A method for recovering and preparing a purified solution from iron phosphate slag

The stepwise purification process for preparing purified liquid from iron phosphate slag solves the problem of incomplete resource utilization of iron phosphate slag, and enables the preparation of high-purity ferrous oxalate and lithium dihydrogen phosphate, thereby improving product added value and resource utilization efficiency.

CN123128306APending Publication Date: 2026-11-20HUNAN LIHUITONG NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611457791.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing technologies for the resource utilization of ferric phosphate slag are incomplete, impurities are not fully removed, ferric iron reduction efficiency is low, and the process lacks systematicity, resulting in low added value and low purity of the product.

Method used

A stepwise purification process is adopted, which includes acid pickling to remove aluminum, acid leaching, resin to remove copper, oxidation precipitation to remove manganese, and iron powder reduction. By controlling the acid leaching conditions and using copper chelating resin, selective removal of impurities and efficient reduction of ferric iron are achieved, thus preparing a high-purity purified solution.

Benefits of technology

This method enables the efficient recovery and high-value utilization of iron and phosphorus resources in ferric phosphate slag, producing high-purity ferrous oxalate and lithium dihydrogen phosphate, thus broadening product channels and reducing reagent consumption and energy consumption.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The application discloses a method for recovering and preparing a purified solution from iron phosphate slag, and the method comprises the following steps: sequentially removing aluminum by dilute acid washing, acid leaching, removing copper by copper chelating resin, removing manganese by oxidation and precipitation, and reducing by iron powder, so as to obtain a purified solution containing ferrous ions and phosphate ions, and the purified solution can be used for preparing ferrous oxalate and lithium dihydrogen phosphate. The process realizes systematic and selective removal of impurities through step-by-step purification, and guarantees high purity of the purified solution. The acid leaching does not add a reducing agent, so that the iron exists in the form of trivalent iron, and the oxidant is not consumed in vain when manganese is oxidized and precipitated. The iron powder reduction simultaneously realizes efficient reduction of trivalent iron and serves as an iron source supplement, and the reagent consumption is reduced. The whole process is systematically integrated, efficient recovery of iron and phosphorus resources and high-quality preparation of the purified solution are realized, the high-value utilization level of the iron phosphate slag is improved, product channels are widened, and the problems of low product added value, incomplete impurity removal, low trivalent iron reduction efficiency and lack of systematicness in the prior art are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of battery material recycling technology, specifically relating to a method for recovering and preparing a purified liquid from iron phosphate slag. Background Technology

[0002] With the rapid development of the new energy vehicle industry, the market share of lithium iron phosphate batteries continues to grow. It is estimated that by 2030, the world will generate 2 million tons of retired lithium batteries annually. Retired lithium iron phosphate batteries contain valuable elements such as lithium, iron, phosphorus, aluminum, and copper, and have extremely high recycling and reuse value.

[0003] Currently, the recycling of retired lithium iron phosphate batteries mainly focuses on the selective leaching recovery of lithium, which has been industrialized. However, the iron phosphate slag remaining after lithium extraction (mainly composed of FePO4 and a small amount of impurities) has not yet been effectively utilized for resource recovery. Iron phosphate slag contains abundant iron and phosphorus resources; direct disposal not only wastes resources but also creates environmental pressure. Therefore, developing high-value recycling processes for iron phosphate slag is of significant resource and environmental importance.

[0004] In existing technologies, some solutions involve the recycling and treatment of iron phosphate slag or lithium iron phosphate waste. Solution one involves direct acid leaching-chemical precipitation of iron phosphate slag to recover iron phosphate. This method first mixes iron phosphate slag with water to form a slurry, then reacts it with acid. After solid-liquid separation, a leachate containing iron and phosphorus ions is obtained. This leachate is then purified by iron displacement to remove copper and resin removal to remove aluminum. The phosphorus-to-iron ratio is adjusted by adding phosphate, and the pH is adjusted by adding an oxidant and ammonia to obtain the iron phosphate precursor precipitate. This route is currently the mainstream technology for iron phosphate slag recycling, and the resulting iron phosphate can be used as a precursor for lithium iron phosphate cathode materials, demonstrating clear industrial application value. Solution two involves oxalic acid leaching-iron powder reduction of lithium iron phosphate waste. This method involves adding lithium iron phosphate powder to an oxalic acid solution, stirring to dissolve it, adjusting the pH, filtering, adding a reducing agent to the filtrate to reduce ferric iron to ferrous iron, and then obtaining ferrous oxalate through precipitation.

