Airflow pulverizing and grading system suitable for tantalum powder and tantalum powder preparation method thereof

By combining an airflow pulverization and classification system with periodic interference airflow and a classifier wheel for compensation and adjustment, the problems of wide particle size distribution, over-pulverization, and coarse particles being lost during the airflow pulverization of tantalum powder were solved. This improved pulverization efficiency and finished product particle size stability, reduced metal impurities and oxygen content, and met the capacitor-grade requirements of high-purity tantalum powder.

CN123128089APending Publication Date: 2026-11-20NINGXIA ORIENT TANTALUM INDUSTRY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611413772.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing tantalum powder airflow milling technology has problems such as wide particle size distribution of finished products, coexistence of over-milling and coarse particles, low milling capacity, and high metal impurities and oxygen content.

Method used

An airflow pulverization and classification system is adopted, including a pulverization and classification unit, a dust removal unit, and a control unit. It utilizes a vertical fluidized bed to construct a three-dimensional micro-vortex flow field for high-density materials by combining a jet-type airflow pulverizer, a cyclone separator, and a dust collection tank with periodic disturbance airflow and compensation adjustment of the classifying wheel. Through multi-stage classification modules and high-purity lining materials, efficient classification and dust removal of tantalum powder are achieved.

Benefits of technology

This resulted in a more concentrated particle size distribution of tantalum powder, improved particle size stability, an increase in yield of approximately 20%, and a reduction in metal impurities and oxygen content, meeting the capacitor-grade requirements for high-purity tantalum powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123128089A_ABST
    Figure CN123128089A_ABST
Patent Text Reader

Abstract

The present application relates to a kind of airflow pulverization classification system suitable for tantalum powder and its tantalum powder preparation method, belong to metal powder preparation technical field, solve the existing tantalum powder airflow pulverization process Wide particle size distribution, over-pulverization and coarse particle run coarse coexist, pulverization production capacity is low and the technical problems such as the increase of metal impurity and oxygen in pulverization process.The airflow pulverization classification system suitable for tantalum powder includes pulverization classification unit, dust removal unit, induced draft fan and control unit;Pulverization classification unit is used to pulverize and classify tantalum powder, including vertical fluidized bed counter-jet airflow pulverizer and supplementary classification module;Dust removal unit is used to recover tantalum dust, including cyclone separator and dust tank;Induced draft fan is used to provide wind power for pulverization classification unit and dust removal unit;Control unit is used to control the operation of pulverization classification unit, dust removal unit and induced draft fan.The present application method does not need to blindly improve main airflow pressure, high-purity pollution-resistant lining and high-purity inert atmosphere protection, reduce the oxidation of powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metal powder preparation technology, and specifically relates to an airflow pulverization and classification system suitable for tantalum powder and its tantalum powder preparation method. Background Technology

[0002] Tantalum powder is primarily used in the manufacture of anode materials for tantalum electrolytic capacitors. The Fisher particle size, particle size distribution, particle morphology, specific surface area, oxygen content, and the content of metallic impurities such as Fe, Cr, and Ni are important factors affecting the pressing performance, sintering performance, capacitance, and leakage current performance of tantalum powder. Airflow milling utilizes high-speed airflow to cause inter-particle collisions, shearing, and friction in tantalum powder particles, offering advantages such as less contamination, lower temperature rise, and suitability for the dry preparation of high-purity tantalum powder. Since tantalum has a density of approximately 16.69 g / cm³... 3 Tantalum powder has a high density, making it prone to over-grinding during fluidized bed jet milling, resulting in an increased proportion of fine powder and a wider particle size distribution. Current tantalum powder jet milling technologies primarily focus on adjusting the grinding air pressure and the frequency of the classifier wheel. While simply increasing the grinding air pressure or the classifier wheel frequency can improve the grinding effect to some extent, it also exacerbates wear on the nozzles, classifier wheel blades, and the inner wall of the grinding chamber, shortening the equipment's lifespan and increasing contamination from metallic impurities such as Fe, Cr, and Ni. Summary of the Invention

[0003] In view of the above-mentioned technical status, the present invention provides an airflow pulverization and classification system for tantalum powder and a method for preparing tantalum powder, in order to solve at least one of the technical problems in the existing airflow pulverization process of tantalum powder, such as wide particle size distribution of finished tantalum powder, coexistence of over-pulverization and coarse particles, low pulverization capacity, and high increase in metal impurities and oxygen during the pulverization process.

[0004] The objective of this invention is mainly achieved through the following technical solutions: This invention provides an airflow pulverization and classification system suitable for tantalum powder, including a pulverization and classification unit, a dust removal unit, an induced draft fan, and a control unit; The pulverizing and classifying unit is used to pulverize and classify tantalum powder, including a vertical fluidized bed jet mill and a supplementary classification module; The dust removal unit is used to recover tantalum dust, including a cyclone separator and a dust collection tank; the induced draft fan is used to provide airflow to the crushing and classifying unit and the dust removal unit; the control unit is used to control the operation of the crushing and classifying unit, the dust removal unit and the induced draft fan; The vertical fluidized bed jet mill includes a feeding module, a grinding and classification module, and a collection module. The feeding module feeds tantalum powder raw materials into the grinding and classification module under the action of inert gas. The main body of the grinding and classification module is a cylindrical cavity structure, and the cylindrical cavity is lined with high-purity alumina or silicon carbide all-ceramic material. The grinding and classification module is used to grind the incoming tantalum powder and transport the pre-finished tantalum powder to the supplementary classification module. The collection module is used to collect coarse powder that exceeds the particle size of the pre-finished tantalum powder. The supplementary grading module includes a supplementary grading machine and a finished product collection tank. The supplementary grading machine is used to further grade the pre-finished tantalum powder into finished tantalum powder and tantalum dust. The finished product collection tank is used to collect the finished tantalum powder, and the tantalum dust enters the dust removal unit. Tantalum dust flowing out from the supplementary grading module enters the cyclone separator of the dust removal unit. The dust collection tank is used to collect the tantalum dust, and the exhaust gas after dust removal is discharged from the exhaust port of the cyclone separator.

[0005] Furthermore, the pulverizing and classifying module is divided into a powder collection zone, a pulverizing zone, a transmission zone, and a turbine classification zone from bottom to top inside the cavity; several pairs of opposing-spray Laval nozzles are distributed on the same horizontal cavity circumference at the middle position of the pulverizing zone in the axial direction; and periodic interference airflow intake components are distributed on the same horizontal cavity circumference below the plane of the opposing-spray Laval nozzles.

[0006] Furthermore, the inner diameter D1 of the crushing zone is 200~500mm, and the height H1 is 0.8D1~2.5D1; the opposing spray Laval nozzles are on the same horizontal cavity circumference at a height of 0.25H1~0.75H1 from the bottom surface of the crushing zone; the periodic interference airflow inlet assembly is on the same horizontal cavity circumference at a height of 0.02H1~0.35H1 from the bottom surface of the crushing zone.

[0007] Furthermore, the ratio of the total throat cross-sectional area of ​​several pairs of opposing-spray Laval nozzles to the cross-sectional area of ​​the pulverizing zone is 0.0003~0.0008; the air intake assembly includes multiple sets of air intake ports, which are evenly distributed on the circumference of the cavity. The direction of the air intake ports is inclined upward, and the angle β between the axial direction of the air intake port and the horizontal plane is 15°~75°. The deflection angle α formed by the projection of the axial direction of the air intake port on the bottom surface of the pulverizing zone and the axial section of the pulverizing zone intersecting on the circumference of the pulverizing zone is 5°~45°, and the deflection direction is consistent.

[0008] Furthermore, the turbine grading zone has a cylindrical or near-cylindrical structure, and a first turbine grading wheel is installed in the central region along the axial direction of the turbine grading zone.

[0009] Furthermore, the supplementary grading module includes a first supplementary grading machine and a second collection tank, or a first supplementary grading machine and a second collection tank, a second supplementary grading machine and a third collection tank.

[0010] In addition, the present invention also provides a method for preparing tantalum powder using the above system, comprising the following steps: Step S1: Pretreatment of tantalum powder raw materials; Step S2: Equipment inertization; Step S3: Start the pulverizing airflow; Step S4: Activate the first turbine classifier in the crushing and classifying module, and the second turbine classifier or the second turbine classifier and the third turbine classifier in the supplementary classifying module; Step S5: Feeding and crushing; Step S6: Apply periodic disruptive airflow; Step S7: Grade wheel compensation adjustment; Step S8: Tantalum powder classification and collection; Step S9: Detection and closed-loop adjustment.

[0011] Furthermore, in step S3, the absolute pressure of the pulverizing airflow is 0.6~12MPa; and / or, in step S4, the basic rotational speed of the first turbine classifier is 1000~12000rpm, and the outer edge linear velocity of the blades of the first turbine classifier is 25~90m / s; the basic rotational speed of the second turbine classifier or the second turbine classifier and the third turbine classifier is 1.12~1.15 times the basic rotational speed of the first turbine classifier, and the outer edge linear velocity of the blades of the second turbine classifier or the second turbine classifier and the third turbine classifier is 1.12~1.15 times the outer edge linear velocity of the blades of the first turbine classifier.

[0012] Furthermore, in step S5, the material holding capacity per unit cross-sectional area of ​​the crushing zone is 40~300 kg / m². 2 Within this range, the material holding capacity accounts for 10% to 30% of the effective volume of the crushing zone, the apparent cross-sectional air velocity within the crushing zone is in the range of 0.15 to 0.60 m / s, the total system air volume is 15 to 200 Nm³ / h, and the gas-solid ratio is 1.5 to 8.0 Nm³ / h. 3 / kg.

[0013] Furthermore, in step S6, the periodic interference airflow operates in two modes: one is a staggered start-stop mode, where multiple sets of inlet ports of the periodic interference airflow inlet assembly alternately start and stop sequentially within one pulse cycle, and then repeat cyclically. Within one pulse cycle, each set of inlet ports starts and stops once. When one set of inlet ports starts, the other inlet ports stop, and when one set of inlet ports stops, another set starts. The other mode is a synchronous start-stop mode, where multiple sets of inlet ports of the periodic interference airflow inlet assembly start and stop simultaneously, repeating cyclically. Within one pulse cycle, all inlet ports start and stop once. The pulse frequency of the periodic interference airflow is 0.2~10Hz, the duty cycle is 10%~60%, the pressure of the periodic interference airflow is 20%~90% of the pulverizing airflow pressure, and the average flow rate is 2%~15% of the total flow rate of the pulverizing airflow. And / or, in step S7, when the average flow rate of the periodic disturbance airflow increases, the rotational speed of each classifier wheel is increased; when the pressure difference at the bottom of the crushing layer decreases and the product particle size tends to stabilize, the rotational speed of each classifier wheel is decreased; the compensation adjustment amount of the classifier wheel is 1% to 15% of the base rotational speed of the classifier wheel.

[0014] Compared with the prior art, the present invention can achieve at least one of the following technical effects: 1. The system of this invention features a periodically interfering air intake component with an upward tilt and tangential deflection at a specific height in the crushing zone. Combined with an upper tapered frustum-shaped transmission zone and a multi-stage series turbine classification module, it constructs a three-dimensional micro-vortex flow field specifically for high-density materials. The air intake component does not directly impact the main spray zone and classification wheel. While protecting the main crushing energy focus, it controls the lifting and redispersing of heavy tantalum powder at the bottom of the chamber, prompting it to enter the spray zone for collision in a timely manner. The crushed particles smoothly enter the multi-stage classification wheel for precise classification with the tapered airflow. This equipment configuration eliminates over-crushing and coarsening caused by bottom deposition, resulting in finer tantalum powder at the fine end (D). 10 The diameter increased from 1.91 μm to 2.25 μm, D 95 The particle size distribution decreased from 5.22μm to 4.89μm, resulting in a more concentrated particle size distribution and completely eliminating the phenomenon of coarse particles being carried away.

