A quick curing construction method for natural lacquer-based color drawing
By leveraging the synergistic effect of Cu(II)-amine complex catalyst and ultraviolet light irradiation, the problem of low curing efficiency in traditional natural lacquer painting processes has been solved, achieving rapid curing and high-quality natural lacquer painting, which is suitable for arts and crafts, furniture, and architectural decoration.
Patent Information
- Application Number
- CN202611291560.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-20
AI Technical Summary
Traditional natural lacquer painting techniques have low curing efficiency and cannot meet the needs of large-scale production. Existing ultraviolet curing solutions use synthetic UV resins, which leads to a loss of the texture and environmental friendliness of natural lacquer.
Using Cu(II)-amine complex as a catalyst, combined with ultraviolet light irradiation, rapid curing of natural lacquer is achieved, including multi-stage construction of primer, painted lacquer and topcoat. The synergistic effect of ultraviolet light and catalyst accelerates the film formation process.
It achieves rapid curing of natural lacquer, shortens the construction cycle, improves the hardness and adhesion of the lacquer film, maintains the environmental friendliness and texture of natural lacquer, and is suitable for handicrafts and large-scale production.
Smart Images

Figure CN123128199A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lacquerware craftsmanship, specifically to a rapid curing method for painting using natural lacquer. Background Technology
[0002] Lacquer painting is an important part of traditional lacquer art. Natural lacquer is mainly composed of urushiol. After curing, the lacquer film formed has the characteristics of high hardness, strong adhesion, chemical corrosion resistance, excellent durability and environmental protection. It is widely used in arts and crafts, furniture, architectural decoration and other fields.
[0003] Traditional lacquer painting relies on air-drying curing in a shaded room, with each layer requiring 24-48 hours to cure. The entire production cycle can take weeks to months, resulting in extremely low efficiency and making it unsuitable for large-scale production. To improve curing efficiency, ultraviolet (UV) curing solutions have emerged, using synthetic UV paints for application and curing. However, this solution uses acrylic-based synthetic UV resin coatings, not natural lacquer. The chemical structures and curing mechanisms of the two are fundamentally different, and the finished product loses the unique texture, environmental friendliness, and durability of natural lacquer, failing to meet the quality requirements of traditional lacquer art.
[0004] In recent years, academic research has focused on the curing of natural lacquer under ultraviolet light, confirming that natural lacquer can cure into a film in a short time under ultraviolet irradiation without the addition of an external photoinitiator. Simultaneously, Cu(II)-amine complexes can simulate laccase-catalyzed urushiol oxidation polymerization, accelerating the drying and film formation of lacquer, and the resulting coating retains all the properties of natural lacquer. However, these studies remain at the laboratory material research stage and have not yet developed a complete construction method compatible with the painting process, nor have they combined ultraviolet curing with catalyst curing and applied it to painting construction. Summary of the Invention
[0005] The purpose of this invention is to address the shortcomings of existing technologies by providing a rapid curing construction method for painting based on natural lacquer, which fully preserves the traditional advantages of natural lacquer, such as being environmentally friendly, having a durable film, and a warm and smooth texture.
[0006] To address the aforementioned technical problems, this invention provides a rapid curing construction method for colored paintings based on natural lacquer, comprising: The dried wood is processed into a base; Lay cloth on the base; Mix raw lacquer with tile ash and apply it to the surface of the base; A primer is sprayed onto the surface of the undercarriage, the primer comprising natural lacquer and Cu(II)-amine complex; After the primer surface has cured, the pattern is applied to the base surface by stenciling or hand-painting with colored lacquer. Each layer of colored lacquer is quickly set by ultraviolet light. The colored lacquer includes natural raw lacquer, natural mineral pigments and Cu(II)-amine complex. Apply topcoat paint to the completed base surface; Polishing is performed.
[0007] In some embodiments, the mass of the Cu(II)-amine complex in the primer is a% of the mass of the natural lacquer, and the mass of the Cu(II)-amine complex in the painted lacquer is b% of the mass of the natural lacquer, with a ≥ b.
[0008] In some embodiments, the painted lacquer comprises 100 parts by weight of natural raw lacquer, 10-30 parts by weight of natural mineral pigments, 10-20 parts by weight of turpentine, and 0.3-0.8 parts by weight of Cu(II)-amine complex.
[0009] In some embodiments, the primer is cured solely by Cu(II)-amine complex.