[0005] However, with the rapid expansion of iron phosphate production capacity, market supply has become relatively abundant, leading to increasingly fierce competition due to product homogeneity. The ferrous oxalate-lithium dihydrogen phosphate route, as another precursor solution for lithium iron phosphate materials, has different market positioning and application value in specific application scenarios. Furthermore, existing processes lack a systematic step-by-step design for removing impurities such as aluminum, copper, and manganese, especially paying insufficient attention to manganese removal; residual impurities directly affect the purity and quality of subsequent products. Moreover, the reduction of trivalent iron in existing technologies mostly relies on electrochemical methods or large amounts of reducing agents, resulting in high energy consumption and high costs. In addition, existing technologies are mostly optimizations of single stages, lacking a complete system design for the entire process from iron phosphate slag to the purification solution for the preparation of ferrous oxalate and lithium dihydrogen phosphate. Summary of the Invention

[0006] In view of the problems existing in the background art, this application provides a method for recovering and preparing purified liquid from ferric phosphate slag.

[0007] To achieve the above objectives, this application adopts the following technical solution: A method for recovering and preparing purified liquid from ferric phosphate slag is provided, comprising: The ferric phosphate slag was subjected to a first acid leaching reaction using a first acid solution. After solid-liquid separation, ferric phosphate slag cake and aluminum-containing pickling solution were obtained. The ferric phosphate slag cake was subjected to a second acid leaching using a second acid solution to obtain a leachate and a leaching residue; the temperature of the second acid leaching was 50~95℃. The leachate is adsorbed by an ion exchange column of copper chelating resin to obtain an adsorbed liquid. An oxidant was added to the adsorbed liquid, and the pH was adjusted to 0.8-1.85 to carry out a precipitation reaction. After solid-liquid separation, the precipitated liquid and the precipitate were obtained. Iron powder was added to the precipitate solution to carry out a reduction reaction, resulting in a purified solution containing ferrous ions and phosphate ions.

[0008] Compared with the prior art, one or more of the above technical solutions can achieve at least one of the following beneficial effects: (1) A method is provided for recovering iron and phosphorus resources from iron phosphate slag and preparing a purified liquid, which can be used to prepare ferrous oxalate and lithium dihydrogen phosphate, thereby realizing the high-value utilization of iron phosphate slag and broadening product channels.

[0009] (2) Through the stepwise purification process of “aluminum removal by pickling → copper removal by acid leaching → copper removal by resin → manganese removal by oxidation precipitation → iron powder reduction”, the impurities are systematically and selectively removed, ensuring the high purity of the purification solution, which is conducive to the preparation of high-value-added high-purity products, and the Fe and P losses are low during the purification process; no reducing agent is added during acid leaching, so that iron exists in the trivalent form, avoiding the ineffective consumption of oxidant during manganese precipitation; solving the problems of low added value of existing products, incomplete removal of impurities, low reduction efficiency of trivalent iron and lack of systematic process in the existing technology.

[0010] (3) Through the iron powder reduction process, the efficient reduction of ferric iron is achieved simultaneously in the acidic leaching system. Iron powder is used as both a reducing agent and an iron source supplement, thereby reducing reagent consumption.

[0011] (4) Through the system integration of the whole process, the efficient recovery of valuable elements in ferric phosphate slag and the high-quality preparation of purified liquid are achieved. Detailed Implementation

[0012] To address the shortcomings of the existing technologies, this invention provides a method for the high-value recycling and utilization of ferric phosphate slag. This method aims to solve the problems of low product added value, incomplete impurity removal, low reduction efficiency of ferric iron, and lack of systematic process in the existing technologies. It achieves efficient recovery and high-value utilization of iron and phosphorus resources in ferric phosphate slag, and obtains a purified solution for the preparation of high-purity ferrous oxalate and lithium dihydrogen phosphate.

