A method of synergistically regulating the physical and chemical environment of an ore pulp to improve the utilization of a collector
By synergistically controlling the flotation environment and pulp parameters, the problem of low collector utilization rate is solved, achieving efficient utilization of collectors, reducing production costs and environmental pressure, and making it suitable for various flotation processes.
Patent Information
- Application Number
- CN202611325235.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-20
AI Technical Summary
In existing technologies, collectors have low utilization rates during mineral flotation due to oxidation, unsuitable pH values, temperature fluctuations, and mismatches in pulp concentration and fineness, which increases production costs and environmental pressures, and there is a lack of systematic solutions.
By synergistically regulating the flotation environment and pulp parameters, including controlling the low-oxygen environment, precise pH value, temperature, and concentration fineness, the collector is ensured to adsorb efficiently under optimal conditions. Specific measures include introducing inert gas, adding pH adjusters, and controlling temperature and concentration fineness.
It significantly improves the utilization rate of collectors, reduces reagent consumption, lowers production costs, and reduces the burden of tailings treatment. It is suitable for various flotation processes, and is particularly effective for the flotation of sulfide ores.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of mineral flotation technology, specifically relating to a method for synergistically regulating the physicochemical environment of the pulp to improve the utilization rate of collectors. Background Technology
[0002] In the field of mineral processing, flotation is a key technology for separating and enriching mineral resources. Its core principle is to utilize collectors to selectively adsorb onto the surface of target minerals, causing them to float hydrophobically. Collectors, especially xanthates, dioxins, and sulfur-nitrogen compounds for sulfide minerals, constitute one of the main costs of mineral processing plants. In actual production, a considerable portion of collectors is not effectively adsorbed onto the surface of the target minerals, but is lost due to oxidation and decomposition, ineffective adsorption, or poor operating conditions. This results in high reagent consumption, increased production costs, and environmental pressures.
[0003] The main reasons for the reduced efficacy of harvesting agents include the following: (1) Oxidative decomposition: Traditional flotation often uses air as the gas source. The oxygen in the air will oxidize and decompose the collector molecules. In particular, xanthate collectors are easily oxidized into substances such as bixanthate, which have reduced or no efficacy, leading to an increase in their consumption.
[0004] (2) Inappropriate pH value: The pH value of the slurry directly affects the form of the collector, the electrical properties and solubility of the mineral surface. An unsuitable pH value will weaken the selectivity and adsorption strength of the collector.
[0005] (3) Temperature fluctuation: Too low a temperature will reduce the diffusion rate of the collector molecules and their reactivity with the mineral surface; too high a temperature will accelerate the decomposition and ineffective consumption of the agent.
[0006] (4) Mismatch between slurry concentration and fineness: If the slurry concentration is too high or too low, or the particle size distribution is too coarse or too fine, it will affect the mineralization process of bubbles, the degree of dispersion of reagents, and the probability of collision between minerals and reagents, resulting in a decrease in reagent utilization.
[0007] Currently, methods to reduce collector usage mainly focus on developing new, highly efficient collectors or adding synergists, but these methods suffer from high costs or limited applicability. There is still no comprehensive method that systematically optimizes the physicochemical environment of the entire flotation system to fundamentally suppress ineffective collector loss and comprehensively improve its utilization efficiency. Summary of the Invention
[0008] The purpose of this invention is to provide a method for synergistically regulating the physicochemical environment of slurry to improve the utilization rate of collectors.
[0009] The objective of this invention is achieved as follows: the method for synergistically regulating the physicochemical environment of the slurry to improve collector utilization involves synergistically regulating the flotation environment and slurry parameters during flotation operations, specifically by simultaneously implementing the following measures: (1) Controlling the low-oxygen environment: Inert gas is introduced into the flotation system so that the volume ratio of inert gas in the gas phase medium is ≥70%; (2) Adjusting the pH value of the pulp: Adjust the pH value of the flotation pulp to the optimal range according to the type of target mineral and the type of collector used; (3) Adjusting the pulp temperature: Adjust the temperature of the flotation pulp to 20~45℃; (4) Adjusting the concentration and fineness of the flotation pulp: Adjust the concentration of the flotation pulp to a solid weight concentration of 25-35%; the fineness requirement is that the liberation degree of the target mineral is ≥90%.