[0015] 2. In the tantalum powder preparation method of the present invention, at the instant the periodic disturbance airflow pulsation is activated, the control system synchronously implements dynamic upward speed feedforward compensation for each classifier in the first turbine classifier and the supplementary classifier module, accurately offsetting the instantaneous aerodynamic thrust surge caused by the pulsation disturbance, so that the gas-solid balance point inside and outside the classifier remains constant throughout the pulsation cycle, eliminating the impact of pulsating airflow on the particle size of the classifier, preventing the escape of coarse powder that has not been fully dissociated, and ensuring the particle size stability of the finished tantalum powder between batches and in continuous production.

[0016] 3. The tantalum powder preparation method of this invention adopts a periodic interfering airflow and a staged wheel compensation adjustment mechanism, which solves the industry pain point of easy deposition and low fluidization of high-density tantalum powder. Compared with non-interfering airflow, the yield is increased by about 20%; compared with continuous blowing, it avoids diluting the energy of the pulverizing airflow, and the gas-solid ratio is significantly reduced to 4.11 Nm. 3 / kg.

[0017] 4. The tantalum powder preparation method of the present invention does not require blindly increasing the main gas flow pressure. With the combination of high-purity anti-pollution lining and high-purity inert atmosphere protection, the wear of the cavity and classifier wheel and the oxidation of the powder surface are greatly reduced. The increase of Fe, Cr and Ni impurities in a single crushing is no more than 3 ppm, and the increase of oxygen (ΔO) is less than 500 ppm, which meets the requirements of capacitor-grade high-purity tantalum powder. Attached Figure Description

[0018] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.

[0019] Figure 1 This is a schematic diagram showing the connections of each unit in the airflow pulverization and classification system for tantalum powder according to the present invention; Figure 2 for Figure 1 A schematic diagram of the axial cross-sectional structure of the crushing zone, the conveying zone, and the turbine classification zone in the crushing and classification module of the present invention; Figure 3 A top view of the intake assembly for periodically interfering airflow; In the diagram: 1-Grinding and classifying unit; 11-Vertical fluidized bed jet mill; 111-Feeding module; 1111-Hopper; 1112-Feeder; 1113-Ejector mixing chamber; 11131-Ejector gas inlet; 1114-Feed pipe; 112-Grinding and classifying module; 1121-Powder collection zone; 1122-Grinding zone; 11220-Laval nozzle; 11221-Periodic interference airflow inlet assembly; 1123-Transfer zone; 1124-Turbine classifier Zone; 11241-First turbine classifier; 11242-First motor; 113-Collection module; 1131-First collection tank; 1132-First solenoid valve; 1133-Second solenoid valve; 12-Supplementary classification module; 121-First supplementary classifier; 1211-Second turbine classifier; 1212-Second motor; 122-Second collection tank; 123-Second supplementary classifier; 1231-Third turbine classifier; 1232-Third motor; 124-Third collection tank; 2-Dust removal unit; 21-Cyclone separator; 211-Dust collection chamber; 212-Exhaust gas outlet; 22-Dust collection tank; 3-Exhaust fan; 4-Control unit; D1 - Inner diameter of the crushing zone; H1 - Height of the crushing zone; D 2a -Inner diameter at the lower end of the transmission area; D 2b - Inner diameter of the upper end of the transmission zone; H2 - Height of the transmission zone; D3 - Inner diameter of the turbine stage zone; H3 - Height of the turbine stage zone; β - Angle between the axial direction of the intake port of the intake assembly and the horizontal plane; α - Deflection angle formed by the projection of the axial direction of the intake port of the intake assembly onto the bottom surface of the crushing zone and the intersection of the axial section of the crushing zone with the circumference of the crushing zone; A, B, C - Three sets of intake ports of the intake assembly. Detailed Implementation

[0020] The following detailed description, in conjunction with specific embodiments, provides an airflow pulverization and classification system suitable for tantalum powder and a method for preparing tantalum powder thereof. These embodiments are for comparative and illustrative purposes only, and the present invention is not limited to these embodiments.

[0021] First, this invention proposes an airflow pulverization and classification system suitable for tantalum powder, the system comprising a pulverization and classification unit, a dust removal unit, an induced draft fan, and a control unit; The pulverizing and classifying unit is used to pulverize and classify tantalum powder, including the main equipment, a vertical fluidized bed jet mill, and a supplementary classification module. The dust removal unit is used to recover tantalum dust and includes a cyclone separator and a dust collection tank; The induced draft fan is used to provide airflow to the crushing and grading unit and the dust removal unit; the control unit is used to control the operation of the crushing and grading unit, the dust removal unit and the induced draft fan.

[0022] Figure 1 This is a schematic diagram of the connection of each unit in the airflow pulverization and classification system applicable to tantalum powder of the present invention. In the figure, 1 is the pulverization and classification unit, 11 is the vertical fluidized bed counter-jet airflow pulverizer, 12 is the supplementary classification module, 2 is the dust removal unit, 21 is the cyclone separator, 22 is the dust collection tank, 3 is the induced draft fan, and 4 is the control unit.

[0023] The vertical fluidized bed jet mill has a periodic interfering airflow inlet assembly distributed below the plane of the jet Laval nozzle in the grinding zone. The supplementary classification module is located after the vertical fluidized bed and further classifies the powder after grinding by the vertical fluidized bed.

[0024] Tantalum powder raw material first enters the vertical fluidized bed jet mill in the pulverizing and classifying unit. The pulverized tantalum powder is then further classified by a supplementary classification module. The classified and optimized tantalum powder then enters the dust removal unit, where tantalum dust is collected, and the exhaust gas is discharged. The induced draft fan provides airflow to the pulverizing and classifying unit and the dust removal unit; the control unit controls the operation of the pulverizing and classifying unit, the dust removal unit, and the induced draft fan.

[0025] Specifically, the vertical fluidized bed jet mill includes a feeding module, a grinding and grading module, and a collection module. The feeding module is used to feed tantalum powder raw materials into the grinding and grading module under the action of inert gas ejection. The feeding module includes a hopper, a feeder, an ejector mixing chamber, and a feeding pipe. The hopper stores the tantalum powder raw materials, and the feeder transports the tantalum powder raw materials from the hopper into the ejector mixing chamber. The ejector mixing chamber has an ejector gas inlet at the top, through which inert gas enters the ejector mixing chamber. Then, the tantalum powder raw materials in the ejector mixing chamber are ejected obliquely downwards into the grinding and grading module through the feeding pipe. The upper end of the feeding pipe connects to the lower part of the ejector mixing chamber, and the lower end connects to the upper side of the transmission area of ​​the grinding and grading module. The feeding pipe runs obliquely downwards. Figure 1 In the diagram, 111 is the feeding module, 1111 is the hopper, 1112 is the feeder, 1113 is the ejector mixing chamber, 11131 is the ejector gas inlet, 1114 is the feeding pipe, 112 is the crushing and grading module, and 113 is the collection module.

[0026] The main body of the crushing and grading module is a cylindrical cavity structure. Inside the cavity, from bottom to top, it is divided into a powder collection area, a crushing area, a transmission area, and a turbine grading area. The cylindrical cavity of the crushing and grading module has a pollution-proof lining, which is made of high-purity alumina or silicon carbide all-ceramic material to prevent or reduce the introduction of metal impurities such as Fe, Cr, and Ni.

[0027] In terms of overall system structure, the present invention adopts an integrated vertical stacked layout of powder collection zone, crushing zone, transmission zone and turbine classification zone from bottom to top, and cooperates with the feed pipe to feed the material obliquely downward from the upper part of the transmission zone. Its basic function is to build a smooth fluidization channel and realize the continuous operation of crushing and classification in the same cavity. Furthermore, the above-mentioned layout has a significant synergistic effect when processing high-density heavy tantalum powder: tantalum powder (density approximately 16.69 g / cm³) has a strong gravity settling effect. The downward trajectory of the feed pipe allows the raw material particles to directly pass through the stable transmission zone and naturally sink to the crushing zone under the combined effect of initial momentum and gravity, effectively avoiding the short-circuiting and coarsening of coarse particles caused by the direct influx of feed into the upper turbine classification zone. At the same time, the vertically coaxial stacked layout physically separates the lower "high-turbulence, high-collision crushing zone" from the upper "stable-flow, rectified turbine classification zone". Combined with the gradually narrowing transmission zone in the middle, a closed-loop synergistic mechanism is formed in the entire cavity: "smooth feeding from the upper side - efficient collision self-grinding in the middle and lower part - stable flow fine classification in the middle and upper part - bottom settling discharge", completely eliminating turbulent backflow and repeated over-crushing of particles.

[0028] The powder collection zone, located at the bottom of the crushing and grading module, is an inverted cone structure with a full cone angle of 60-80°. It is used to collect the deposited tantalum powder during the crushing and grading process. High-density tantalum powder has a large angle of repose and high wall sliding friction resistance. Setting this range ensures that the settled heavy powder flows smoothly under its own weight and collects in the collection module. If the full cone angle does not fall within this range, the following adverse effects will occur: if the full cone angle is greater than 80°, the cone generatrix is ​​too gently inclined, and heavy tantalum powder is prone to sticking and bridging on the cone wall, leading to caking and dead zones at the bottom; if the full cone angle is less than 60°, the axial height of the powder collection zone will be excessively elongated, increasing the ineffective volume of the equipment and severely weakening the pneumatic cleaning disturbance force during bottom backflushing. Therefore, controlling the full cone angle at 60-80° ensures that the high-density tantalum powder flows smoothly under gravity, while maintaining a compact lower cavity and a stable flow field.

[0029] The crushing zone is located above the powder collection zone. The crushing zone has a cylindrical or near-cylindrical structure. Several pairs of opposing-spray Laval nozzles are distributed on the same horizontal cavity surface at a certain height from the bottom of the crushing zone. The basic function of the Laval nozzles is to accelerate the expansion of the introduced high-pressure inert gas into a supersonic jet. The effect is to form a high-energy collision focus at the center of the crushing zone, causing the entrained tantalum powder particles to undergo violent self-collision and shearing, thereby avoiding direct impact of high-speed particles on the inner wall of the cavity and minimizing the wear of the ceramic lining and the introduction of metal impurities.

[0030] In one possible design, the inner diameter D1 of the crushing zone is approximately 200-500 mm. At the midpoint of the crushing zone's axial direction, at a height of 0.25H1-0.75H1 from the bottom surface of the crushing zone, several pairs of opposing Laval nozzles (e.g., 1-4 pairs) are distributed on the same horizontal cavity circumference. Two opposing Laval nozzles on the same diameter of the cylindrical cavity are referred to as a pair of opposing Laval nozzles. The height H1 is approximately 0.8D1-2.5D1. The throat diameter of a single nozzle is d. t The diameter is 1.5~8.0 mm, and the designed Mach number Ma is 1.2~3.0; the ratio of the total throat cross-sectional area of ​​several pairs of nozzles to the cross-sectional area of ​​the crushing zone is maintained at 0.0003~0.0008. The Laval nozzles are positioned at a midpoint height of 0.25H1~0.75H1 from the bottom surface of the crushing zone, with a height ratio H1 / D1 limited to 0.8~2.5. This allows the nozzles to be stably submerged in the fluidized bed with a specific bed thickness, providing sufficient space below the nozzles for periodically pulsating fluidized airflow to activate the bottom deposited material, while also maintaining a suitable gas-solid buffer release height above the nozzles to prevent insufficiently collided high-energy airflow from directly impacting the top classifier. Furthermore, the designed Mach number Ma of 1.2~3.0 is matched with the throat diameter d. tThe diameter is 1.5~8.0mm, ensuring that the high-pressure gas is transformed into a supersonic collision field with extremely high kinetic energy under the operating pressure of 0.6~12MPa, which can overcome the high toughness of high-density tantalum metal and achieve efficient fracture refinement. Furthermore, the ratio of the total throat cross-sectional area of ​​several pairs of nozzles to the cross-sectional area of ​​the crushing zone is controlled at 0.0003~0.0008, which is the core guarantee for maintaining the apparent cross-sectional gas velocity of the crushing zone at 0.15~0.60m / s. If this ratio is less than 0.0003, the amount of expanding gas and kinetic energy entering the crushing chamber is insufficient, making it difficult to effectively agitate and fluidize the high-density tantalum powder bed. If this ratio is greater than 0.0008, the gas velocity per unit cross-sectional area is too high, which will not only cause violent gas surge in the bed and disperse and dilute the collision energy of the main nozzle, but also cause coarse particles that have not been fully collided and dissociated to be prematurely blown up to the turbine classification zone, seriously damaging the classification accuracy and causing coarse particles to penetrate and run away.