[0013] This invention provides a method for recovering and preparing purified liquid from ferric phosphate slag, the process flow of which is as follows: Ferric phosphate slag → Acid washing to remove aluminum → Solid-liquid separation → Ferric phosphate slag (after aluminum removal) → Acid leaching → Solid-liquid separation → Iron-phosphorus leaching solution → Resin to remove copper → Oxidation precipitation to remove manganese → Iron powder reduction → Purified solution (containing Fe) 2+ and PO4 3- The purified solution can be used to prepare high-purity ferrous oxalate and high-purity lithium dihydrogen phosphate, respectively.

[0014] A typical implementation provides a method for recovering and preparing purified liquid from ferric phosphate slag, comprising: (1) Aluminum removal by ferric phosphate washing: The ferric phosphate slag was subjected to a first acid leaching reaction using a first acid solution. After solid-liquid separation, ferric phosphate slag cake and aluminum-containing pickling solution were obtained. Aluminum in ferric phosphate slag exists in the form of alumina or metallic aluminum, and dissolves into the solution under acidic conditions. Al2O3+ 3H2SO4→ Al2(SO4)3+ 3H2O Ferric phosphate (FePO4) has low solubility in sulfuric acid. By controlling the pickling conditions (lower acid concentration, appropriate temperature and time), aluminum can be selectively dissolved while ferric phosphate remains in the solid phase. The aluminum-containing pickling solution enters the wastewater treatment system, and after neutralization and precipitation, it is discharged in compliance with standards or reused.

[0015] (2) Acid leaching of ferric phosphate slag: The ferric phosphate slag cake was subjected to a second acid leaching using a second acid solution to obtain a leachate and a leaching residue; the temperature of the second acid leaching was 50~95℃. Ferric phosphate dissolves under acidic conditions: 2FePO4+ 3H2SO4→ Fe2(SO4)3+ 2H3PO4 The aluminum-removed ferric phosphate slag is mixed with sulfuric acid solution and subjected to direct acid leaching under stirring. Unlike existing reduction leaching processes, this step does not add iron powder or other reducing agents. The leaching rate is ensured by increasing the sulfuric acid concentration, raising the leaching temperature, and extending the leaching time. After the reaction, solid-liquid separation is performed to obtain Fe-containing... 3+ and PO4 3- Leachate and leaching residue.

[0016] In this step, iron exists in the leachate as ferric ions. Studies have shown that under optimized conditions, the leaching rates of both iron and phosphorus can reach over 97%. By increasing the acid concentration and temperature, the redeposition of FePO4·2H2O can be effectively suppressed, ensuring a high leaching rate.

[0017] (3) Copper removal with resin: The leachate is adsorbed by an ion exchange column of copper chelating resin to obtain an adsorbed liquid. The Fe-containing material obtained in step (2) 3+ and PO4 3- The leachate is pumped into an ion exchange column packed with copper chelating resin, where copper is removed by adsorption under specific pH and flow rate conditions. The saturated resin is then regenerated by desorption with sulfuric acid solution, allowing for recycling. The copper chelating resin binds to Cu through its functional groups. 2+ Chelating chemisorption occurs, achieving selective separation. This resin exhibits high selectivity for copper ions, with a copper removal efficiency of up to 99% and residual copper content reduced to below 1 mg / L.

[0018] (4) Oxidation precipitation to remove manganese: An oxidant is added to the adsorbed liquid, and the pH value is adjusted to 0.8~1.85, for example, 0.8, 1, 1.2, 1.5, 1.6, 1.8, etc., to carry out a precipitation reaction. After solid-liquid separation, the precipitated liquid and precipitate are obtained. The copper-removed solution (containing Fe) 3+ and PO4 3- It contains virtually no Fe. 2+ Adjust to a suitable pH value, add a strong oxidizing agent, and remove Mn from the solution. 2+ It is oxidized to a higher oxidation state and precipitates as manganese dioxide under weakly acidic conditions. Since iron exists in the solution in its trivalent form, the oxidant is not consumed by the Fe... 2+ →Fe 3+ The oxidation reaction is carried out, thus significantly reducing the amount of oxidant used. After the reaction, solid-liquid separation is performed to obtain a purified liquid after manganese removal and a precipitate containing manganese dioxide.

