A multi-stage coating process for corrosion protection of recycled aluminum wheels and a wheel
By combining sandblasting, nitric acid and hydrofluoric acid pickling, and KSL primer, the problem of Fe and Cu precipitates on the surface of multi-stage recycled aluminum wheels was solved, forming a dense composite protective coating and improving corrosion resistance.
Patent Information
- Application Number
- CN202611466659.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-20
- Publication Date
- 2026-11-20
AI Technical Summary
Existing coating processes cannot effectively handle the Fe- and Cu-rich precipitates on the surface of multi-stage recycled aluminum wheels, causing the coating to easily blister and peel off in corrosive environments, resulting in substandard corrosion protection life.
The oxide scale is removed by sandblasting, and impurities are removed by acidic cleaning solutions mainly composed of nitric acid and hydrofluoric acid to form a nano-scale microporous passivation film. KSL anti-corrosion transparent primer is then sprayed onto the passivation film to construct a multi-layer composite protection system.
By thoroughly removing the surface oxide layer through physical and chemical means, a dense and uniform anti-corrosion coating is formed, which solves the problem of substandard anti-corrosion performance of multi-stage recycled aluminum wheels and achieves long-term and stable coating protection.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of wheel coating technology, and more specifically, it relates to a multi-stage recycled aluminum wheel anti-corrosion coating process and wheel. Background Technology
[0002] Currently, the wheel manufacturing industry mainly uses #A356 recycled material for primary utilization. However, the total amount of recyclable recycled aluminum scrap wheels will account for a relatively low proportion of the total aluminum used in new wheel production. Therefore, it is necessary to begin using other grades of recycled aluminum scrap on the market to expand the application scope and create multi-stage recycled aluminum.
[0003] Compared to primary recycled aluminum, multi-stage recycled aluminum has significantly higher Fe content (approximately 0.25%) and Cu content (approximately 0.2%) (primary recycled aluminum contains only approximately 0.002% Cu). Since Fe and Cu have higher electrode potentials than Al, they form localized electrode pairs in corrosive media, accelerating preferential corrosion of Al. Therefore, multi-stage recycled aluminum requires higher corrosion resistance.
[0004] The current conventional coating process is as follows: raw material → pretreatment → base powder spraying → baking → color paint spraying → baking → bright powder spraying → baking → off-line. In the coating of multi-stage recycled aluminum wheels, the conventional pretreatment (mainly phosphoric acid / sulfuric acid) is difficult to effectively treat the unevenly distributed Fe-rich and Cu-rich precipitates on the substrate surface. This leads to the subsequent coating being prone to blistering and peeling in corrosive environments, and the corrosion protection life is far from meeting the quality requirements of wheel products. Summary of the Invention
[0005] The purpose of this invention is to provide a coating process for corrosion protection of multi-stage recycled aluminum wheels, aiming to solve the problem that conventional pretreatment cannot effectively treat the Fe-rich and Cu-rich precipitates on the surface of multi-stage recycled aluminum substrates, resulting in substandard corrosion protection performance after coating.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is: to provide a multi-stage corrosion-resistant coating process for recycled aluminum wheels, comprising the following steps performed in sequence: sandblasting, pretreatment, anti-corrosion transparent primer spraying, first curing, base powder or transparent powder spraying, second curing, color paint spraying, third curing, transparent powder spraying, and fourth curing. The pretreatment process includes degreasing, pickling, and passivation processes performed in sequence. The degreasing process is used to remove residual grease, release agent, and adsorbed dirt from the surface of recycled aluminum; The pickling process uses an acidic cleaning solution mainly composed of nitric acid and hydrofluoric acid, with added corrosion inhibitors and surfactants, to remove the oxide layer and impurity elements on the surface of recycled aluminum and expose the fresh metal lattice of the aluminum substrate. The passivation process uses a chromium-free passivation solution to form a dense, uniform chemical conversion film with a nanoscale microporous structure on the surface of the acid-washed and activated aluminum substrate.
[0007] In one possible implementation, the anti-corrosion transparent primer used in the anti-corrosion transparent primer spraying process is KSL anti-corrosion transparent primer, selected from one or two of hyperbranched polyester / amino system and acrylic / amino system. The anti-corrosion transparent primer has a hydroxyl value of 140-180 mgKOH / g and is an amino and hydroxyl curing system at 140℃ for 15-25 min. The solid content during application is 20%-25%, the viscosity during application is 18-22 s, and the film thickness during spraying is 20-25 μm. In the first curing process, the wheel body temperature is maintained above 140℃, and the curing time is 15-25 minutes.
[0008] In one possible implementation, the sandblasting process employs a dry sandblasting technique, using non-ferrous spherical abrasives with a particle size range of φ0.3mm-0.5mm. The injection pressure is 0.4-0.6MPa, the angle between the nozzle and the wheel hub surface is 70°-85°, and the injection distance is 150-250mm; The arithmetic mean roughness Ra of the wheel hub surface after sandblasting is 2.5μm-4.0μm.
[0009] In one possible implementation, the non-ferrous spherical abrasive is stainless steel pellets or ceramic pellets; After sandblasting is completed, the pretreatment process begins within 4 hours.
[0010] In one possible implementation, in the degreasing process, a weakly alkaline or neutral degreasing agent is used, and the process is sprayed at 50-60°C for 1-5 minutes with a spray pressure of 1.0-1.5 kg / cm² and a free alkali point of 2-4. In the pickling process, the spray treatment is carried out at room temperature for 1-4 minutes, the spray pressure is 0.6-1.0 kg / cm², and the acid point is 6-7 points; In the passivation process, the chromium-free passivation solution is a zirconium-based, titanium-based, or silane-based passivation solution, treated at room temperature for 1-5 minutes, with a spray pressure of 0.6-1.0 kg / cm², a conductivity of 400-600 µS / cm, and a pH of 2.5-3.5.