[0010] In some embodiments, 0.3 ≤ b ≤ 0.8.
[0011] In some embodiments, the topcoat comprises 100 parts by weight of natural lacquer and 0.3 to 0.5 parts by weight of Cu(II)-amine complex.
[0012] In some embodiments, after the topcoat is sprayed onto the completed base coat surface, ultraviolet light is used for rapid setting.
[0013] In some embodiments, performing rapid UV light irradiation for setting after each layer of painting is completed includes: Irradiate the painted layer with a UV-LED lamp for 3-8 minutes to quickly set the surface. Once the painted layer is no longer sticky to the touch, the next layer can be applied. The UV-LED lamp's irradiance is 100-300 mW / cm². 2 .
[0014] In some embodiments, the thickness of each layer of paint is controlled to be 20~40μm.
[0015] In some embodiments, applying fabric to the base material includes: Place fine linen or summer cloth on the surface of the base, then evenly apply natural raw lacquer diluted with turpentine onto the fine linen or summer cloth, press it firmly to remove air bubbles, and leave it at 25~30℃ and 75~85% relative humidity for 4~6 hours.
[0016] In some embodiments, during the application of primer and topcoat, the thickness of each layer of primer and topcoat is controlled between 15 and 25 μm. After each layer of primer or topcoat is applied, the next layer must be applied only after the surface of that layer has cured.
[0017] The beneficial effects of this invention are as follows: 1. This invention constructs a complete process system for rapid curing and painting with pure natural lacquer. Using natural raw lacquer as the sole film-forming substance, Cu(II)-amine complexes, turpentine, and other additives serve only as functional auxiliaries and do not participate in the main construction of the film-forming network. This fully preserves the traditional advantages of natural lacquer—its green and environmentally friendly nature, durable film, and warm texture—distinguishing it from existing rapid curing and painting solutions that use synthetic UV resins.
[0018] 2. This invention utilizes the synergistic effect of ultraviolet light and a catalyst for curing. The photothermal effect of ultraviolet light rapidly activates the catalytic activity of the Cu(II)-amine complex, while simultaneously accelerating the evaporation of the thinner and improving the leveling properties of the paint film, achieving rapid surface setting within 3-8 minutes to meet the needs of continuous construction. After the light exposure stops, the catalyst continues to function, ensuring complete deep curing of the paint film. Compared to pure catalytic curing, the amount of catalyst used in the painted layer is reduced by approximately 2 / 3, the drying time is shortened, the pencil hardness of the paint film is increased, and the adhesion is better.
[0019] 3. This invention effectively reduces the impact of mineral pigments on ultraviolet light by controlling the thickness of a single layer of paint to 20~40μm, applying layers to ultra-thick areas, and using workpiece rotation or multi-angle lamp irradiation technology, thus ensuring complete curing of all parts of the paint layer.
[0020] 4. This invention significantly shortens the construction cycle while ensuring quality. The active construction cycle from the application of the sealing primer to the completion of the topcoat only takes 6 to 8 hours. Compared with the traditional pure catalytic curing process, the efficiency is improved by more than 70%, which can realize continuous painting operations. It is suitable for both handicraft art creation and large-scale industrial production.
[0021] 5. The primer of the present invention adopts a catalytic curing scheme, which not only avoids the problem that the primer cannot be exposed to ultraviolet light after being covered by the painting layer, but also forms chemical bonds with the painting layer through the active sites remaining on the surface of the primer, which significantly improves the adhesion between the multi-layer coatings and avoids delamination and peeling during use. Attached Figure Description
[0022] Figure 1 This is a process flow diagram of the present invention; Figure 2 This is a schematic diagram of the structure of the UV curing chamber of the present invention; Figure 3 This is a cross-sectional view of the lacquerware of the present invention.
[0023] Attached reference numerals: 1. Cabinet body; 2. UV-LED lamp; 3. Control cabinet door; 4. Hollowed-out storage platform; 5. Inner heat dissipation grille; 6. Touch control panel; 7. Temperature control device; 8. Storage cabinet door; 9. Ventilation louvers. Detailed Implementation
[0024] To make the technical problems to be solved, the technical solutions, and the beneficial effects of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only for explaining the present invention and are not intended to limit the present invention.
[0025] This invention provides a rapid curing construction method for colored paint based on natural lacquer. The overall process is divided into five stages: substrate pretreatment, sealing primer application, colored paint layer application and curing, transparent protective topcoat application, and polishing. The details are as follows: I. Substrate Pretreatment.