[0019] Sodium persulfate decomposes in solution to produce highly oxidizing sulfate radicals (SO4· ... - ) and hydroxyl radicals (·OH), which will cause Mn 2+ Oxidation to a higher oxidation state: S2O8 2- + 2e - → 2SO4 2- Mn 2+ → Mn 4+ (After oxidation, it precipitates as MnO2) The leachate from existing reduction leaching processes contains a large amount of Fe. 2+ In the oxidation precipitation process, sodium persulfate will preferentially remove Fe. 2+ Oxidized to Fe 3+ (Fe) 2+ →Fe 3+ + e - This method consumes a large amount of oxidizing agent. However, this invention uses direct acid leaching (without a reducing agent), and the iron in the leachate is in the form of Fe. 3+ It exists in a form that does not consume oxidizing agents; the oxidizing agent is only used for Mn. 2+ Oxidation precipitation.

[0020] (5) Iron powder reduction: Iron powder was added to the precipitate solution to carry out a reduction reaction, resulting in a purified solution containing ferrous ions and phosphate ions.

[0021] The manganese-removed solution (containing Fe) 3+ and PO4 3- The mixture was transferred to a reduction reactor, and iron powder was added to initiate the reduction reaction. After the reaction was complete, solid-liquid separation was performed to obtain a product containing Fe. 2+ and PO4 3- The purified liquid and a small amount of unreacted iron powder (can be recycled).

[0022] Iron powder reduces ferric iron in the solution to ferrous iron: Fe + Fe2(SO4)3 → 3FeSO4 Fe produced by the reaction 2+ With PO4 in solution 3- It coexists in the purification solution, which can be used for the subsequent preparation of ferrous oxalate (precipitated with oxalic acid) and lithium dihydrogen phosphate (after further processing).

[0023] In some preferred embodiments, in step (1), the hydrogen ion concentration of the first acid solution is 0.1~1 mol / L, for example, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1 mol / L, etc.; the first acid solution is a sulfuric acid solution. It should be noted that the provided embodiment uses a sulfuric acid solution as the first acid solution, and its hydrogen ion concentration is calculated based on 2 mol / L of sulfuric acid per 1 mol / L.

[0024] In some preferred embodiments, in step (1), the temperature of the first acid leaching is 30~80℃, for example 30℃, 40℃, 50℃, 60℃, 70℃, 80℃, etc.

[0025] In a partially preferred embodiment, in step (1), the solid-liquid ratio of the first acid leaching is 1t:(1.5~6)m 3 For example, 1t:1.5m 3 1t:2m 3 1t:2.5m 3 1t:3m 3 1t:3.5m 3 1t:4m 3 1t:4.5m 3 1t:5m 3 1t:5.5m 3 1t:6m 3 wait.

[0026] In some preferred embodiments, in step (1), the first acid leaching time is 30~120min, for example 30min, 45min, 60min, 75min, 90min, 105min, 120min, etc.

[0027] In some preferred embodiments, in step (1), the first acid leaching is carried out under stirring conditions; the stirring speed is 100~500 rpm, for example 100 rpm, 200 rpm, 300 rpm, 400 rpm, 500 rpm, etc.

[0028] In some preferred embodiments, in step (2), the hydrogen ion concentration of the second acid solution is 2~7 mol / L, for example, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, 5 mol / L, 5.5 mol / L, 6 mol / L, 6.5 mol / L, 7 mol / L, etc.; the second acid solution is a sulfuric acid solution. It should be noted that the provided embodiment uses a sulfuric acid solution as the first acid solution, and its hydrogen ion concentration is calculated based on 2 mol / L of sulfuric acid per 1 mol / L.

[0029] In some preferred embodiments, in step (2), the temperature of the second acid leaching is 50~90℃, for example 50℃, 60℃, 70℃, 80℃, 90℃, etc.

[0030] In a partially preferred embodiment, in step (2), the solid-liquid ratio of the second acid leaching is 1t:(2~5.5)m. 3 For example, 1t:2m 3 1t:2.5m 3 1t:3m 3 1t:3.5m 3 1t:4m 3 1t:4.5m 31t:5m 3 1t:5.5m 3 wait.