[0031] Several pairs of opposing-jet Laval nozzles are mainly used to pulverize tantalum powder particles through inter-particle collisions using multiple high-speed jet streams. Below the plane of the opposing-jet Laval nozzles, on the same horizontal cavity circumference at a height of 0.02H1~0.35H1 from the bottom of the pulverization zone, periodically interfering airflow inlet components are distributed. These inlet components include multiple sets of inlet ports. Two opposing inlet ports on the same diameter of the cylindrical cavity are called a set of inlet ports, such as 2~4 sets. These sets of inlet ports are evenly distributed on the cavity circumference, meaning the central angle formed by two adjacent inlet ports is equal everywhere. The inlet components are positioned 0.02H1~0.35H1 below the plane of the opposing-jet nozzles. 1. On the low circumferential surface, the bottom dead zone where high-density tantalum powder is most prone to agglomeration and caking due to gravity sedimentation is precisely targeted; through multiple sets of pipes arranged symmetrically at equal angles around the circumference, momentum input is achieved in the entire circumferential direction, ensuring that the material on the bottom cross-section of the entire crushing zone is subjected to uniform force and fluidized throughout the entire area, eliminating bed flow deviation, asymmetric turbulent vortex and localized violent splashing caused by unidirectional air blowing. Moreover, this position is strictly layered in space with the main anti-spray plane above, which can achieve directional activation and lifting of heavy materials in the lower part without completely destroying the integrity of the collision flow field at the center of the main nozzle.

[0032] Furthermore, the direction of the air intake is inclined upward, and the angle β between the axial direction of the air intake and the horizontal plane is about 15°~75°. The projection of the axial direction of the air intake on the bottom surface of the crushing zone intersects with the axial section of the crushing zone on the circumference of the crushing zone, forming a deflection angle α. The deflection directions are all consistent, such as all deflecting clockwise or all deflecting counterclockwise. The deflection angle α is about 5°~45°. An elevation angle β (15°~75°) imparts a vertical momentum component to the disturbing airflow, which generates a lifting force that penetrates the dense settling layer. This causes the coarse tantalum powder particles settled at the bottom to periodically loosen, suspend, and be directionally transported to the suction and entrainment zone of the main Laval nozzle for re-collision. If β is less than 15°, the vertical momentum is insufficient to lift the heavy tantalum powder with a density as high as 16.69 g / cm³. If β is greater than 75°, the airflow is excessively vertical, easily penetrating the main jetting area and disturbing the classification flow field, even blowing undissociated coarse material directly into the classifier wheel. Tangential deflection angle α (5°~ If α is less than 5°, a regular circumferential swirling flow cannot be formed, and it easily evolves into a chaotic flow field with central impaction. If α is greater than 45°, the tangential rotational momentum is too strong and the axial lifting kinetic energy is drastically weakened. This not only fails to effectively achieve upward fluidization of the bottom material, but also greatly aggravates the rotational tangential erosion of the gas and solid relative to the inner wall of the cylinder.

[0033] The periodic interference airflow inlet assembly is used to apply periodic pulsating interference airflow below the pulverizing zone, eliminate the dead zone at the bottom of the high-density tantalum powder deposition, promote the re-entry of coarse particles into the spray zone of the vertical fluidized bed airflow mill, and improve pulverizing efficiency.

[0034] The transport zone and the turbine classification zone are coaxially and vertically stacked above the grinding zone. Addressing the characteristics of tantalum powder—its extremely high density (approximately 16.69 g / cm³), rapid settling, and susceptibility to turbulent flow—this invention constructs a transport zone with a gradually tapering transition from small to large at the bottom between the two zones. This tapering structure eliminates powder retention and wall backflow that can easily occur with a straight, uniform-diameter cylinder transition, effectively buffering the dynamic pressure impact from the lower grinding jet. Furthermore, the smooth contraction of the cross-section controls the acceleration of the rising airflow, providing a stable upward drag force to the high-density fine powder. This guides qualified powder to be smoothly transported to the classification zone, completely resolving the contradiction between fine powder falling back into the grinding zone and coarse powder being carried away by turbulent flow.

[0035] In terms of specific dimensions, the lower inner diameter D of the transmission area 2a The inner diameter of the crushing zone, D1, should be controlled to be 0.8 to 1.2 times; if D... 2aIf the diameter is too small, it will create stepped dead zones at the edges, exacerbating localized wear and material splashing; if it is too large, it will increase the ineffective dead zone at the edges, causing airflow to adhere to the wall and detach and settle. The inner diameter D at the upper end of the transmission zone... 2b Control it to be 0.35D1~0.85D1; if D 2b If the air velocity is too high, insufficient air velocity will cause high-density fine powder to fall back due to gravity; if it is too low, throttling jets will be generated at the top, forcibly blowing coarse particles into the classifier wheel, causing severe coarseness. The height H2 of the transfer zone is set to 0.3D1~1.5D1 to provide sufficient turbulent dissipation and rectification stroke; if it is too short, the lower turbulent flow will directly impact the classifier wheel, disturbing the centrifugal flow field; if it is too long, it will increase the flow resistance along the path and easily cause heavy powder to slide and stick to the wall.

[0036] Specifically, the transmission zone is located above the crushing zone. The transmission zone has a transitional structure that is smaller at the top and larger at the bottom, resembling a frustum, cone, or trapezoid. The inner diameter D at the lower end of the transmission zone... 2a Approximately 0.8D1~1.2D1, the inner diameter D at the upper end of the transmission area. 2b The diameter D3 is approximately 0.35D1~0.85D1, and the height H2 is approximately 0.3D1~1.5D1. It is mainly used to transport the pulverized tantalum powder particles with the rising airflow to the turbine classification zone. The turbine classification zone is located above the transport zone. It is a cylindrical or near-cylindrical structure with an inner diameter D3 of approximately 0.35D1~0.90D1 and a height H3 of approximately 0.3D1~1.2D1. A first turbine classifier is installed in the central region along the axial direction of the turbine classification zone. The radial direction of the first turbine classifier is consistent with the radial direction of the turbine classification zone, and the axial direction of the first turbine classifier is consistent with the axial direction of the turbine classification zone. The diameter D of the first turbine classifier is... c The height H of the first turbine stage wheel is approximately 0.25D3 to 0.85D3. c Approximately 0.10D c ~0.60D c A first motor for driving the first turbine classifying wheel is installed above the top surface of the turbine classifying zone along the axial direction. The turbine classifying zone is mainly used for particle size classification of crushed tantalum powder particles.

[0037] The turbine grading zone is cylindrical or nearly cylindrical in shape, with an inner diameter D3 of approximately 0.35D1 to 0.90D1 and a height H3 of approximately 0.3D1 to 1.2D1. Inside, a first turbine grading wheel, driven by a top motor, is installed for high-precision cutting and sorting. The diameter D of the first turbine grading wheel is... c The value is controlled within the range of 0.25D3 to 0.85D3 to define a reasonable annular feed channel; if D c If the diameter is too large and the annular gap is too narrow, it will cause a sudden increase in local air resistance and exacerbate the erosion and wear of the inner wall of the equipment by the high-hardness tantalum powder; if D cIf the height is too small, the centripetal velocity distribution of the gas-solid flow will be uneven, and fine particles at the edges will easily escape directly from the centrifugal force field, reducing the sharpness of the stage. Furthermore, the height H of the first turbine stager... c Controlled to 0.10D c ~0.60D c If H c If the inlet is too small, insufficient effective area will reduce the system's hourly output; if H c If the velocity is too high, it will cause severe uneven radial suction velocity at different points along the grading wheel axis. Excessive drag near the suction port will pull coarse powder through, while material at the far end will be excessively repelled and retained, ultimately resulting in blurred grading and cutting points and a wider particle size distribution. Figure 2 This is a schematic diagram of the axial cross-sectional structure of the crushing zone, the transmission zone, and the turbine classification zone in the crushing and classification module of the present invention. In the figure, 1122 is the crushing zone, 11220 is the counter-spray type Laval nozzle, 11221 is the air intake assembly, angle β is the angle between the axial direction of the air intake port and the horizontal plane, 1123 is the transmission zone, and 1124 is the turbine classification zone. Figure 3 This is a top view of the air intake assembly, which includes 3 groups of 6 air intake ports, namely group A, group B, and group C. Angle α is the deflection angle formed by the projection of the axial direction of the air intake port onto the bottom surface of the crushing zone and the intersection of the cross section of the crushing zone with the circumference of the crushing zone.

[0038] The collection module is used to collect coarse powder after air jet milling. It includes a first collection tank and solenoid valves. The first collection tank is located directly below the milling and grading module and is connected to the collection area of ​​the milling and grading module via a pipeline controlled by solenoid valves. There are two solenoid valves, one lower and one higher. The lower solenoid valve, closer to the collection tank, controls the connection or closure between the milling area and the collection tank. The upper solenoid valve, closer to the first collection area, controls the backflushing airflow during powder discharge. Given the physical characteristics of high-density tantalum powder, which is prone to compaction and caking, this dual-solecular-valve collaborative control structure has significant discharge advantages: during normal system operation, both valves remain closed to maintain the fluidization and airtightness of the milling chamber; during shutdown and powder discharge, the lower first solenoid valve opens to connect to the collection tank, while the upper second solenoid valve, closer to the collection area, is used to pulse-introduce the backflushing airflow. This backflushing airflow can instantly break down the bottom bridging and dense caking of the tantalum powder deposited in the collection area, allowing the heavy powder to flow smoothly downwards into the collection tank with pneumatic assistance, avoiding the drawbacks of conventional gravity discharge that results in incomplete discharge or the need for manual knocking to clean the equipment.

[0039] The supplementary grading module includes a supplementary grader and a finished product collection tank, such as a first supplementary grader and a second collection tank. The first supplementary grader is a cylindrical or near-cylindrical cavity structure. The inner diameter of the first supplementary grader is equal to the inner diameter of the turbine grading zone of the crushing and grading module. A second turbine grading wheel is installed in the upper axial region of the cylindrical cavity. The radial direction of the second turbine grading wheel is consistent with the radial direction of the cylindrical cavity, and the axial direction of the second turbine grading wheel is consistent with the axial direction of the cylindrical cavity. The diameter and height of the second turbine grading wheel are equal to the diameter and height of the first turbine grading wheel, respectively. A second motor for driving the second turbine grading wheel is installed above the top surface of the cylindrical cavity in the axial direction. The cylindrical cavity sidewall corresponding to the second turbine grading wheel is connected to the outlet of the turbine grading zone to perform a second grading on the tantalum powder flowing from the first turbine grading wheel, thereby optimizing the grading effect. For extremely dense tantalum powder, a single classifier wheel, under conditions of high gas-to-solid ratio and bottom pulsating fluidization, cannot completely prevent the escape of a few high-kinetic-energy coarse particles. Using a first supplementary classifier of identical size allows for the in-situ replication of the same fluid dynamics environment (i.e., similar radial pressure and wall boundary layer effects) within the classifier's chamber. The airflow carrying pre-processed tantalum powder is introduced from the turbine classifier outlet into the sidewall of the second turbine classifier wheel. Based on this consistent flow field, a second motor at the top imparts a higher rotational speed to the classifier wheel, enabling precise secondary momentum centrifugal interception of any coarse particles that may have escaped during the initial classification, thus significantly optimizing the classification sharpness. The lower part of the classifier has an inverted conical structure; the qualified tantalum powder that has been secondary-intercepted and falls ultimately settles by gravity into the second collection tank at the bottom.

