treatment as described in claim 1 or 2, characterized in that, include: Activated carbon is immersed in a first acid solution for the first time to obtain pre-expanded carbon; The pre-expanded carbon is immersed in a second acid solution for a second time to obtain functionalized activated carbon with a pore structure; A precursor solution is introduced into the pore structure of the functionalized activated carbon to obtain activated carbon that adsorbs titanium metal ions. The precursor solution includes a titanium-containing metal precursor and a complexing agent; The activated carbon that adsorbs titanium metal ions is mixed with an aqueous solution of titanium metal ligand to obtain a mixture, and then titanium metal MOF crystals are grown in situ to obtain an activated carbon-supported titanium metal MOF intermediate. The activated carbon-supported titanium metal MOF intermediate was subjected to heat treatment and post-treatment in sequence to obtain the catalyst for wastewater treatment.

4. The method for preparing the catalyst for wastewater treatment according to claim 3, characterized in that, The first acid solution is a dilute nitric acid solution with a mass fraction of 13-18%; And / or, the first soaking time is 2-3 hours; And / or, the activated carbon is selected from columnar activated carbon; And / or, the second acid solution is a mixed acid solution of nitric acid and sulfuric acid, wherein the mass fraction of nitric acid is 10-25% and the mass fraction of sulfuric acid is 5-18%; And / or, the second soaking is performed under aeration conditions for 3-5 hours; And / or, the titanium metal precursor is selected from tetrabutyl titanate; And / or, the titanium metal concentration in the precursor solution is 0.05~0.5 mol / L; And / or, the complexing agent is selected from citric acid; And / or, the molar ratio of the complexing agent to the titanium metal in the titanium metal precursor is 1:(1.8-2.2). And / or, the step of introducing a precursor solution into the pore structure of the functionalized activated carbon includes: placing the functionalized activated carbon in a container, first evacuating it to (-0.13)-(-0.17) MPa and holding it for 10-30 min; then reducing the pressure to (-0.18)-(-0.22) MPa and holding it for 10-30 min; subsequently maintaining the pressure and adding the precursor solution to soak for 4-8 h.

5. The method for preparing the catalyst for wastewater treatment according to claim 3, characterized in that, The titanium metal ligands in the aqueous solution of the titanium metal ligands include 2-methylimidazole and amino-2-methylimidazole; And / or, the total concentration of titanium metal ligands in the aqueous solution of the titanium metal ligands is 0.1~0.8 mol / L; And / or, the in-situ growth of titanium metal MOF crystals includes: first heating the mixture to 50-70°C to induce nucleation, followed by a second heating to 80-100°C for crystal growth.

6. The method for preparing the catalyst for wastewater treatment according to claim 5, characterized in that, The mass fraction of amino-2-methylimidazole in the titanium metal ligand is 10%-20%; And / or, the induction of nucleation time is 1.5-2.5 h; And / or, the heating rate for the first heating is 1.8-2.2℃ / min; And / or, the crystal growth time is 6~10h; And / or, the heating rate for the second heating is 0.4-0.6℃ / min.

7. The method for preparing the catalyst for wastewater treatment according to claim 3, characterized in that, The heat treatment includes a first-stage heat treatment and a second-stage heat treatment performed sequentially under a protective gas atmosphere. The temperature of the first-stage heat treatment is 280-320℃, and the holding time is 50-70 min. The temperature of the second-stage heat treatment is 550-650℃, and the holding time is 2-3 h.

8. The method for preparing the catalyst for wastewater treatment according to claim 7, characterized in that, The heating rate of the first stage of heat treatment is 1.5-2.5℃ / min; And / or, the heating rate of the two-stage heat treatment is 0.8-1.2℃ / min; And / or, the post-processing includes: immersing the heat-treated product in a sodium hydroxide solution, followed by washing and drying.

9. A method for wastewater treatment, characterized in that, In the presence of an oxidant, wastewater containing organophosphorus compounds with a pH of 3-7 is brought into contact with the catalyst described in any one of claims 1-2 to carry out a catalytic oxidation reaction, thereby obtaining wastewater containing orthophosphate.

10. The wastewater treatment method according to claim 9, characterized in that, The oxidant is selected from persulfate; And / or, the mass ratio of the oxidant to the organic phosphorus in the wastewater to be treated is 5~10:1; And / or, the catalyst is packed in a fixed bed reaction, and the flow rate of the wastewater to be treated through the catalyst bed is 1~4 BV / h; And / or, the temperature for the catalytic oxidation reaction is 15-30℃.