[0011] In one possible implementation, the anti-corrosion transparent primer spraying process adopts rotary cup spraying, with two spray guns set at the outer wheel flange and outer wheel rim positions, and at the front wheel flange and front wheel center positions, and the wheel is sprayed once in both clockwise and counterclockwise rotation. The spraying voltage for each location is 40±15Kv, the forming pressure is 0.20-0.30MPa, the spraying time is 3-5s, the paint output is 70-150cc / min, and the coating thickness is 20-25μm.
[0012] In one possible implementation, in the base powder spraying process, the base powder is selected as epoxy polyester powder, which is a carboxyl and amino curing system at 180℃ / 10-15min, and the sprayed film thickness is 100-120μm. In the transparent powder spraying process, the transparent powder is an acrylic transparent powder, which is a ring-opening addition reaction system of carboxylic acid and epoxy group at 180℃ / 10-20min, and the spraying film thickness is 100-120μm; In the paint spraying process, the paint is selected from one or two of the oil-based polyester / amino systems, which are amino and hydroxyl curing systems with a temperature of 140℃ for 15-25 minutes. The hiding power is ≤10μm and the sprayed film thickness is 15-25μm.
[0013] In one possible implementation, an online film thickness detection device is provided between the anti-corrosion transparent primer spraying process and the first curing process, between the base powder or transparent powder spraying process and the second curing process, between the color paint spraying process and the third curing process, and between the transparent powder spraying process and the fourth curing process. The online film thickness detection device adopts one or more combinations of infrared spectroscopy, X-ray fluorescence, or laser triangulation. The online film thickness detection device performs non-contact real-time film thickness detection on uncured wet film or powder coating after spraying. The detection data is transmitted to the control system in real time. The control system compares the measured film thickness with the preset target film thickness. When the deviation exceeds the preset threshold, it automatically adjusts the paint / powder output and / or spraying time of the corresponding spray gun.
[0014] In one possible implementation, the control system monitors the continuous film thickness distribution curve along the rotation direction on the wheel surface in real time. When a standing wave node is detected in the film thickness distribution curve, which is formed by the interference of the sprayed airflow with the incident airflow after reflection on the complex curved surface of the wheel, that is, when the film thickness shows a periodic peak-valley alternating distribution at a specific angular position and the film thickness difference between adjacent peaks and valleys is ≥1μm, the control system determines that there is a spraying standing wave effect at that position. The control system calculates the standing wave wavelength λw based on the number of standing wave nodes and the distance between adjacent standing wave nodes, and generates a compensation spraying scheme with opposite phase and equal amplitude to the standing wave waveform. It controls the corresponding spray gun to increase the paint / powder output by ΔQc at the standing wave trough and decrease the paint / powder output by ΔQc at the standing wave peak. The formula for calculating ΔQc is as follows: Where Aw is the standing wave amplitude, in μm, and Aw is determined by half the difference between the peak and trough of the measured film thickness distribution curve. λw is the distance between adjacent standing wave nodes, in mm, λw = 10-50 mm; x is the arc length coordinate along the direction of wheel rotation, in mm; φ is the initial phase angle, in rad, which is determined by the angle difference between the position of the first node of the standing wave and the initial spray point of the spray gun. k is the standing wave compensation gain coefficient, k = 0.5-1.5; γ is the curvature compensation coefficient, γ = 0.1-0.5; d²ε / dx² is the second spatial derivative of the film thickness deviation along the direction of wheel rotation, with units of μm / mm², and characterizes the curvature of the film thickness variation; v is the linear velocity of the wheel rotation, in mm / s; Δt is the spraying cycle, measured in seconds.
[0015] The beneficial effects of the multi-stage recycled aluminum wheel anti-corrosion coating process provided by this invention are as follows: Compared with the prior art, this invention first introduces a sandblasting process to thoroughly remove the oxide scale on the surface of the casting and form a uniform rough surface through physical means; secondly, the pickling solution in the pretreatment is replaced with an acidic cleaning solution mainly composed of nitric acid and hydrofluoric acid, which utilizes its strong complexing and dissolving ability for Fe and Cu elements to remove or expose the enriched phases on the substrate surface; thirdly, a KSL anti-corrosion transparent primer process is added between passivation and base powder. This primer has a high cross-linking density and excellent resistance to media penetration, and can form a dense and continuous chemically inert organic barrier on the passivation film. Through the combination of the above-mentioned sandblasting, pickling solution replacement, and the addition of KSL primer, a composite protective system of passivation film, KSL primer, and multi-layer powder coating is finally formed, solving the problem of substandard anti-corrosion performance of multi-stage recycled aluminum due to high Fe and Cu content.
[0016] The present invention also provides a wheel, which is prepared by the multi-stage recycled aluminum wheel anti-corrosion coating process described above. The wheel surface is formed from the inside out by a passivation film layer, a KSL anti-corrosion transparent primer layer, a base powder layer or a transparent powder layer, a color paint layer and a transparent powder layer. The KSL anti-corrosion transparent primer layer has a film thickness of 20-25μm, the base powder layer or transparent powder layer has a film thickness of 100-120μm, the color paint layer has a film thickness of 15-25μm, and the transparent powder layer has a film thickness of 130-150μm.