[0026] S1. Base tire making and drying.
[0027] Select high-quality wood with uniform texture, put it into a drying equipment for dehydration treatment, and control the wood moisture content to 8%~12%; process the wood into a base according to the product design requirements, and use 120 grit, 240 grit and 400 grit sandpaper to polish the surface of the base step by step to remove burrs and processing marks until the surface is smooth and flat.
[0028] S2, Fabric mounting.
[0029] Fine linen or ramie fabric is selected as the reinforcing backing material. Natural lacquer and turpentine are mixed and stirred evenly at a mass ratio of 1:0.3~0.5 to obtain a diluted backing varnish. The fine linen or ramie fabric is laid flat on the base material, and the diluted backing varnish is evenly applied to the fabric surface. A scraper is used to press the varnish firmly from the center outwards, thoroughly removing any air bubbles between the fabric layer and the base material. After construction, the base material is placed in an environment with a temperature of 25~30℃ and a relative humidity of 75%~85% for 4~6 hours to complete the backing process. The resulting backing layer improves the crack resistance and structural strength of the base material.
[0030] S3, scraping off the putty.
[0031] Use raw lacquer mixed with tile ash to level the surface of the base coat, applying it in the order of coarse tile ash, medium tile ash, and fine tile ash. After each layer of ash is applied, place the base coat in an environment with a temperature of 25-30℃ and a relative humidity of 75%-85% for 3-4 hours. Once the ash layer is surface dry, sand it smooth with 240-grit sandpaper. Repeat the application 2-3 times to form a uniform and dense ash layer on the surface of the base coat.
[0032] 2. Apply a sealing primer.
[0033] S4. Spray a sealing primer.
[0034] The primer contains natural lacquer, turpentine and Cu(II)-amine complex. The components are in the following proportions by weight: 100 parts natural lacquer, 30-50 parts turpentine, and 0.8 parts Cu(II)-amine complex.
[0035] During construction, first mix and dilute the natural lacquer and turpentine at a mass ratio of 1:0.3~0.5, then add the corresponding proportion of Cu(II)-amine complex as a catalyst, stir thoroughly for 5~10 minutes until uniform, and then use a spraying device to evenly coat the surface of the base coat after applying putty.
[0036] During the spraying process, the thickness of each layer of primer should be controlled between 15 and 30 μm. If it is necessary to increase the thickness of the primer, a layered spraying method should be adopted. After the surface of the previous layer of primer has cured, the next layer should be sprayed to avoid sagging or uneven curing caused by a single thick coating.
[0037] The primer uses a catalytic curing method. After spraying, the primer is placed in an environment with a temperature of 15~30℃ and a relative humidity of 50%~85% for 1~2 hours. The primer surface will be surface dry, meeting the requirements for the next construction process. The primer needs to be left at room temperature for 24~48 hours to fully cure and reach its final performance.
[0038] The catalytically cured primer used in this invention has two considerations: First, the primer is located below the painted layer and cannot be exposed to ultraviolet light after being covered by the painted layer. Catalytic curing can ensure that the primer is fully cross-linked. Second, the primer surface after catalytic drying has residual catalytic active sites, which can form chemical bonds with urushiol in the subsequent painted layer, significantly improving the interlayer adhesion between the primer and the painted layer. If ultraviolet light catalysis is used, its surface will be highly dense, and the subsequent painted layer can only form physical adhesion, with weak interlayer bonding, which easily leads to coating delamination and peeling.
[0039] The preparation method of the Cu(II)-amine complex used in this invention is as follows: triethylenetetramine and copper chloride (CuCl2・2H2O) are dissolved in anhydrous ethanol at a molar ratio of 2:1, heated to 60°C and stirred under reflux for 4 hours. After the reaction is completed, the solvent is removed by vacuum distillation to obtain a blue-green solid product, which is then ground into powder and sealed for later use.
[0040] III. Painting and curing of the colored layers.
[0041] S5, Preparation of Painted Lacquer.