[0040] Furthermore, based on the higher process requirements for extremely narrow particle size distribution of the finished product, the supplementary classification module can also include a second supplementary classifier and a third collection tank. The second supplementary classifier has the same structure and dimensions as the first supplementary classifier, and also includes a third turbine classifier and a third motor driving the third turbine classifier. The third collection tank has the same structure and dimensions as the second collection tank, and the connection method between the second supplementary classifier and the third collection tank is exactly the same as that between the first supplementary classifier and the second collection tank. The tantalum powder flowing out of the first supplementary classifier enters the second supplementary classifier for a third classification, and the classified tantalum powder product finally enters the third collection tank. This multi-stage, equal-scale series physical architecture, combined with subsequent progressive classification speed control, completely eliminates the possibility of heavy coarse powder being entrained and carried away from the hardware flow field, and strictly locks the coarse end boundary of the finished tantalum powder. ).

[0041] Tantalum dust flowing from the supplementary classification module enters the cyclone separator of the dust removal unit. If the supplementary classification module only includes a first supplementary classifier and a second collection tank, the tantalum dust flowing from the first supplementary classifier enters the cyclone separator of the dust removal unit. If the supplementary classification module includes a first supplementary classifier, a second collection tank, a second supplementary classifier, and a third collection tank, the tantalum dust flowing from the second supplementary classifier enters the cyclone separator of the dust removal unit. The dust collection chamber and dust collection tank at the bottom of the cyclone separator are connected to collect tantalum dust, while the exhaust gas after dust removal is discharged from the exhaust gas outlet. Taking advantage of the high density and extremely high economic value of ultrafine tantalum powder, the cyclone separator utilizes the strong centrifugal settling effect generated by the airflow rotation to efficiently separate the extremely fine tantalum dust carried in the exhaust gas. The separated fine tantalum dust falls into the connected dust collection chamber at the bottom and is collected by the dust collection tank with a high recovery rate, while the purified exhaust gas is safely discharged from the exhaust gas outlet, preventing the loss of high-purity materials and eliminating dust pollution.

[0042] The induced draft fan provides airflow to the crushing and grading unit and the dust removal unit; the control unit controls the operation of the crushing and grading unit, the dust removal unit, and the induced draft fan. The induced draft fan is located at the end of the system and provides a precisely adjustable negative pressure driving force for the global gas-solid two-phase flow of the crushing and grading unit and the dust removal unit, ensuring that high-density tantalum powder particles remain in a stable suspended conveying state throughout the fluidization, tapering, and multi-stage grading channels, avoiding deposition along the pipeline. The control unit (such as a PLC control system) coordinates the automated and collaborative operation of the crushing and grading unit, the dust removal unit, and the induced draft fan; in particular, this control unit is equipped with a feedforward control module, which simultaneously performs high-precision dynamic speed compensation adjustment of the drive motors of each stage of the turbine grading wheel upon receiving a signal indicating the start of periodic interfering airflow pulsation at the bottom of the crushing zone, thereby ensuring that the cut particle size remains constant under complex flow field disturbances.

[0043] Secondly, this invention proposes a method for preparing tantalum powder using the above-mentioned airflow pulverization and classification system, comprising the following steps: Step S1: Pretreatment of tantalum powder raw materials; Step S2: Equipment inertization; Step S3: Start the pulverizing airflow; Step S4: Activate the first turbine classifier in the crushing and classifying module, and the second turbine classifier or the second turbine classifier and the third turbine classifier in the supplementary classifying module; Step S5: Feeding and crushing; Step S6: Apply periodic disruptive airflow; Step S7: Grade wheel compensation adjustment; Step S8: Tantalum powder classification and collection; Step S9: Detection and closed-loop adjustment.

[0044] Specifically, in step S1, the tantalum powder raw material is pretreated, including sieving, drying, and impurity removal, to meet the requirements of airflow milling. Preferably, all the tantalum powder raw material passes through a 0.175mm sieve, and the moisture content is not higher than 0.05%.

[0045] In step S2, nitrogen or argon is used to purify all equipment in the crushing and grading unit and the dust removal unit of the system, such as the hopper, feeder, ejector mixing chamber and feed pipe in the feeding module, the chamber and collection tank in the crushing and grading module, the supplementary grading chamber and collection tank in the supplementary grading module, the cyclone separator and dust collection tank in the dust removal unit, and the connecting pipes between the units, so that the equipment is in a low-oxygen, low-moisture state. Preferably, after purging, the oxygen content of the protective gas in the system meets the requirements of O2 ≤ 500 ppm and the gas dew point ≤ -40°C. o C, preferably ≤-50 o C.

[0046] In step S3, the pulverizing gas flow is activated, causing the inert gas to form a high-speed jet through a counter-jet Laval nozzle. The inert gas used is nitrogen or argon. The absolute pressure of the pulverizing gas flow is 0.6~12MPa, preferably 0.7~8MPa, and can be set according to the particle size of the tantalum powder raw material and the particle size of the target product.

[0047] In step S4, the initial classifying wheel frequency of each turbine classifying wheel is set so that the classifying and cutting particle size matches the target product particle size. The basic rotational speed of the first turbine classifying wheel is 1000~12000 rpm, and the outer edge linear velocity of the classifying wheel blades is controlled at 25~90 m / s. The basic rotational speed of the second and third turbine classifying wheels in the supplementary classification module is 1.12~1.15 times that of the first turbine classifying wheel, and the corresponding outer edge linear velocity of the classifying wheel blades is also 1.12~1.15 times that of the first turbine classifying wheel blades.

[0048] In step S5, the pretreated tantalum powder raw material is continuously or intermittently fed into the crushing and grading unit through the feeding module, so that the tantalum powder particles are crushed by inter-particle collision, shearing and friction under the action of high-speed jet flow in the crushing zone.

[0049] Specifically, tantalum powder raw materials are stored in a silo. A feeder transports the tantalum powder raw materials from the silo into the ejector mixing chamber. Inert gas enters the ejector mixing chamber through the ejector gas inlet. The inert gas used is the same gas as the pulverizing gas flow, such as nitrogen or argon. Then, the tantalum powder raw materials in the ejector mixing chamber are injected obliquely downwards into the pulverizing and classifying module through the feed pipe. The pressure of the inert gas is 0.2~0.4MPa, and the gas-solid ratio is 0.2Nm. 3 / kg, meaning that 0.2 Nm³ of gas is consumed per kilogram of tantalum powder transported. 3 .

[0050] During the crushing process, the material holding capacity of the unit crushing zone cross-sectional area is controlled at 40~300kg / m². 2 Preferred weight: 45~220 kg / m 2 The material holding capacity accounts for 10% to 30% of the effective volume of the crushing zone; the apparent cross-sectional air velocity within the crushing zone is maintained within the range of 0.15 to 0.60 m / s, i.e., the gas velocity per unit cross-sectional area of ​​the crushing zone is 0.15 to 0.60 m / s; the total system air volume is set to 15 to 200 Nm³ / h (preferably 20 to 160 Nm³ / h) based on the matching of the inner diameter of the crushing zone and the apparent air velocity; the gas-solid ratio is 1.5 to 8.0 Nm³ / h. 3 / kg, meaning that the gas consumption per kilogram of tantalum powder is 1.5~8.0 Nm³. 3 Preferably 2.5~5.0 Nm 3 / kg.

[0051] In step S6, a periodic disturbance airflow is initiated, which enters the crushing zone periodically from the lower side wall of the crushing zone, disturbing the tantalum powder particles deposited at the bottom of the crushing zone. This causes the deposited tantalum powder to periodically loosen, rise, and redisperse, and then re-enter the high-speed jet crushing zone to participate in collision crushing.

[0052] Specifically, the periodic interference airflow operates in two modes. One is a staggered start-stop mode, where multiple sets of air inlets in the periodic interference airflow inlet assembly alternately start and stop sequentially within a pulse cycle, and then repeat cyclically. Within one pulse cycle, each set of air inlets starts and stops once. When one set of air inlets starts, the others stop, and when one set stops, another set starts. For example, the periodic interference airflow inlet assembly includes three sets of air inlets: A, B, and C. Set A starts, while sets B and C stop; when set A stops, set B starts, while set C remains stopped; when set B stops, set C starts, while set A remains stopped; when set C stops, one pulse cycle is completed; then, when set C stops, set A starts again, and this cycle repeats. The pulse frequency is 0.2~10Hz, preferably 0.5~5Hz, with a duty cycle of 10%~60%, controlled by a high-speed electromagnetic pulse valve. The staggered start-stop mode is more suitable for medium to large-sized vertical fluidized bed jet mills with large production capacity.

[0053] Another mode of periodic airflow disturbance is the synchronous start-stop mode. Multiple sets of inlet ports in the periodic airflow disturbance inlet assembly start and stop simultaneously, cycling through the process. Within one pulse cycle, all inlet ports start and stop once. For example, if the periodic airflow disturbance inlet assembly includes three sets of inlet ports, A, B, and C, sets A, B, and C start simultaneously, then stop simultaneously, and then start simultaneously again. One pulse cycle is completed precisely at the point when sets A, B, and C start simultaneously again, and this cycle repeats continuously. The pulse frequency is 0.2~10Hz, preferably 0.5~5Hz, with a duty cycle of 10%~60%, controlled by a high-speed electromagnetic pulse valve. The synchronous start-stop mode is more suitable for small-scale vertical fluidized bed jet mills with lower production capacity.

[0054] The periodic disturbance airflow uses the same inert gas as the pulverizing airflow. The pressure of the periodic disturbance airflow is 20% to 90% of the pressure of the pulverizing airflow, and the average flow rate is 2% to 15% of the total flow rate of the pulverizing airflow (the corresponding average flow rate is usually 0.3 to 30 Nm³ / h).

[0055] It should be noted that when there is no periodic turbulent airflow at the bottom of the vertical fluidized bed, the density is as high as approximately 16.69 g / cm³. 3 The tantalum powder particles tend to form a settling dead zone in the lower part of the grinding chamber, making it difficult to fully enter the main anti-spray collision zone, resulting in low grinding efficiency and increased circulating load; moreover, the already ground fine particles are retained in the chamber and repeatedly circulated, which can easily lead to severe over-grinding, resulting in a high proportion of fine powder and a wider particle size distribution.

[0056] In addition, existing tantalum powder airflow pulverization processes mainly adjust the fineness by simply increasing the pressure of the main pulverizing airflow or increasing the speed of the classifier wheel. However, high-pressure and high-speed scouring will drastically increase the wear of the nozzle, classifier wheel blades and the inner wall of the cavity, seriously increase the contamination of metal impurities such as Fe, Cr, and Ni, and exacerbate the oxidation of the new surface of the powder. On the other hand, conventional fluidization methods are very easy to destroy the energy of the main jet focal point, making it difficult to achieve an extremely narrow particle size distribution and efficient and stable production while ensuring high purity and low oxygen increment.

[0057] In step S7, the rotational speed of each classifier is adjusted to compensate for changes in the total system air volume, crushing zone pressure difference, classifier current, classifier torque, or product particle size caused by periodic disturbance airflow, so as to keep the particle size cut by the classifier stable.

[0058] Preferably, when the average flow rate of the periodic disturbance airflow increases, the rotational speed of each stage of the classifying impeller is increased to prevent coarse particles from entering the finished powder with the airflow. Specifically, the increase in the average flow rate of the periodic disturbance airflow and the increase in the rotational speed of each stage of the classifying impeller satisfy a positive dynamic feedforward compensation relationship: the increase in the proportion of the average flow rate of the periodic disturbance airflow to the total flow rate of the main grinding airflow is ΔQ.比 Based on this, the percentage increase in the speed compensation Δn of each stage's impeller relative to its corresponding base speed n0 satisfies the following: for every 1% increase in the average flow rate of the periodic disturbance airflow to the total flow rate of the main crushing airflow, the speed of each stage's impeller increases by 0.5% to 2.5% of its base speed, preferably by 1.0% to 1.8%, and further preferably by 1.2% to 1.6%. The dynamic compensation gain coefficient for the impeller speed is k = (Δn / n0) / (ΔQ / Q). 主 The value of ΔQ should be controlled within the range of 0.5 to 2.5, preferably within the range of 1.0 to 1.8. 比 =ΔQ / Q 主 .