[0017] The beneficial effects of the wheel provided by this invention are as follows: Compared with the prior art, this wheel constructs a composite protective system on the substrate surface through a passivation film layer, a KSL anti-corrosion transparent primer layer, a base powder layer or transparent powder layer, a color paint layer, and a transparent powder layer arranged sequentially from the inside out. Specifically, the KSL anti-corrosion transparent primer layer forms an independent chemically inert barrier between the passivation film and the subsequent powder coating, working synergistically with the base powder / transparent powder layer, color paint layer, and transparent powder layer to ensure the long-term stability of the composite coating system. This effectively solves the problem of substandard anti-corrosion performance of multi-stage recycled aluminum wheels due to the high Fe and Cu content in the substrate. Detailed Implementation
[0018] To make the technical problems, technical solutions, and beneficial effects of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0019] Unless otherwise explicitly specified, the use of terms such as "first," "second," or "third" is intended to distinguish different objects, not to describe a specific order.
[0020] Unless otherwise expressly defined, the use of directional terms such as “center,” “lateral,” “longitudinal,” “horizontal,” “vertical,” “top,” “bottom,” “inner,” “outer,” “upper,” “lower,” “front,” “rear,” “left,” “right,” “clockwise,” “counterclockwise,” “high,” and “low” to indicate orientation or positional relationships is merely for the convenience of describing the present invention and simplifying the description, and is not intended to indicate or imply that the device or element referred to must have a specific orientation or be constructed and operated in a specific orientation, and therefore should not be construed as limiting the specific scope of protection of the present invention.
[0021] The present invention provides a multi-stage anti-corrosion coating process for recycled aluminum wheels. This multi-stage anti-corrosion coating process for recycled aluminum wheels includes the following steps performed in sequence: sandblasting, pretreatment, anti-corrosion transparent primer spraying, first curing, base powder or transparent powder spraying, second curing, color paint spraying, third curing, transparent powder spraying, and fourth curing. The pretreatment step includes, in sequence, a degreasing step, an acid pickling step, and a passivation step.
[0022] The above sequence of processes constitutes the complete process route of this invention. The order of each process should not be arbitrarily changed to avoid poor adhesion of the subsequent coating or a decrease in anti-corrosion performance due to the incomplete completion of the preceding process.
[0023] Sandblasting is the pretreatment foundation for the entire coating process. After the wheels are cast, the surface is left with oxide scale, release agent and other casting contaminants. Moreover, the oxide layer composition of the multi-stage recycled aluminum substrate is more complex due to the presence of impurities such as Fe and Cu.
[0024] This process employs dry blasting, using non-ferrous spherical abrasives, preferably stainless steel or ceramic shot, with a particle size range of φ0.3mm-0.5mm. The blasting pressure is controlled at 0.4-0.6MPa, the nozzle-hull surface angle is maintained at 70°-85°, and the blasting distance is maintained at 150-250mm.
[0025] After sandblasting, the arithmetic mean roughness Ra value of the wheel hub surface is controlled within the range of 2.5μm-4.0μm.
[0026] After sandblasting, the aluminum should be moved to the next pretreatment process within 4 hours, or temporarily stored in a dry, clean, and inert environment to prevent secondary oxidation of the fresh aluminum surface and ensure the quality of the pretreatment conversion film.
[0027] The pretreatment process includes degreasing, pickling, and passivation, which are carried out in sequence.
[0028] In the degreasing process, a weak alkaline or neutral degreasing agent is used. The agent is sprayed at 50-60℃ for 1-5 minutes with a spray pressure of 1.0-1.5 kg / cm² and a free alkali point of 2-4 points. This thoroughly removes various greases, release agents and adsorbed dirt from the surface of the recycled aluminum, while avoiding excessive corrosion of the aluminum material.
[0029] In the pickling process, an acidic cleaning solution mainly composed of nitric acid and hydrofluoric acid with added corrosion inhibitors and surfactants is used. The solution is sprayed at room temperature for 1-4 minutes with a spray pressure of 0.6-1.0 kg / cm² and an acid point of 6-7 points.
[0030] The pickling solution formulation is the key difference between this invention and conventional phosphoric acid / sulfuric acid pickling. Nitric acid and hydrofluoric acid have strong complexing and dissolving abilities on the Fe-rich and Cu-rich precipitates on the surface of multi-stage recycled aluminum substrates. They can effectively remove or expose the impurity-rich areas on the substrate surface, exposing fresh metal lattices to the aluminum substrate and providing a uniform and highly reactive activated surface for subsequent passivation processes.
[0031] In the passivation process, a chromium-free passivation process is adopted, preferably using zirconium-based, titanium-based, or silane-based passivation solutions. The solution is treated at room temperature for 1-5 minutes, with a spray pressure of 0.6-1.0 kg / cm², a conductivity of 400-600 µS / cm, and a pH of 2.5-3.5.
[0032] This process forms a dense, uniform chemical conversion film with a nanoscale microporous structure on the surface of the acid-etched and activated aluminum substrate. The pore size of these nanoscale micropores is approximately tens to hundreds of nanometers. This microporous structure provides the basic anti-corrosion performance as a morphological feature of the conversion film itself, and also provides a crucial micromechanical interlocking interface for the physical penetration and anchoring of the subsequent KSL anti-corrosion transparent primer. If the passivation film is too dense and non-porous, the subsequent KSL primer cannot form a penetration and anchoring effect; if the micropores are too large or unevenly distributed, it will affect the continuity of the primer film formation.
[0033] The anti-corrosion transparent primer spraying process and the first curing process are important steps in constructing the composite protection system of this invention. The anti-corrosion transparent primer used is KSL anti-corrosion transparent primer, which is selected from one or two of the hyperbranched polyester / amino system and acrylic / amino system.