[0042] Painted lacquer uses natural lacquer as the sole film-forming substance and comprises natural lacquer, natural mineral pigments, turpentine, and Cu(II)-amine complex functional additives. The components, by weight, are: 100 parts natural lacquer, 10-30 parts natural mineral pigments, 10-20 parts turpentine, and 0.3-0.8 parts Cu(II)-amine complex. The preferred ratio is 100 parts natural lacquer, 15-25 parts natural mineral pigments, 12-18 parts turpentine, and 0.3-0.5 parts Cu(II)-amine complex. The aforementioned film-forming substance refers to the main material constituting the continuous phase of the lacquer film (i.e., natural lacquer). The catalyst is merely an aid to accelerate the cross-linking of urushiol and does not alter the essential natural lacquer properties of the lacquer film.
[0043] The preparation method for painted lacquer includes: mixing natural raw lacquer with turpentine, stirring evenly, adding Cu(II)-amine complex, stirring thoroughly for 5-10 minutes, then adding natural mineral pigments, and grinding the mixture in a three-roll mill until the lacquer fineness is ≤20μm, thus obtaining the painted lacquer. Since the catalyst activity gradually decreases over time, the prepared painted lacquer should be used within 2 hours; if left for more than 2 hours, 0.1-0.2 parts by weight of Cu(II)-amine complex should be added to compensate for the loss of activity before continued use.
[0044] S6. Color painting.
[0045] After the primer surface has cured, the pattern is transferred to the base surface using either a powder transfer method or by hand painting. Before the actual painting, gently brush away any residual powder from the base surface with a soft brush to prevent the powder from blocking ultraviolet light and causing poor local curing.
[0046] When drawing patterns, the thickness of each layer of paint should be controlled between 20 and 40 μm. If a thick coating effect is required in a part of the pattern and the thickness of a single layer exceeds 40 μm, multiple layers should be applied to avoid problems such as UV light not being able to penetrate and incomplete curing of the underlying layer due to a single thick coating.
[0047] S7, the painted layer cures quickly.
[0048] After each layer of color painting is completed, a rapid UV light curing process is performed. During and after the rapid UV light curing process, the catalyst continues to slowly cure the coating, forming a combined curing mode of rapid UV light curing and catalyst post-curing.
[0049] The method for rapid curing with ultraviolet light includes: placing the completed workpiece in an ultraviolet curing chamber and controlling the irradiation intensity to be 100~300mW / cm². 2Irradiate for 3-8 minutes to quickly set the painted layer until it is no longer sticky to the touch, then proceed to the next layer. For workpieces with three-dimensional structures or raised or recessed shapes, rotate the workpiece 90° once during the irradiation process, or use a combination of top and side lighting to ensure that all sides of the thick painted lines are fully illuminated, avoiding any hard-to-cure areas. Figure 2 As shown, this invention uses a UV curing chamber to irradiate workpieces with ultraviolet light. The UV curing chamber includes a chamber body 1. An operating cabinet door 3 and a storage cabinet door 8 are rotatably mounted on one side of the chamber body 1. The operating cabinet door is located above the storage cabinet door. The interior of the chamber corresponding to the storage cabinet door is used for storage, while the interior of the chamber corresponding to the operating cabinet door is used for UV irradiation. A perforated platform 4 and UV-LED lamps 2 are installed inside the chamber, allowing UV-LED lamps to be installed on all surfaces of the chamber to ensure curing coverage in all areas. Internal heat dissipation grilles 5 and ventilation louvers 9 are respectively installed on the walls of the chamber corresponding to the operating cabinet door and the storage cabinet door. The chamber body also includes a temperature control device 7 and a touch control panel 6. The touch control panel is used to control the on / off state of the UV-LED lamps, and the temperature control device is used to monitor the temperature inside the chamber and adjust the power of the UV-LED lamps according to the temperature inside the chamber.
[0050] After the light exposure ends, the next layer of coating can be applied. The Cu(II)-amine complex catalyst continues the post-curing reaction. The paint film (i.e., the coating) will reach a dry state in about 4 to 6 hours, and subsequent operations such as sanding and packaging can be carried out. The paint film needs to be left at room temperature for 24 to 48 hours to fully cure and reach its maximum hardness.
[0051] During the curing process described above, the photothermal effect of ultraviolet light and the Cu(II)-amine complex catalyst exhibit a significant synergistic effect: In addition to ultraviolet radiation, the UV-LED lamps also emit significant thermal radiation, raising the ambient temperature inside the curing equipment to 40-60°C. This heat significantly increases the reaction rate of urushiol oxidation polymerization, rapidly activating the catalyst and allowing even low-dose catalysts to exert highly efficient catalytic effects. Furthermore, it accelerates the evaporation of turpentine thinner from the paint film, reducing film viscosity, improving the leveling properties of the paint, and resulting in a smoother and denser final film. After the light exposure stops, the catalyst continues to provide chemical catalytic energy, ensuring complete deep cross-linking of the paint film, ultimately achieving rapid application and complete curing.