[0059] The fluid dynamics mechanism and synergistic effect of the above-mentioned quantitative matching relationship lie in the following: based on the principle of balance between centrifugal force and centripetal aerodynamic drag force in the gas-solid two-phase flow inside the turbine stager, the staged cutting particle size d c It is positively correlated with the radial airflow velocity (determined by the total air volume passing through the classifier wheel) and negatively correlated with the classifier wheel rotation speed (determining the outer edge tangential velocity and centrifugal force field strength). When the periodic interfering airflow jet at the bottom of the grinding chamber is activated, the instantaneous upward air volume in the grinding zone increases, and the centripetal aerodynamic drag force between the classifier wheel blades increases instantaneously. If the classifier wheel rotation speed compensation ratio is less than 0.5% (insufficient compensation), the centripetal drag force will be significantly greater than the outward centrifugal force, causing a large number of incompletely dissociated high-density coarse particles to directly penetrate the classifier wheel blades and enter the finished product with the instantaneous air surge, resulting in product D. 95 The centrifugal force field is too strong, causing excessive coarse powder to escape from the grinding zone. If the centrifugal speed compensation ratio of the classifier wheel exceeds 2.5% (overcompensation), the excessive centrifugal force field will not only obstruct the smooth discharge of qualified fine powder, but also force it to re-settle and fall back into the grinding zone, resulting in secondary over-grinding and an abnormally high proportion of fine powder (D). 10 Reducing output (due to excessively large specific surface area of ​​the finished product) and decreasing hourly output will cause overload of the grading motor current and exacerbate wear on the grading wheel blades. By precisely locking the compensation ratio within the above range, the gas-solid balance point inside and outside the grading wheel can maintain constant momentum throughout the entire cycle of pulsation disturbance, ensuring dynamic stability of the grading and cutting particle size.

[0060] Preferably, the compensation adjustment amount of the stage wheel is 1% to 15% of the base speed of the stage wheel, that is, the compensation adjustment amount of the first turbine stage wheel is 100 to 1800 rpm, and the compensation adjustment amount of the second and third turbine stage wheels is 112 to 2070 rpm.

[0061] It should be noted that periodic disturbances in the airflow can cause periodic changes in the total air volume, local pressure, and particle conveying status within the pulverizing zone. Without compensation control, this could affect the particle size cut by the turbine classifier, leading to particle size fluctuations or entrainment of coarse particles. Therefore, this invention includes a classifier compensation control step.

[0062] In step S8, the first turbine classifier in the crushing and classifying module transports the pre-finished tantalum powder to the supplementary classification module. The first collection tank of the collection module collects coarse tantalum powder that does not enter the pre-finished tantalum powder under the control of the first and second solenoid valves. The coarse tantalum powder is returned to the crushing zone for further crushing. The pre-finished tantalum powder is classified by the supplementary classifier in the supplementary classification module and collected in the second collection tank or the second and third collection tanks to obtain finished tantalum powder. The classified tantalum dust flows out of the supplementary classification module and enters the cyclone separator of the dust removal unit. After passing through the cyclone separator, tantalum dust is obtained in the dust collection tank. The exhaust gas after dust removal is discharged from the exhaust gas outlet.

[0063] In step S9, the output per unit time is counted, and the D of the finished tantalum powder is detected. 10 D 50 D 90 D 95 The parameters include the Fisher particle size (Fsss), oxygen content, and metal impurity content. Based on the test results, the crushing airflow pressure, feed rate, classifier frequency, periodic interference airflow inlet pressure, flow rate, pulsation frequency, duty cycle, and opening mode are adjusted.

[0064] Control unit with product D 10 D 50 D 90 D 95 Alternatively, the Fisher particle size (Fsss) can be used as a feedback index to perform closed-loop regulation of periodically disturbing airflow parameters and staged impeller speed. Wherein, D... 10 D 50 D 90 D 95 These represent the particle sizes corresponding to cumulative volume distributions of 10%, 50%, 90%, and 95%, respectively; Fsss represents the Fisher particle size. When D 10 If the value is too small, it indicates over-grinding and excessively fine particle size. In this case, the speed of the classifier wheel should be reduced and / or the duty cycle of the periodic interfering airflow should be shortened; when D... 50 When D is too large, it indicates that the overall powder particle size is too coarse and the grinding is insufficient. In this case, the classifier speed should be increased and / or the periodic disturbance gas flow rate should be increased; conversely, when D is too small... 50 If the particle size is too small, it indicates that the overall powder particle size is too fine and the powder has been over-grinded. In this case, the classifier speed should be reduced and / or the feed rate increased. 90 D 95 If the value is too high, it indicates that the finished product contains coarse powder, or that the distribution curve shows a peak / shoulder peak at the coarse end. In this case, the speed of the classifier wheel should be increased and / or the flow rate of the periodic interference air should be reduced. All of the above should be adjusted by about 5%.

[0065] Finally, according to the requirements of tantalum powder for capacitors, the obtained tantalum powder is subjected to acid washing, vacuum heat treatment, deoxidation, secondary acid washing, drying and sieving to obtain high voltage and high specific capacitance tantalum powder products.

[0066] Compared with existing technologies that do not employ periodic interference airflow and staged wheel compensation adjustment, the method of this invention solves the industry pain point of easy deposition and low fluidization of high-density tantalum powder, and has the following technical effects: (1) Improved efficiency and reduced consumption: Compared with undisturbed airflow, the output is increased by about 20%; compared with continuous blowing, the dilution of the pulverizing airflow energy is avoided, and the gas-solid ratio is significantly reduced to 4.11 Nm. 3 / kg.

[0067] (2) Extremely narrow particle size distribution (eliminating coarse particles): Through dynamic feedforward compensation of the grading wheel speed, the disturbance of the grading cutting point by the instantaneous pulsation is eliminated, such as the finished product D 10 The diameter increased from 1.91 μm to 2.25 μm, D 95 The particle size decreased from 5.22μm to 4.89μm, with no coarse particles being removed.

[0068] (3) Ultra-low impurities and low oxidation pollution: There is no need to blindly increase the main gas flow pressure. With the high-purity anti-pollution lining and high-purity inert atmosphere protection, the wear of the cavity and classifier wheel and the oxidation of the powder surface are greatly reduced. The increase of Fe, Cr and Ni impurities in a single crushing does not exceed 3ppm, and the increase of oxygen (ΔO) is less than 500ppm, which meets the requirements of capacitor-grade high-purity tantalum powder.

[0069] Example 1 An airflow pulverization and classification system for tantalum powder is disclosed. The system includes a pulverization and classification unit, a dust removal unit, an induced draft fan, and a control unit. The pulverization and classification unit is used to pulverize and classify tantalum powder, including a main unit, a vertical fluidized bed jet pulverizer, and a supplementary classification module. The dust removal unit is used to recover tantalum dust, including a cyclone separator and a dust collection tank. The induced draft fan provides airflow to the pulverization and classification unit and the dust removal unit. The control unit controls the operation of the pulverization and classification unit, the dust removal unit, and the induced draft fan.

[0070] The vertical fluidized bed jet mill includes a feeding module, a grinding and grading module, and a collection module. The feeding module is used to feed tantalum powder raw materials into the grinding and grading module under the action of inert gas ejection. The feeding module includes a hopper, a feeder, an ejector mixing chamber, and a feeding pipe. The hopper stores the tantalum powder raw materials, and the feeder transports the tantalum powder raw materials from the hopper into the ejector mixing chamber. The ejector mixing chamber has an ejector gas inlet at the top, through which inert gas enters the ejector mixing chamber. Then, the tantalum powder raw materials in the ejector mixing chamber are ejected obliquely downwards into the grinding and grading module through the feeding pipe. The upper end of the feeding pipe connects to the lower part of the ejector mixing chamber, and the lower end of the feeding pipe connects to the upper side of the transmission area of ​​the grinding and grading module. The feeding pipe runs obliquely downwards.

[0071] The main body of the crushing and grading module is a cylindrical cavity structure. Inside the cavity, from bottom to top, it is divided into a powder collection zone, a crushing zone, a conveying zone, and a turbine grading zone. The cylindrical cavity of the crushing and grading module has a contamination-proof lining made of 99.5% high-purity alumina ceramic material to prevent or reduce the introduction of metallic impurities such as Fe, Cr, and Ni. The powder collection zone is located at the bottom of the crushing and grading module and is an inverted cone structure with a full cone angle of 60°, used to collect deposited tantalum powder during the crushing and grading process. The crushing zone is above the powder collection zone and is a cylindrical structure with an inner diameter D1 of 200 mm and a height H1 of 300 mm (1.5D1). Four (two pairs) of opposing Laval nozzles are distributed on the same horizontal cavity circumference at a height of 150 mm (0.50H1) from the bottom of the crushing zone. Two opposing Laval nozzles on the same diameter of the cylindrical cavity are called a pair of opposing Laval nozzles. The throat diameter d of a single nozzle... t The thickness is 1.8 mm, and the designed Mach number is 2.2; the ratio of the total throat cross-sectional area of ​​the two pairs of nozzles to the cross-sectional area of ​​the crushing zone is maintained at 0.000324. Several pairs of opposing-jet Laval nozzles are mainly used to crush tantalum powder particles by inter-particle collision through multiple high-speed opposing jets. Below the plane of the opposing Laval nozzle and at a height of 45 mm (0.15H1) above the bottom surface of the pulverizing zone, periodic interfering airflow intake components are distributed on the circumference of the same horizontal cavity. Each intake component includes four (two groups) air inlets. Two opposing air inlets on the same diameter of the cylindrical cavity are referred to as one group. The two groups of air inlets are evenly distributed on the circumference of the cavity, with a central angle of 90° formed by two adjacent air inlets. All air inlets are inclined upwards, with an axial angle β of 45° between the air inlet and the horizontal plane. The deflection angle α formed by the intersection of the air inlet's axial projection on the bottom surface of the pulverizing zone and the axial section of the pulverizing zone on the circumference of the pulverizing zone is consistent, clockwise, and 15°. The transmission zone is above the pulverizing zone and has a frustum-shaped structure, smaller at the top and larger at the bottom. The inner diameter D at the lower end of the transmission zone... 2a The inner diameter D at the upper end of the transmission area is 200mm (1.0D1).2b The diameter D3 is 120mm (0.60D1), and the height H2 is 180mm (0.9D1). The turbine classification zone is above the transmission zone. The turbine classification zone has a cylindrical structure with an inner diameter D3 of 130mm (0.65D1) and a height H3 of 150mm (0.75D1). A first turbine classifier is installed in the central axial region of the turbine classification zone. The radial direction of the first turbine classifier is consistent with the radial direction of the turbine classification zone, and the axial direction of the first turbine classifier is consistent with the axial direction of the turbine classification zone. The diameter D of the first turbine classifier is... c The height H of the first turbine stage wheel is 100.1 mm (0.77D3). c 30mm (0.30D) c A first motor for driving the first turbine stage wheel is installed above the top surface of the turbine stage zone along the axial direction.

[0072] The collection module is used to collect coarse powder after air jet milling. It includes a first collection tank and solenoid valves. The first collection tank is located directly below the milling and grading module and is connected to the powder collection area of ​​the milling and grading module via a pipeline controlled by the solenoid valves. There are two solenoid valves, one lower and one higher. The lower solenoid valve, closer to the collection tank, controls the connection or closure between the milling area and the collection tank. The upper solenoid valve, closer to the first powder collection area, controls the backflushing airflow during powder discharge, making it easier for the tantalum powder to descend. Both solenoid valves are closed during the operation of the air jet mill; they only open when discharging powder after the air jet milling process.