[0034] The anti-corrosion transparent primer has a hydroxyl value of 140-180 mgKOH / g and is an amino and hydroxyl curing system at 140℃ for 15-25 min. The solid content during application is 20%-25%, the viscosity during application is 18-22 s, and the film thickness is 20-25 μm.
[0035] The KSL primer can penetrate into the nanoscale micropores of the passivation film in a liquid state. After curing, it forms a dual interface of physical anchoring and chemical bonding. At the same time, its high crosslinking density gives the coating excellent resistance to media penetration.
[0036] Specifically, to achieve consistency in product appearance, film thickness, and corrosion resistance, this process employs a rotary cup spraying method. Two spray guns are installed at each of the outer wheel rim and outer wheel flange positions, and at each of the front wheel rim and front wheel center positions. The wheel is sprayed once in both clockwise and counter-clockwise rotations. The spraying voltage at each position is 40±15Kv, the forming pressure is 0.20-0.30MPa, the spraying time is 3-5s, and the paint output is 70-150cc / min.
[0037] After spraying, the first curing process is carried out, with the wheel temperature maintained above 140℃ and the curing time being 15-25 minutes, preferably 15-20 minutes. If the curing temperature is below 140℃ or the curing time is less than 15 minutes, the cross-linking density of the KSL primer will be insufficient, resulting in a decrease in anti-corrosion performance; if the curing temperature is too high or the time is too long, it may lead to excessive aging of the coating or affect the adhesion of subsequent interlayers.
[0038] The base powder or transparent powder spraying process and the second curing process provide the main protective layer of the composite protective system. There are two parallel implementation schemes for this process: one is to spray base powder, and the other is to spray transparent powder, and one of the two can be used.
[0039] When using a base powder coating method, the base powder is an epoxy polyester powder, a carboxyl and amino group curing system cured at 180℃ for 10-15 min. Electrostatic spraying is used, with two spray guns each at the front rim, front center hole, outer rim, and inner rim. The wheel is sprayed once in both clockwise and counter-clockwise directions. The spraying voltage for each location is 55±10 kV, the spraying time is 10-20 s, the powder output is 25±10 m³ / h, and the coating thickness is 100-120 μm. During base powder curing, the wheel body temperature is maintained above 180℃, and the curing time is 10-15 min.
[0040] When using a transparent powder coating scheme, an acrylic transparent powder is selected, which is a ring-opening addition reaction system of carboxylic acid and epoxy group at 180℃ for 10-20min. Electrostatic spraying is used, with two spray guns each at the outer rim, center hole, outer rim, and inner rim positions. The wheel is sprayed once in both clockwise and counter-clockwise directions. The spraying voltage is 50±5Kv, the spraying time is 10-20s, the powder output is 25±5m³ / h, and the coating thickness is 100-120μm. During transparent powder curing, the wheel body temperature is maintained above 180℃, and the curing time is 10-20min.
[0041] The difference between epoxy polyester base powder and acrylic transparent powder is that the base powder has better filling ability for substrate defects and lower cost, making it suitable for occasions where appearance requirements are not strict; the transparent powder has high transparency and good leveling properties, making it suitable for occasions that require a metallic texture or special color effect.
[0042] The paint spraying process and the third curing process provide a decorative color layer for the wheels and also serve as an auxiliary protective function. The paint is selected from one or two oil-based polyester / amino systems, both of which are amino and hydroxyl curing systems cured at 140℃ for 15-25min, with a hiding power ≤10μm.
[0043] This process uses a combination of rotary cup and air gun spraying. The rotary cup is used to spray the front of the wheel, with a spraying voltage of 40±15Kv, a forming pressure of 0.20-0.30MPa, a spraying time of 9-15s, a paint output of 100-250cc / min, and a coating thickness of 15-25μm. The air gun is used to spray the wheel window, with a spraying voltage of 50±10Kv, an atomization pressure of 0.10-0.20MPa, a fan-shaped pressure of 0.10-0.20MPa, a spraying time of 12-20s, a paint output of 50-150cc / min, and a coating thickness of 10-20μm. The inner and outer rim paints are applied by free adsorption.
[0044] Rotary cup spraying uses centrifugal force generated by high-speed rotation to atomize paint into tiny droplets, making it suitable for coating large front areas with high efficiency and excellent surface quality; air gun spraying uses compressed air to atomize paint, making it suitable for fine coating of complex shaped areas such as windows.
[0045] After the spraying is completed, the third curing process is carried out. The wheel body temperature is kept above 140℃ and the curing time is 15-25 minutes, preferably 15-20 minutes.
[0046] The transparent powder coating process and the fourth curing process provide the outer wear-resistant and weather-resistant protective layer for the wheels. The transparent powder used is an acrylic transparent powder, which is a ring-opening addition reaction system of carboxylic acid and epoxy group at 180℃ / 10-20min.
[0047] Electrostatic spraying is used, with two spray guns each at the outer rim, center hole, outer rim, and inner rim. The wheel is sprayed once in both clockwise and counter-clockwise directions. The spraying voltage is 50±5 kV, the spraying time is 10-20 seconds, the powder output is 35±5 m³ / h, and the coating thickness is 130-150 μm. In the fourth curing process, the wheel temperature is maintained above 180℃, and the curing time is 10-20 minutes.
[0048] This transparent powder layer is the outermost barrier of the composite protection system. It is the thickest layer in the entire coating system and provides excellent scratch resistance, stone chip resistance, and UV aging resistance. This layer and the KSL primer layer are on the outside and inside of the coating system, respectively resisting external mechanical damage and internal electrochemical corrosion, forming a complete protective closed loop.