[0031] In some preferred embodiments, in step (2), the second acid leaching time is 60~180 min, for example 60 min, 75 min, 90 min, 105 min, 120 min, 135 min, 150 min, 165 min, 180 min, etc., preferably 90~150 min.

[0032] In some preferred embodiments, in step (2), the second acid leaching is carried out under stirring conditions; the stirring speed is 100~500 rpm, for example 100 rpm, 200 rpm, 300 rpm, 400 rpm, 500 rpm, etc.

[0033] In some preferred embodiments, in step (3), the copper chelating resin is a copper chelating resin containing any one of the functional groups of pyridine nitrogen, carboxyl and hydroxyl.

[0034] In some preferred embodiments, in step (3), the pH value of the adsorption is 0.6~1.0, for example 0.6, 0.7, 0.8, 0.9, 1.0, etc.

[0035] In some preferred embodiments, in step (3), the flow rate of the leachate is 1~10 BV / h (resin bed volume / hour).

[0036] In some embodiments, in step (3), the desorbent is a 1~5 mol / L sulfuric acid solution, such as 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, etc.

[0037] In some preferred embodiments, in step (3), the adsorption temperature is 25~50℃, for example 25℃, 30℃, 40℃, 50℃, etc.

[0038] In some preferred embodiments, in step (3), the ion exchange column of the copper chelating resin after adsorption is eluted with sulfuric acid solution to obtain a copper-containing solution.

[0039] In some preferred embodiments, in step (4), the temperature of the precipitation reaction is 60~95℃, for example 60℃, 70℃, 80℃, 90℃, 95℃, etc., preferably 80~90℃.

[0040] In some preferred embodiments, in step (4), the precipitation reaction time is 30~120 min, for example 30 min, 45 min, 60 min, 75 min, 90 min, 105 min, 120 min, etc.

[0041] In some preferred embodiments, in step (4), the precipitation is carried out under stirring conditions; the stirring speed is 100~500 rpm.

[0042] In some preferred embodiments, in step (4), the oxidant is sodium persulfate.

[0043] In some preferred embodiments, in step (4), the amount of oxidant used is the amount of Mn in the solution. 2+ The amount of oxidant used is 1.2 to 3 times that of the molar number, for example, 1.2 times, 1.5 times, 1.8 times, 2 times, 2.2 times, 2.5 times, 2.8 times, and 3 times, which reduces the amount of oxidant used by 30 to 50% compared to the reduction leaching process.

[0044] In some preferred embodiments, in step (5), the amount of iron powder added is 0.3 to 0.6 times the molar amount of ferric ions in the solution, for example, 0.3 times, 0.4 times, 0.5 times, 0.6 times, etc.

[0045] In some preferred embodiments, in step (5), the particle size of the iron powder is 100~400 mesh, such as 100 mesh, 125 mesh, 200 mesh, 300 mesh, 400 mesh, etc.

[0046] In some preferred embodiments, in step (5), the temperature of the reduction reaction is 20~60℃, for example 20℃, 30℃, 40℃, 50℃, 60℃, etc.

[0047] In some preferred embodiments, in step (5), the reduction reaction time is 30~120 min, for example 30 min, 45 min, 60 min, 75 min, 90 min, 105 min, 120 min, etc.

[0048] In some preferred embodiments, in step (5), the reduction reaction is carried out under stirring conditions; the stirring speed is 100~500 rpm.

[0049] Reaction endpoint determination: Fe in solution 3+ The concentration dropped to below 10 mg / L.

[0050] The purified liquid prepared by this invention (containing Fe) 2+ and PO4 3- It can be used for: (1) Preparation of ferrous oxalate: Oxalic acid (H2C2O4) is added to the purified solution, and the pH is controlled at 2.0~4.0 to induce a precipitation reaction: Fe 2+ + C2O4 2- + 2H2O → FeC2O4·2H2O↓ The ferrous oxalate product is obtained after filtration, washing, and drying.