[0052] IV. Apply a transparent protective topcoat.
[0053] S8. Apply topcoat.
[0054] After all the painted patterns are completed, a transparent protective topcoat is sprayed onto the surface of the workpiece. The topcoat consists of natural lacquer and Cu(II)-amine complex, and by weight, it contains 100 parts of natural lacquer and 0.3 parts of Cu(II)-amine complex.
[0055] During application, mix and dilute natural lacquer and turpentine at a mass ratio of 1:0.5~0.8, add the corresponding proportion of Cu(II)-amine complex, stir evenly, and then spray. The thickness of each topcoat should be controlled at 15~25μm; if it is necessary to increase the thickness of the topcoat, it should be applied in layers, and the next layer should be sprayed after the previous layer has cured.
[0056] S9, Topcoat Curing.
[0057] After the topcoat is applied, it is cured using the same UV rapid setting + catalyst post-curing method as the color painting layer: the workpiece is placed under a 365nm UV-LED lamp with an irradiation intensity of 100~300mW / cm². 2 The surface is rapidly shaped by irradiation for 3-8 minutes, followed by curing at room temperature using a Cu(II)-amine complex catalyst. The topcoat takes approximately 4-6 hours to fully dry and 24-48 hours to fully cure.
[0058] The amount of catalyst used in the topcoat is lower than that in the color layer, which can reduce the impact of catalyst residue on the appearance and color of the transparent film, while ensuring the curing performance and transparent texture of the topcoat.
[0059] V. Polishing process.
[0060] S10, graded grinding and polishing.
[0061] After the topcoat has fully cured, the surface of the paint film is successively wet-polished using 600-grit, 1000-grit, 1500-grit, and 2000-grit sandpaper to remove surface particles and imperfections. Then, a wool wheel is used with polishing compound to perform mirror polishing, resulting in a glossy and smooth finished lacquer painting.
[0062] like Figure 3 As shown, the final lacquerware structure, from bottom to top, consists of a wooden base, a cloth layer, an ash layer, a sealing primer layer, two painted layers, and a transparent topcoat layer.
[0063] The technical effects of the present invention will be further illustrated below through specific embodiments and comparative experiments.
[0064] The parameters of the substrate pretreatment process (S1~S3) in each embodiment and the control group were kept consistent: Phoebe zhennan wood with a moisture content of 10% was selected and processed into a flat base, which was sanded step by step and then covered with summer cloth. The ratio of raw lacquer to turpentine was 1:0.4, and it was placed in an environment of 28°C and 80% relative humidity for 5 hours. Raw lacquer was mixed with tile ash and scraped three times in the order of coarse, medium and fine. After each layer was placed at 28°C for 3.5 hours, it was sanded smooth.
[0065] The only difference between each embodiment and the control group is the curing conditions of the primer and the paint layer. Based on the above results, we can conclude that: Control Group 1: Natural lacquer dries extremely slowly at room temperature (25℃) without any catalyst or ultraviolet light, with a surface drying time > 24 hours and a complete drying time > 7 days. This is due to the inherent characteristics of lacquer; the oxidative polymerization reaction of urushiol has an extremely low reaction rate without a catalyst and at room temperature. This control group demonstrates that natural lacquer cannot be quickly applied by simply brushing and letting it dry naturally; it must be accelerated with the help of catalysts or ultraviolet light.
[0066] Control Group 2: Under catalyst-free conditions, with only UV irradiation (chamber temperature 40~60℃), the surface drying time was shortened to 3~5 minutes, proving that the thermal effect of UV light can quickly evaporate the solvent and cure the paint film surface. However, actual drying still takes several hours, the pencil hardness is only 4H, the adhesion is only grade 2, and the bottom layer of the paint film is not completely cured. This indicates that although UV irradiation alone can achieve rapid surface drying, due to the lack of a catalyst's continued catalytic effect after the light irradiation stops, the deeper layers of the paint film cannot be completely cross-linked and cured, resulting in poor paint film hardness and adhesion, which cannot meet the requirements of practical use.