[0073] The supplementary classification module includes a first supplementary classifier and a second collection tank. The first supplementary classifier has a cylindrical cavity structure, and its inner diameter is equal to the inner diameter of the turbine classification zone of the pulverizing and classification module. A second turbine classification wheel is installed in the upper axial region of the cylindrical cavity. The radial direction of the second turbine classification wheel is consistent with the radial direction of the cylindrical cavity, and its axial direction is consistent with the axial direction of the cylindrical cavity. The diameter and height of the second turbine classification wheel are equal to those of the first turbine classification wheel. A second motor for driving the second turbine classification wheel is installed above the top surface of the cylindrical cavity in the axial direction. The side wall of the cylindrical cavity corresponding to the second turbine classification wheel is connected to the outlet of the turbine classification zone to perform a second classification on the tantalum powder flowing from the first turbine classification wheel, thereby optimizing the classification effect. The axial height of the cylindrical cavity of the first supplementary classifier is equal to that of the cylindrical cavity structure of the pulverizing and classification module. The lower part of the cylindrical cavity is an inverted conical structure used to collect the deposited tantalum powder during the classification process. The second collection tank is located directly below the cylindrical cavity and is connected to or closed to the inverted conical structure at the bottom of the cylindrical cavity. The tantalum powder finished product after being classified by the second turbine classifier finally enters the second collection tank.

[0074] Tantalum powder flowing from the supplementary grading module enters the cyclone separator of the dust removal unit. If the supplementary grading module only includes a first supplementary classifier and a second collection tank, the tantalum powder flowing from the first supplementary classifier enters the cyclone separator of the dust removal unit. If the supplementary grading module only includes a first supplementary classifier, a second collection tank, a second supplementary classifier, and a third collection tank, the tantalum powder flowing from the second supplementary classifier enters the cyclone separator of the dust removal unit. The dust collection chamber and dust collection tank at the bottom of the cyclone separator are connected to collect tantalum dust, while the exhaust gas after dust removal is discharged from the exhaust gas outlet.

[0075] The induced draft fan is used to provide airflow to the crushing and grading unit and the dust removal unit; the control unit is used to control the operation of the crushing and grading unit, the dust removal unit and the induced draft fan.

[0076] A method for preparing tantalum powder using the above-mentioned airflow pulverization and classification system includes the following steps: Step S1: Pretreatment of tantalum powder raw materials; Step S2: Equipment inertization; Step S3: Start the pulverizing airflow; Step S4: Activate the first turbine classifier in the crushing and classifying module, and the second turbine classifier in the supplementary classifying module; Step S5: Feeding and crushing; Step S6: Apply periodic disruptive airflow; Step S7: Grade wheel compensation adjustment; Step S8: Tantalum powder classification and collection; Step S9: Detection and closed-loop adjustment.

[0077] Specifically, in step S1, the tantalum powder raw material is pretreated, including sieving, drying, and impurity removal, to meet the requirements of airflow pulverization. All tantalum powder raw materials pass through a 0.175mm sieve (80 mesh), and the moisture content is 200ppm (0.02%).

[0078] In step S2, all equipment in the nitrogen replacement system's crushing and grading unit and dust removal unit, including the hopper, feeder, ejector mixing chamber, and feed pipe in the feeding module; the chamber and collection tank in the crushing and grading module; the supplementary grading machine chamber and collection tank in the supplementary grading module; the cyclone separator and dust collection tank in the dust removal unit; and the connecting pipes between the units, are used to bring the equipment to a low-oxygen, low-moisture state. After replacement, the oxygen and moisture content in the system meets the requirements for preparing tantalum powder for capacitors. The O2 content in the system after replacement is 100 ppm (i.e., 0.01%), and the dew point is -50°C. o C.

[0079] In step S3, the pulverizing gas flow is initiated, causing the inert gas to form a high-speed jet through a counter-jet Laval nozzle. The inert gas used is nitrogen. The absolute pressure of the pulverizing gas flow is 5 MPa.

[0080] In step S4, the initial classifying wheel frequency of each turbine classifying wheel is set so that the classifying and cutting particle size matches the target product particle size. The basic rotational speed of the first turbine classifying wheel is 6500 rpm, and the outer edge linear velocity of the classifying wheel blades is controlled at 34 m / s. The basic rotational speed of the second turbine classifying wheel in the supplementary classification module is 7400 rpm, and the outer edge linear velocity of the classifying wheel blades is 38.7 m / s.

[0081] In step S5, the pretreated tantalum powder raw material is continuously or intermittently fed into the crushing and grading unit through the feeding module, so that the tantalum powder particles are crushed by inter-particle collision, shearing and friction under the action of high-speed jet flow in the crushing zone.

[0082] Specifically, tantalum powder raw materials are stored in a silo. The feeder transports the tantalum powder raw materials from the silo into the ejector mixing chamber. Inert gas enters the ejector mixing chamber through the ejector gas inlet. The inert gas used is the same gas as the pulverizing gas flow. Then, the tantalum powder raw materials in the ejector mixing chamber are injected obliquely downwards into the pulverizing and classifying module through the feed pipe. The pressure of the inert gas is 0.30 MPa, and the gas-solid ratio is 0.20 Nm³ / kg, that is, 0.20 Nm³ of gas is consumed for every kilogram of tantalum powder transported.

[0083] During the crushing process, the material holding capacity per unit cross-sectional area of ​​the crushing zone is controlled at 47.8 kg / m². 2 The bed holding capacity is 1.5 kg, which accounts for 12% of the effective volume of the crushing zone; the apparent cross-sectional gas velocity (i.e., the gas velocity per unit cross-sectional area of ​​the crushing zone) is 0.21 m / s; and the gas-solid ratio is 4.11 Nm. 3 / kg, meaning that 4.11 Nm³ of gas is consumed per kilogram of tantalum powder. 3 .

[0084] In step S6, nitrogen is used for the periodic disturbance airflow. The periodic disturbance airflow is started and periodically enters the crushing zone from the lower side wall of the crushing zone, disturbing the tantalum powder particles deposited at the bottom of the crushing zone. This causes the deposited tantalum powder to periodically loosen, rise and redisperse, and then re-enter the high-speed jet crushing zone to participate in collision crushing.

[0085] Specifically, the periodic interference airflow operates in a synchronized start-stop mode, with both sets of inlet ports of the periodic interference airflow inlet assembly starting and stopping simultaneously in a cycle. Within one pulse cycle, all inlet ports start and stop once. The pulse frequency is 2Hz, with a duty cycle of 35%, controlled by a high-speed electromagnetic pulse valve. The periodic interference airflow pressure is 50% of the pulverizing airflow pressure (i.e., 2.5MPa), and the average flow rate is 2.9% of the total pulverizing airflow flow rate. The pulsed average increase in flow rate is 0.63 Nm³ / h, and the total system air volume is 23.43 Nm³ / h (corresponding to an apparent cross-sectional air velocity of 0.21 m / s in the pulverizing zone).

[0086] In step S7, at the instant the periodic disturbance airflow pulsation is activated, the control system (PLC) synchronously applies dynamic upward compensation of +250rpm and +285rpm (upward compensation of 3.85%) to the first turbine stager inverter and the second turbine stager inverter, respectively; during the pulsation shutdown interval, the pulsation speeds are restored to 6500rpm and 7400rpm, respectively.

[0087] In step S8, the first turbine classifier in the crushing and classifying module transports the pre-finished tantalum powder to the supplementary classification module. The first collection tank of the collection module collects coarse tantalum powder that does not enter the pre-finished tantalum powder under the control of the first and second solenoid valves. The coarse tantalum powder is returned to the crushing zone for further crushing. The pre-finished tantalum powder is classified by the supplementary classifier in the supplementary classification module and collected in the second collection tank or the second and third collection tanks to obtain finished tantalum powder. The classified tantalum dust flows out of the supplementary classification module and enters the cyclone separator of the dust removal unit. After passing through the cyclone separator, tantalum dust is obtained in the dust collection tank. The exhaust gas after dust removal is discharged from the exhaust gas outlet.

[0088] In step S9, the D of the finished tantalum powder is detected. 10 D 50 D 90 D 95 The parameters include Fisher particle size (Fsss), oxygen content, and metallic impurity content. The finished tantalum powder test data are: D 10 =2.253μm, D 50 =3.561μm, D 95 =4.892μm, Fisher particle size Fsss is 1.85μm; Fe increment is 3ppm, Cr increment is 3ppm, Ni increment is 3ppm, and the total O content of the finished tantalum powder is 2200ppm. Among them, the oxygen increment ΔO during the crushing process is only 250ppm compared with the raw material tantalum powder (initial oxygen content is 1950ppm); the unit time output is 5.7kg / h. The process parameters and test data of this embodiment are shown in Table 1.

[0089] Finally, according to the requirements of tantalum powder for capacitors, the obtained tantalum powder is subjected to acid washing, vacuum heat treatment, deoxidation, secondary acid washing, drying and sieving to obtain high voltage and high specific capacitance tantalum powder products.

[0090] Example 2 An airflow pulverization and classification system for tantalum powder is disclosed. The system includes a pulverization and classification unit, a dust removal unit, an induced draft fan, and a control unit. The pulverization and classification unit is used to pulverize and classify tantalum powder, including a main unit, a vertical fluidized bed jet pulverizer, and a supplementary classification module. The dust removal unit is used to recover tantalum dust, including a cyclone separator and a dust collection tank. The induced draft fan provides airflow to the pulverization and classification unit and the dust removal unit. The control unit controls the operation of the pulverization and classification unit, the dust removal unit, and the induced draft fan.

[0091] The vertical fluidized bed jet mill includes a feeding module, a grinding and grading module, and a collection module. The feeding module is used to feed tantalum powder raw materials into the grinding and grading module under the action of inert gas ejection. The feeding module includes a hopper, a feeder, an ejector mixing chamber, and a feeding pipe. The hopper stores the tantalum powder raw materials, and the feeder transports the tantalum powder raw materials from the hopper into the ejector mixing chamber. The ejector mixing chamber has an ejector gas inlet at the top, through which inert gas enters the ejector mixing chamber. Then, the tantalum powder raw materials in the ejector mixing chamber are ejected obliquely downwards into the grinding and grading module through the feeding pipe. The upper end of the feeding pipe connects to the lower part of the ejector mixing chamber, and the lower end of the feeding pipe connects to the upper side of the transmission area of ​​the grinding and grading module. The feeding pipe runs obliquely downwards.

[0092] The main body of the crushing and grading module is a cylindrical cavity structure. Inside the cavity, from bottom to top, it is divided into a powder collection zone, a crushing zone, a conveying zone, and a turbine grading zone. The cylindrical cavity of the crushing and grading module has a contamination-proof lining made of 99.5% high-purity alumina ceramic material to prevent or reduce the introduction of metallic impurities such as Fe, Cr, and Ni. The powder collection zone is located at the bottom of the crushing and grading module and is an inverted cone structure with a full cone angle of 60°, used to collect deposited tantalum powder during the crushing and grading process. The crushing zone is above the powder collection zone and is a cylindrical structure with an inner diameter D1 of 500 mm and a height H1 of 750 mm (1.5D1). Six (3 pairs) of opposing Laval nozzles are distributed on the same horizontal cavity circumference at a height of 375 mm (0.50H1) from the bottom of the crushing zone. Two opposing Laval nozzles on the same diameter of the cylindrical cavity are called a pair of opposing Laval nozzles. The throat diameter d of a single nozzle... tThe diameter is 4.5 mm, and the designed Mach number is 2.2. The ratio of the total throat cross-sectional area of ​​the three pairs of nozzles to the cross-sectional area of ​​the crushing zone is maintained at 0.000486. Several pairs of opposing-jet Laval nozzles are mainly used to crush tantalum powder particles by inter-particle collision through multiple high-speed opposing jets. Below the plane of the opposing Laval nozzle and at a height of 112.5 mm (0.15H1) above the bottom surface of the pulverizing zone, periodic interfering airflow intake components are distributed on the circumference of the same horizontal cavity. The intake components include 6 (3 groups) intake ports. Two opposing intake ports on the same diameter of the cylindrical cavity are referred to as one group of intake ports. The three groups of intake ports are evenly distributed on the circumference of the cavity, with a central angle of 60° formed by two adjacent intake ports. The intake ports are all inclined upwards, with an axial angle β of 45° between the intake port and the horizontal plane. The deflection angle α formed by the intersection of the axial projection of the intake port on the bottom surface of the pulverizing zone and the axial section of the pulverizing zone on the circumference of the pulverizing zone is consistent, all clockwise, and the deflection angle α is 15°. The transmission zone is above the pulverizing zone and has a frustum-shaped structure that is smaller at the top and larger at the bottom. The inner diameter D at the lower end of the transmission zone is... 2a The inner diameter D at the upper end of the transmission area is 500mm (1.0D1). 2b The diameter D3 is 300mm (0.60D1), and the height H2 is 375mm (0.75D1). The turbine classification zone is above the transmission zone. The turbine classification zone has a cylindrical structure with an inner diameter D3 of 325mm (0.65D1) and a height H3 of 195mm (0.39D1). A first turbine classifier is installed in the central axial region of the turbine classification zone. The radial direction of the first turbine classifier is consistent with the radial direction of the turbine classification zone, and the axial direction of the first turbine classifier is consistent with the axial direction of the turbine classification zone. The diameter D of the first turbine classifier is... c The height H of the first turbine stage wheel is 250.25mm (0.77D3). c It is 75.08mm (i.e., 0.30D). c A first motor for driving the first turbine stage wheel is installed above the top surface of the turbine stage zone along the axial direction.