[0049] In a preferred embodiment of the present invention, an online film thickness detection device is also provided after each spraying process and before the corresponding curing process.
[0050] Specifically, the online film thickness detection device is installed between the anti-corrosion transparent primer spraying process and the first curing process, between the base powder or transparent powder spraying process and the second curing process, between the color paint spraying process and the third curing process, and between the transparent powder spraying process and the fourth curing process.
[0051] This device uses one or more combinations of infrared spectroscopy, X-ray fluorescence, or laser triangulation to perform non-contact real-time film thickness detection on uncured wet films or powder coatings after spraying.
[0052] The detection data is transmitted to the control system in real time. The control system compares the measured film thickness with the preset target film thickness. When the deviation exceeds the preset threshold, it automatically adjusts the paint / powder output and / or spraying time of the corresponding spray gun.
[0053] Taking infrared spectroscopy as an example, its principle is that different film thicknesses absorb infrared light of a specific wavelength differently. By calibrating the quantitative relationship between absorption intensity and film thickness, rapid and non-destructive testing can be achieved. X-ray fluorescence method calculates film thickness by detecting the fluorescence intensity of characteristic elements in the coating, and is suitable for coating systems containing specific metal element markings. Laser trigonometry calculates coating thickness by the position difference of the laser reflection spot on the coating surface and the substrate surface, which belongs to geometric optics measurement method.
[0054] As a further preferred embodiment of the above-mentioned online film thickness detection and control system, the control system also has standing wave node identification and adaptive compensation functions.
[0055] During the wheel-rotating spraying process, the paint airflow ejected from the fixed spray gun is reflected when it encounters the complex curved surface of the high-speed rotating wheel. The incident and reflected flows interfere and superimpose near the gas-solid interface, forming a standing wave field in an aerodynamic sense. The antinodes of this standing wave field correspond to the longest airflow residence time and the largest paint deposition (film thickness peak), while the nodes correspond to the shortest airflow residence time and the smallest paint deposition (film thickness trough).
[0056] After identifying the periodic distribution pattern of the standing wave, the standing wave compensation scheme actively generates compensation waveforms with opposite phases to achieve interference cancellation.
[0057] Specifically, the control system monitors the continuous film thickness distribution curve along the rotation direction on the wheel surface in real time. When a standing wave node is detected in the film thickness distribution curve, which is formed by the interference of the sprayed airflow with the incident airflow after reflection on the complex curved surface of the wheel, that is, when the film thickness shows a periodic peak-valley alternating distribution at a specific angle position and the film thickness difference between adjacent peaks and valleys is ≥1μm, the control system determines that there is a spraying standing wave effect at that position.
[0058] The control system calculates the standing wave wavelength λw based on the number of standing wave nodes and the spacing between adjacent nodes, and generates a compensation spraying scheme with the opposite phase and equal amplitude to the standing wave waveform. This scheme controls the corresponding spray gun to increase the paint / powder output by ΔQc at the trough of the standing wave and decrease it by ΔQc at the peak. The formula for calculating ΔQc is: Where Aw is the standing wave amplitude (μm), determined by half the difference between the peak and trough of the measured film thickness distribution curve; λw is the distance between adjacent standing wave nodes (mm), λw = 10-50mm; x is the arc length coordinate along the wheel rotation direction (mm); φ is the initial phase angle (rad), determined by the angle difference between the position of the first node of the standing wave and the initial spray point of the spray gun; k is the standing wave compensation gain coefficient, k = 0.5-1.5; γ is the curvature compensation coefficient, γ = 0.1-0.5; d²ε / dx² is the second spatial derivative of the film thickness deviation along the wheel rotation direction (μm / mm²), characterizing the curvature of the film thickness change; v is the wheel rotation linear velocity (mm / s); Δt is the spraying period (s). In the formula, the sine term is the main compensation component, used to offset the periodic standing wave distribution; the second derivative term is the curvature correction component, used to compensate for the influence of the curvature change of the complex surface of the wheel hub on the coating deposition efficiency. The physical meaning of this formula is: increase the amount of paint output at the trough of the standing wave (negative sin value) and decrease the amount of paint output at the peak of the standing wave (positive sin value). At the same time, the compensation amount is finely adjusted according to the curvature of the film thickness deviation along the space to avoid over-compensation or under-compensation.
[0059] The present invention also provides a wheel, which is prepared using any of the above-described coating processes. The surface of the wheel is formed, from the inside out, in the following order: a passivation film layer, a KSL anti-corrosion transparent primer layer, a base powder layer or a transparent powder layer, a color paint layer, and a transparent powder layer.
[0060] The film thicknesses of each layer are as follows: KSL anti-corrosion transparent primer layer 20-25μm, base powder layer or transparent powder layer 100-120μm, color paint layer 15-25μm, transparent powder layer 130-150μm.
[0061] It should be noted that the base powder layer or transparent powder layer refers to the fact that the actual product contains only one of the base powder layer and the transparent powder layer. One of the two is selected, not both. When the base powder is selected in the process, the product presents the base powder layer, and when the transparent powder is selected in the process, the product presents the transparent powder layer, in order to meet different appearance requirements.
[0062] The technical effects of the present invention are verified below through specific embodiments and comparative embodiments.
[0063] Example 1 Multi-stage recycled aluminum wheels are produced using the following process: multi-stage recycled aluminum material → sandblasting → pretreatment → spraying KSL (anti-corrosion transparent primer) → baking → spraying base powder / transparent powder → baking → spraying color paint → baking → spraying transparent powder → baking → off-line.