[0067] Control group 3: Under conditions of adding 1.5% Cu(II)-amine complex and without UV irradiation, the drying time was 6-8 hours, which was shorter than that of control group 4 (0.8%, 8-12 hours). However, with the catalyst dosage nearly doubled, the drying time was only shortened by about 25%, indicating that simply increasing the catalyst dosage has a diminishing marginal effect on improving the curing speed. In addition, excessive catalyst dosage can also increase the brittleness of the paint film and the risk of color darkening.
[0068] Control Group 4: Under conditions of adding 0.8% Cu(II)-amine complex and without UV irradiation, curing was carried out at room temperature (25°C) for 8-12 hours, achieving a hardness of 5H, an adhesion grade of 1, and complete film curing. This scheme demonstrates the feasibility of a curing pathway relying solely on a catalyst. In contrast, Example 2, using 0.3% catalyst (less than 40% of Control Group 4) combined with UV irradiation, actually shortened the drying time to 4-6 hours (a reduction of approximately 40-50%) and increased the hardness to 6-7H. This comparison fully demonstrates that catalytic curing and UV curing are not simply additive but exhibit a significant synergistic effect.
[0069] Example 1: Under conditions of adding 0.5% Cu(II)-amine complex and supplementing with ultraviolet light irradiation (chamber temperature 40~60℃), the surface drying time was 3~5 minutes, the pencil hardness increased to 6H, and the adhesion was grade 1, which was significantly improved compared with control group 2 (only light irradiation, no catalyst, hardness 4H, adhesion grade 2), proving that the catalyst is indispensable for the final curing quality. However, actual drying still required several hours, and deep curing still required post-curing. This indicates that although the pure light curing method introduces a catalyst, the catalyst in the primer is rapidly consumed during the light irradiation stage, and there is no continuous catalytic activity after the light irradiation stops, so deep curing is still incomplete.
[0070] Example 2: The primer was cured at 25°C with 0.8% Cu catalyst in the absence of light; the color layer was rapidly set by irradiation with 0.3% Cu(II)-amine complex for 6 minutes (40-60°C in the chamber), followed by curing at room temperature (25°C). Surface drying time was only 2-5 minutes, and actual drying time was shortened to 4-6 hours. Pencil hardness reached 6-7H, adhesion was grade 1, and the paint film surface was smooth and fully cured. As a preferred embodiment of the present invention, the primer is cured only with catalyst, ensuring deep curing of the subsequent primer; the catalyst dosage for the color layer is only 0.3%, far lower than the 0.8% in control group 4, but the actual drying time is shortened by 40%-50%, and the pencil hardness is increased by 1-2 grades, fully demonstrating that there is a synergistic effect between the ultraviolet photothermal effect and the Cu(II)-amine complex, rather than a simple functional additive effect. This scheme simultaneously achieves rapid continuous construction and excellent paint film performance, resulting in the best overall effect.
[0071] Example 3: Based on Example 2, the catalyst dosage for the paint layer was increased to 0.8%, further shortening the drying time to 3-5 hours, achieving a pencil hardness of 7H, adhesion grade 1, and complete curing of the paint film. Compared to control group 4 (0.8% catalyst, no light exposure), the drying time was shortened from 8-12 hours to 3-5 hours (a reduction of approximately 58-60%), and the hardness increased from 5H to 7H (an improvement of 2 grades), fully demonstrating the activating effect of UV photothermal effect on catalyst activity; the higher the catalyst dosage, the more significant the synergistic effect. Compared to Example 2 (0.3% catalyst + light exposure, drying time 4-6 hours, hardness 6-7H), the catalyst dosage increased by approximately 167%, while the drying time was only shortened by approximately 17-25%, and the hardness improvement was limited, indicating that simply increasing the catalyst dosage has diminishing marginal returns on the improvement of curing speed. Considering catalyst cost, paint film performance, and construction efficiency, Example 2 (0.3% catalyst + light exposure) is the optimal solution, achieving near-high-dosage effects with the lowest catalyst dosage.
[0072] In Example 3, a low-dose catalyst of 0.3% achieves an effect close to that of a high-dose catalyst of 0.8%. Rapid curing can be achieved within the range of 0.3% to 0.8%, but considering the cost of the catalyst, the optimal solution is to choose the lower value of 0.3%. In practical applications, if the ultimate efficiency is sought, 0.8% can be selected, while 0.3% to 0.5% can be selected to balance cost and efficiency.