[0051] (2) Preparation of lithium dihydrogen phosphate: After removing residual iron and oxalate by adding quicklime to the purified liquid, it is mixed with an external lithium source (such as lithium carbonate or lithium hydroxide), and the lithium dihydrogen phosphate product is obtained by reaction, crystallization, separation and drying.

[0052] To facilitate understanding of this application, the following description will be provided in more detail with reference to the embodiments, but the scope of protection of this application is not limited to the following specific embodiments.

[0053] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of this application.

[0054] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this application are available on the market or can be prepared by existing methods.

[0055] Example 1 Methods for recovering and preparing purified liquid from ferric phosphate slag include: (1) Under stirring conditions, use a 0.2 mol / L sulfuric acid solution (each 1 mol of H2SO4 is used at a concentration of 2 mol of H2SO4). + (Calculation) The ferric phosphate slag was subjected to an acid leaching reaction with a solid-liquid ratio of 1t:5m. 3 The reaction temperature was 60℃, the reaction time was 120 min, and the stirring speed was 300 rpm. After the reaction, solid-liquid separation was performed to obtain iron phosphate slag filter cake after aluminum removal and aluminum-containing pickling solution. The leaching rates of Fe and P were approximately 1.0% and 0.8%, respectively. The aluminum-containing pickling solution entered the wastewater treatment system, and after neutralization and precipitation, it was discharged in compliance with standards or reused.

[0056] (2) The aluminum-removed iron phosphate slag filter cake was mixed with sulfuric acid solution and subjected to direct acid leaching under stirring conditions to obtain iron-phosphorus leachate; the concentration of sulfuric acid solution was 2 mol / L, and the solid-liquid ratio of acid leaching was 1t:4.5m. 3 The acid leaching temperature was 75℃, the acid leaching time was 120 min, and the stirring speed was 300 rpm; according to the test and calculation, the leaching rates of iron and phosphorus were 95% and 98%, respectively. (3) Take the Fe-containing sample obtained in step (2) 3+ and PO4 3-The leachate was pumped into an ion exchange column (bispyridineamine type) packed with copper chelating resin. The pH of the leachate was adjusted to 0.8, and copper removal was performed at a flow rate of 1 BV / h. After adsorption saturation, the resin was regenerated by desorption with a 3 mol / L sulfuric acid solution. The copper in the desorbate (copper-rich) was recovered separately, and the resin was recycled. The adsorption and desorption temperature was 25℃. The residual copper content in the post-adsorption solution was 2 ppm. The calculated copper ion removal rate was 98%. (4) Adjust the pH of the adsorbed solution to 1.5±0.1, add sodium persulfate, and stir at 80℃ for 120 min at a stirring speed of 300 rpm; the amount of sodium persulfate added is twice the molar amount of manganese ions in the adsorbed solution; after the reaction, perform solid-liquid separation to obtain a manganese-removed solution and a precipitate. The manganese ion concentration in the manganese-removed solution is 5 ppm. The removal rate of Mn in this step is about 98%, and the loss of Fe and P into the precipitate is small. According to the test and calculation, the loss of Fe is 0.5% and the loss of P is 0.5%. (5) Add 0.5 times the molar amount of ferric ions (Cu < 20 ppm, Mn < 50 ppm) of iron powder with a particle size of 200 mesh to the manganese removal solution in a closed container (non-open container). Stir the reaction at 45°C to obtain a purified solution. The stirring speed is 300 rpm. After reacting for 60 min, take a sample to determine the Fe content. 3+ If residual Fe 3+ If the concentration is >50 mg / L, add iron powder until the total amount does not exceed 0.6 times the original amount. The total reaction time is 120 min, and the endpoint is controlled by Fe. 3+ ≤15mg / L. Immediately after the reaction, filter to remove unreacted iron powder. Store the filtrate in an oxygen-free environment and analyze as soon as possible. Analysis results show that Fe in the purified solution... 3+ The concentration is 15 mg / L.

[0057] The desorption solution (copper-rich solution) obtained in step (3) is first diluted or neutralized to an acidity of ≤0.5mol / L, iron powder is added, and after reaction, it is filtered to obtain sponge copper and reaction solution. The reaction solution is returned to step (2) for use.