[0064] Step 1 (sandblasting): Stainless steel shot is preferred, with a particle size of φ0.3mm, a spraying pressure of 0.6MPa, an angle of 80° between the nozzle and the wheel hub surface, a spraying distance of 150-250mm, and the surface roughness Ra value after sandblasting is controlled at 2.5μm-4.0μm.
[0065] Step 2 (Pretreatment): Degreasing uses a weak alkaline degreasing agent at a temperature of 50-60℃, a spray pressure of 1.0-1.5 kg / cm², and a free alkaline point of 2-4 points; pickling uses an acidic cleaning solution mainly composed of nitric acid and hydrofluoric acid, sprayed at room temperature for 1-4 minutes, with a spray pressure of 0.6-1.0 kg / cm² and an acid point of 6-7 points; passivation uses an organic-inorganic hybrid chromium-free passivating agent at room temperature, a spray pressure of 0.6-1.0 kg / cm², a conductivity of 400-600 µs / cm, and a pH of 2.5-3.5.
[0066] Step 3 (Spraying KSL Anti-corrosion Transparent Primer): Use German Leucer hyperbranched polyester / amino transparent primer with a hydroxyl value of 160 mg KOH / g, a construction solids content of 22%, and a construction viscosity of 20s (Ford Cup 4). Use a rotary cup sprayer, placing spray guns at the front rim and front center, and at the outer rim and outer rim positions. Spray clockwise for 5 seconds, then counterclockwise for 5 seconds. Spraying voltage is 40 kV, forming pressure is 0.25 MPa, and paint flow rates at each position are 70 cc / min for the front center, 150 cc / min for the front rim, 90 cc / min for the outer rim, and 150 cc / min for the outer rim. The resulting film thickness is 20-25 μm.
[0067] Step 4 (KSL curing): Keep the workpiece at a solid temperature of 140℃ or above for 15 minutes.
[0068] Step 5 (Spraying base powder or transparent powder): Two schemes were verified in this embodiment. Scheme A: Spraying base powder (Akzo epoxy polyester black powder EN018CS) using 8 electrostatic spray guns at 50kV. The powder was sprayed clockwise for 7 seconds and then counterclockwise for 7 seconds at the outer wheel rim, near the center hole, the outer rim, and the inner rim, with powder output of 30m³ / h, 25m³ / h, 25m³ / h, and 35m³ / h respectively, and a film thickness of 100-120μm. Scheme B: Spraying transparent powder (Akzo acrylic transparent powder CZ007) with the same spraying parameters as Scheme A.
[0069] Step 6 (Curing base powder or transparent powder): Base powder curing temperature above 180℃, hold for 10 minutes; transparent powder curing temperature above 180℃, hold for 15 minutes.
[0070] Step 7 (Painting): Using an oil-based polyester / amino resin system, the front of the wheel is coated with a rotary cup sprayer (voltage 40KV, spraying the front rim, center, and center hole for 3 seconds each, forming pressures of 0.30, 0.25, and 0.20MPa respectively, paint output of 250, 200, and 120cc / min respectively, and film thickness of 20-25μm). The windows are coated with an air gun (voltage 40KV, spraying the large window, small angle, left rib, and right rib for 3 seconds each, atomization pressure and fan-shaped pressure are both 0.15MPa, paint output of 150, 50, 100, and 100cc / min respectively, and film thickness of 15-20μm).
[0071] Step 8 (Color Paint Curing): Keep the workpiece at a temperature above 140℃ for 15 minutes.
[0072] Step 9 (Spraying transparent powder): Akzo acrylic transparent powder CZ007 is used, with 8 electrostatic spray guns and a voltage of 50Kv. Spray the outer ear edge, center hole, outer rim, and inner rim positions clockwise for 7 seconds and then counterclockwise for 7 seconds. The powder output is 35, 30, 30, and 35 m³ / h, respectively, and the coating thickness is 130-150μm.
[0073] Step 10 (Curing transparent powder): Keep the workpiece at a solid temperature of 180℃ or above for 15 minutes.
[0074] Comparative Example 1 The only difference from Example 1 is the thickness of the KSL primer coating. In this comparative example, the coating thickness is 10-15 μm (achieved by reducing the paint output: 50cc / min for the front wheel center, 120cc / min for the front wheel rim, 70cc / min for the outer wheel rim, and 120cc / min for the outer wheel rim). The remaining processes and parameters are exactly the same as in Example 1.
[0075] Comparative Example 2 The KSL anti-corrosion transparent primer spraying process and its corresponding curing process are cancelled. The process route is as follows: multi-stage recycled aluminum material → sandblasting → pretreatment → spraying primer or transparent powder → baking → spraying color paint → baking → spraying transparent powder → baking → unloading. The remaining parameters are the same as in Example 1.
[0076] Comparative Example 3 Compared to Example 1, the coating sequence is different. The process route is: multi-stage recycled aluminum material → sandblasting → pretreatment → spraying primer or transparent powder → baking → spraying color paint → baking → spraying KSL (anti-corrosion transparent primer) → baking → spraying transparent powder → baking → off-line. That is, the KSL primer spraying process has been adjusted to be after the color paint has cured and before the transparent powder spraying. The remaining parameters are the same as in Example 1.
[0077] Comparative Example 4 The only difference from Example 1 is the composition of the pickling solution. In this comparative example, the pickling uses an acidic cleaning solution mainly composed of phosphoric acid and sulfuric acid, with added corrosion inhibitors and surfactants. The acid point is controlled at 5-6 points, and the remaining procedures and parameters are exactly the same as in Example 1.