[0073] The definitions of surface dry, hard dry, and fully cured above are as follows: Surface dry: The surface is not sticky to the touch. A continuous thin film has formed on the surface of the paint film. It is not sticky to the touch and does not leave fingerprints, but the interior of the paint film is still liquid or semi-solid. The touch test is used to determine this: touch the surface of the paint film with your finger every 5 to 10 minutes until it is no longer sticky, referring to standard GB / T 1728-2020 (Method A).
[0074] Practical application: The paint film has formed a complete solid continuous phase, possessing initial mechanical strength and capable of withstanding light external forces (such as sanding and handling), but has not yet reached its final performance peak. The next process (such as sanding and packaging) can then be carried out. The filter paper pressing method is used for determination: Filter paper is placed flat on the paint film surface, and a weight (200g, dry filter paper method) is gently placed on top. After 30 seconds, the weight and filter paper are removed, and it is observed whether the filter paper adheres to the paint film, referring to standard GB / T 1728-2020 (Method B).
[0075] Complete Curing: The cross-linking reaction of the paint film is basically completed, and various properties such as hardness, adhesion, and chemical resistance reach their design maximum values. Thereafter, no significant changes occur, achieving the final performance indicators and the maximum degree of hardening. Pencil hardness test: Pencil hardness is measured every 24 hours until the hardness value remains unchanged after two consecutive tests. Refer to standard GB / T 6739-2022.
[0076] The above-described embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention, and should all be included within the protection scope of the present invention.
Claims
1. A rapid curing construction method for painted decoration based on natural lacquer, characterized in that, include: The dried wood is processed into a base; Lay cloth on the base; Mix raw lacquer with tile ash and apply it to the surface of the base; A primer is sprayed onto the surface of the undercarriage, the primer comprising natural lacquer and Cu(II)-amine complex; After the primer surface has cured, the pattern is applied to the base surface by stenciling or hand-painting with colored lacquer. Each layer of colored lacquer is quickly set by ultraviolet light. The colored lacquer includes natural raw lacquer, natural mineral pigments and Cu(II)-amine complex. Apply topcoat paint to the completed base surface; Polishing is performed.
2. The rapid curing construction method for colored paintings based on natural lacquer according to claim 1, characterized in that, The mass of the Cu(II)-amine complex in the primer is a% of the mass of the natural lacquer, and the mass of the Cu(II)-amine complex in the painted lacquer is b% of the mass of the natural lacquer, with a ≥ b.
3. The rapid curing construction method for colored paintings based on natural lacquer according to claim 1, characterized in that, The primer is cured solely by Cu(II)-amine complex.
4. The rapid curing construction method for colored paintings based on natural lacquer according to claim 2, characterized in that, 0.3≤b≤0.8。 5. The rapid curing construction method for colored paintings based on natural lacquer according to claim 4, characterized in that, The topcoat comprises 100 parts by weight of natural lacquer and 0.3 to 0.5 parts by weight of Cu(II)-amine complex.
6. The rapid curing construction method for colored paintings based on natural lacquer according to claim 4, characterized in that, After the base coat is painted, it is quickly set by ultraviolet light.
7. The rapid curing construction method for colored paintings based on natural lacquer according to any one of claims 1 to 6, characterized in that, After each layer of painting is completed, a rapid UV light treatment is performed to set the color, including: Irradiate the paint layer with a UV-LED lamp for 3-8 minutes to quickly set the surface. Once the surface is no longer sticky, proceed to the next layer. The UV-LED lamp's irradiance is 100-300 mW / cm². 2 .
8. The rapid curing construction method for colored lacquer based on any one of claims 1 to 6, characterized in that, The thickness of each layer of paint is controlled between 20 and 40 μm.
9. The rapid curing construction method for colored lacquer based on any one of claims 1 to 6, characterized in that, The fabric applied to the base includes: Place fine linen or summer cloth on the surface of the base, then evenly apply natural raw lacquer diluted with turpentine onto the fine linen or summer cloth, press it firmly to remove air bubbles, and leave it at 25~30℃ and 75~85% relative humidity for 4~6 hours.
10. The rapid curing construction method for colored lacquer based on any one of claims 1 to 6, characterized in that, During the application of primer and topcoat, the thickness of each layer of primer and topcoat should be controlled between 15 and 25 μm. After each layer of primer or topcoat is applied, the next layer should be applied only after the surface of the current layer has cured.