[0010] Compared with the prior art, the technical solution described in this invention has the following advantages: (1) Under anaerobic or low-oxygen conditions, the oxidative decomposition pathway of xanthate collectors (especially thiolated compounds) is blocked, and the collector molecules remain in active form, which can exist more stably in the slurry. Unoxidized collectors can be fully adsorbed on the surface of the target mineral, rather than becoming ineffective due to oxidation or forming non-selective products. This can significantly reduce the waste of collectors caused by decomposition, which is more fundamental, more economical, and has no secondary pollution than simply increasing the amount of collector or adding antioxidants.
[0011] (2) Since excessively high or low pH values can change the surface charge of minerals and the adsorption capacity of collectors, the pH value is precisely controlled within the range where the specific collector has the strongest collecting ability and the highest selectivity for the target mineral. This ensures that the collector exists in the best ionic form and undergoes the most effective adsorption with the mineral surface, thus improving the adsorption strength. This process is more precise and scientific than traditional processes, and reduces ineffective adsorption and reagent consumption caused by unsuitable pH values.
[0012] (3) Precise control of the slurry temperature range ensures that the collector molecules have sufficient kinetic energy, diffusion rate, and collision frequency to quickly reach the mineral surface and complete adsorption. The temperature is below 45℃, which effectively inhibits the thermal decomposition rate of the collector and avoids rapid failure of the agent due to excessive temperature. Within this range, both high adsorption rate and low decomposition rate are satisfied, and the chemical activity and stability of the collector are optimally balanced.
[0013] (4) Optimizing the slurry concentration and grinding fineness ensures a high probability of collision and adhesion efficiency among mineral particles, reagents, and bubbles. A suitable concentration ensures that the slurry has sufficient viscosity to effectively mineralize bubbles, while a suitable fineness ensures that the mineral surface is fully exposed, allowing the collector to be efficiently adsorbed without generating excessive sludge, increasing reagent consumption, and reducing physical losses such as "carrying" or "wrapping".
[0014] Through the synergistic implementation of the above four measures, this invention creates a stable and efficient operating environment for the collector, significantly improving the effective utilization rate of collector molecules by addressing both "reducing decomposition" and "promoting adsorption." Practice has proven that, under the premise of achieving the same or better mineral indicators, the technical solution described in this invention can systematically reduce the amount of collector used by 15-30% and reduce the burden of subsequent tailings water treatment. It is applicable to various flotation processes, especially showing significant effects in the flotation of sulfide ores, resulting in significant economic and environmental benefits. Detailed Implementation
[0015] The present invention will be further described below, but this is not intended to limit the invention in any way. Any modifications or substitutions made based on the teachings of the present invention shall fall within the scope of protection of the present invention.
[0016] The method for synergistically regulating the physicochemical environment of the slurry to improve collector utilization, as described in this invention, involves synergistically regulating the flotation environment and slurry parameters during flotation operations. Specifically, the following measures are implemented simultaneously: (1) Controlling the low oxygen environment: Introduce inert gas into the flotation system. The inert gas can be any one of nitrogen or argon or a combination thereof. Adjust the valve according to the volume of the flotation cell and the gas filling requirements to replace the air in the gas phase medium in the flotation machine with inert gas, or make the volume ratio of inert gas in the gas phase medium in the flotation machine ≥70%, so as to ensure that the oxygen content in the flotation system is significantly reduced.
[0017] Before and during the flotation operation, the following parameters are monitored and adjusted in real time using online detection instruments and an automatic control system: (2) Adjusting the pH value of the pulp: Based on the type of target mineral and the type of collector used, the pH value of the flotation pulp is adjusted to the optimal range by adding a pH adjuster.