[0093] The collection module is used to collect coarse powder after air jet milling. It includes a first collection tank and solenoid valves. The first collection tank is located directly below the milling and grading module and is connected to the powder collection area of ​​the milling and grading module via a pipeline controlled by the solenoid valves. There are two solenoid valves, one lower and one higher. The lower solenoid valve, closer to the collection tank, controls the connection or closure between the milling area and the collection tank. The upper solenoid valve, closer to the first powder collection area, controls the backflushing airflow during powder discharge, making it easier for the tantalum powder to descend. Both solenoid valves are closed during the operation of the air jet mill; they only open when discharging powder after the air jet milling process.

[0094] The supplementary classification module includes a first supplementary classifier and a second collection tank. The first supplementary classifier has a cylindrical cavity structure, and its inner diameter is equal to the inner diameter of the turbine classification zone of the pulverizing and classification module. A second turbine classification wheel is installed in the upper axial region of the cylindrical cavity. The radial direction of the second turbine classification wheel is consistent with the radial direction of the cylindrical cavity, and its axial direction is consistent with the axial direction of the cylindrical cavity. The diameter and height of the second turbine classification wheel are equal to those of the first turbine classification wheel. A second motor for driving the second turbine classification wheel is installed above the top surface of the cylindrical cavity in the axial direction. The side wall of the cylindrical cavity corresponding to the second turbine classification wheel is connected to the outlet of the turbine classification zone to perform a second classification on the tantalum powder flowing from the first turbine classification wheel, thereby optimizing the classification effect. The axial height of the cylindrical cavity of the first supplementary classifier is equal to that of the cylindrical cavity structure of the pulverizing and classification module. The lower part of the cylindrical cavity is an inverted conical structure used to collect the deposited tantalum powder during the classification process. The second collection tank is located directly below the cylindrical cavity and is connected to or closed to the inverted conical structure at the bottom of the cylindrical cavity. The tantalum powder finished product after being classified by the second turbine classifier finally enters the second collection tank.

[0095] Tantalum powder flowing from the supplementary grading module enters the cyclone separator of the dust removal unit. If the supplementary grading module only includes a first supplementary classifier and a second collection tank, the tantalum powder flowing from the first supplementary classifier enters the cyclone separator of the dust removal unit. If the supplementary grading module only includes a first supplementary classifier, a second collection tank, a second supplementary classifier, and a third collection tank, the tantalum powder flowing from the second supplementary classifier enters the cyclone separator of the dust removal unit. The dust collection chamber and dust collection tank at the bottom of the cyclone separator are connected to collect tantalum dust, while the exhaust gas after dust removal is discharged from the exhaust gas outlet.

[0096] The induced draft fan is used to provide airflow to the crushing and grading unit and the dust removal unit; the control unit is used to control the operation of the crushing and grading unit, the dust removal unit and the induced draft fan.

[0097] A method for preparing tantalum powder using the above-mentioned airflow pulverization and classification system includes the following steps: Step S1: Pretreatment of tantalum powder raw materials; Step S2: Equipment inertization; Step S3: Start the pulverizing airflow; Step S4: Activate the first turbine classifier in the crushing and classifying module, and the second turbine classifier in the supplementary classifying module; Step S5: Feeding and crushing; Step S6: Apply periodic disruptive airflow; Step S7: Grade wheel compensation adjustment; Step S8: Tantalum powder classification and collection; Step S9: Detection and closed-loop adjustment.

[0098] Specifically, in step S1, the tantalum powder raw material is pretreated, including sieving, drying, and impurity removal, to meet the requirements of airflow milling. All the tantalum powder raw material passes through a 0.175mm sieve (80 mesh), and the moisture content is 0.02% (i.e., 200ppm). In step S2, all equipment in the nitrogen replacement system's crushing and grading unit and dust removal unit, including the hopper, feeder, ejector mixing chamber, and feed pipe in the feeding module; the chamber and collection tank in the crushing and grading module; the supplementary grading machine chamber and collection tank in the supplementary grading module; the cyclone separator and dust collection tank in the dust removal unit; and the connecting pipes between the units, are used to bring the equipment to a low-oxygen, low-moisture state. After replacement, the oxygen and moisture content in the system meets the requirements for preparing tantalum powder for capacitors. The O2 content in the system after replacement is 100 ppm (i.e., 0.01%), and the dew point is -50°C. o C.

[0099] In step S3, the pulverizing gas flow is initiated, causing the inert gas to form a high-speed jet through a counter-jet Laval nozzle. The inert gas used is nitrogen. The absolute pressure of the pulverizing gas flow is 5 MPa.

[0100] In step S4, the initial classifying wheel frequency of each turbine classifying wheel is set so that the classifying and cutting particle size matches the target product particle size. The basic rotational speed of the first turbine classifying wheel is 2600 rpm, and the outer edge linear velocity of the classifying wheel blades is 34 m / s. The basic rotational speed of the second and third turbine classifying wheels in the supplementary classification module is 2960 rpm (1.138 times the basic rotational speed of the first turbine classifying wheel), and the outer edge linear velocity of the classifying wheel blades is 38.7 m / s (1.138 times the outer edge linear velocity of the first turbine classifying wheel blades).

[0101] In step S5, the pretreated tantalum powder raw material is continuously or intermittently fed into the crushing and grading unit through the feeding module, so that the tantalum powder particles are crushed by inter-particle collision, shearing and friction under the action of high-speed jet flow in the crushing zone.

[0102] Specifically, tantalum powder raw materials are stored in a silo. The feeder transports the tantalum powder raw materials from the silo into the ejector mixing chamber. Inert gas enters the ejector mixing chamber through the ejector gas inlet. The inert gas used is the same gas as the pulverizing gas flow. Then, the tantalum powder raw materials in the ejector mixing chamber are injected obliquely downwards into the pulverizing and classifying module through the feed pipe. The pressure of the inert gas is 0.30 MPa, and the gas-solid ratio of the ejector feed is 0.20 Nm³ / kg, that is, 0.20 Nm³ of gas is consumed per kilogram of tantalum powder.

[0103] During the crushing process, the material holding capacity per unit cross-sectional area of ​​the crushing zone is 47.7 kg / m², which means the absolute material holding capacity of the bed is 9.37 kg, accounting for 12% of the effective volume of the crushing zone; the apparent cross-sectional gas velocity (i.e., the gas velocity of the airflow passing through the unit cross-sectional area of ​​the crushing zone) in the crushing zone is 0.21 m / s; the gas-solid ratio of the system is 4.11 Nm³ / kg, which means that 4.11 Nm³ of gas is consumed per kilogram of finished tantalum powder.

[0104] In step S6, nitrogen is used for the periodic disturbance airflow. The periodic disturbance airflow is started and periodically enters the crushing zone from the lower side wall of the crushing zone, disturbing the tantalum powder particles deposited at the bottom of the crushing zone. This causes the deposited tantalum powder to periodically loosen, rise and redisperse, and then re-enter the high-speed jet crushing zone to participate in collision crushing.

[0105] Specifically, the periodic interference airflow operates in a staggered start-stop mode. The three sets of inlet ports of the periodic interference airflow inlet assembly alternately start and stop sequentially within one pulse cycle, then repeat cyclically. Within one pulse cycle, each set of inlet ports starts and stops once; when one set of inlet ports starts, the others stop, and when one set stops, another set starts. The pulse frequency is 1.5Hz, the duty cycle is 33.3%, and it is controlled by a high-speed electromagnetic pulse valve. The periodic interference airflow pressure is 50% of the pulverizing airflow pressure (i.e., 2.5MPa), and the average flow rate is 2.9% of the total pulverizing airflow flow rate. The pulsed average increase in flow rate is 3.93 Nm³ / h, and the total system air volume is 146.4 Nm³ / h (corresponding to an apparent cross-sectional air velocity of 0.21 m / s in the pulverizing zone).

[0106] In step S7, at the instant the periodic disturbance airflow pulsation is activated, the control system (PLC) synchronously applies dynamic upward compensation of +120rpm and +137rpm (upward compensation of 4.62%) to the first turbine stager inverter and the second turbine stager inverter, respectively; during the pulsation shutdown interval, the pulsation speed is restored to 2600rpm and 2960rpm, respectively.

[0107] In step S8, the first turbine classifier in the crushing and classifying module transports the pre-finished tantalum powder to the supplementary classification module. The first collection tank of the collection module collects coarse tantalum powder that does not enter the pre-finished tantalum powder under the control of the first and second solenoid valves. The coarse tantalum powder is returned to the crushing zone for further crushing. The pre-finished tantalum powder is classified by the supplementary classifier in the supplementary classification module and collected in the second collection tank or the second and third collection tanks to obtain finished tantalum powder. The classified tantalum dust flows out of the supplementary classification module and enters the cyclone separator of the dust removal unit. After passing through the cyclone separator, tantalum dust is obtained in the dust collection tank. The exhaust gas after dust removal is discharged from the exhaust gas outlet.

[0108] In step S9, the D of the finished tantalum powder is detected. 10D 50 D 90 D 95 The test data for the finished tantalum powder, including the Fisher particle size (Fsss), oxygen content, and metal impurity content, are as follows: D 10 =2.221μm, D 50 =3.520μm, D 95 =4.860μm, Fisher particle size (Fsss) is 1.82μm; Fe increment is 3ppm, Cr increment is 3ppm, Ni increment is 3ppm, and the total O content of the finished product is 2213ppm (of which, compared with the initial oxygen content of 1950ppm raw material, the oxygen increment ΔO during the crushing process is 263ppm), and the output per unit time is 35.6kg / h. The process parameters and test data of this embodiment are shown in Table 1.

[0109] Finally, according to the requirements of tantalum powder for capacitors, the obtained tantalum powder is subjected to acid washing, vacuum heat treatment, deoxidation, secondary acid washing, drying and sieving to obtain high voltage and high specific capacitance tantalum powder products.

[0110] Comparative Example 1 The airflow pulverizing and classifying system in this comparative example is exactly the same as that in Example 1.

[0111] The tantalum powder preparation method in this comparative example differs from that in Example 1 in that it does not employ the periodic interfering airflow and the staged impeller compensation adjustment mechanism; that is, steps S6 and S7 are omitted. The rest are identical. The total system gas volume is 22.8 Nm³. 3 / h, operating gas-solid ratio is 4.80 Nm 3 / kg.