[0078] Performance Tests and Results The wheel samples prepared in Example 1 and Comparative Examples 1-4 were subjected to copper accelerated acetic acid salt spray test (CASS test) according to the wheel industry standard test method. The corrosion creep value Ud on the front of the wheel was used as the evaluation index (the smaller the Ud value, the better the corrosion resistance). The pass standard was Ud≤1.0mm. The test results are shown in Table 1.
[0079] The results in Table 1 show that: Example 1 uses the complete technical solution of the present invention (nitric acid + hydrofluoric acid pickling + KSL primer film thickness 20-25μm + KSL located before the base powder after passivation), and the Ud values are 0.64mm (base powder solution) and 0.54mm (transparent powder solution), which are far superior to the qualified standard Ud≤1.0mm.
[0080] In Comparative Example 1, when the KSL film thickness was reduced to 10-15 μm, the Ud values were 1.16 mm and 1.01 mm, respectively, which were slightly higher than the qualified standard. This indicates that the KSL primer film thickness needs to reach 20-25 μm to provide sufficient isolation and protection.
[0081] In Comparative Example 2, after removing the KSL primer, the Ud values reached 3.27 mm and 3.03 mm respectively, far exceeding the qualified standard, indicating that a single powder coating system without KSL primer cannot meet the corrosion protection requirements of multi-stage recycled aluminum.
[0082] In Comparative Example 3, after the KSL primer was adjusted to a colored paint and then sprayed, the Ud values were 2.85mm and 2.69mm, respectively, which far exceeded the qualified standard. This indicates that the KSL primer must be located in the innermost layer of the coating system (closely attached to the passivation film) in order to perform its core functions of sealing the micropores of the passivation film and isolating the substrate from the corrosive medium. If it is placed in the outer layer, it cannot prevent the corrosive medium from penetrating from the primer / substrate interface.
[0083] Comparative Example 4 uses phosphoric acid + sulfuric acid pickling solution instead of nitric acid + hydrofluoric acid pickling solution. The Ud values are 1.74 mm and 1.59 mm, respectively, which far exceed the qualified standard. This shows that the combination of nitric acid + hydrofluoric acid has a complexation and dissolution ability on the Fe-rich and Cu-rich precipitates on the surface of multi-stage recycled aluminum that cannot be replaced by the phosphoric acid + sulfuric acid system. Conventional phosphoric acid / sulfuric acid pickling cannot effectively remove the enriched phases, resulting in local galvanic corrosion continuing to occur during service.
[0084] Based on the analysis of the above test results, the uniform rough surface provided by the sandblasting process provides an adhesion basis for the passivation film. The acid washing with nitric acid and hydrofluoric acid removes the enriched phase and provides an activated surface with uniform composition for the passivation film. The nanopores of the passivation film provide a penetration and anchoring interface for the KSL primer. The KSL primer forms a dense chemical inert barrier on the passivation film.
[0085] The above four steps are interconnected. The absence of any step (such as the absence of KSL primer in Comparative Example 2) or the deviation of any step from the optimal conditions (such as the low film thickness in Comparative Example 1, the incorrect order in Comparative Example 3, and the inappropriate pickling solution in Comparative Example 4) will lead to a significant decrease in the final anti-corrosion performance. This synergistic effect exceeds the expected linear superposition of the individual contributions of each technical feature.
[0086] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A multi-stage corrosion-resistant coating process for recycled aluminum wheels, characterized in that, The process includes the following steps performed in sequence: sandblasting, pretreatment, anti-corrosion transparent primer spraying, first curing, base powder or transparent powder spraying, second curing, color paint spraying, third curing, transparent powder spraying, and fourth curing. The pretreatment process includes degreasing, pickling, and passivation processes performed in sequence. The degreasing process is used to remove residual grease, release agent, and adsorbed dirt from the surface of recycled aluminum; The pickling process uses an acidic cleaning solution mainly composed of nitric acid and hydrofluoric acid, with added corrosion inhibitors and surfactants, to remove the oxide layer and impurity elements on the surface of recycled aluminum and expose the fresh metal lattice of the aluminum substrate. The passivation process uses a chromium-free passivation solution to form a dense, uniform chemical conversion film with a nanoscale microporous structure on the surface of the acid-washed and activated aluminum substrate.
2. The coating process for corrosion protection of multi-stage recycled aluminum wheels as described in claim 1, characterized in that, In the process of applying the anti-corrosion transparent primer, the anti-corrosion transparent primer used is KSL anti-corrosion transparent primer, which is selected from one or two of the hyperbranched polyester / amino system and acrylic / amino system. The anti-corrosion transparent primer has a hydroxyl value of 140-180 mgKOH / g and is an amino and hydroxyl curing system at 140℃ for 15-25 min. The solid content during application is 20%-25%, the viscosity during application is 18-22 s, and the film thickness during spraying is 20-25 μm. In the first curing process, the wheel body temperature is maintained above 140℃, and the curing time is 15-25 minutes.
3. The coating process for corrosion protection of multi-stage recycled aluminum wheels as described in claim 1, characterized in that, The sandblasting process adopts a dry sandblasting process, using non-ferrous spherical abrasives with a particle size range of φ0.3mm-0.5mm; The injection pressure is 0.4-0.6MPa, the angle between the nozzle and the wheel hub surface is 70°-85°, and the injection distance is 150-250mm; The arithmetic mean roughness Ra of the wheel hub surface after sandblasting is 2.5μm-4.0μm.