[0058] Example 2 The only difference between this embodiment and Example 1 is that the concentration of the sulfuric acid solution in step (1) is 0.5 mol / L, and the leaching rates of Fe and P are approximately 4.1% and 3.3%, respectively.

[0059] Example 3 The only difference between this embodiment and Example 1 is that the concentration of sulfuric acid solution in step (2) is 1.2 mol / L. According to the test and calculation, the leaching rates of iron and phosphorus are 86.3% and 87.2%, respectively.

[0060] Example 4 The only difference between this embodiment and Example 1 is that the concentration of the sulfuric acid solution in step (2) is 3 mol / L. According to the test and calculation, the leaching rates of iron and phosphorus are 99% and 99.5%, respectively.

[0061] Example 5 The only difference between this embodiment and embodiment 1 is that the acid leaching temperature in step (2) is 50°C. According to the test and calculation, the leaching rates of iron and phosphorus are 83.5% and 84.1%, respectively.

[0062] Example 6 The only difference between this embodiment and embodiment 1 is that the acid leaching temperature in step (2) is 90°C. According to the test and calculation, the leaching rates of iron and phosphorus are 97% and 99%, respectively.

[0063] Example 7 The only difference between this embodiment and embodiment 1 is that in step (4), the pH value of the adsorbed liquid is adjusted to 0.8, the manganese ion concentration in the manganese removal solution is 10.5 ppm, the removal rate of Mn in this step is about 95.5%, and the loss of Fe and P into the precipitate is small. According to the test calculation, the loss of Fe is 0.3% and the loss of P is 0.3%.

[0064] Example 8 The only difference between this embodiment and Example 1 is that in step (4), the pH value of the adsorbed liquid is adjusted to 1.75~1.85, the manganese ion concentration in the manganese removal solution is 1ppm, the removal rate of Mn in this step is about 99.5%, the loss of Fe and P into the precipitate is increased but still within an acceptable range, and the Fe loss is calculated to be 2.8% and the P loss is 1.9%.

[0065] Comparative Example 1 The difference between this comparative example and Example 1 is that steps (3) and (4) are reversed in order, specifically: (3) Take the Fe-containing sample obtained in step (2) 3+ and PO4 3- The pH of the leachate was adjusted to 1.0, sodium persulfate was added, and the mixture was stirred at 80°C for 120 min at a stirring speed of 300 rpm. The amount of sodium persulfate added was twice the molar amount of manganese ions in the leachate. After the reaction, solid-liquid separation was performed to obtain a manganese-removed solution and a precipitate. The manganese ion concentration in the manganese-removed solution was 9 ppm. The removal rate of Mn in this step was approximately 96%, and the loss of Fe and P into the precipitate was minimal. Calculations showed that the Fe loss was 0.49% and the P loss was 0.45%. (4) The manganese removal solution from step (3) was pumped into an ion exchange column packed with copper chelating resin for adsorption and copper removal at a pH of 0.8 and a flow rate of 1 BV / h. The resin after adsorption saturation was desorbed and regenerated with 4 mol / L sulfuric acid solution for recycling; the adsorption and desorption temperature was 25℃; the residual copper content in the adsorption solution was 6 ppm; and the copper ion removal rate was calculated to be 94%.

[0066] Comparative Example 2 The difference between this comparative example and Example 1 is that the concentration of sulfuric acid solution in step (1) is 0.04 mol / L, the leaching rate of Al is 67.8%, and the leaching rates of Fe and P are approximately 0.2% and 0.1%, respectively. The Al content in the purified solution obtained in step (5) is as high as 100 ppm, which is significantly excessive.

[0067] Comparative Example 3 The difference between this comparative example and Example 1 is that the concentration of sulfuric acid solution in step (1) is 0.6 mol / L, the leaching rate of Al is 99%, and the leaching rates of Fe and P are approximately 6% and 5%, respectively.

[0068] Comparative Example 4 The difference between this comparative example and Example 1 is that the hydrogen ion concentration of the sulfuric acid solution in step (2) is 1.5 mol / L (each 1 mol of H2SO4 is used as 2 mol of H+). + According to calculations, the leaching rates of iron and phosphorus were 78.5% and 79.6%, respectively.