[0112] The finished tantalum powder test data is: D 10 =1.914μm, D 50 =3.473μm, D 95 =5.221μm, Fisher particle size (Fsss) is 1.45μm; Fe increment is 7ppm, Cr increment is 4ppm, Ni increment is 3ppm, O content is 2800ppm (of which, compared with the initial oxygen content of 1950ppm, the oxygen increment ΔO during the crushing process is 850ppm), and the yield per unit time is 4.75kg / h. The process parameters and test data of this comparative example are shown in Table 1.

[0113] Comparative Example 2 The airflow pulverizing and classifying system in this comparative example is exactly the same as that in Example 1.

[0114] The tantalum powder preparation method in this comparative example differs from that in Example 1 in that the bottom interfering airflow is 100% continuously on, i.e., the duty cycle is 100%, the pulsation frequency is 0Hz, and no staged wheel compensation adjustment mechanism is applied; otherwise, they are identical. Because the bottom interfering airflow is 100% continuously on, the air volume is increased but the collision efficiency is not significantly improved; the total system air volume is 24.6 Nm³. 3 / h, operating gas-solid ratio is 4.75Nm 3 / kg.

[0115] The finished tantalum powder test data is: D 10 =2.043μm, D 50 =3.492μm, D 95 =5.192μm, Fisher particle size (Fsss) is 1.62μm; Fe increment is 5ppm, Cr increment is 4ppm, Ni increment is 3ppm, O content is 2470ppm (of which, compared with the initial oxygen content of 1950ppm raw material, the oxygen increment ΔO during the crushing process is 520ppm), and the yield per unit time is 5.18kg / h. The process parameters and test data of this comparative example are shown in Table 1.

[0116] Table 1. Process parameters and test data for the examples and comparative examples.

[0117] As shown in Table 1, Example 1 and Comparative Examples 1 and 2 used the same system equipment and basic process conditions. Comparative Example 1 did not apply periodic interfering airflow or staged impeller compensation adjustment, Comparative Example 2 applied interfering airflow with a duty cycle of 100% and did not apply staged impeller compensation adjustment, while Example 1 applied periodic interfering airflow with a duty cycle of 35% and synchronous start-stop and staged impeller compensation adjustment. The unit time output of Example 1 was 5.7 kg / h, which was 20% higher than that of Comparative Example 1 (4.75 kg / h) and 10% higher than that of Comparative Example 2 (5.18 kg / h). The gas-solid ratio of Example 1 was 4.11 Nm³. 3 / kg, compared to 4.80 Nm in Comparative Example 1. 3 / kg decreased by 14.4%, compared to 4.75 Nm in Comparative Example 2. 3 / kg decreased by 13.5%; indicating that periodic interference airflow can improve pulverization efficiency while reducing the amount of pulverizing airflow. In Comparative Example 1, without periodic interference airflow, high-density tantalum powder was deposited at the bottom of the pulverization chamber, resulting in low pulverization efficiency. In Comparative Example 2, the application of continuous interference airflow slightly improved the bottom deposition, but it also diluted the collision energy of the pulverizing airflow and easily caused undispersed coarse particles to be blown up and entrained. Although it had an effect, the effect was limited.

[0118] Particle size analysis of the finished tantalum powder showed that the average particle size of Example 1 was 1.85 μm, D 102.25μm, D 50 3.56μm, D 95 The average particle size was 4.89 μm; while the average particle size of Comparative Example 1 was 1.45 μm, D 10 1.91μm, D 50 3.47μm, D 95 The average particle size was 5.22 μm; the average particle size of Comparative Example 2 was 1.62 μm, D 10 2.04μm, D 50 3.49μm, D 95 The value is 5.19 μm; this indicates that the adoption of a dynamic feedforward compensation adjustment mechanism for the grading wheel can eliminate the disturbance of the grading cutting point caused by the instantaneous pulsation, thereby improving the average particle size and making the particle size distribution more concentrated, thus eliminating coarse particles.

[0119] Oxygen and metal impurity content tests showed that the increase in Fe, Cr, and Ni impurities in Example 1 was 3 ppm, and the increase in oxygen ΔO was 250 ppm. The increases in Fe, Cr, Ni, and O impurities in Comparative Example 1 were 7 ppm, 4 ppm, 3 ppm, and 850 ppm, respectively, and the increases in Fe, Cr, Ni, and O impurities in Comparative Example 2 were 5 ppm, 4 ppm, 3 ppm, and 520 ppm, respectively. It is evident that the increase in Fe, Cr, and O impurities in Example 1 during the pulverization process was superior to that in Comparative Example 1 and Comparative Example 2, especially in terms of oxygen increase. This indicates that when there is no turbulent airflow, the tantalum powder accumulated at the bottom is subjected to continuous high-frequency friction from the high-speed rotating airflow and intense shear force above, generating a local micro-regional thermal effect. Meanwhile, the already pulverized fine powder undergoes excessive pulverization due to repeated cyclic friction in the bottom region, continuously exposing newly formed dangling crystal faces with extremely high energy. Under the dual action of heat and a large number of newly formed active crystal faces, intense local thermal oxidation is formed, leading to an increase in oxygen content.

[0120] Example 2, using the same basic process parameters as Example 1, scaled up the equipment and employed a periodic interfering airflow with staggered start-stop to suit medium-sized and larger vertical fluidized bed jet milling with larger production capacity. Operational results showed that the milling efficiency, particle size, oxygen content, and metal impurity content of the finished tantalum powder were the same as or similar to those of Example 1, with a yield of 35.60 kg / h, achieving high-efficiency, narrow-distribution, and high-purity preparation under industrial scale-up conditions.

[0121] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.

Claims

1. An airflow milling and classification system suitable for tantalum powder, characterized in that, The system includes a crushing and grading unit, a dust removal unit, an induced draft fan, and a control unit; The pulverizing and classifying unit is used to pulverize and classify tantalum powder, including a vertical fluidized bed jet mill and a supplementary classification module. The dust removal unit is used to recover tantalum dust and includes a cyclone separator and a dust collection tank; the induced draft fan is used to provide airflow to the crushing and grading unit and the dust removal unit; the control unit is used to control the operation of the crushing and grading unit, the dust removal unit and the induced draft fan; The vertical fluidized bed jet mill includes a feeding module, a grinding and grading module, and a collection module. The feeding module feeds tantalum powder raw materials into the grinding and grading module under the action of inert gas. The main body of the grinding and grading module is a cylindrical cavity structure, and the cylindrical cavity is lined with high-purity alumina or silicon carbide all-ceramic material. The grinding and grading module is used to grind the incoming tantalum powder and transport the pre-finished tantalum powder to the supplementary grading module. The collection module is used to collect coarse powder that exceeds the particle size of the pre-finished tantalum powder. The supplementary grading module includes a supplementary grading machine and a finished product collection tank. The supplementary grading machine is used to further grade the pre-finished tantalum powder into finished tantalum powder and tantalum dust. The finished product collection tank is used to collect the finished tantalum powder and the tantalum dust enters the dust removal unit. Tantalum dust flowing out from the supplementary grading module enters the cyclone separator of the dust removal unit. The dust collection tank is used to collect tantalum dust, and the exhaust gas after dust removal is discharged from the exhaust gas outlet of the cyclone separator.

2. The system according to claim 1, characterized in that, The pulverizing and classifying module is divided into a powder collection zone, a pulverizing zone, a transmission zone, and a turbine classification zone from bottom to top inside the cavity; several pairs of opposing-spray Laval nozzles are distributed on the same horizontal cavity circumference at the middle position of the axial direction of the pulverizing zone; and periodic interference airflow intake components are distributed on the same horizontal cavity circumference below the plane of the opposing-spray Laval nozzles.

3. The system according to claim 2, characterized in that, The inner diameter D1 of the pulverizing zone is 200~500mm, and the height H1 is 0.8D1~2.5D1; the opposing spray-type Laval nozzles are on the same horizontal cavity circumference at a height of 0.25H1~0.75H1 from the bottom surface of the pulverizing zone; the periodic interference airflow inlet assembly is on the same horizontal cavity circumference at a height of 0.02H1~0.35H1 from the bottom surface of the pulverizing zone.

4. The system according to claim 2, characterized in that, The ratio of the total throat cross-sectional area of ​​the plurality of pairs of opposing spray Laval nozzles to the cross-sectional area of ​​the pulverizing zone is 0.0003 to 0.0008; the air intake assembly includes multiple sets of air intake ports, which are evenly distributed at intervals on the circumference of the cavity. The direction of the air intake ports is inclined upward, and the angle β between the axial direction of the air intake ports and the horizontal plane is 15° to 75°. The deflection angle α formed by the projection of the axial direction of the air intake ports onto the bottom surface of the pulverizing zone and the axial section of the pulverizing zone intersecting on the circumference of the pulverizing zone is 5° to 45°, and the deflection direction is consistent.

5. The system according to claim 2, characterized in that, The turbine grading zone is a cylindrical or near-cylindrical structure, and a first turbine grading wheel is installed in the central region along the axial direction of the turbine grading zone.

6. The system according to claim 1, characterized in that, The supplementary grading module includes a first supplementary grading machine and a second collection tank, or a first supplementary grading machine and a second collection tank, a second supplementary grading machine and a third collection tank.

7. A method for preparing tantalum powder using the system described in any one of claims 1 to 6, characterized in that, The method includes the following steps: Step S1: Pretreatment of tantalum powder raw materials; Step S2: Equipment inertization; Step S3: Start the pulverizing airflow; Step S4: Activate the first turbine classifier in the crushing and classifying module, and the second turbine classifier or the second turbine classifier and the third turbine classifier in the supplementary classifying module; Step S5: Feeding and crushing; Step S6: Apply periodic disruptive airflow; Step S7: Grade wheel compensation adjustment; Step S8: Tantalum powder classification and collection; Step S9: Detection and closed-loop adjustment.

8. The method according to claim 7, characterized in that, In step S3, the absolute pressure of the pulverizing airflow is 0.6~12MPa; and / or, in step S4, the basic rotational speed of the first turbine classifier is 1000~12000rpm, and the outer edge linear velocity of the first turbine classifier blade is 25~90m / s; the basic rotational speed of the second turbine classifier or the second turbine classifier and the third turbine classifier is 1.12~1.15 times the basic rotational speed of the first turbine classifier, and the outer edge linear velocity of the blade of the second turbine classifier or the second turbine classifier and the third turbine classifier is 1.12~1.15 times the outer edge linear velocity of the blade of the first turbine classifier.

9. The method according to claim 7, characterized in that, In step S5, the material holding capacity per unit cross-sectional area of ​​the crushing zone is 40~300 kg / m². 2 Within this range, the material holding capacity accounts for 10% to 30% of the effective volume of the crushing zone, the apparent cross-sectional air velocity within the crushing zone is in the range of 0.15 to 0.60 m / s, the total system air volume is 15 to 200 Nm³ / h, and the gas-solid ratio is 1.5 to 8.0 Nm³ / h. 3 / kg.

10. The method according to claim 7, characterized in that, In step S6, the periodic interference airflow operates in two modes: a staggered start-stop mode, where multiple sets of inlet ports of the periodic interference airflow inlet assembly alternately start and stop sequentially within a pulse cycle, and then repeat cyclically; within one pulse cycle, each set of inlet ports starts and stops once, and when one set of inlet ports starts, the other sets stop, and when one set of inlet ports stops, another set starts simultaneously; and a synchronous start-stop mode, where multiple sets of inlet ports of the periodic interference airflow inlet assembly start and stop simultaneously, repeating cyclically; within one pulse cycle, all inlet ports start and stop once. The pulse frequency of the periodic interference airflow is 0.2~10Hz, the duty cycle is 10%~60%, the pressure of the periodic interference airflow is 20%~90% of the pulverizing airflow pressure, and the average flow rate is 2%~15% of the total flow rate of the pulverizing airflow. And / or, in step S7, when the average flow rate of the periodic interfering airflow increases, the rotational speed of each classifier wheel is increased; when the pressure difference at the bottom of the crushing layer decreases and the product particle size tends to stabilize, the rotational speed of each classifier wheel is decreased; the compensation adjustment amount of the classifier wheel is 1% to 15% of the base rotational speed of the classifier wheel.