4. The coating process for corrosion protection of multi-stage recycled aluminum wheels as described in claim 3, characterized in that, The non-ferrous spherical abrasive is stainless steel shot or ceramic shot. After sandblasting is completed, the pretreatment process begins within 4 hours.
5. The coating process for corrosion protection of multi-stage recycled aluminum wheels as described in claim 1, characterized in that, In the degreasing process, a weak alkaline or neutral degreasing agent is used, and the agent is sprayed at 50-60°C for 1-5 minutes with a spray pressure of 1.0-1.5 kg / cm² and a free alkali point of 2-4 points. In the pickling process, the spray treatment is carried out at room temperature for 1-4 minutes, the spray pressure is 0.6-1.0 kg / cm², and the acid point is 6-7 points; In the passivation process, the chromium-free passivation solution is a zirconium-based, titanium-based, or silane-based passivation solution, treated at room temperature for 1-5 minutes, with a spray pressure of 0.6-1.0 kg / cm², a conductivity of 400-600 µS / cm, and a pH of 2.5-3.
5.
6. The coating process for corrosion protection of multi-stage recycled aluminum wheels as described in claim 1, characterized in that, The anti-corrosion transparent primer spraying process adopts rotary cup spraying, with two spray guns set at the outer wheel flange and outer wheel rim position, and two spray guns at the front wheel flange and front wheel center position, and the wheel is sprayed once in both clockwise and counterclockwise rotation. The spraying voltage for each location is 40±15Kv, the forming pressure is 0.20-0.30MPa, the spraying time is 3-5s, the paint output is 70-150cc / min, and the coating thickness is 20-25μm.
7. The coating process for corrosion protection of multi-stage recycled aluminum wheels as described in claim 1, characterized in that, In the base powder spraying process, the base powder is an epoxy polyester powder, which is a carboxyl and amino curing system at 180℃ for 10-15min, and the sprayed film thickness is 100-120μm. In the transparent powder spraying process, the transparent powder is an acrylic transparent powder, which is a ring-opening addition reaction system of carboxylic acid and epoxy group at 180℃ / 10-20min, and the spraying film thickness is 100-120μm; In the paint spraying process, the paint is selected from one or two of the oil-based polyester / amino systems, which are amino and hydroxyl curing systems with a temperature of 140℃ for 15-25 minutes. The hiding power is ≤10μm and the sprayed film thickness is 15-25μm.
8. The multi-stage recycled aluminum wheel anti-corrosion coating process as described in claim 1, characterized in that, An online film thickness detection device is provided between the anti-corrosion transparent primer spraying process and the first curing process, between the base powder or transparent powder spraying process and the second curing process, between the color paint spraying process and the third curing process, and between the transparent powder spraying process and the fourth curing process. The online film thickness detection device adopts one or more combinations of infrared spectroscopy, X-ray fluorescence, or laser triangulation. The online film thickness detection device performs non-contact real-time film thickness detection on uncured wet film or powder coating after spraying. The detection data is transmitted to the control system in real time. The control system compares the measured film thickness with the preset target film thickness. When the deviation exceeds the preset threshold, it automatically adjusts the paint / powder output and / or spraying time of the corresponding spray gun.
9. The multi-stage recycled aluminum wheel anti-corrosion coating process as described in claim 8, characterized in that, The control system monitors the continuous film thickness distribution curve along the rotation direction on the wheel surface in real time. When a standing wave node is detected in the film thickness distribution curve, which is formed by the interference of the sprayed airflow with the incident airflow after reflection on the complex curved surface of the wheel, that is, when the film thickness shows a periodic peak-valley alternating distribution at a specific angle position and the film thickness difference between adjacent peaks and valleys is ≥1μm, the control system determines that there is a spraying standing wave effect at that position. The control system calculates the standing wave wavelength λw based on the number of standing wave nodes and the distance between adjacent standing wave nodes, and generates a compensation spraying scheme with opposite phase and equal amplitude to the standing wave waveform. It controls the corresponding spray gun to increase the paint / powder output by ΔQc at the standing wave trough and decrease the paint / powder output by ΔQc at the standing wave peak. The formula for calculating ΔQc is as follows: Where Aw is the standing wave amplitude, in μm, A w It is determined by half the difference between the peaks and troughs of the measured film thickness distribution curve; λw is the distance between adjacent standing wave nodes, in mm, λw = 10-50 mm; x is the arc length coordinate along the direction of wheel rotation, in mm; φ is the initial phase angle, in rad, which is determined by the angle difference between the position of the first node of the standing wave and the initial spray point of the spray gun. k is the standing wave compensation gain coefficient, k = 0.5-1.5; γ is the curvature compensation coefficient, γ = 0.1-0.5; d²ε / dx² is the second spatial derivative of the film thickness deviation along the direction of wheel rotation, with units of μm / mm², and characterizes the curvature of the film thickness variation; v is the linear velocity of the wheel rotation, in mm / s; Δt is the spraying cycle, measured in seconds.
10. A wheel, characterized in that, The coating process for corrosion protection of recycled aluminum wheels as described in any one of claims 1-9 is used to prepare the wheels. The wheel surface is formed from the inside out in sequence as follows: a passivation film layer, a KSL anti-corrosion transparent primer layer, a base powder layer or a transparent powder layer, a color paint layer, and a transparent powder layer. The KSL anti-corrosion transparent primer layer has a film thickness of 20-25μm, the base powder layer or transparent powder layer has a film thickness of 100-120μm, the color paint layer has a film thickness of 15-25μm, and the transparent powder layer has a film thickness of 130-150μm.