[0069] Comparative Example 5 The difference between this comparative example and Example 1 is that the acid leaching temperature in step (2) is 30°C. According to the test and calculation, the leaching rates of iron and phosphorus are 74.9% and 81.2%, respectively.

[0070] Comparative Example 6 The difference between this comparative example and Example 1 is that in step (4), the pH value of the adsorbed liquid is adjusted to 2.5, the manganese ion concentration in the manganese removal solution is 1 ppm, the removal rate of Mn in this step is about 99.5%, and the loss of Fe and P into the precipitate is large. According to the test calculation, the loss of Fe is 19% and the loss of P is 17%.

[0071] The above description is only a preferred embodiment of this application. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of this application, and these improvements and modifications should also be considered within the scope of protection of this application.

Claims

1. A method for recovering and preparing purified liquid from ferric phosphate slag, characterized in that, include: The ferric phosphate slag was subjected to a first acid leaching reaction using a first acid solution. After solid-liquid separation, ferric phosphate slag cake and aluminum-containing pickling solution were obtained. The ferric phosphate slag cake was subjected to a second acid leaching using a second acid solution to obtain a leachate and a leaching residue; the temperature of the second acid leaching was 50~95℃. The leachate is adsorbed by an ion exchange column of copper chelating resin to obtain an adsorbed liquid. An oxidant was added to the adsorbed liquid, and the pH was adjusted to 0.8-1.85 to carry out a precipitation reaction. After solid-liquid separation, the precipitated liquid and the precipitate were obtained. Iron powder was added to the precipitate solution to carry out a reduction reaction, resulting in a purified solution containing ferrous ions and phosphate ions.

2. The method for preparing purified liquid from ferric phosphate slag as described in claim 1, characterized in that, The hydrogen ion concentration of the first acid solution is 0.1~1 mol / L; the first acid solution is a sulfuric acid solution.

3. The method for preparing purified liquid from ferric phosphate slag as described in claim 1, characterized in that, The temperature of the first acid leaching is 30~80℃; The solid-liquid ratio of the first acid leaching is 1t:(1.5~6)m 3 ; The first acid leaching time is 30~120 min; The first acid leaching is carried out under stirring conditions; the stirring speed is 100~500 rpm.

4. The method for preparing purified liquid from ferric phosphate slag as described in claim 1, characterized in that, The hydrogen ion concentration of the second acid solution is 2~7 mol / L; the second acid solution is a sulfuric acid solution.

5. The method for preparing purified liquid from ferric phosphate slag as described in claim 1, characterized in that, The temperature of the second acid leaching is 50~95℃; The solid-liquid ratio of the second acid leaching is 1t:(2~5.5)m 3 ; The second acid leaching time is 60~180min, preferably 90~150min; The second acid leaching is carried out under stirring conditions; the stirring speed is 100~500 rpm.

6. The method for preparing purified liquid from ferric phosphate slag as described in claim 1, characterized in that, The copper chelating resin is a copper chelating resin containing any one of the functional groups of pyridine nitrogen, carboxyl and hydroxyl groups; The pH value for adsorption is 0.6~1.0; The flow rate of the leachate is 1~10 BV / h; The adsorption temperature is 25~50℃; The copper chelating resin ion exchange column after adsorption was eluted with sulfuric acid solution to obtain a copper-containing solution.

7. The method for preparing purified liquid from ferric phosphate slag as described in claim 1, characterized in that, The precipitation reaction is carried out at a temperature of 60-95℃, preferably 80-90℃. The precipitation reaction time is 30~120 min; The precipitation is carried out under stirring conditions; the stirring speed is 100~500 rpm; The oxidant is sodium persulfate; The amount of oxidant used is 1.2 to 3 times the number of moles of manganese ions in the solution.

8. The method for preparing purified liquid from ferric phosphate slag as described in claim 1, characterized in that, The amount of iron powder added is 0.3 to 0.6 times the molar amount of ferric ions in the solution; The iron powder has a particle size of 100-400 mesh; The temperature of the reduction reaction is 20~60℃; The reduction reaction takes 30-120 minutes; The reduction reaction is carried out under stirring conditions; the stirring speed is 100~500 rpm.