[0018] (3) Adjusting the temperature of the slurry: Adjust the temperature of the flotation slurry to 20~45℃; in cold regions or seasons, the slurry can be preheated to above 20℃ by a slurry heater (such as a steam coil); in hot regions, the slurry temperature can be controlled below 45℃ by adding water or a cooling device.
[0019] (4) Controlling pulp concentration and fineness: By adjusting the grinding and classification operation, the concentration and particle size composition of the pulp entering the flotation operation are controlled. The concentration is adjusted by adding water or thickening underflow, and the fineness is achieved by controlling the particle size of the classification overflow. The flotation pulp concentration is adjusted to a solid weight concentration of 25-35%; the fineness requirement is that the liberation degree of the target mineral is ≥90%.
[0020] The process of introducing inert gas into the flotation system preferably involves ensuring that the volume percentage of inert gas in the gas phase is ≥95% and / or that the dissolved oxygen concentration in the pulp is ≤2.0 mg / L.
[0021] When the collector is a xanthate-based flotation agent for copper sulfide ore or sphalerite, the pH of the flotation pulp is adjusted to 9-12. When the collector is a xanthate-based flotation agent for copper oxide ore or galena, the pH of the flotation pulp is adjusted to 8-10. When the collector is a xanthate-based flotation agent for molybdenite, the pH of the flotation pulp is adjusted to 7-9.
[0022] The pH adjustment of the flotation pulp requires selecting the type and amount of pH adjuster according to the type of target mineral, and adjusting the pH of the flotation pulp to the optimal range. The pH adjuster can be lime, sodium carbonate, sulfuric acid, etc. For example, when flotating chalcopyrite, lime is commonly used to adjust the pH to 10.5~11.5.
[0023] The temperature of the flotation slurry is preferably controlled to be 30~35℃.
[0024] The fineness needs to be controlled to -0.074mm (-200 mesh), with a content of 80-90%.
[0025] The method described in this invention can be applied to the flotation process of various metallic and non-metallic minerals, and is especially suitable for the flotation of sulfide minerals (such as copper, lead, zinc, molybdenum, nickel, etc.) where the collector is easily oxidized.
[0026] Example 1
[0027] A copper ore beneficiation plant was conducting flotation on copper sulfide ore. The original process used air, and the amount of butyl xanthate collector was 100g / t of raw ore.
[0028] The technical solution described in this invention is adopted: (1) Controlling the low oxygen environment: In the aeration device of the flotation machine, nitrogen is introduced. According to the volume of the flotation cell and the aeration volume requirements, the valve is adjusted so that the volume ratio of nitrogen in the gas phase medium in the flotation machine reaches 80%.
[0029] (2) Adjusting the pH value of the slurry: By adding lime, the pH value of the flotation slurry is adjusted to 11.0±0.3.
[0030] (3) Adjusting the pulp temperature: Using the natural heating in the process, the temperature of the flotation pulp is adjusted to 32℃.
[0031] (4) Adjusting the concentration and fineness of the slurry: By adjusting the grinding and classification operation, the concentration and particle size composition of the slurry entering the flotation operation are controlled, and the concentration of the flotation slurry is adjusted to a solid weight concentration of 30%; the fineness is controlled to a content of -0.074mm (-200 mesh) of 88%.
[0032] While maintaining the same grade and recovery rate of copper concentrate, the dosage of butyl xanthate was reduced to 75g / t of raw ore, a reduction of 25%.
[0033] Example 2
[0034] The target mineral and collector are the same as in Example 1.
[0035] The technical solution described in this invention is adopted: (1) Controlling the low oxygen environment: Argon gas is introduced into the gas charging device of the flotation machine. According to the volume of the flotation cell and the gas charging requirements, the valve is adjusted so that the volume ratio of argon gas in the gas phase medium in the flotation machine reaches 90%.
[0036] (2) Adjusting the pH value of the slurry: By adding lime, the pH value of the flotation slurry is adjusted to 11.0±0.2.
[0037] (3) Adjusting the pulp temperature: Utilize the natural heating in the process to adjust the temperature of the flotation pulp to 35℃.
[0038] (4) Adjusting the concentration and fineness of the pulp: By adjusting the grinding and classification operation, the concentration and particle size composition of the pulp entering the flotation operation are controlled, and the concentration of the flotation pulp is adjusted to a solid weight concentration of 30%; the fineness is controlled to a content of -0.074mm (-200 mesh) of 84%.
[0039] While maintaining the same grade and recovery rate of copper concentrate, the amount of butyl xanthate used was reduced to 71g / t of raw ore, a reduction of 29%.
[0040] Example 3
[0041] —Comparative Example The original process at this plant involved air filling, resulting in pH fluctuations between 10.5 and 11.5, which were not precisely controlled. The slurry temperature also fluctuated between 15 and 50°C depending on the season, and the collector dosage was 100 g / t. The indicators showed significant fluctuations, with reagent consumption being particularly noticeable during the high-temperature season.
[0042] As can be seen from the embodiments and comparative examples, the technical solution described in this invention can stabilize the flotation environment and significantly reduce reagent consumption.
Claims
1. A method for synergistically regulating the physicochemical environment of a slurry to improve collector utilization, characterized in that, In flotation operations, the flotation environment and pulp parameters are coordinated and controlled, specifically by simultaneously implementing the following measures: (1) Controlling the low-oxygen environment: Inert gas is introduced into the flotation system so that the volume ratio of inert gas in the gas phase medium is ≥70%; (2) Adjusting the pH value of the pulp: Adjust the pH value of the flotation pulp to the optimal range according to the type of target mineral and the type of collector used; (3) Adjusting the pulp temperature: Adjust the temperature of the flotation pulp to 20~45℃; (4) Adjusting the concentration and fineness of the flotation pulp: Adjust the concentration of the flotation pulp to a solid weight concentration of 25-35%; the fineness requirement is that the liberation degree of the target mineral is ≥90%.
2. The method for synergistically regulating the physicochemical environment of the slurry to improve the utilization rate of the collector according to claim 1, characterized in that, The flotation system is introduced with inert gas so that the volume percentage of inert gas in the gas phase is ≥95%.
3. The method for synergistically regulating the physicochemical environment of the slurry to improve the utilization rate of the collector according to claim 2, characterized in that, The inert gas is introduced into the flotation system to make the dissolved oxygen concentration in the pulp ≤2.0mg / L.
4. The method for synergistically regulating the physicochemical environment of the slurry to improve the utilization rate of the collector according to claim 1, characterized in that, When the collector is xanthate-based for flotation of copper sulfide ore or sphalerite, the pH of the flotation pulp is adjusted to 9-12.
5. The method for synergistically regulating the physicochemical environment of the slurry to improve the utilization rate of the collector according to claim 1, characterized in that, When the collector is a xanthate-based flotation agent for copper oxide ore or galena, the pH of the flotation pulp is adjusted to 8-10.
6. The method for synergistically regulating the physicochemical environment of the slurry to improve the utilization rate of the collector according to claim 1, characterized in that, When the collector is xanthate-based flotation of molybdenite, the pH of the flotation pulp is adjusted to 7-9.
7. The method for synergistically regulating the physicochemical environment of a slurry to improve collector utilization according to any one of claims 1, 4, 5, and 6, characterized in that, The pH value of the flotation pulp needs to be adjusted according to the type of target mineral, and the type and amount of pH adjuster should be selected to adjust the pH value of the flotation pulp to the optimal range.
8. The method for synergistically regulating the physicochemical environment of slurry to improve collector utilization according to claim 1, characterized in that, The temperature of the flotation slurry is controlled to 30~35℃.
9. The method for synergistically regulating the physicochemical environment of slurry to improve collector utilization according to claim 1, characterized in that, The fineness needs to be controlled to -0.074mm, with a content of 80-90%.